Preparation method of infrared broadband radar flexible camouflage carbon felt car cover
By pre-treating and functionalizing carbon fiber felt, and combining it with infrared camouflage and electromagnetic shielding treatments, a flexible camouflage carbon felt car cover for infrared broadband radar was prepared. This solved the shortcomings of existing materials in multi-spectral camouflage and electromagnetic shielding, and achieved lightweight, efficient multi-band camouflage effect and long-term stable camouflage.
Patent Information
- Application Number
- CN202411414765.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-11
AI Technical Summary
Existing flexible camouflage materials are difficult to achieve effective camouflage in multi-spectral environments, especially due to insufficient compatibility with infrared, thermal infrared and radar bands, and lack of electromagnetic shielding function, which cannot meet the multi-band camouflage requirements of mobile secure conference vehicles. At the same time, traditional materials have insufficient performance stability and service life in harsh environments.
Using carbon fiber felt as the base material, and through pretreatment such as cleaning, carbon ball stirring and saturated sodium chloride solution spraying, combined with infrared camouflage and electromagnetic shielding treatment, a flexible camouflage carbon felt car cover for infrared broadband radar is prepared, which has the functions of preventing infrared reconnaissance, preventing multi-band radar reconnaissance and electromagnetic attack protection.
It achieves a multi-spectral camouflage effect that is lightweight, wind-resistant, and highly adaptable to various environments, significantly improving the camouflage performance and service life of the mobile conference vehicle, reducing the probability of the target being detected, and ensuring electromagnetic protection capabilities.
Smart Images

Figure CN119022719A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of multi-spectrum camouflage, and in particular relates to a method for preparing an infrared broadband radar flexible camouflage carbon felt vehicle cover. Background Art
[0002] With the complication of the international strategic situation and the application of high-precision weapons in modern warfare, the demand for anti-reconnaissance camouflage functions of mobile temporary confidential conference venues has increased dramatically in countries around the world. The improvement of multi-spectral (synthetic aperture radar, visible light / far infrared imager, hyperspectral imaging detector) detection capabilities of satellites, high-altitude reconnaissance aircraft, drones, etc. has made the reconnaissance detection accuracy reach the centimeter level. Imaging reconnaissance satellites can quickly and accurately grasp the dynamics and real-time situation of ground targets through panoramic high-resolution imaging of the battlefield and monitoring, tracking and detection and identification of key targets, providing strong information support for the precise strike of targets. Therefore, it is urgent to reduce the detectability of mobile confidential conference vehicles to achieve the purpose of all-round camouflage in a high-precision reconnaissance detection environment. For mobile conference vehicle targets, how to effectively and efficiently avoid satellite reconnaissance, reduce the probability of target discovery, and resist close-range electromagnetic attacks have become the core factors to ensure the self-protection capability and wartime survivability of key mobile targets.
[0003] The base materials of flexible camouflage products that are currently widely used in my country are mostly composite materials made of synthetic compounds such as polyester, polyamide or polyester braid and metal fiber. They have high-efficiency camouflage functions in single frequency bands such as visible light camouflage, infrared camouflage or radar camouflage, but there is still a certain gap in the product's multi-spectrum compatibility and performance consistency. It is difficult to simultaneously meet the actual camouflage function requirements of flexible camouflage materials in multiple frequency bands such as near-infrared, thermal infrared, radar, etc.; it lacks electromagnetic shielding and other functions, and it is difficult to protect against close-range electromagnetic interference; due to the poor environmental adaptability of the base material itself, when used in harsh environments such as coastal areas, deserts, and plateaus, the performance stability and service life will be severely reduced, and it is difficult to meet future use requirements; and the existing camouflage materials are not suitable for the appearance structure and surface paint color of mobile confidential conference vehicles.
[0004] Therefore, there is an urgent need for camouflage covers for mobile confidential conference vehicles, which will not affect the operation of the conference vehicle and can also achieve good multi-spectrum camouflage functions. This type of cover should have the advantages of light weight, good wind resistance, anti-infrared reconnaissance camouflage, anti-multi-band radar reconnaissance camouflage, easy disassembly and assembly, and excellent environmental adaptability. At present, there is no mature design scheme, preparation process and detail processing technology for this type of cover in China, and this field is still in a market blank. Summary of the invention
[0005] In response to the above technical problems, the present invention provides a method for preparing an infrared broadband radar flexible camouflage carbon felt car cover. The prepared camouflage carbon felt car cover has the functions of covering anti-infrared reconnaissance camouflage, anti-multi-band radar reconnaissance camouflage and electromagnetic attack protection, and has the characteristics of good wind resistance, low density and strong environmental adaptability.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A method for preparing an infrared broadband radar flexible camouflage carbon felt car cover comprises the following steps:
[0008] S1. Raw material pretreatment: The carbon fiber felt is sequentially subjected to cleaning pretreatment, carbon ball stirring pretreatment, and saturated sodium chloride solution spraying process;
[0009] S2, cutting: cutting the skeleton net and cutting the carbon fiber felt processed in step S1;
[0010] S3, infrared camouflage treatment: performing infrared camouflage treatment on the upper surface of the carbon fiber felt cut in step S2;
[0011] S4, electromagnetic shielding treatment: performing electromagnetic shielding treatment on the lower surface of the carbon fiber felt after the infrared camouflage treatment in step S3;
[0012] S5, cutting and binding the carbon fiber felt after the electromagnetic shielding treatment into a net; and binding the carbon fiber felt after the net and the skeleton net cut in step S2 for edge wrapping.
[0013] In step S1, the cleaning pretreatment refers to: firstly treating the carbon fiber felt by heating and drying for 1 to 2 hours; then removing impurities on the surface of the carbon fiber felt by solvent cleaning, and finally performing drying treatment.
[0014] In step S1, the carbon ball stirring pretreatment refers to: adding distilled water, carbon fiber felt and high-purity carbon balls into a magnetic stirring container, stirring slowly at 300 to 600 rpm for 5 to 10 hours, and forming microporous defects on the surface of the carbon fiber felt through mutual collision and friction between the carbon balls and the carbon fiber felt.
[0015] In step S1, the saturated sodium chloride solution spraying process refers to: evenly spraying the saturated sodium chloride solution on the upper and lower surfaces of the carbon fiber felt, keeping it horizontally dry at room temperature, placing it in a cool and dark place for a period of time, and then rinsing it with deionized water.
[0016] The surface of the carbon fiber felt is 2-3g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry for 5 to 10 minutes at room temperature, and then spray the surface of the carbon fiber at 2 to 3 g / m 2Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry at room temperature for 5 to 10 minutes, place it in a cool and dark place (ambient humidity> 20%) for 144 to 240 hours, rinse it with deionized water 3 to 5 times, and place it in a dry and cool place for use.
[0017] In the step S3: the infrared camouflage paint is dispersed for 10 to 20 minutes, and then the infrared camouflage paint is sprayed on the upper surface of the carbon fiber felt; after the spraying is completed, the carbon fiber felt is placed horizontally in a clean and ventilated place, and after the coating surface is dry, it is folded and stored in a dry and ventilated place, completing the infrared camouflage treatment process on the upper surface of the carbon fiber felt.
[0018] In the step S4: the carbon nano conductive coating is dispersed for 5 to 10 minutes, and then the conductive coating is sprayed on the lower surface of the carbon fiber felt; after the spraying is completed, the carbon fiber felt is placed horizontally in a clean and ventilated place, and after the coating surface is dry, it can be folded and stored in a dry and ventilated place to complete the electromagnetic shielding treatment process of the lower surface of the carbon fiber felt.
[0019] The step S4 is performed sequentially 24 hours after the step S3 is completed.
[0020] In step S5, the flower cutting refers to: placing the spliced carbon fiber felt on a flower cutting machine; laying the carbon fiber felt flat, laying 20 to 30 layers per plate, the edges of the fabric should be neat, and the upper and lower errors should not be greater than 5mm; after the carbon fiber felt is stacked, it is neatly and parallelly placed on a flower cutting machine of the corresponding flower pattern as required to cut the flower;
[0021] The binding into a net refers to: spreading the carbon fiber felt flat on the work surface, and then spreading the skeleton net on the carbon fiber felt, and adjusting it to be even and flat; using binding wire for binding, the binding structure is diamond-shaped, the binding density, the number of bindings per square meter is controlled at 25 to 35 knots, the knotting type is self-tightening, one knot is tied 3 to 5 times, the direction of winding is positive and negative, it is tied and tightened, and the knot head is left 20mm to 30mm long.
[0022] In step S5, the hemming means: aligning the carbon fiber felt and the skeleton net, and completely wrapping the two layers together with the edge rope into the hemming strip, sewing the stitches evenly, without skipped stitches or broken threads; the sutures of the connecting loop rope and the skeleton net should be re-sewn 3-5 times, the repeated stitch length should be completely covered, the connecting loop rope should not be missing, and the sewing stitches should be flat and firm;
[0023] The length and spacing of the connecting rings must be within the tolerance range, the length of the connecting ring rope is 200mm±20mm, and the spacing of the connecting ring rope is 200mm±20mm;
[0024] Make cuts of about 15 to 25 mm in depth every 150 to 250 mm on the fabric strips to facilitate the rope production;
[0025] When hemming, the edge rope joints are sewn at the center of any length of the four sides, and sewing at the four corners is not allowed.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. For the first time, a preparation method of a new infrared / broadband radar flexible camouflage carbon felt car cover is proposed to solve the anti-reconnaissance problem of mobile conference cars. The prepared infrared / broadband radar flexible camouflage carbon felt car cover can have comprehensive camouflage functions.
[0028] 2. Selection of raw material components and preparation method of new infrared / broadband radar flexible camouflage carbon felt car cover. The important innovation is to use carbon fiber felt, skeleton mesh and functional coating as raw materials, and carry out surface pretreatment, layout cutting, upper and lower surface spraying, cutting, binding into nets, hemming and other processes to prepare infrared / broadband radar flexible camouflage carbon felt car cover that can be used for mobile confidential conference car camouflage.
[0029] 3. The preparation process and process parameters of the new infrared / broadband radar flexible camouflage carbon felt car cover. Important innovations include the overall structural design, carbon fiber felt surface modification, functional coating spraying and other process flows and process parameters.
[0030] At present, there is no mature infrared / broadband radar flexible camouflage carbon felt car cover that can be used for multi-band comprehensive protection of mobile confidential conference cars. Through the design and application of new protective materials, a series of comprehensive protective camouflage products that can be used for mobile conference cars are realized, covering anti-infrared reconnaissance camouflage, anti-multi-band radar reconnaissance camouflage and electromagnetic interference protection. The infrared / broadband radar flexible camouflage carbon felt car cover based on the content of the present invention has a surface density reduced to 200g / m compared with existing camouflage materials. 2 , thickness is less than 1cm; on the basis of meeting the camouflage performance, it significantly improves the environmental adaptability performance, with a service life of not less than 2 years, ensuring the stability and reliability of the long-term camouflage protection effect, and providing a guarantee for improving the safety factor of mobile conference vehicles.
[0031] It mainly makes up for the following deficiencies of existing technologies:
[0032] 1. Currently, there is no lightweight, quick-disassembly infrared / broadband radar flexible camouflage material with excellent performance. The scarcity of lightweight and high-performance materials limits the development and production of camouflage car covers for mobile confidential conference vehicles.
[0033] 2. Traditional camouflage materials do not have anti-electromagnetic shielding function, and camouflage materials that have anti-near infrared, thermal infrared, and radar wave functions are heavy (usually composed of a multi-layer structure, weighing 500 to 1000 grams per square meter) and occupy a large amount of internal loading space in the vehicle (the volume of a traditional 25 square meter camouflage net is about 0.5 cubic meters), which causes inconvenience to the operation of the mobile confidential conference car and the disassembly and assembly of the camouflage car cover.
[0034] 3. Traditional camouflage materials usually require the use of metal components to achieve broadband radar camouflage and electromagnetic shielding, which will produce oxidation during long-term outdoor use, and their performance will be greatly reduced.
[0035] 4. Most traditional carbon fiber felt surface treatment processes use strong oxidants such as strong acids and alkalis, which not only pose safety risks in the production process, but also seriously pollute the environment with wastewater and waste generated. The present invention achieves functional modification of the entire carbon fiber felt and key surface locations by simply using non-toxic and harmless raw materials such as high-purity carbon balls and sodium chloride. After the present invention is cleaned, pre-treated with carbon ball stirring, and treated with a saturated sodium chloride solution spraying process, extremely fine nano-scale grooves appear on the surface of a single fiber of the carbon fiber felt. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the roll of the infrared / broadband radar flexible camouflage carbon felt car cover product of the present invention;
[0037] Figure 2 It is a structural schematic diagram of the infrared / broadband radar flexible camouflage carbon felt car cover of the present invention;
[0038] Figure 3 is a top view of the carbon fiber felt / skeleton mesh structure of the present invention;
[0039] Figure 4 This is a structural morphology diagram of the carbon fiber felt of the present invention;
[0040] Figure 5 This is a microscopic morphology diagram of the carbon fiber felt of the present invention;
[0041] Figure 6 This is a detailed view of the surface of a single fiber of the original carbon fiber felt of the present invention;
[0042] Figure 7 This is a detailed view of the surface of a single fiber of the carbon fiber felt after being cleaned, pre-treated by stirring carbon balls, and sprayed with a saturated sodium chloride solution;
[0043] Figure 8 Schematic diagram of the microstructure of the carbon nano conductive coating of the present invention;
[0044] Fig. 9 is a test curve diagram of the reflectivity of the sample in the first embodiment of the present invention;
[0045] Fig.10 is the sample reflectivity test curve in Example 2 of the present invention;
[0046] Fig.11 This is the reflectivity test curve of the sample in Example 3 of the present invention. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.
[0048] like Figure 1-8 As shown, a method for preparing an infrared broadband radar flexible camouflage carbon felt car cover comprises the following steps:
[0049] Main raw material selection:
[0050] ①Fiber felt:
[0051] Carbon fiber wire diameter: 15~30μm
[0052] Impurity content: <10ppm
[0053] Density: Three levels are set according to radar wave / infrared camouflage requirements. Level A is 0.07g / cm 3 , B grade 0.08g / cm 3 , C grade A grade 0.09g / cm 3 . The performance level increases step by step from A to C.
[0054] ②Infrared camouflage treatment on the upper surface of carbon fiber felt: infrared camouflage paint
[0055] Ingredients: Polyurethane resin, fluorocarbon resin, and dimethyl silicone resin coatings containing low-emissivity fillers such as MgO, FeO, and ZnO.
[0056] ③ Electromagnetic shielding treatment of carbon fiber felt bottom: carbon nano conductive coating
[0057] Ingredients: Polyurethane and epoxy resin coatings containing pure carbon conductive fillers such as graphene, Mexene, and highly conductive graphite.
[0058] Square resistance after coating is dry: <0.1Ω / sq
[0059] ④Skeleton network:
[0060] Main ingredient: Nylon thread
[0061] Wire type: Warp (840D / 3), Weft (840D / 3)
[0062] Aperture: (50±10)mm×(50±10)mm
[0063] ⑤Carbon ball:
[0064] Carbon content: >99.9%
[0065] Carbon ball diameter: 3~5μm
[0066] Main preparation process
[0067] S1. Raw material pretreatment:
[0068] (1) Cleaning and pre-treating the raw materials (carbon fiber felt). This is mainly to remove the active agent and adsorbed water remaining on the surface of the powder during the preparation process, so as to reduce the adverse effects of impurities on the material properties in the later stage of the reaction. The present invention removes impurities on the surface of the raw materials by heating (120°C to 160°C) and drying for 1 to 2 hours, and washing with a solvent (ethanol, acetone), and then drying the raw materials.
[0069] (2) Functionalize the surface of carbon fiber felt to improve the adhesion of subsequent surface functional coatings. Add distilled water: carbon fiber felt: high-purity carbon balls in a mass fraction ratio of 10L: 100g: 200g into a magnetic stirring container, and stir slowly at 300-600 rpm for 5-10 hours to ensure that the carbon fiber felt and carbon balls rotate in a circle in the distilled water. Through the collision and friction between the carbon balls and the carbon fiber felt, microporous defects are formed on the surface of the carbon fiber felt. After the reaction is completed, the carbon fiber felt is removed and rinsed with deionized water for 3-5 times. Finally, it is placed in a 50℃ oven to dry for 12-16 hours and placed in a dry and cool place for standby use; the remaining carbon balls are filtered from the remaining solution and reused after the quality is determined to meet the parameter requirements.
[0070] (3) After the previous step is completed, the carbon fiber felt is in the same surface functional pretreatment state as a whole. The focus of this process is to treat the upper and lower surfaces of the carbon fiber felt. A precision spray control system is used to spray the upper surface of the carbon fiber felt at a rate of 2 to 3 g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry for 5 to 10 minutes at room temperature, and then spray the surface of the carbon fiber at 2 to 3 g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep horizontal drying at room temperature for 5 to 10 minutes, place in a cool and dark place (ambient humidity> 20%) for 144 to 240 hours, rinse with deionized water 3 to 5 times, and place in a dry and cool place for use. Through this process, further functional modification of the upper and lower surfaces of the carbon fiber felt is achieved. It will not be difficult to control the surface modification effect of the carbon fiber like traditional strong oxidants such as nitric acid, which will cause the performance of the carbon fiber felt to decline, and a continuous groove microstructure can be formed on the surface. In the subsequent process of spraying the coating on the upper and lower surfaces of the carbon fiber felt, the coating components can penetrate into the groove gaps, and after curing, the mechanical interlocking effect with the carbon fiber surface is obvious, which significantly improves the interface strength and effectively improves the adhesion of the coating after curing.
[0071] Figure 7 It can be clearly seen that the surface details of a single fiber of the carbon fiber felt after cleaning, carbon ball stirring pretreatment, and saturated sodium chloride solution spraying process: extremely fine nano-scale grooves appear on the fiber surface; Figure 6Shown are the surface details of a single fiber of the original carbon fiber felt: the fiber surface is flat and smooth.
[0072] S2, cutting: cutting the skeleton net and cutting the carbon fiber felt processed in step S1;
[0073] (1) Cut the carbon fiber felt. According to the layout size, the thickness of the carbon fiber felt is controlled at 5-8 mm, and the edges are neat and burr-free.
[0074] (2) The mesh specifications of the skeleton net must be accurate, and the number of meshes must be calculated accurately when cutting. The size of each skeleton mesh is (50±10)mm×(50±10)mm.
[0075] S3, infrared camouflage treatment: performing infrared camouflage treatment on the upper surface of the carbon fiber felt cut in step S2;
[0076] (1) The infrared camouflage paint is dispersed at a speed of 100 rpm for 10 to 20 minutes, and the infrared camouflage paint is sprayed on the upper surface of the carbon fiber felt using the following spraying process.
[0077]
[0078] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 4 hours. After the coating surface is dry, fold it and store it in a dry and ventilated place for 96 hours to complete the infrared camouflage treatment process on the surface of the carbon fiber felt.
[0079] S4, electromagnetic shielding treatment: performing electromagnetic shielding treatment on the lower surface of the carbon fiber felt after the infrared camouflage treatment in step S2;
[0080] (1) The carbon nano conductive coating is dispersed at a speed of 100 rpm for 5 to 10 minutes, and the conductive coating is sprayed on the lower surface of the carbon fiber felt using the following spraying process.
[0081]
[0082] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 2 hours. After the coating surface is dry, it can be folded and stored in a dry and ventilated place for 48 hours to complete the electromagnetic shielding treatment process of the lower surface of the carbon fiber felt.
[0083] Note: Step 4 should be performed 24 hours after step 3. The order of steps 3 and 4 cannot be reversed.
[0084] S5, cutting and binding the carbon fiber felt after the electromagnetic shielding treatment into a net; and binding the carbon fiber felt after the net and the skeleton net cut in step S2 for edge wrapping.
[0085] Cutting flowers: (1) First, the cutting notch size should be R (15-20) mm as required by the design drawing, and the spliced carbon fiber felt should be placed on the cutting machine. (2) The carbon fiber felt should be laid flat, with 20-30 layers per plate. The edges should be neat, and the upper and lower errors should not be greater than 5 mm. Unqualified or substandard carbon fiber felts should not be cut or punched. After stacking, the carbon fiber felts should be neatly placed on the cutting machine of the corresponding flower pattern as required, ready for cutting. (3) Setting data for the cutting machine: Cutting stroke: 180 mm, pressure 0.15-0.3 MPa.
[0086] Binding into a net: (1) Laying: First lay the carbon fiber felt flat on the work surface, then lay the skeleton net flat on the carbon fiber felt, and adjust it to be even and flat. (2) Binding: Use binding wire for binding. The binding structure is diamond-shaped. The binding density is controlled at 25 to 35 knots per square meter. The knotting type is self-tightening. One knot is tied 3 to 5 times. The winding direction is positive and negative. Tie it tightly and leave the knot 20mm to 30mm long.
[0087] Binding: (1) The carbon fiber felt and skeleton net should be aligned up and down, and the edge rope should be completely wrapped in the binding strip. The sewing stitches should be even, and there should be no skipped stitches or broken threads. The seams between the connecting ring rope and the skeleton net should be re-sewn 3-5 times, and the repeated stitch length should be completely covered. The connecting ring rope should not be missing, and the sewing stitches should be flat and firm. (2) The length and spacing of the connecting ring should be within the tolerance range. The length of the connecting ring rope is 200mm±20mm, and the spacing of the connecting ring rope is 200mm±20mm.
[0088] (3) Make cuts about 15 to 25 mm deep on the fabric strips at intervals of 150 to 250 mm to facilitate the production of the rope.
[0089] (4) When hemming, the edge rope joints are sewn at the center of any length of the four sides. Sewing at the four corners is not allowed.
[0090] It also includes finished product inspection and packaging: the sewn camouflage carbon felt car cover is spread out horizontally, debris is removed, thread ends are cut, it is rolled up, and packed into packaging bags to complete the entire camouflage car cover preparation process.
[0091] For further explanation, the following embodiments are provided:
[0092] Embodiment 1:
[0093] 1. Raw material pretreatment
[0094] (1) The raw material (B-grade carbon fiber felt) is cleaned and pretreated. The main purpose is to remove the active agent and adsorbed water remaining on the surface of the powder during the preparation process to reduce the adverse effects of impurities on the material properties in the later stage of the reaction. The present invention heats the raw material to 120°C for 2 hours, then ultrasonically cleans the raw material with acetone and ethanol, and filters and dries it at room temperature.
[0095] (2) Functionalize the surface of carbon fiber felt to improve the adhesion of subsequent surface functional coatings. Add distilled water: carbon fiber felt: high-purity carbon balls in a mass fraction ratio of 10L: 100g: 200g into a magnetic stirring container, and stir slowly at 600 rpm for 5 hours to ensure that the carbon fiber felt and carbon balls rotate in a circle in the distilled water. After the reaction is completed, remove the carbon fiber felt and rinse it with deionized water 5 times. Finally, put it in a 50°C oven to dry for 16 hours and place it in a dry and cool place for use; filter the remaining carbon balls from the remaining solution and reuse them after the quality is determined to meet the parameter requirements.
[0096] (3) After the previous step is completed, the carbon fiber felt is in the same surface functional pretreatment state as a whole. The focus of this process is to treat the upper and lower surfaces of the carbon fiber felt. A precision spray control system is used to spray the upper surface of the carbon fiber felt at a rate of 2.5 g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry at room temperature for 8 minutes, and then spray the surface of the carbon fiber at 2.5g / m 2 Spray density, spray saturated sodium chloride solution evenly, keep horizontal drying at room temperature for 8 minutes, place in a cool and dark place (ambient humidity> 20%), rinse with deionized water 4 times after 196 hours, and place in a dry and cool place for use. Through this process, the key functional modification of the upper and lower surfaces of the carbon fiber felt is achieved.
[0097] 2. Cutting composite carbon felt and skeleton mesh
[0098] (1) Cut the composite carbon felt. According to the layout size, the thickness of the carbon fiber felt is controlled at 8 mm, and the edge of the fabric is neat and burr-free.
[0099] (2) The mesh specifications of the skeleton net must be accurate, and the number of meshes must be calculated accurately when cutting. The size of each skeleton mesh is 50mm×50mm.
[0100] 3. Infrared camouflage treatment on the upper surface of carbon fiber felt
[0101] (1) The infrared coating is dispersed at a speed of 100 rpm for 10 minutes, and the infrared camouflage coating is sprayed on the upper surface of the carbon fiber felt using the following spraying process.
[0102]
[0103] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 4 hours. After the coating surface is dry, fold it and store it in a dry and ventilated place for 96 hours to complete the infrared camouflage treatment process on the surface of the carbon fiber felt.
[0104] 4. Electromagnetic shielding treatment on the lower surface of carbon fiber felt
[0105] (1) The carbon nano conductive coating was dispersed at a speed of 100 rpm for 5 minutes, and the electromagnetic shielding coating was sprayed on the lower surface of the carbon fiber felt using the following spraying process.
[0106]
[0107] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 2 hours. After the coating surface is dry, it can be folded and stored in a dry and ventilated place for 48 hours to complete the electromagnetic shielding treatment process of the lower surface of the carbon fiber felt.
[0108] Note: Step 4 should be performed 24 hours after step 3. The order of steps 3 and 4 cannot be reversed.
[0109] 5. Cut Flowers
[0110] (1) First, the cutting notch size should be R15mm according to the design drawing requirements, and the spliced carbon fiber felt should be placed on the cutting machine.
[0111] (2) Lay the carbon fiber felt flat, with 25 layers per plate. The edges of the fabric should be neat and the upper and lower errors should not be greater than 5 mm. Unqualified or substandard carbon fiber felts should not be cut or punched. After stacking the carbon fiber felts, place them neatly and parallelly on the corresponding flower cutting machine as required, ready for cutting.
[0112] (3) Flower cutter setting data
[0113] Flower cutting stroke: 200mm, pressure 0.20MPa.
[0114] 6. Tie into a net
[0115] (1) Tiling
[0116] First, spread the carbon fiber felt on the work surface, then spread the skeleton mesh on the carbon fiber felt, and adjust it to be even and flat.
[0117] (2) Binding
[0118] Use binding wire for binding. The binding structure is diamond-shaped. The binding density is controlled at 25 knots per square meter. The knotting type is self-tightening. One knot is tied 5 times. The direction of winding is positive and negative. Tie it tightly and leave the knot 25mm long.
[0119] 7. Hemming
[0120] (1) The carbon fiber felt and the skeleton net should be aligned up and down, and the two layers together with the edge rope should be completely wrapped in the edge strip. The sewing stitches should be even, and there should be no skipped stitches or broken threads. The seams between the connecting ring rope and the skeleton net should be re-sewn 3 times, and the repeated stitch length should be completely covered. The connecting ring rope should not be missing, and the sewing stitches should be flat and firm.
[0121] (2) The length and spacing of the connecting rings must be within the tolerance range. The length of the connecting ring rope is 200mm and the spacing of the connecting ring rope is 200mm.
[0122] (3) Make cuts about 25 mm deep every 150 mm on the fabric strip to facilitate the rope production.
[0123] (4) When hemming, the edge rope joints are sewn at the center of any length of the four sides. Sewing at the four corners is not allowed.
[0124] 8 Finished product inspection and packaging
[0125] The sewn camouflage carbon felt car cover is spread out horizontally, debris is removed, thread ends are cut, the car cover is rolled up, and the car cover is packed in a packaging bag to complete the entire camouflage car cover preparation process.
[0126] The sample prepared in Example 1 can significantly reduce the infrared energy difference between the target and the background, improve the consistency of the infrared characteristics of the vehicle and the background, and the average thermal radiation temperature difference with the typical background is no more than 4°C.
[0127] like Fig. 9 As shown, the product has excellent radar wave stealth performance.
[0128] Embodiment 2:
[0129] 1. Raw material pretreatment
[0130] (1) The raw material (grade A carbon fiber felt) is cleaned and pretreated. The main purpose is to remove the active agent and adsorbed water remaining on the surface of the powder during the preparation process to reduce the adverse effects of impurities on the material properties in the later stage of the reaction. The present invention heats the raw material to 140°C for 1.5 hours, then ultrasonically cleans the raw material with acetone and ethanol, and filters and dries it at room temperature.
[0131] (2) Functionalize the surface of carbon fiber felt to improve the adhesion of subsequent surface functional coatings. Add distilled water: carbon fiber felt: high-purity carbon balls in a mass fraction ratio of 10L: 100g: 200g into a magnetic stirring container, and stir slowly at 300 rpm for 10 hours to ensure that the carbon fiber felt and carbon balls rotate in a circle in the distilled water. After the reaction is completed, remove the carbon fiber felt and rinse it with deionized water three times. Finally, put it in a 50°C oven to dry for 12 hours and place it in a dry and cool place for use; filter the remaining carbon balls from the remaining solution and reuse them after the quality is determined to meet the parameter requirements.
[0132] (3) After the previous step is completed, the carbon fiber felt is in the same surface functional pretreatment state as a whole. The focus of this process is to treat the upper and lower surfaces of the carbon fiber felt. A precision spray control system is used to spray the upper surface of the carbon fiber felt at a rate of 2g / m 2Spray the saturated sodium chloride solution evenly, keep it horizontally dry for 5 minutes at room temperature, and then spray the surface of the carbon fiber at 2g / m 2 Spray the saturated sodium chloride solution evenly at a spray density of 10000, keep it horizontally dry for 5 minutes at room temperature, place it in a cool and dark place (ambient humidity>20%), rinse it with deionized water 3 times after 144 hours, and place it in a dry and cool place for use. Through this process, the key functional modification of the upper and lower surfaces of the carbon fiber felt is achieved.
[0133] 2. Cutting composite carbon felt and skeleton mesh
[0134] (1) Cut the composite carbon felt. According to the layout size, the thickness of the carbon fiber felt is controlled at 6 mm, and the edge of the fabric is neat and burr-free.
[0135] (2) The mesh specifications of the skeleton net must be accurate, and the number of meshes must be calculated accurately when cutting. The size of each skeleton mesh is 60mm×60mm.
[0136] 3. Infrared camouflage treatment on the upper surface of carbon fiber felt
[0137] (1) The infrared coating is dispersed at a speed of 100 rpm for 15 minutes, and the infrared camouflage coating is sprayed on the upper surface of the carbon fiber felt using the following spraying process.
[0138]
[0139] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 4 hours. After the coating surface is dry, fold it and store it in a dry and ventilated place for 96 hours to complete the infrared camouflage treatment process on the surface of the carbon fiber felt.
[0140] 4. Electromagnetic shielding treatment on the lower surface of carbon fiber felt
[0141] (1) The carbon nano conductive coating was dispersed at a speed of 100 rpm for 8 minutes, and the electromagnetic shielding coating was sprayed on the lower surface of the carbon fiber felt using the following spraying process.
[0142]
[0143] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 2 hours. After the coating surface is dry, it can be folded and stored in a dry and ventilated place for 48 hours to complete the electromagnetic shielding treatment process of the lower surface of the carbon fiber felt.
[0144] Note: Step 4 should be performed 24 hours after step 3. The order of steps 3 and 4 cannot be reversed.
[0145] 5. Cut Flowers
[0146] (1) First, according to the design drawing requirements, the cutting notch size should be R18mm, and the spliced carbon fiber felt should be placed on the cutting machine.
[0147] (2) Lay the carbon fiber felt flat, with 30 layers per plate. The edges of the fabric should be neat and the upper and lower errors should not be greater than 5 mm. Unqualified or substandard carbon fiber felts should not be cut or punched. After stacking, the carbon fiber felts should be neatly and parallelly placed on the corresponding flower cutting machine as required, ready for cutting.
[0148] (3) Flower cutter setting data
[0149] Flower cutting stroke: 180mm, pressure 0.15MPa.
[0150] 6. Tie into a net
[0151] (1) Tiling
[0152] First, spread the carbon fiber felt on the work surface, then spread the skeleton mesh on the carbon fiber felt, and adjust it to be even and flat.
[0153] (2) Binding
[0154] Use binding wire for binding. The binding structure is diamond-shaped. The binding density is controlled at 30 knots per square meter. The knotting type is self-tightening, with one knot tied 4 times. The direction of winding is positive and negative. Tie it tightly and leave the knot 20mm long.
[0155] 7. Hemming
[0156] (1) The carbon fiber felt and the skeleton net should be aligned up and down, and the two layers together with the edge rope should be completely wrapped in the edge strip. The sewing stitches should be even, and there should be no skipped stitches or broken threads. The seams between the connecting ring rope and the skeleton net should be re-sewn 5 times, and the repeated stitch length should be completely covered. The connecting ring rope should not be missing, and the sewing stitches should be flat and firm.
[0157] (2) The length and spacing of the connecting rings must be within the tolerance range. The length of the connecting ring rope is 220mm, and the spacing of the connecting ring rope is 220mm.
[0158] (3) Make cuts about 15 mm deep every 250 mm on the fabric strip to facilitate the rope production.
[0159] (4) When hemming, the edge rope joints are sewn at the center of any length of the four sides. Sewing at the four corners is not allowed.
[0160] 8 Finished product inspection and packaging
[0161] The sewn camouflage carbon felt car cover is spread out horizontally, debris is removed, thread ends are cut, the car cover is rolled up, and the car cover is packed in a packaging bag to complete the entire camouflage car cover preparation process.
[0162] The sample prepared in Example 2 can significantly reduce the infrared energy difference between the target and the background, improve the consistency of the infrared characteristics of the vehicle and the background, and the average thermal radiation temperature difference with the typical background is no more than 4°C.
[0163] like Fig.10 As shown, the product has excellent radar wave stealth performance.
[0164] Embodiment three:
[0165] 1. Raw material pretreatment
[0166] (1) The raw material (C-grade carbon fiber felt) is cleaned and pretreated. The main purpose is to remove the active agent and adsorbed water remaining on the surface of the powder during the preparation process to reduce the adverse effects of impurities on the material properties in the later stage of the reaction. The present invention heats the raw material to 160°C for 1.0 hour, then ultrasonically cleans the raw material with acetone and ethanol, and filters and dries it at room temperature.
[0167] (2) Functionalize the surface of carbon fiber felt to improve the adhesion of subsequent surface functional coatings. Add distilled water: carbon fiber felt: high-purity carbon balls in a mass fraction ratio of 10L: 100g: 200g into a magnetic stirring container, and stir slowly at 400 rpm for 8 hours to ensure that the carbon fiber felt and carbon balls rotate in a circle in the distilled water. After the reaction is completed, remove the carbon fiber felt and rinse it with deionized water 4 times. Finally, put it in a 50°C oven to dry for 14 hours and place it in a dry and cool place for use; filter the remaining carbon balls from the remaining solution and reuse them after the quality is determined to meet the parameter requirements.
[0168] (3) After the previous step, the carbon fiber felt is in the same surface functional pretreatment state. The focus of this process is to treat the upper and lower surfaces of the carbon fiber felt. A precision spray control system is used to spray the upper surface of the carbon fiber felt at a rate of 3g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry for 10 minutes at room temperature, and then spray the surface of the carbon fiber at 3g / m 2 Spray the saturated sodium chloride solution evenly at a spray density of 10000, keep it horizontally dry at room temperature for 10 minutes, place it in a cool and dark place (ambient humidity>20%), rinse it with deionized water 5 times after 240 hours, and place it in a dry and cool place for use. Through this process, the key functional modification of the upper and lower surfaces of the carbon fiber felt is achieved.
[0169] 2. Cutting composite carbon felt and skeleton mesh
[0170] (1) Cut the composite carbon felt. According to the layout size, the thickness of the carbon fiber felt is controlled at 5 mm, and the edge of the fabric is neat and burr-free.
[0171] (2) The mesh specifications of the skeleton net must be accurate, and the number of meshes must be calculated accurately when cutting. The size of each skeleton mesh is 40mm×40mm.
[0172] 3. Infrared camouflage treatment on the upper surface of carbon fiber felt
[0173] (1) The infrared coating is dispersed at a speed of 100 rpm for 20 minutes, and the infrared camouflage coating is sprayed on the upper surface of the carbon fiber felt using the following spraying process.
[0174]
[0175] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 4 hours. After the coating surface is dry, fold it and store it in a dry and ventilated place for 96 hours to complete the infrared camouflage treatment process on the surface of the carbon fiber felt.
[0176] 4. Electromagnetic shielding treatment on the lower surface of carbon fiber felt
[0177] (1) The carbon nano conductive coating was dispersed at a speed of 100 rpm for 10 minutes, and the electromagnetic shielding coating was sprayed on the lower surface of the carbon fiber felt using the following spraying process.
[0178]
[0179] (2) After spraying, place the carbon fiber felt horizontally in a clean and ventilated place for 2 hours. After the coating surface is dry, it can be folded and stored in a dry and ventilated place for 48 hours to complete the electromagnetic shielding treatment process of the lower surface of the carbon fiber felt.
[0180] Note: Step 4 should be performed 24 hours after step 3. The order of steps 3 and 4 cannot be reversed.
[0181] 5. Cut Flowers
[0182] (1) First, the cutting notch size should be R20mm according to the design drawing requirements, and the spliced carbon fiber felt should be placed on the cutting machine.
[0183] (2) Lay the carbon fiber felt flat, with 20 layers per plate. The edges of the fabric should be neat and the upper and lower errors should not be greater than 5 mm. Unqualified or substandard carbon fiber felts should not be cut or punched. After stacking, the carbon fiber felts should be neatly and parallelly placed on the corresponding flower cutting machine as required, ready for cutting.
[0184] (3) Flower cutter setting data
[0185] Flower cutting stroke: 180mm, pressure 0.30MPa.
[0186] 6. Tie into a net
[0187] (1) Tiling
[0188] First, spread the carbon fiber felt on the work surface, then spread the skeleton mesh on the carbon fiber felt, and adjust it to be even and flat.
[0189] (2) Binding
[0190] Use binding wire for binding. The binding structure is diamond-shaped. The binding density is controlled at 35 knots per square meter. The knotting type is self-tightening. One knot is tied 3 times. The direction of winding is positive and negative. Tie it tightly and leave the knot 30mm long.
[0191] 7. Hemming
[0192] (1) The carbon fiber felt and the skeleton net should be aligned up and down, and the two layers together with the edge rope should be completely wrapped in the edge strip. The sewing stitches should be even, and there should be no skipped stitches or broken threads. The seams between the connecting ring rope and the skeleton net should be re-sewn 4 times, and the repeated stitch length should be completely covered. The connecting ring rope should not be missing, and the sewing stitches should be flat and firm.
[0193] (2) The length and spacing of the connecting rings must be within the tolerance range. The length of the connecting ring rope is 180mm, and the spacing of the connecting ring rope is 180mm.
[0194] (3) Make cuts about 20 mm deep every 200 mm on the fabric strip to facilitate the rope production.
[0195] (4) When hemming, the edge rope joints are sewn at the center of any length of the four sides. Sewing at the four corners is not allowed.
[0196] 8 Finished product inspection and packaging
[0197] The sewn camouflage carbon felt car cover is spread out horizontally, debris is removed, thread ends are cut, the car cover is rolled up, and the car cover is packed in a packaging bag to complete the entire camouflage car cover preparation process.
[0198] The sample prepared in Example 3 can significantly reduce the infrared energy difference between the target and the background, improve the consistency of the infrared characteristics of the vehicle and the background, and the average thermal radiation temperature difference with the typical background is no more than 4°C.
[0199] like Fig.11 As shown, the product has excellent radar wave stealth performance.
[0200] Only the preferred embodiments of the present invention have been described in detail above, but the present invention is not limited to the above embodiments.
Claims
1. A method for preparing an infrared broadband radar flexible camouflage carbon felt car cover, characterized in that: The following steps are involved: S1. Raw material pretreatment: The carbon fiber felt is sequentially subjected to cleaning pretreatment, carbon ball stirring pretreatment, and saturated sodium chloride solution spraying process; S2, cutting: cutting the skeleton net and cutting the carbon fiber felt processed in step S1; S3, infrared camouflage treatment: performing infrared camouflage treatment on the upper surface of the carbon fiber felt cut in step S2; S4, electromagnetic shielding treatment: performing electromagnetic shielding treatment on the lower surface of the carbon fiber felt after the infrared camouflage treatment in step S3; S5, cutting and binding the carbon fiber felt after the electromagnetic shielding treatment into a net; and binding the carbon fiber felt after the net and the skeleton net cut in step S2 for edge wrapping.
2. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In step S1, the cleaning pretreatment refers to: firstly treating the carbon fiber felt by heating and drying for 1 to 2 hours; then removing impurities on the surface of the carbon fiber felt by solvent cleaning, and finally performing drying treatment.
3. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In step S1, the carbon ball stirring pretreatment refers to: adding distilled water, carbon fiber felt and high-purity carbon balls into a magnetic stirring container, stirring slowly at 300 to 600 rpm for 5 to 10 hours, and forming microporous defects on the surface of the carbon fiber felt through mutual collision and friction between the carbon balls and the carbon fiber felt.
4. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In step S1, the saturated sodium chloride solution spraying process refers to: evenly spraying the saturated sodium chloride solution on the upper and lower surfaces of the carbon fiber felt, keeping it horizontally dry at room temperature, placing it in a cool and dark place for a period of time, and then rinsing it with deionized water.
5. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 4, characterized in that: The surface of the carbon fiber felt is 2-3g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry for 5 to 10 minutes at room temperature, and then spray the surface of the carbon fiber at 2 to 3 g / m 2 Spray density, evenly spray saturated sodium chloride solution, keep it horizontally dry at room temperature for 5 to 10 minutes, place it in a cool and dark place (ambient humidity> 20%) for 144 to 240 hours, rinse it with deionized water 3 to 5 times, and place it in a dry and cool place for use.
6. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In the step S3: the infrared camouflage paint is dispersed for 10 to 20 minutes, and then the infrared camouflage paint is sprayed on the upper surface of the carbon fiber felt; After spraying, place the carbon fiber felt horizontally in a clean and ventilated place. After the coating surface is dry, fold it and store it in a dry and ventilated place to complete the infrared camouflage treatment process on the surface of the carbon fiber felt.
7. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In the step S4: the carbon nano conductive coating is dispersed for 5 to 10 minutes, and then the conductive coating is sprayed on the lower surface of the carbon fiber felt; After spraying, place the carbon fiber felt horizontally in a clean and ventilated place. After the coating surface is dry, fold it and store it in a dry and ventilated place to complete the electromagnetic shielding treatment process on the lower surface of the carbon fiber felt.
8. A method for preparing an infrared broadband radar flexible camouflage carbon felt car cover according to any one of claims 1, 6 and 7, characterized in that: The step S4 is performed sequentially 24 hours after the step S3 is completed.
9. The method for preparing a infrared broadband radar flexible camouflage carbon felt car cover according to claim 1, characterized in that: In step S5, the flower cutting refers to: placing the spliced carbon fiber felt on a flower cutting machine; laying the carbon fiber felt flat, laying 20 to 30 layers per plate, the edges of the fabric should be neat, and the upper and lower errors should not be greater than 5mm; after the carbon fiber felt is stacked, it is neatly and parallelly placed on a flower cutting machine of the corresponding flower pattern as required to cut the flower; The binding into a net refers to: spreading the carbon fiber felt flat on the work surface, and then spreading the skeleton net on the carbon fiber felt, and adjusting it to be even and flat; using binding wire for binding, the binding structure is diamond-shaped, the binding density, the number of bindings per square meter is controlled at 25 to 35 knots, the knotting type is self-tightening, one knot is tied 3 to 5 times, the direction of winding is positive and negative, it is tied and tightened, and the knot head is left 20mm to 30mm long.
10. The method for preparing a flexible camouflage carbon felt car cover for infrared broadband radar according to claim 1, characterized in that: In step S5, the hemming means: aligning the carbon fiber felt and the skeleton net, and completely wrapping the two layers together with the edge rope into the hemming strip, sewing the stitches evenly, without skipped stitches or broken threads; the sutures of the connecting loop rope and the skeleton net should be re-sewn 3-5 times, the repeated stitch length should be completely covered, the connecting loop rope should not be missing, and the sewing stitches should be flat and firm; The length and spacing of the connecting rings must be within the tolerance range, the length of the connecting ring rope is 200mm±20mm, and the spacing of the connecting ring rope is 200mm±20mm; Make cuts of about 15 to 25 mm in depth every 150 to 250 mm on the fabric strips to facilitate the rope production; When hemming, the edge rope joints are sewn at the center of any length of the four sides, and sewing at the four corners is not allowed.
Citation Information
Patent Citations
Flexible wave-absorbing non-woven fabric and preparation method thereof
CN106079673A
Single-layer coating carbon fiber fabric for electromagnetic shielding field and preparation method thereof
CN111705514A
Carbon fiber radar wave-absorbing material
CN112941905A
Multiband-radar stealth compatible multifunctional camouflage net and preparation method thereof
CN115752095A
MXene modified carbon fiber non-woven felt with multi-layer structure and preparation method of MXene modified carbon fiber non-woven felt
CN117947633A