Method for rapidly evaluating corrosion resistance of zinc coating
By accelerating corrosion tests by using color developer and specific corrosion solutions on the galvanized layer, the problems of long test cycles and single evaluation angles in the prior art are solved, and a rapid and quantitative corrosion resistance evaluation of galvanized layer is achieved, providing Scientific basis for optimizing anti-corrosion measures.
Patent Information
- Application Number
- CN202410927685.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-26
AI Technical Summary
The existing accelerated corrosion test detection methods have problems such as long test cycle, single corrosion resistance evaluation angle, difficulty in quantification, and insufficient real-time data monitoring, making it difficult to effectively evaluate the corrosion resistance of the galvanized layer.
The corrosion solution and supplementary solution are soaked with a base containing color developer, and the reaction is stirred by a constant temperature shaker to adjust the pH value and temperature, and the absorbance of the corrosion sample solution is measured to evaluate the corrosion resistance of the galvanized layer. The corrosion resistance of the sulfosalicylic acid is used. Components such as acetic acid, sodium nitrate and sodium chloride accelerate the corrosion process of the zinc layer.
It has achieved the simulation of material corrosion conditions in a short time, quickly evaluated the corrosion resistance of the galvanized layer, provided scientific basis to optimize corrosion protection measures, and reduced safety and economic losses caused by corrosion.
Smart Images

Figure CN119023547A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of corrosion resistance detection of zinc coatings, and in particular relates to a method for rapidly evaluating the corrosion resistance of zinc coatings. Background Art
[0002] Corrosion tests include laboratory corrosion tests and field corrosion tests. Laboratory corrosion tests can be divided into room temperature or heated liquid immersion corrosion and gas corrosion and salt spray tests. Field corrosion tests are also diverse, such as atmospheric corrosion, seawater and freshwater immersion, soil corrosion, coupon tests, etc. According to the nature of the corrosive medium, it can be divided into acidic, alkaline, neutral salt corrosion and other types.
[0003] The corrosion test conditions need to be formulated according to the technical standards of the test materials or the conditions of use of the materials. The pH value of the solution, the amount of dissolved gas, the concentration of dissolved ions, the solution temperature and flow rate, etc., will directly affect the corrosion reaction of the material. It is generally believed that the dissolved gas in the solution, especially the oxygen content in the neutral solution, has a great influence on the cathode reaction of the corrosion process, and the liquid temperature not only affects the reaction speed, but also has a certain influence on the reaction type.
[0004] Current accelerated corrosion test methods include:
[0005] 1. Liquid immersion method: This test method is suitable for occasions where the performance of materials under periodic or alternating environmental conditions needs to be evaluated, such as materials in the fields of ocean, automobile, construction and bridge. It is particularly important for studying the corrosion behavior of materials under cyclic stress, the peeling of coatings, and the fatigue life of materials. In order to achieve dry-wet alternation, the sample can be alternately immersed in and taken out of the solution; or the sample can be fixed and the solution can be raised and lowered relative to the sample. It is usually easier to move the sample than to move the corrosive medium.
[0006] This test method is suitable for situations where the performance of materials under periodic or alternating environmental conditions needs to be evaluated, such as materials in the fields of ocean, automobile, construction and bridge. It is particularly important for studying the corrosion behavior of materials under cyclic stress, the peeling of coatings, and the fatigue life of materials. In order to achieve dry-wet alternation, the specimen can be alternately immersed in and out of the solution; or the specimen can be fixed and the solution can be raised and lowered relative to the specimen. It is usually easier to move the specimen than to move the corrosive medium.
[0007] 2. Neutral salt spray test: Neutral salt spray test is a commonly used artificial accelerated corrosion test. It simulates the coastal atmospheric environment, where the warm sea evaporates into the cold air and the tiny droplets containing chloride ions splash into the space under the impact of waves, forming a fine mist medium to corrode the metal. A certain concentration of sodium chloride solution is used to spray in a fine mist under pressure. Since the mist particles fall evenly on the surface of the sample and continuously maintain the renewal of the liquid film, the corrosion of the material conforms to the basic principle of atmospheric corrosion and achieves accelerated corrosion. The neutral salt spray test checks the metal matrix or surface treatment layer's resistance to neutral salt spray corrosion, and can also test the discontinuity of the surface treatment layer (such as pores and other defects).
[0008] However, the neutral salt spray test cannot perfectly simulate the corrosion of metals under atmospheric conditions. In addition, there are many factors that affect corrosion, which makes the test conditions difficult to control, etc., and the reproducibility is often poor, so it can only be used as a comparison of the relative corrosion resistance of the same type of materials under this condition. Practice shows that it has a better corrosion resistance effect on anodic coatings (such as zinc and cadmium layers on steel substrates), while for cathodic coatings, it can only reveal the porosity and defect degree of the coating, indirectly reflecting the corrosion resistance of the coating.
[0009] 3. Copper salt accelerated acetate spray test: Copper salt accelerated acetate spray test is an improved method of neutral salt water spray test. Because it is acidified with acetic acid in sodium chloride solution and copper chloride is added to increase the corrosion rate and effect on certain metal coatings, it has achieved good results that the corrosion mode of cathodic coating on steel substrate is close to the actual environment. Compared with neutral salt water spray, CASS method not only accelerates the corrosion rate, but also has better reproducibility, so it is gradually replacing neutral salt water spray for corrosion resistance test of cathodic coating. This method is suitable for corrosion resistance test of cathodic coating (copper, nickel, chromium coating, etc.) on steel substrate and anodic oxide film on aluminum or aluminum alloy.
[0010] The copper salt accelerated acetate spray test equipment is roughly the same as the salt spray test equipment, except that the high temperature resistance of the box is higher (50±1℃). At present, in addition to the equipment specifically used for CASS testing, there are also equipment that is common to salt spray testing. Except for the test temperature of 50±1℃, other conditions are the same as those of the salt spray test.
[0011] Through the analysis of existing relevant accelerated corrosion test detection methods, it is not difficult to see that the existing methods have the problems of long test cycle, single angle of analyzing the corrosion resistance of materials, mainly qualitative evaluation results, and difficult to quantify. In addition, the real-time nature of data monitoring is insufficient. In view of the above shortcomings, it is necessary to develop an evaluation method for the corrosion resistance of galvanized layers. Summary of the invention
[0012] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0013] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0014] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for quickly evaluating the corrosion resistance of a galvanized layer.
[0015] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:
[0016] After pretreatment, the galvanized steel sheet samples containing the galvanized layer are placed in parallel and immersed in a basic immersion corrosion solution containing a color developer, and the reaction is stirred on a constant temperature shaker. During the reaction, a supplementary solution containing a color developer is added to adjust the pH to the initial pH, and the reaction is performed for 6 to 8 hours to obtain a corrosion sample and a corrosion sample solution;
[0017] The absorbance of the corrosion sample solution is measured by a spectrophotometer. The greater the absorbance, the higher the iron content in the corrosion sample solution, and the more serious the corrosion, which means that the corrosion resistance of the galvanized layer is evaluated.
[0018] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the basic immersion corrosion solution containing a developer comprises the following components:
[0019] 2% color developer + 5% HAc + 0.05% NaNO3 + 0.8% + 5% NaCl.
[0020] 2% Sulfosalicylic acid: Sulfosalicylic acid is an organic compound containing a sulfonic acid group, which may have a certain chelating ability and can form a stable complex with metal ions. For galvanized steel, it may increase the rate of zinc dissolution because it can form a complex with zinc ions, thereby removing zinc ions from the metal surface, breaking the passivation state of the surface and accelerating the corrosion process.
[0021] 5% HAc (acetic acid): Acetic acid is a weak organic acid that can dissolve the zinc layer to form zinc acetate and may further corrode the exposed steel substrate. The presence of acetic acid lowers the local pH and facilitates the dissolution of zinc.
[0022] 0.05% NaNO3 (sodium nitrate): Sodium nitrate releases nitrate (NO 3-), which can participate in the electrochemical corrosion process as oxidants and promote the anodic dissolution process of zinc and iron. Nitric acid provides additional nitrate ions, which participate in the electrochemical corrosion process and promote metal dissolution.
[0023] 0.8% NaNO3 (sodium persulfate): Sodium persulfate is a strong oxidant that can accelerate corrosion by oxidizing the metal surface. In electrochemical corrosion, it may promote the oxygen reduction reaction in the cathode area, thereby increasing the dissolution of zinc in the anode area.
[0024] 5% NaCl (sodium chloride): Sodium chloride provides chloride ions (Cl-), which are particularly prone to penetrating the protective layer on the metal surface, causing pitting and crevice corrosion, especially when the zinc layer has been locally damaged.
[0025] Combining the mechanisms of action of these components, it is possible to predict the corrosion of galvanized steel in this solution:
[0026] Rapid dissolution of zinc: The zinc coating may corrode rapidly due to the presence of various components that promote zinc dissolution (sulfosalicylic acid, acetic acid, nitrates, and persulfates).
[0027] Pitting and localized corrosion: Chloride ions can cause pitting on the zinc coating, especially under the action of sulfosalicylic acid and oxidants, these pitting can quickly evolve into localized corrosion.
[0028] Corrosion of underlying steel: Once the galvanized layer is penetrated, the exposed steel will begin to corrode, forming iron extracts, especially in the presence of acetic acid and sodium chloride.
[0029] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the initial pH of the basic immersion corrosion solution is 2 to 2.6.
[0030] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the initial pH of the basic immersion corrosion solution is 2.1.
[0031] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the initial pH of the basic immersion corrosion solution is adjusted by a saturated Na2CO3 solution.
[0032] As a preferred embodiment of the method for evaluating the corrosion resistance of the galvanized layer of the present invention, the replenishing solution comprises the following components: 30% developer + 0.5% HNO3 + 1% Na2S2O8.
[0033] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the replenishing liquid is added when the pH of the basic immersion corrosion solution reaches 3.0.
[0034] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a zinc coating according to the present invention, the color developer is 5-sulfosalicylic acid dihydrate.
[0035] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer of the present invention, the reaction temperature of the stirring reaction on a constant temperature shaking table is 35-40°C.
[0036] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer according to the present invention, the stirring speed of the constant temperature shaking table stirring reaction is 50 to 200 rpm.
[0037] As a preferred embodiment of the method for rapidly evaluating the corrosion resistance of a galvanized layer of the present invention, the content of iron in the corrosion sample solution is calculated by establishing a standard curve.
[0038] Beneficial effects of the present invention:
[0039] The present invention proposes a method for quickly evaluating the corrosion resistance of a galvanized layer. By changing the corrosion conditions to accelerate the corrosion process of the material, it can simulate the corrosion of the material in a relatively short period of time. This method is of great significance for evaluating the corrosion resistance of the galvanized layer, predicting its lifespan, and optimizing anti-corrosion measures. Through accelerated corrosion testing, we can obtain data on the corrosion of the material more quickly, so that we can take corresponding protective measures or replace damaged materials in time to reduce safety accidents and economic losses caused by corrosion. This process is simple, rapid and cost-effective, and is very suitable for rapid testing under field or laboratory conditions. Through the research of the present invention, we can not only evaluate the corrosion resistance of the galvanized layer, but also explore new methods and materials to improve the corrosion resistance of the galvanized layer, providing a scientific basis for the design, production and application of the galvanized layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0041] Figure 1 This is the standard working curve of iron ions in Example 2 of the present invention.
[0042] Figure 2 The corrosion sample images are obtained after the corrosion test is carried out under different types of basic corrosion solution conditions in Example 2 of the present invention.
[0043] Figure 3This is an absorbance test graph of the corrosion sample solution obtained after the corrosion test was carried out under different types of basic corrosion solution conditions in Example 2 of the present invention.
[0044] Figure 4 This is a test graph of absorbance of the corrosion sample solution obtained after the corrosion test under different pH conditions of the corrosion solution in Example 3 of the present invention.
[0045] Figure 5 This is an absorbance test graph of the corrosion sample solution obtained after the corrosion test at different corrosion reaction temperatures in Example 5 of the present invention.
[0046] Figure 6 This is an absorbance test graph of the corrosion sample solution obtained after the corrosion test was carried out at different corrosion reaction speeds in Example 6 of the present invention.
[0047] Figure 7 is Fe in Example 7 of the present invention 3+ Standard curve graph.
[0048] Figure 8 The different color developers in Example 7 of the present invention are 2+ Anti-interference ability comparison chart.
[0049] Fig. 9 This is a physical picture of the solution of different color developers at different pH values in Example 7 of the present invention.
[0050] Fig.10 This is a test diagram of absorbance of different color developers at different pH values in Example 7 of the present invention.
[0051] Fig.11 This is a graph showing the test results of the metal impurity resistance of sulfosalicylic acid in Example 7 of the present invention.
[0052] Fig.12 This is a graph showing the antioxidant capacity test results of sulfosalicylic acid in Example 7 of the present invention.
[0053] Fig.13 This is a comparison chart of the anti-interference capabilities of o-phenanthroline and sulfosalicylic acid as color developers in Example 7 of the present invention. DETAILED DESCRIPTION
[0054] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0055] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0056] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0057] The material used in this test is galvanized steel, and the galvanized steel is 150mm*25mm*4mm with holes The sheet material has a zinc coating thickness of 40 to 120 μm and the zinc coating is pure zinc (more than 99.995%).
[0058] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art. The list of drugs used is shown in Table 1.
[0059] Table 1
[0060] Drug Name source <![CDATA[Sodium persulfate (Na2S2O8)]]> Shanghai Sinopharm Group Sodium chloride (NaCl) Shanghai Sinopharm Group <![CDATA[Sodium nitrate (NaNO3)]]> Shanghai Sinopharm Group <![CDATA[Sodium bisulfate (NaHSO4)]]> Shanghai Sinopharm Group <![CDATA[Ethanol (CH3CH2OH)]]> Shanghai Sinopharm Group <![CDATA[Acetone (CH3COCH3)]]> Shanghai Sinopharm Group <![CDATA[Concentrated nitric acid (HNO3)]]> Shanghai Sinopharm Group 5-Sulfosalicylic acid dihydrate / Sulfosalicylic acid(Ssal) Shanghai Sinopharm Group Potassium thiocyanate Shanghai Sinopharm Group Iron standard solution Shanghai Sinopharm Group
[0061] The list of instruments used is shown in Table 2.
[0062] Table 2
[0063] Instrument Name model Company and Origin UV-Vis Spectrophotometer UV-5200 Shanghai Yuanxi Instrument Co., Ltd. pH meter 7100 BPH
[0064] Example 1
[0065] This embodiment provides a method for evaluating the corrosion resistance of a galvanized layer, specifically:
[0066] S1: Pretreatment of galvanized steel sheet samples containing zinc coating;
[0067] The samples to be tested are cleaned with anhydrous ethanol (to remove oil), deionized water, and anhydrous ethanol (to remove water) in sequence, and then dried with cold air from a hair dryer, thus achieving sample pretreatment;
[0068] S2: preparing a basic immersion corrosion solution containing a color developer and a replenisher containing a color developer;
[0069] Prepare a basic immersion corrosion solution with the following components:
[0070] 2% 5-sulfosalicylic acid dihydrate + 5% HAc + 0.05% NaNO3 + 0.8% Na2S2O8 + 5% NaC.
[0071] Prepare a replenisher containing the colorimetric reagent according to the following composition:
[0072] 30% dihydrate-5-sulfosalicylic acid + 0.5% HNO3 + 1% Na2S2O 8;
[0073] S3: Conduct corrosion reaction experiment;
[0074] After pretreatment, the galvanized steel sheet samples containing the zinc coating were placed in parallel in the basic immersion corrosion solution containing the developer, so that the samples were completely immersed in the solution, the pH value was adjusted to 2.1 using Na2CO3, and the constant temperature shaker was used for stirring and heating reaction, the heating temperature was 40°C, and the stirring speed was 50rpm;
[0075] During the reaction, the pH of the reaction solution was tested in real time. When the pH reached 3, a supplementary solution containing a color developer was added, and the pH was adjusted to 2.1 before continuing the reaction. The total reaction time was 6 h, and a corrosion sample and a corrosion sample solution were obtained.
[0076] S4: Test the absorbance of the corrosion sample solution to determine the corrosion resistance of the sample;
[0077] Using the basic immersion corrosion solution G without color developer as solvent, 1, 2, 4, 6, and 8 μg / ml of Fe 3+ The standard solution uses dihydrated 5-sulfosalicylic acid as the color developer and G as the reference solution. The spectrophotometer is used to scan the 400-800nm band and select the maximum absorption wavelength of 456nm. At the wavelength of 456nm, different concentrations of Fe 3+ The absorbance of the standard solution is plotted to obtain the absorbance-concentration working curve;
[0078] Pipette 5 ml of the corrosion sample solution, test the absorbance of the corrosion sample solution at a wavelength of 456 nm, and calculate the iron content in the corrosion sample solution through the absorbance-concentration working curve. The greater the absorbance, the more severe the corrosion, and the higher the iron content, which means that the corrosion resistance of the galvanized layer has been evaluated.
[0079] Example 2
[0080] This example uses scientific verification methods to explore the influence of the type of basic immersion corrosion solution of this application on the evaluation of the corrosion resistance of the zinc coating, specifically:
[0081] Different basic immersion corrosion solutions were configured as shown in Table 3;
[0082] Table 3
[0083]
[0084]
[0085] 1) Drawing of standard working curve of iron ion;
[0086] The absorbance of the galvanized steel corrosion solution was tested by spectrophotometry using potassium thiocyanate as a colorimetric agent. The absorbance A of the corrosion solution and the corrosion time t (h) were recorded.
[0087] Using corrosion solution G as solvent, prepare 1, 2, 4, 6, and 8 μg / ml Fe 3+ Standard solution. Use potassium thiocyanate as the colorimetric agent and G as the reference solution. Use a spectrophotometer to scan the 400-800nm band and select the maximum absorption wavelength of 456nm.
[0088] The standard working curve of iron ion was drawn, and different concentrations of Fe were tested at a wavelength of 456nm. 3+ The absorbance of the standard solution was used to draw the absorbance-concentration working curve, R 2 =0.998, A = 0.0448C (μg / mL), such as Figure 1 shown.
[0089] 2) Conduct corrosion experiments;
[0090] After pretreatment, the galvanized steel sheet (galvanized layer thickness 60μm) was placed flat in a flat-bottomed reaction dish, and the corrosion solutions in the above table were added to just immerse the test piece to conduct corrosion reactions and investigate the corrosion of the galvanized steel sheet in different solutions; the solution was changed every 30 minutes, and the absorbance was measured before changing the solution. The experiment was completed after 6 hours of reaction, and the corrosion sample and corrosion sample solution were obtained. The corrosion sample was photographed and preserved. The results are shown in Figure 2 shown.
[0091] from Figure 2 It can be seen that there are obvious bubbles escaping during the corrosion reaction of corrosion solutions D, E, F, and G, while the bubbles in the corrosion reactions of A, B, and C are not obvious. After 6 hours of reaction, the galvanized steel samples immersed in the corrosion solutions D, E, F, and G changed from bright to dark, and the surface of the test piece in the G solution was gray-black; the samples in the A, B, and C solutions were relatively bright.
[0092] The absorbance of different corrosion solutions was tested respectively, and the results were as follows Figure 3 As shown. It can be seen that the absorbance of all the corrosion solutions from the beginning of the reaction of the seven corrosion solutions to 4 hours is close to 0, indicating that no iron element appears in the solution at this stage. After immersion and corrosion for 4.5 hours, the absorbance of the E, F, and G solutions is relatively close, all greater than 0, indicating that there is already iron in the solution and the corrosion has destroyed the substrate iron. The absorbance of the AD solution is still close to 0. After the reaction for 6.0 hours, the absorbance of the G solution is the largest, reaching 0.24; the absorbance of the A solution is the smallest, and the order of the absorbance from large to small is G>F>E>D>C>B>A. The greater the absorbance, the higher the iron content in the solution and the more severe the corrosion. Among this group of corrosion test solutions, the G solution has the strongest corrosion to galvanized steel, and the A solution has the weakest corrosion performance.
[0093] In summary, the results of this embodiment show that the corrosion of galvanized steel in a solution containing acetic acid, sodium nitrate, sodium persulfate and sodium chloride is a complex process involving zinc dissolution under acidic conditions, oxidation by strong oxidants, and penetration and local corrosion by chloride ions. These factors work together to accelerate the consumption of the zinc layer and lead to the formation of gray-black powdery corrosion products. In such a complex solution, the corrosion behavior of galvanized steel will be affected by multiple factors, and each additive has its specific mechanism of action.
[0094] By optimizing the composition and ratio of the corrosion solution, a mixed acid solution system for evaluating the corrosion resistance of the galvanized layer in this application was determined, which has the optimal corrosion experiment acceleration ratio. Sulfosalicylic acid and acetic acid provide a stable corrosion environment, while the presence of nitric acid, sodium nitrate and sodium persulfate will greatly accelerate the corrosion process. Sodium chloride will cause pitting corrosion on the surface of galvanized steel, which can cause the galvanized layer to be completely penetrated in a short period of time, exposing the underlying steel substrate, thereby initiating iron corrosion, and this process may be accompanied by obvious deposition of corrosion products.
[0095] Example 3
[0096] This example uses scientific verification methods to explore the effect of the pH of the basic immersion corrosion solution on the evaluation of the corrosion resistance of the zinc coating in this application, specifically:
[0097] 1) Adjust the pH of the basic etching solution to 1.5, 2.5, 3.5, 4.5, and 5.5 respectively;
[0098] Take 5 pieces of galvanized steel with the same coating thickness (40μm) as the corrosion test objects. After pretreatment, immerse them in corrosion solutions with pH values of 1.5, 2.5, 3.5, 4.5, and 5.5 for corrosion reaction. Change the solution every 30 minutes, and absorb 5ml of the corrosion solution to test the absorbance. The results are as follows: Figure 4 shown.
[0099] from Figure 4 It can be seen that in the corrosion solutions under these five pH conditions, the absorbance of the corrosion solutions with different pH values remained basically unchanged within the first 4 hours, all close to 0; after corrosion for 5.5 hours, the color of the corrosion solution with a pH value of 1.5 changed significantly, and the absorbance reached 0.11, while the absorbance of the corrosion solutions under other pH conditions was still relatively low; after corrosion for 6.0 hours, the absorbance of the corrosion solutions with pH values of 2.5 and pH values of 1.5 increased to 0.10 and 0.19 respectively; when the pH value was between 3.5 and 5.5, the reaction time was 6.5 hours, and the absorbance of the solution was still relatively low.
[0100] The above experimental phenomena show that the weaker the acidity of the corrosion solution, the longer it takes for obvious absorbance to appear in the reaction solution. A corrosion solution with a stronger acidity is conducive to shortening the corrosion test cycle; however, the corrosion rate is too fast, making it difficult to distinguish the corrosion resistance of different galvanized steels. Therefore, it is more appropriate to select a pH value of 2 to 3 for the corrosion solution.
[0101] 2) Test Fe under different pH conditions 3+ The concentration when precipitation began to occur is shown in Table 4.
[0102] Table 4
[0103] Fe3+ concentration (mg / L) pH Fe3+ concentration (mg / L) pH 1 3.11 0.1 3.45 2 3.02 0.2 3.35 3 2.96 0.3 3.29 4 2.92 0.4 3.25 5 2.88 0.5 3.22 6 2.86 0.6 3.19 7 2.83 0.7 3.17 8 2.82 0.8 3.15 9 2.80 0.9 3.13 10 2.78 <![CDATA[0.56(1×10 -5 mol / L)]]> 3.20 35 2.60 560(0.01mol / L) 2.20 56 2.53 5600(0.1mol / L) 1.87 100 2.45 56000(1mol / L) 1.53
[0104] As can be seen from the above, due to the corrosion product Fe 3+ The precipitation started in the solution with pH 2.7 and was complete at pH 3.2. Therefore, in order to make Fe 3+ No precipitation occurred in a sufficiently large concentration range, and the pH value of the corrosion solution was selected to be 2.0-2.6 as the condition for subsequent research.
[0105] Example 4
[0106] This example uses scientific verification methods to explore the influence of the components of the supplementary solution in this application on the evaluation of the corrosion resistance of the zinc coating, specifically:
[0107] 1) Take 3 pieces of galvanized steel with the same coating thickness (80 μm) as corrosion test objects, place them in three different reaction dishes (A, B, C) after pretreatment, add an equal amount of the basic immersion corrosion solution containing the developer in Example 1, so that the galvanized steel is completely immersed in the corrosion solution;
[0108] The initial pH value of the corrosion solution was adjusted to 2.1 using Na2CO3 and the reaction was carried out at a constant temperature of 40°C, wherein:
[0109] A: continuous reaction without adding supplementary solution;
[0110] B. Measure the pH value in real time. When the pH value of the solution reaches 3.0, add corrosion solution B (30% SSal + 0.5HNO3 + 1% Na2S2O8) to a pH value of 2.1;
[0111] C. Measure the pH value in real time. When the pH value of the solution reaches 3.0, add corrosion solution C (10% HCl + 1% HNO3 + 5% Na2S2O8) to a pH value of 2.1.
[0112] Continue the reaction and record the experimental phenomena and the absorbance of the test solution.
[0113] The experimental results show that obvious bubbles are generated in the three solutions from the beginning of the reaction to 30 minutes. As the reaction proceeds, the amount of bubbles in the solution reaction gradually decreases. When the reaction time is 20 minutes, the pH values of the three solutions are all about 3.1. After adding solutions to B and C respectively, the bubbles generated by solution B are similar to those in the first 30 minutes; the corrosion rate of solution C is significantly faster than that of solution B.
[0114] After about 100 minutes of reaction, the color of solution C deepened sharply, and the absorbance reached 0.656, while the colors of solutions A and B were similar to the initial ones. When the reaction continued for 300 minutes, the absorbance of solution B was 0.076, and the color gradually deepened; when the reaction lasted for 330 minutes, the absorbance was 0.137; when the reaction continued for about 400 minutes, the color of the solution also deepened sharply, and the absorbance reached 0.618. However, when the reaction lasted for 400 minutes, the color of solution A did not change significantly, and the absorbance was 0.03; the reaction continued to extend to 600 minutes, and the color of the solution still did not change significantly.
[0115] The initial corrosion reaction of solution A is similar to that of solution B and solution C, both of which are quite obvious. As the reaction proceeds, the corrosive substances in solution A, such as H + and oxidative substances NO 3- and S2O8 2- The concentration of the corrosion factor in the reaction process of this method is uneven, and the time required is longer than 10 hours, which is not suitable for the rapid evaluation of the corrosion resistance of galvanized steel in this application.
[0116] The solution supplemented by C is hydrochloric acid containing strong acid, which corrodes the zinc coating rapidly and the reaction rate is too fast. The corrosion rate of B solution containing SSal is significantly lower than that of C solution. Because SSal is a medium-strong acid, it slowly releases H while maintaining a pH value of 2 to 3. + Reacts with the zinc layer to make the corrosion reaction more uniform.
[0117] In addition, during the corrosion test, a large amount of zinc ions and some other ions such as aluminum ions will accumulate in the solution system. These metal ions will produce soluble colorless complexes with sulfosalicylic acid and consume the color developer, greatly reducing the concentration of sulfosalicylic acid. Therefore, sufficient sulfosalicylic acid must be added during the test. In summary, in order to effectively distinguish the corrosion resistance of different galvanized steels, the preferred B supplementary liquid is 30% SSal + 0.5HNO3 + 1% Na2S2O8.
[0118] Example 5
[0119] This example uses scientific verification methods to explore the influence of temperature on the evaluation of the corrosion resistance of the galvanized layer in this application, specifically:
[0120] Five pieces of galvanized steel with the same coating thickness (40 μm) were taken as corrosion test objects. After pretreatment, they were immersed in the corrosion solution described in Example 1 and heated to 25° C., 30° C., 35° C., 40° C., and 45° C. in a constant temperature water bath for corrosion reaction.
[0121] The pH value was measured every 30 minutes and the pH value of the solution was adjusted to between 2.1. At a wavelength of 486nm, the absorbance of the corrosion solution was tested at different corrosion times using a spectrophotometer. The results are as follows: Figure 5 shown.
[0122] Results In the corrosion solution, the absorbance of different corrosion solutions remained basically unchanged in the first 5 hours, all close to 0. After corrosion for 5.5 hours, the color of the corrosion solution at 45°C changed significantly, and the absorbance reached 0.11, while the absorbance of the corrosion solutions under other temperature conditions was still close to 0. After corrosion for 6.0-6.5 hours, the corrosion solutions at 30-45°C all showed obvious absorbance. And it followed the following rules: under the same corrosion time conditions, as the temperature increased, the absorbance gradually increased; in the same corrosion solution, the absorbance of the corrosion solution at 6.5 hours was significantly greater than that at 6.0 hours.
[0123] The results show that, under the same other conditions, within the range of 25-45°C, the higher the reaction temperature, the darker the color of the solution and the greater the absorbance of the solution, indicating that the increase in temperature can accelerate the corrosion reaction rate. However, when the temperature is greater than 50°C, zinc may produce a "potential reversal effect". Therefore, in order to achieve rapid detection of the corrosion resistance of the galvanized layer and ensure scientificity, it is appropriate to select 40°C as the corrosion reaction temperature.
[0124] Example 6
[0125] This example uses scientific verification methods to explore the influence of the reaction speed on the evaluation of the corrosion resistance of the galvanized layer in this application, specifically:
[0126] Six galvanized steel test pieces with a zinc coating of 60 μm were placed flat in six corrosion dishes respectively. After pretreatment, they were immersed in the corrosion solution described in Example 1 and placed in a constant temperature (40° C.) shaking table. The shaking table speed was adjusted to 0, 50, 100, 150, 200, and 250 r.mp respectively for corrosion reaction. During the experiment, supplementary solution was added according to Example 1. The absorbance of the solution at different reaction times and speeds was tested. The results are as follows: Figure 6 shown.
[0127] It can be seen that when the corrosion reaction is 2h, the substrate has not yet been corroded, and the absorbance of the solution is relatively weak, and the absorbance of the solution at different rotation speeds is relatively close. When the corrosion time reaches 5h and 6h, the absorbance of the solution in the static reaction (0r.mp) is significantly weaker than that in other shaking states. This may be because the corrosion reaction is more uniform in the shaking state, and the corrosion products on the surface of the test piece, such as H2 bubbles, are promptly washed away by the solution and dispersed into the solution, while in the reaction system in the prohibited state, the corrosion products are easily covered on the surface of the test piece, reducing the corrosion reaction sites and slowing down the corrosion rate. The results show that the difference in absorbance under different reaction times is most obvious when the rotation speed is 50rpm. Therefore, the reaction speed of the present application is preferably 50rpm.
[0128] Example 7
[0129] This example uses scientific verification methods to explore the influence of the type of developer in this application on the evaluation of the corrosion resistance of the zinc coating, specifically:
[0130] In order to study the valence state of iron in a corrosive environment (corrosive solution composition 5% HAc + 0.05% NaNO3 + 0.8% Na2S2O8 + 5% NaC, reaction temperature 40°C), Fe 3+ / Fe 2+ Standard solution, design the following experiment.
[0131] 1) Different proportions of Fe 2+ :Fe 3+ Preparation of standard solution with constant total iron content
[0132] Configure Fe 2+ and Fe 3+ The standard solution is prepared as follows:
[0133] Fe 2+ Standard solution: Fe 2+ Standard stock solution [ρ(Fe) = 10 mg / mL], weigh 0.1756 g of ammonium ferrous sulfate [Fe(NH4)2(SO4)2·6H2O], dissolve it in a small amount of pure water, add 1 mL of high-grade concentrated hydrochloric acid, dilute to 250 mL in a volumetric flask with pure water, shake well, and set aside.
[0134] Fe 3+ Standard solution: Fe 3+ Standard stock solution [ρ(Fe)=10mg / mL], weigh 0.4317g of ferric ammonium sulfate [FeNH4(SO4)2·12H2O] and dissolve it in 10mL of 1:1 hydrochloric acid solution, transfer it into a 500mL volumetric flask, dilute it to the scale with water, the iron ion content of this solution is 10mg / mL, shake well and set aside.
[0135] Prepared with different proportions of Fe 3+ and Fe 2+ Standard solution. Use a 20μL pipette to accurately transfer 20μL of 10mg / L Fe 3+ The stock solution was placed in a 5 mL centrifuge tube and diluted to 2 mL with pure water to obtain 100 μg / mL Fe 3+ According to this method, different proportions of Fe 3+ and Fe 2+ The liquid used is as shown in Table 5.
[0136] Table 5
[0137] 10:0 9:1 8:2 7:3 6:4 5:5 4:6 3:7 2:8 1:9 0:10 <![CDATA[Fe 3+ / uL]]> 20 18 16 14 12 10 8 6 4 2 0 <![CDATA[Fe 2+ / uL]]> 0 2 4 6 8 10 12 14 16 18 20
[0138] 2) Standard curve;
[0139] Sulfosalicylic acid was used as the color developer (C = 2 × 10 -4 mol / L), at a wavelength of 510nm, test different concentrations of Fe 3+ The absorbance of the standard solution was used to draw the absorbance-concentration working curve, R 2 =0.99267, A = 0.6394C-0.01492 (mmol / L), such as Figure 7 shown.
[0140] 3)Fe 2+ , Fe 3+
[0141] 20 μL of 0.02 mol / L sulfosalicylic acid was added to the prepared iron standard solutions of different proportions, and the absorbance was measured at 510 nm. The content was calculated according to the standard curve. The results are shown in Table 6. The recovery rate of this method is 96.7% to 101.2%, indicating that the corrosion solution is mainly composed of Fe 3+ .
[0142] Table 6
[0143] 10:0 9:1 8:2 7:3 6:4 5:5 4:6 3:7 2:8 1:9 0:10 Total iron actual / (ug / mL) 100 100 100 100 100 100 100 100 100 100 100 Total iron test / (ug / mL) 101.2 100.5 100.1 99.5 101.4 100.9 98.6 98.0 98.1 98.8 96.7 Recovery rate % 101.2 100.5 100.1 99.5 101.4 100.9 98.6 98.0 98.1 98.8 96.7
[0144] 4) Effect of different color developers on Zn 2+ Comparison of anti-interference capabilities;
[0145] Sulfosalicylic acid and potassium thiocyanate were selected as the color developing agents for Fe under the interference of coexisting ions. 3+ Perform identification detection. The test results are as follows Figure 8 As shown, the left picture is sulfosalicylic acid and the right picture is potassium thiocyanate, and the concentrations of both are 200 μM.
[0146] The results showed that with the increase of zinc ion content, the absorption peak of potassium thiocyanate at 460nm became lower and lower. When the zinc ion content reached 100 times, the absorbance decreased by 0.13, indicating that zinc ions interfered with the determination of iron by potassium thiocyanate, thus affecting the accuracy of the test results; while the absorbance of sulfosalicylic acid did not change much even under the interference of 100 times the amount of zinc ions, and the absorption at 510nm only increased by 0.03, indicating that sulfosalicylic acid can effectively resist the interference of zinc ions.
[0147] 5) Comparison of the anti-interference ability of different color developers at different pH values;
[0148] Two commercial color developing agents, 5-sulfosalicylic acid dihydrate (hereinafter referred to as sulfosalicylic acid) and potassium thiocyanate, were selected to test their anti-interference ability at different pH values. The results are as follows Fig. 9 As shown in the figure, the upper figure is sulfosalicylic acid and the lower figure is potassium thiocyanate. It can be seen that sulfosalicylic acid can identify iron in a wide range of pH values visible to the naked eye from 2 to 9. The color decreases slightly from 10 to 11, and turns yellow at pH 12. It is speculated that iron ions generate iron hydroxide in a strong alkaline environment. Potassium thiocyanate does not develop color well, so the test concentration is changed to 2×10 -3 mol / L, and with the increase of pH value, the color of the complex gradually decreased, and at pH value>10, precipitation occurred.
[0149] Fig.10 The absorbance test results of different color developers under different pH conditions. The left picture is sulfosalicylic acid and the right picture is potassium thiocyanate. It can be seen that under the conditions of pH 2-5, as the acidity decreases, the absorption of sulfosalicylic acid gradually increases, reaching a maximum value of 0.39 at pH 5, and can well identify and detect iron in a wide range of pH 2-10; potassium thiocyanate can also well identify and detect iron in the pH range of 2-8, but its sensitivity is not high.
[0150] 6) Test on the ability of sulfosalicylic acid to resist metal impurities;
[0151] The impurity elements in steel are mainly composed of inorganic elements such as sulfur, phosphorus, silicon and metallic element manganese. The zinc ingots used in the galvanizing process meet the requirements of GB / T 470-2008. In addition to iron, the impurity metal elements in the zinc ingots also include lead, manganese, copper, tin and aluminum. Therefore, it is necessary to test the resistance of the preferred color developer sulfosalicylic acid to metal impurities.
[0152] The results are as follows Fig.11 As shown, five times the amount of impurity ions (1000 μM Cu 2+ , Mn 2+ Sn 2+ , Pd 2+ 、Al2+ ) and then add 200 μM Fe 3+ The absorption spectrum changes after Fig.11 (Left) and relative intensity change bar at 510nm Fig.11 (right), Fig.11 1-6 in (right) represent non-interfering ions, Cu 2+ , Mn 2+ Sn 2 + , Pd 2+ 、Al 3+ ). The absorbance was only slightly lower than that without adding metal impurities. The results showed that sulfosalicylic acid has a good ability to resist interference from other metal impurities.
[0153] 7) Antioxidant capacity test of sulfosalicylic acid;
[0154] The results are as follows Fig.12 As shown, in the condition of containing corrosive solution (5% HAc + 0.05% NaNO3 + 0.8% Na2S2O8 + 5% NaC), 1eq of Fe 3+ , the absorbance of SSal hardly changed within 8 hours, indicating that it has good antioxidant capacity test.
[0155] 8) Comparison with other chromogens;
[0156] O-Phenanthroline: Fig.13 (The left picture shows o-phenanthroline, the right picture shows sulfosalicylic acid, the color developer concentration is 200 μM, and the iron ion concentration is 200 μM) The results show that when o-phenanthroline is used as the color developer, as Fe 3+ When the content of Fe increases from 1:1 to 1:100, the absorption peak at 510nm disappears. 2+ There is a strong interference in the measurement of Fe. 2+ When the content of Fe increases to 100 times, the absorbance changes little, and Fe 3+ It has good quantitative detection ability, which shows that since o-phenanthroline does not have a good anti-interference effect, it is not suitable as a color developer in this application.
[0157] In summary, when evaluating the corrosiveness of galvanized steel, it is important to accurately determine the iron ions (Fe 3+ ) concentration is a key indicator for evaluating the degree of corrosion. Sulfosalicylic acid is used as a colorimetric agent to determine Fe 3+ Concentration has significant advantages, including high selectivity, sensitivity, ease of operation and stability, which helps to accurately and efficiently evaluate the degree of corrosion of galvanized steel.
[0158] Comparative Example 1
[0159] This comparative example compares the corrosion resistance evaluation test method of the galvanized layer in the present application with other methods in the prior art, and the results are shown in Table 7.
[0160] Table 7
[0161]
[0162]
[0163] By comparing the existing relevant accelerated corrosion test evaluation methods, it is not difficult to see that the existing evaluation test cycle is long, the corrosion resistance of the analysis material is single, the evaluation results are mainly qualitative and difficult to quantify, and the data monitoring is not real-time enough. The method of the present invention is simple, rapid and cost-effective, and is very suitable for rapid detection under field or laboratory conditions.
[0164] In summary, the present invention proposes a method for quickly evaluating the corrosion resistance of the galvanized layer. By changing the corrosion conditions to accelerate the corrosion process of the material, it can simulate the corrosion of the material in a shorter time. This method is of great significance for evaluating the corrosion resistance of the galvanized layer, predicting its lifespan, and optimizing anti-corrosion measures. Through accelerated corrosion testing, we can obtain data on the corrosion of the material more quickly, so as to take corresponding protective measures or replace damaged materials in time to reduce safety accidents and economic losses caused by corrosion. Through the method of the present invention, we can not only evaluate the corrosion resistance of the galvanized layer, but also explore new methods and materials to improve the corrosion resistance of the galvanized layer, providing a scientific basis for the design, production and application of the galvanized layer.
[0165] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A method for quickly evaluating the corrosion resistance of a galvanized layer, characterized in that: include, After pretreatment, the galvanized steel sheet samples containing the galvanized layer are placed in parallel and immersed in a basic immersion corrosion solution containing a color developer, and the reaction is stirred on a constant temperature shaker. During the reaction, a supplementary solution containing a color developer is added to adjust the pH to the initial pH, and the reaction is performed for 6 to 8 hours to obtain a corrosion sample and a corrosion sample solution; The absorbance of the corrosion sample solution is measured by a spectrophotometer. The greater the absorbance, the higher the iron content in the corrosion sample solution, and the more serious the corrosion, which means that the corrosion resistance of the galvanized layer is evaluated.
2. The method for rapidly evaluating the corrosion resistance of a zinc coating as claimed in claim 1, characterized in that: The basic immersion etching solution containing the developer comprises the following components: 2% color developer + 5% HAc + 0.05% NaNO3 + 0.8% Na2S2O8 + 5% NaCl.
3. The method for rapidly evaluating the corrosion resistance of a galvanized layer according to any one of claims 1 or 2, characterized in that: The initial pH of the basic immersion corrosion solution is 2-2.
6.
4. The method for rapidly evaluating the corrosion resistance of a galvanized layer according to any one of claims 1 or 2, characterized in that: The initial pH of the basic immersion corrosion solution was 2.
1.
5. The method for rapidly evaluating the corrosion resistance of a zinc coating as claimed in claim 3, characterized in that: The initial pH of the basic immersion corrosion solution was adjusted by saturated Na2CO3 solution.
6. The method for rapidly evaluating the corrosion resistance of a galvanized layer as claimed in claim 1, characterized in that: The replenishing solution includes the following components: 30% color developer + 0.5% HNO3 + 1% Na2S2O8.
7. The method for rapidly evaluating the corrosion resistance of a zinc coating as claimed in claim 1, characterized in that: The replenishing solution is added when the pH of the basic immersion corrosion solution reaches 3.
0.
8. The method for rapidly evaluating the corrosion resistance of a galvanized layer according to any one of claims 2 or 5, characterized in that: The color developer is 5-sulfosalicylic acid dihydrate.
9. The method for rapidly evaluating the corrosion resistance of a zinc coating as claimed in claim 1, characterized in that: The reaction temperature of the constant temperature shaker stirring reaction is 35-40°C.
10. The method for rapidly evaluating the corrosion resistance of a zinc coating as claimed in claim 8, characterized in that: The stirring speed of the constant temperature shaker stirring reaction is 50-200 rpm.
Citation Information
Cited By
Salt spray accelerated testing method for stainless steel
CN121632924A