Platinum plating solution, preparation method and application
By adjusting the concentration of platinum salt and conductive salt, platinum plating solution is prepared and vacuum sintered under an argon atmosphere, the problems of weak binding force and large consumption in the existing platinum plating process are solved, and the dense uniformity and production of the platinum layer are achieved. Improved efficiency.
Patent Information
- Application Number
- CN202411126720.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing platinum plating process has problems such as large plating solution consumption, weak binding force and unevenness under high current density and high temperature conditions, and is not suitable for complex anodes.
The platinum plating solution was prepared by adjusting the types and concentrations of the platinum salt and conductive salt, and vacuum sintered under an argon atmosphere to form a platinum layer with strong binding force and uniform binding force.
The dense and uniform bonding force of the platinum layer is achieved, shortening the production process, reducing production energy consumption, and reducing the cost of platinum plating.
Smart Images

Figure CN119020779A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal plating, and in particular relates to a platinum plating solution, a preparation method and an application thereof. Background Art
[0002] The production of electrolytic copper foil is carried out under the acidic conditions of copper sulfate, and oxygen precipitation reaction occurs on the anode. Since the current production process conditions of electrolytic copper foil are relatively harsh, it is necessary to find a suitable material as the anode, which not only has high electrochemical and electrolytic properties, but also has to withstand high current density and high temperature. Existing anodes mostly use metal electrodes. Although this type of electrode has excellent electrochemical properties, its corrosion resistance and high temperature resistance are relatively weak; platinum is a silvery white and shiny metal with good ductility, conductivity and electrocatalytic activity. It is also an ideal insoluble electrode. Pure platinum has low mechanical strength, is easy to deform, and is expensive. Therefore, pure platinum is generally replaced by plating a platinum layer on the metal substrate, which not only prevents the substrate from being corroded, improves the service life of the product, reduces costs, but also increases the electrochemical properties of the metal electrode.
[0003] Most existing platinum plating processes use electroplating, which consumes a lot of plating solution, has weak and uneven platinum plating adhesion, and is not suitable for certain complex anodes. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a platinum plating solution, a preparation method and an application thereof. The platinum plating solution is prepared by adjusting the types and concentrations of platinum salt and conductive salt, and a platinum plating process of vacuum sintering under an argon atmosphere is adopted, so that the platinum plating solution can form a strongly bonded and uniform platinum layer on the surface of a metal substrate.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A platinum plating solution, wherein the raw materials of the platinum plating solution include platinum salt and conductive salt;
[0007] The platinum salt is dinitrosodiammine platinum;
[0008] The conductive salt includes a stabilizer, a brightener and a complexing agent;
[0009] In the platinum plating solution, the concentration of the platinum salt is 10-100 g / L; the concentration of the stabilizer is 1-20 g / L; the concentration of the brightener is 5-100 ppm; and the concentration of the coordination agent is 1-10 g / L.
[0010] Preferably, the stabilizer is any one of ammonium sulfamate, sodium citrate, and ammonium citrate; the brightener is any one of ammonium sulfinate, sodium sulfinate, and sodium dodecyl sulfate; and the complexing agent is any one of sodium chloride and calcium chloride.
[0011] Preferably, the platinum plating solution raw material also includes a pH regulator, and the pH regulator is hydrochloric acid.
[0012] Preferably, the pH of the platinum plating solution is 1-3.
[0013] A method for preparing a platinum plating solution comprises the following steps:
[0014] S1. Prepare an aqueous solution of a platinum salt;
[0015] S2. Add stabilizer, brightener and complexing agent to the S1 aqueous solution according to the concentration requirements, heat and dissolve, stir and prepare a platinum plating solution;
[0016] S3. Add a pH adjuster to the platinum plating solution in S2 to adjust the pH of the platinum plating solution.
[0017] Preferably, in the S1 platinum salt aqueous solution, the mass ratio of platinum salt to water is 1:6-8.
[0018] Preferably, the heating temperature in S2 is 80-100°C.
[0019] The invention discloses an application of a platinum plating solution in preparing a platinum coating on the surface of an electrolytic copper foil anode metal substrate.
[0020] Preferably, the specific process of preparing the platinum coating is: preheating the substrate, placing the preheated substrate in a vacuum environment and uniformly spraying the platinum plating solution, and then naturally drying the substrate sprayed with the platinum plating solution and performing multiple high-temperature sintering in an argon atmosphere.
[0021] Preferably, the preheating conditions are: preheating temperature is 300-1000° C., and preheating time is 3-10 min; the sintering conditions are: sintering temperature is 450-600° C., sintering times are 5-10 times, and each time is 1-3 hours.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention promotes the recrystallization of platinum by vacuum sintering in an argon atmosphere, so that the sintered platinum layer has a denser and more uniform morphology and a higher bonding strength. At the same time, the vacuum sintering platinum plating process can be sintered together with the precious metal coating, shortening the production process and reducing production energy consumption. This method is easy to operate and has high safety.
[0024] (2) Traditional platinum plating solutions are mostly based on chloroplatinic acid. This platinum salt is easily hydrolyzed and inconvenient to store, which increases the cost of preparing the platinum plating solution. Using dinitrodiammine platinum as a platinum source and high-concentration citrate as a conductive salt does not require the addition of a large amount of free ligands, which can reduce the oxidation of the platinum layer. Compared with other low-concentration stabilizers, the platinum layer plated by this method has stronger bonding strength and longer service life, so the cost of platinum plating is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a physical picture of the platinum-plated layer of Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. The reagents used therein should be understood to be conventional commercial reagents or prepared according to the prior art unless otherwise specified; the operating methods used therein should be understood to be conventional operations in the art unless otherwise specified.
[0027] The invention provides a platinum plating solution, wherein the raw materials of the platinum plating solution include platinum salt and conductive salt; the platinum salt is dinitrosodiammine platinum; and the conductive salt includes a stabilizer, a brightener and a coordination agent.
[0028] In the platinum plating solution, the concentration of platinum salt is 10-100 g / L; the concentration of stabilizer is 1-20 g / L; the concentration of brightener is 5-20 ppm; and the concentration of coordination agent is 1-10 g / L.
[0029] The raw materials of the platinum plating solution of the present invention also include a pH regulator and water; wherein the pH regulator is hydrochloric acid and water is used as a solvent.
[0030] In the embodiment of the present invention, the stabilizer is any one of ammonium sulfamate, sodium citrate, and ammonium citrate; the brightener is any one of ammonium sulfinate, sodium sulfinate, and sodium dodecyl sulfate; and the complexing agent is any one of sodium chloride and calcium chloride.
[0031] The present invention uses dinitrosodiammine platinum as a platinum source and high-concentration citrate as a conductive salt, does not need to add a large amount of free ligands, can reduce the oxidation of the platinum layer, and compared with other low-concentration stabilizers, the platinum layer plated by this method has stronger bonding force and longer service life, so the cost of platinum plating is greatly reduced.
[0032] The platinum plating solution provided by the present invention is used to prepare a platinum coating on the surface of an electrolytic copper foil anode metal substrate, comprising the following steps:
[0033] S1. Substrate pretreatment: The substrate is selected from any one of corrosion-resistant metals such as titanium, nickel, tantalum and stainless steel, and is subjected to sandblasting, pickling and heat correction treatment;
[0034] S2. Preparation of platinum plating solution: first prepare an aqueous solution of platinum salt, then add stabilizer, brightener and ligand into the aqueous solution according to concentration requirements, heat to 80-100°C to dissolve and stir evenly, then add pH adjuster; wherein, in the platinum salt aqueous solution, the mass ratio of platinum salt to water is 1:6-8; the pH of the platinum plating solution is 1-3.
[0035] S3, platinum plating layer; preheating with liquefied gas to remove moisture from the substrate pretreated by S1, the preheating temperature is 300-1000°C, and the preheating time is 3-10 minutes; placing the preheated substrate in a vacuum spraying device and spraying the platinum plating solution prepared by S2 evenly, and after the substrate sprayed with the platinum plating solution is naturally dried, it is subjected to multiple high-temperature sintering in an argon atmosphere, the sintering temperature is 450-600°C, the sintering times are 5-10 times, and each time is 1-3 hours; a platinum layer with metallic luster and uniform thickness can be plated on the surface of the metal substrate.
[0036] The present invention promotes the recrystallization of platinum by vacuum sintering in an argon atmosphere, so that the sintered platinum layer has a denser and more uniform morphology and a higher bonding strength. At the same time, the vacuum sintering platinum plating process can be sintered together with the precious metal coating, shortening the production process and reducing production energy consumption.
[0037] The following is further described in conjunction with specific embodiments.
[0038] Example 1
[0039] A platinum plating solution is used to prepare a platinum coating on the surface of an electrolytic copper foil anode metal substrate, comprising the following steps:
[0040] S1. Pretreatment of substrate: 6mm titanium plate is selected as substrate, brown corundum is used for automatic sandblasting, and then 5% oxalic acid is used for etching for 3 hours, and the plate surface is flattened by heat correction;
[0041] S2, preparation of platinum plating solution; preparing an aqueous solution of dinitrodiammine platinum with a concentration of 10 g / L, then adding 1 g / L of citric acid to the aqueous solution according to the concentration requirement, adding 5 ppm of sodium sulfite, adding 1 g / L of sodium chloride, heating to 100 ° C to dissolve and stir evenly, and then adding hydrochloric acid to adjust the pH of the platinum plating solution to 2;
[0042] S3, platinum plating layer; before platinum plating, use a magnetic stirrer to stir the platinum plating solution evenly and preheat it with liquefied gas to remove moisture from the surface of the titanium plate pretreated by S1, the preheating temperature is 300°C, and the preheating time is 3min; the platinum plating solution prepared by S2 is evenly sprayed on the surface of the preheated titanium plate, and the titanium plate sprayed with the platinum plating solution is naturally dried and then sintered several times at high temperature in an argon atmosphere furnace, the sintering temperature is 600°C, the sintering number is 10 times, and each time is 3 hours; a platinum layer with a metallic luster and uniform thickness can be plated on the surface of the titanium plate, refer to Figure 1 .
[0043] Example 2
[0044] A platinum plating solution is used to prepare a platinum coating on the surface of an electrolytic copper foil anode metal substrate, comprising the following steps:
[0045] S1. Pretreatment of substrate: 3mm tantalum plate is selected as substrate, quartz sand is used for sandblasting 3 times, and then etched with 5% sulfuric acid and heat-corrected;
[0046] S2, preparation of platinum plating solution; prepare an aqueous solution of dinitrodiammine platinum with a concentration of 100 g / L, then add 20 g / L of ammonium citrate to the aqueous solution according to the concentration requirement, add 10 g / L of sodium chloride, add 20 ppm of sodium dodecyl sulfate, heat to 80 ° C to dissolve and stir evenly, add hydrochloric acid to adjust the pH of the platinum plating solution to 1;
[0047] S3, platinum plating layer; before platinum plating, use a magnetic stirrer to stir the platinum plating solution evenly and use liquefied gas to preheat to remove moisture on the surface of the tantalum plate pretreated by S1, the preheating temperature is 300°C, and the preheating time is 3 minutes; the platinum plating solution prepared by S2 is evenly sprayed on the surface of the preheated tantalum plate, and the tantalum plate sprayed with the platinum plating solution is naturally dried and then subjected to multiple high-temperature sintering in an argon atmosphere furnace, the sintering temperature is 450°C, the sintering times are 5 times, and each time is 1 hour; a platinum layer with metallic luster and uniform thickness can be plated on the surface of the tantalum plate.
[0048] Example 3
[0049] A platinum plating solution is used to prepare a platinum coating on the surface of an electrolytic copper foil anode metal substrate, comprising the following steps:
[0050] S1. Pretreatment of substrate: 304 stainless steel was selected as the substrate, and white corundum was used for sandblasting 3 times, and then etched with 5% oxalic acid and heat-corrected;
[0051] S2, preparation of platinum plating solution; preparing an aqueous solution of dinitrodiammine platinum with a concentration of 25g / L, then adding 10g / L of ammonium sulfamate to the aqueous solution according to the concentration requirement, adding 10g / L of sodium chloride, adding 20ppm of sodium dodecyl sulfate, heating to 90°C to dissolve and stir evenly, and adding hydrochloric acid to adjust the pH of the platinum plating solution to 3;
[0052] S3, platinum-plated layer; before platinum plating, use a magnetic stirrer to stir the platinum-plating liquid evenly and use liquefied gas to preheat to remove moisture on the surface of the stainless steel pretreated by S1, the preheating temperature is 1000°C, and the preheating time is 10 minutes; the platinum-plating liquid prepared by S2 is evenly sprayed on the preheated stainless steel surface, and the stainless steel sprayed with the platinum-plating liquid is naturally dried and then subjected to multiple high-temperature sintering in an argon atmosphere furnace, the sintering temperature is 550°C, the number of sintering times is 8 times, and each time is 1.5 hours; a platinum layer with metallic luster and uniform thickness can be plated on the stainless steel surface.
[0053] Example 4
[0054] A platinum plating solution is used to prepare a platinum coating on the surface of an electrolytic copper foil anode metal substrate, comprising the following steps:
[0055] S1, substrate pretreatment: 10mm titanium plate was selected as the substrate, and diamond sandblasting was used for 3 times, and then etched with 10% hydrochloric acid for 2 hours, and heat-corrected;
[0056] S2, preparation of platinum plating solution; preparing an aqueous solution of dinitrodiammine platinum with a concentration of 15g / L, then adding 1.5g / L of sodium citrate to the aqueous solution according to the concentration requirement, adding 4g / L of calcium chloride, adding 10ppm of sodium sulfite, heating to 80°C to dissolve and stir evenly, and adding hydrochloric acid to adjust the pH of the platinum plating solution to 1;
[0057] S3, platinum-plated layer; before platinum plating, use a magnetic stirrer to stir the platinum-plating liquid evenly and use liquefied gas to preheat it to remove moisture on the surface of the titanium plate pretreated by S1, the preheating temperature is 1000°C, and the preheating time is 5 minutes; the platinum-plating liquid prepared by S2 is evenly sprayed on the surface of the preheated titanium plate, and the titanium plate sprayed with the platinum-plating liquid is naturally dried and then subjected to multiple high-temperature sintering in an argon atmosphere furnace, the sintering temperature is 550°C, the number of sintering times is 10 times, and each time is 1.5 hours; a platinum layer with metallic luster and uniform thickness can be plated on the surface of the titanium plate.
[0058] Comparative Example 1
[0059] The titanium plate is electroplated using the platinum plating solution prepared in this comparative example as the electroplating solution, comprising the following steps:
[0060] S1. Use 6mm titanium plate as the substrate, use brown corundum for automatic sandblasting, etch with 5% oxalic acid for 3 hours, and make the plate surface flat by heat correction;
[0061] S2. The platinum plating solution uses 20g / L chloroplatinic acid, adds 2g / L citric acid as a stabilizer, adds 1:1 ethanol and water to dissolve, adds 2g / L sodium chloride, adds 10ppm of sodium dodecylbenzene sulfonate and dioctyl sodium sulfosuccinate, and after fully stirring and dissolving, adopts the brush plating process, the anode is an iridium tantalum electrode, the cathode is the titanium plate to be plated, the current is 7A, and the electroplating time is 40 minutes.
[0062] Table 1 is the platinum content results obtained in Examples 1-4 of the present invention
[0063]
[0064] Table 2 shows the material bonding strength and conductivity results obtained by brush plating in Examples 1-4 of the present invention and Comparative Example 1
[0065] Bonding strength (thermal shock method) Conductivity (national standard method) Example 1 14 times without peeling 3mΩ Example 2 11 times without peeling 6mΩ Example 3 13 times without peeling 3mΩ Example 4 16 times without peeling 4mΩ Comparative Example Brush Plating 9 times without peeling 31mΩ
[0066] The platinum coating effect of Example 1 of the present invention is as follows Figure 1 As shown, it can be seen that the platinum layer is bright white and the coating is uniform;
[0067] The platinum content of the above examples 1-4 was measured by XRF as shown in Table 1; the platinum content was detected at 6 locations of the platinum-plated layer of the metal substrate of each example, and the comparison results of six similar data of each example showed that the platinum content on the surface of the substrate was uniform;
[0068] The results of material bonding strength and conductivity obtained by brush plating in Examples 1-4 of the present invention and Comparative Example 1 are shown in Table 2. The measured bonding strength and conductivity data indicate that the platinum coating obtained by vacuum sintering in an argon atmosphere in the present invention has the characteristics of strong bonding strength and low conductivity; and this method is easy to operate and highly safe.
Claims
1. A platinum plating solution, characterized in that The raw materials of the platinum plating solution include platinum salt and conductive salt; The platinum salt is dinitrosodiammine platinum; The conductive salt includes a stabilizer, a brightener and a complexing agent; In the platinum plating solution, the concentration of the platinum salt is 10-100 g / L; the concentration of the stabilizer is 1-20 g / L; the concentration of the brightener is 5-100 ppm; and the concentration of the coordination agent is 1-10 g / L.
2. The platinum plating solution according to claim 1, characterized in that The stabilizer is any one of ammonium sulfamate, sodium citrate and ammonium citrate; the brightener is any one of ammonium sulfinate, sodium sulfinate and sodium dodecyl sulfate; the complexing agent is any one of sodium chloride and calcium chloride.
3. The platinum plating solution according to claim 1, characterized in that The platinum plating solution raw material also includes a pH regulator, and the pH regulator is hydrochloric acid.
4. The platinum plating solution according to claim 1-3, characterized in that The pH of the platinum plating solution is 1-3.
5. The method for preparing the platinum plating solution according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Prepare an aqueous solution of a platinum salt; S2. Add stabilizer, brightener and complexing agent to the S1 aqueous solution according to the concentration requirements, heat and dissolve, stir and prepare a platinum plating solution; S3. Add a pH adjuster to the platinum plating solution in S2 to adjust the pH of the platinum plating solution.
6. The preparation method according to claim 5, characterized in that: In the S1 platinum salt aqueous solution, the mass ratio of platinum salt to water is 1:6-8.
7. The preparation method according to claim 5, characterized in that: The heating temperature in S2 is 80-100°C.
8. Use of the platinum plating solution according to any one of claims 1 to 4 in preparing a platinum coating on the surface of an electrolytic copper foil anode metal substrate.
9. The use according to claim 8, characterized in that: The specific process of preparing the platinum coating is: preheating the substrate, placing the preheated substrate in a vacuum environment and spraying the platinum plating solution uniformly, and then naturally drying the substrate sprayed with the platinum plating solution and performing multiple high-temperature sintering in an argon atmosphere.
10. The use according to claim 9, characterized in that: The preheating conditions are: preheating temperature is 300-1000°C, and preheating time is 3-10 minutes; the sintering conditions are: sintering temperature is 450-600°C, sintering times are 5-10 times, and each time is 1-3 hours.