High-temperature-resistant carbon fiber composite material and preparation method thereof

By combining modified carbon fibers and modified resins with ore powder and alloy powder, a high-temperature sintered body is formed, which solves the problem of insufficient high temperature and corrosion resistance of existing carbon fiber composite materials, and achieves high thermal conductivity and high temperature and high Impact strength carbon fiber composite material.

CN119020705APending Publication Date: 2024-11-26SUZHOU LIGHTWEIGHT INTELLIGENT MFG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123818.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing carbon fiber composites still have room for improvement in their high temperature and corrosion resistance, especially the thermal conductivity and impact strength are not sufficient to meet the needs of certain high temperature applications.

Method used

Modified carbon fibers and modified resins are used to combine with ore powder and alloy powder after activation treatment and drying, and then sintered to form a high-temperature-resistant carbon fiber composite material, improving its thermal conductivity and impact strength. Specific steps include activating carbon fibers, preparing modified resins, mixing powders and sintering at high temperatures.

Benefits of technology

A carbon fiber composite material with a thermal conductivity of 14.08W/m·K and an impact strength of 56.3KJ/m2 has good high temperature and corrosion resistance, and effectively avoids heat accumulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995806270000111
    Figure BDA0004995806270000111
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant carbon fiber composite material, which belongs to the technical field of carbon fiber composite materials and comprises modified carbon fibers, modified fibers and a modified resin layer. A preparation method of the modified resin comprises the following steps: A, preheating 100 parts of acrylic resin to 50 DEG C; b, 11-18 parts of tris (4-nonylphenyl) phosphite ester is added into acrylic resin, and then the mixture is heated to 108 DEG C; c, dividing 5-7 parts of mineral powder into five equal parts, adding the five parts of mineral powder into the acrylic resin in five times, raising the temperature to 1 DEG C each time, stirring, and naturally cooling to obtain modified resin; and grinding the modified resin into modified resin powder. The heat conductivity coefficient of the prepared high-temperature-resistant carbon fiber composite material is 14.08 W / m.K, the impact strength is 56.3 KJ / m < 2 >, and the high-temperature-resistant carbon fiber composite material has the advantages of high temperature resistance, high impact strength, corrosion resistance and the like, is good in heat conductivity and can effectively avoid heat accumulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber composite materials, and in particular to a high temperature resistant carbon fiber composite material and a preparation method thereof. Background Art

[0002] In recent years, carbon fiber composite materials have been sought after for their excellent performance.

[0003] For example, Chinese patent CN113881228B proposes a high thermal conductivity carbon fiber composite material and its preparation method. Carbon fiber is used as the main building unit of the highly oriented heat transport network, and graphene oxide with self-assembly characteristics and similar lattice structure to carbon fiber is used as a bridging agent. A self-supporting network structure of carbon fiber and graphene oxide three-dimensionally interconnected and highly oriented in a specific direction is constructed by ice template method or hydrothermal reduction assembly, and a composite material with high thermal conductivity is prepared after compounding with a polymer matrix. The highly oriented carbon fiber self-supporting structure uses graphene oxide as a bridging agent, without the wrapping of traditional polymer binders. The carbon fibers are effectively connected to each other through graphene oxide, and together constitute a synergistically oriented three-dimensional thermally conductive enhanced network structure, which significantly improves the thermal conductivity of the composite material at a low filling amount.

[0004] Although the above patent improves thermal conductivity, high temperature resistance and corrosion resistance still need to be improved.

[0005] Based on this, the present invention designs a high temperature resistant carbon fiber composite material and a preparation method thereof to solve the above problems. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high temperature resistant carbon fiber composite material and a preparation method thereof.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A high temperature resistant carbon fiber composite material, comprising modified carbon fiber, modified fiber and modified resin layer;

[0009] The modified resin preparation method is as follows:

[0010] A. Preheat 100 parts of acrylic resin to 50°C;

[0011] B. Add 11-18 parts of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0012] C. Divide 5-7 parts of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0013] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 0.7-1.5:1.

[0014] Furthermore, the modified carbon fiber preparation method is as follows:

[0015] A. Activate 50-80 parts of carbon fiber by 150-200 parts of calcium carbonate solution;

[0016] B. adding 90-110 parts of olefin monomer to the activated carbon fiber and mixing and stirring to obtain a mixed solution A;

[0017] C. Dry the mixed solution A to obtain modified carbon fiber.

[0018] A method for preparing a high temperature resistant carbon fiber composite material;

[0019] Step 1: preparing modified carbon fiber;

[0020] A. Activate 50-80 parts of carbon fiber by 150-200 parts of calcium carbonate solution;

[0021] B. adding 90-110 parts of olefin monomer to the activated carbon fiber and mixing and stirring to obtain a mixed solution A;

[0022] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0023] Step 2: Preparation of modified resin:

[0024] A. Preheat 100 parts of acrylic resin to 50°C;

[0025] B. Add 11-18 parts of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0026] C. Divide 5-7 parts of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0027] The ore is a mixture of pyrophyllite and chabazite;

[0028] Step 3: preparing carbon fiber-alloy powder;

[0029] A. Mix 80-92 parts of nickel aluminum alloy powder, 72-78 parts of silicon nitride powder and 1 / 3-1 / 2 of modified carbon fiber, and obtain a mixed powder by ball milling;

[0030] B. Adding a binder to the mixed powder, stirring evenly and drying, and sintering in a sintering furnace under argon protection to obtain a sintered body;

[0031] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0032] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0033] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for pressing and sintering at a high temperature of 1950-2000°C to obtain the high temperature resistant carbon fiber composite material.

[0034] Furthermore, in step 1, the stirring time is 1-2h.

[0035] Furthermore, in step 2, the particle size of the ore powder is 200 mesh.

[0036] Furthermore, in step three, the sintering temperature is between 1950°C and 2000°C.

[0037] Furthermore, in step three, the adhesive is a cyanoacrylate droplet-free adhesive.

[0038] Furthermore, in step 2, the ratio of pyrophyllite to chabazite is 0.7-1.5:1.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The high temperature resistant carbon fiber composite material prepared by the present invention has a thermal conductivity of 14.08W / m·K and an impact strength of 56.3KJ / m 2 It has the advantages of high temperature resistance, high impact strength, corrosion resistance, and good thermal conductivity, which can effectively avoid heat accumulation. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Embodiment 1

[0043] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0044] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0045] Step 2: preparing modified carbon fiber;

[0046] A. 80 kg of carbon fiber is activated by 200 kg of calcium carbonate solution;

[0047] B. Add 110 kg of olefin monomer to the activated carbon fiber and stir for 2 h to obtain a mixed solution A;

[0048] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0049] Step 3: Preparation of modified resin:

[0050] A. Preheat 100kg acrylic resin to 50℃;

[0051] B. Add 18 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0052] C. Divide 7 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0053] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 1.5:1;

[0054] The particle size of the ore powder is 200 mesh;

[0055] Step 3: preparing carbon fiber-alloy powder;

[0056] A. Mix 92 kg of nickel-aluminum alloy powder, 78 kg of silicon nitride powder and 1 / 2 of modified carbon fiber, and obtain a mixed powder by ball milling;

[0057] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 2000° C. in a sintering furnace under argon protection to obtain a sintered body;

[0058] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0059] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0060] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 2000° C. to obtain the high temperature resistant carbon fiber composite material.

[0061] Embodiment 2

[0062] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0063] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0064] Step 2: preparing modified carbon fiber;

[0065] A. 50 kg of carbon fiber is activated by 150 kg of calcium carbonate solution;

[0066] B. Add 90 kg of olefin monomer to the activated carbon fiber and stir for 1 hour to obtain a mixed solution A;

[0067] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0068] Step 3: Preparation of modified resin:

[0069] A. Preheat 100kg acrylic resin to 50℃;

[0070] B. Add 11 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0071] C. Divide 5 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0072] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 0.7:1;

[0073] The particle size of the ore powder is 200 mesh;

[0074] Step 3: preparing carbon fiber-alloy powder;

[0075] A. 80 kg of nickel-aluminum alloy powder, 72 kg of silicon nitride powder and 1 / 3 of modified carbon fiber were mixed and ball-milled to obtain a mixed powder;

[0076] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 1950° C. in a sintering furnace under argon protection to obtain a sintered body;

[0077] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0078] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0079] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 1950° C. to obtain the high temperature resistant carbon fiber composite material.

[0080] Embodiment 3

[0081] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0082] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0083] Step 2: preparing modified carbon fiber;

[0084] A. 70 kg of carbon fiber was activated by 160 kg of calcium carbonate solution;

[0085] B. Add 102 kg of olefin monomer to the activated carbon fiber and stir for 1.5 h to obtain a mixed solution A;

[0086] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0087] Step 3: Preparation of modified resin:

[0088] A. Preheat 100kg acrylic resin to 50℃;

[0089] B. Add 16 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0090] C. Divide 6 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0091] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 1.1:1;

[0092] The particle size of the ore powder is 200 mesh;

[0093] Step 3: preparing carbon fiber-alloy powder;

[0094] A. Mix 90 kg of nickel-aluminum alloy powder, 75 kg of silicon nitride powder and 5 / 12 of modified carbon fiber, and obtain a mixed powder by ball milling;

[0095] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 1980° C. in a sintering furnace under argon protection to obtain a sintered body;

[0096] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0097] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0098] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 1980° C. to obtain the high temperature resistant carbon fiber composite material.

[0099] Embodiment 4

[0100] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0101] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0102] Step 2: preparing modified carbon fiber;

[0103] A. 65 kg of carbon fiber was activated by 163 kg of calcium carbonate solution;

[0104] B. Add 98 kg of olefin monomer to the activated carbon fiber and stir for 1.5 h to obtain a mixed solution A;

[0105] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0106] Step 3: Preparation of modified resin:

[0107] A. Preheat 100kg acrylic resin to 50℃;

[0108] B. Add 12 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0109] C. Divide 6.2 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0110] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 0.9:1;

[0111] The particle size of the ore powder is 200 mesh;

[0112] Step 3: preparing carbon fiber-alloy powder;

[0113] A. Mix 91 kg of nickel-aluminum alloy powder, 77 kg of silicon nitride powder and 5 / 12 of modified carbon fiber, and obtain a mixed powder by ball milling;

[0114] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 1980° C. in a sintering furnace under argon protection to obtain a sintered body;

[0115] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0116] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0117] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 1980° C. to obtain the high temperature resistant carbon fiber composite material.

[0118] Embodiment 5

[0119] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0120] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0121] Step 2: preparing modified carbon fiber;

[0122] A. 76 kg of carbon fiber was activated by 169 kg of calcium carbonate solution;

[0123] B. Add 91 kg of olefin monomer to the activated carbon fiber and stir for 1.5 h to obtain a mixed solution A;

[0124] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0125] Step 3: Preparation of modified resin:

[0126] A. Preheat 100kg acrylic resin to 50℃;

[0127] B. Add 12 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0128] C. Divide 5.8 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0129] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 1.3:1;

[0130] The particle size of the ore powder is 200 mesh;

[0131] Step 3: preparing carbon fiber-alloy powder;

[0132] A. 88 kg of nickel-aluminum alloy powder, 75 kg of silicon nitride powder and 5 / 12 of modified carbon fiber were mixed and ball-milled to obtain a mixed powder;

[0133] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 1980° C. in a sintering furnace under argon protection to obtain a sintered body;

[0134] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0135] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0136] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 1980° C. to obtain the high temperature resistant carbon fiber composite material.

[0137] Embodiment 6

[0138] This embodiment provides a high temperature resistant carbon fiber composite material, comprising the following steps:

[0139] Step 1: weigh the raw materials: carbon fiber, acrylic resin, tris(4-nonylphenyl)phosphite, pyrophyllite, chabazite, nickel-aluminum alloy powder, and silicon nitride powder;

[0140] Step 2: preparing modified carbon fiber;

[0141] A. 57 kg of carbon fiber was activated by 188 kg of calcium carbonate solution;

[0142] B. Add 105 kg of olefin monomer to the activated carbon fiber and stir for 1.5 h to obtain a mixed solution A;

[0143] C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use;

[0144] Step 3: Preparation of modified resin:

[0145] A. Preheat 100kg acrylic resin to 50℃;

[0146] B. Add 13 kg of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C;

[0147] C. Divide 6.7 kg of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder;

[0148] The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 1.2:1;

[0149] The particle size of the ore powder is 200 mesh;

[0150] Step 3: preparing carbon fiber-alloy powder;

[0151] A. 83 kg of nickel-aluminum alloy powder, 73 kg of silicon nitride powder and 5 / 12 of modified carbon fiber were mixed and ball-milled to obtain a mixed powder;

[0152] B. Adding cyanoacrylate drop-free binder to the mixed powder, stirring evenly and drying, and sintering at 1980° C. in a sintering furnace under argon protection to obtain a sintered body;

[0153] C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder;

[0154] Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material;

[0155] Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for compression molding, and sinter at a high temperature of 1980° C. to obtain the high temperature resistant carbon fiber composite material.

[0156] The carbon fiber composite material prepared in Example 3 was tested for performance, and the results were as follows:

[0157]

[0158] (Similarly, corresponding evaluation tests were conducted on other embodiments, and the test results were not significantly different from the evaluation test results of Embodiment 3, so they will not be elaborated here)

[0159] The high temperature resistant carbon fiber composite material prepared by the present invention has a thermal conductivity of 14.08W / m·K and an impact strength of 56.3KJ / m 2 It has the advantages of high temperature resistance, high impact strength, corrosion resistance, and good thermal conductivity, which can effectively avoid heat accumulation.

[0160] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high temperature resistant carbon fiber composite material, Features: It includes modified carbon fiber, modified fiber and modified resin layer; The modified resin preparation method is as follows: A. Preheat 100 parts of acrylic resin to 50°C; B. Add 11-18 parts of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C; C. Divide 5-7 parts of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder; The ore is a mixture of pyrophyllite and chabazite; the ratio of pyrophyllite to chabazite is 0.7-1.5:

1.

2. The carbon fiber composite material according to claim 1, It is characterized in that The modified carbon fiber preparation method is as follows: A. Activate 50-80 parts of carbon fiber by 150-200 parts of calcium carbonate solution; B. adding 90-110 parts of olefin monomer to the activated carbon fiber and mixing and stirring to obtain a mixed solution A; C. Dry the mixed solution A to obtain modified carbon fiber.

3. A method for preparing a high temperature resistant carbon fiber composite material according to claim 1-2, It is characterized in that Step 1: preparing modified carbon fiber; A. Activate 50-80 parts of carbon fiber by 150-200 parts of calcium carbonate solution; B. adding 90-110 parts of olefin monomer to the activated carbon fiber and mixing and stirring to obtain a mixed solution A; C. Drying the mixed solution A to obtain modified carbon fiber, and dividing the modified carbon fiber into two parts for standby use; Step 2: Preparation of modified resin: A. Preheat 100 parts of acrylic resin to 50°C; B. Add 11-18 parts of tris(4-nonylphenyl)phosphite to acrylic resin and heat to 108°C; C. Divide 5-7 parts of ore powder into five equal parts, add them into acrylic resin in five times, raise the temperature by 1°C each time and stir, and obtain modified resin after natural cooling; grind the modified resin into modified resin powder; The ore is a mixture of pyrophyllite and chabazite; Step 3: preparing carbon fiber-alloy powder; A. Mix 80-92 parts of nickel aluminum alloy powder, 72-78 parts of silicon nitride powder and 1 / 3-1 / 2 of modified carbon fiber, and obtain a mixed powder by ball milling; B. Adding a binder to the mixed powder, stirring evenly and drying the mixture, and sintering the mixture in a sintering furnace under argon protection to obtain a sintered body; C. Grinding the sintered body into fine powder to obtain carbon fiber-alloy powder; Step 4: mixing the remaining modified carbon fiber, modified resin powder and carbon fiber-alloy powder to obtain a carbon fiber composite material; Step 5: Place the high temperature resistant carbon fiber composite material into a product mold for pressing and sintering at a high temperature of 1950-2000°C to obtain the high temperature resistant carbon fiber composite material.

4. The preparation method according to claim 3, It is characterized in that In step 1, the stirring time is 1-2h.

5. The preparation method according to claim 4, It is characterized in that In step 2, the particle size of the ore powder is 200 mesh.

6. The preparation method according to claim 5, It is characterized in that In step three, the sintering temperature is between 1950°C and 2000°C.

7. The preparation method according to claim 6, It is characterized in that In step three, the adhesive is a cyanoacrylate drop-free adhesive.

8. The preparation method according to claim 7, It is characterized in that In step 2, the ratio of pyrophyllite to chabazite is 0.7-1.5:1.