Radio frequency silicon on insulator wafer stage

By using the integrated structure of floating-area silicon-based wafers and well-rich layer in RF devices, the challenges of semiconductor wafers on the insulating layer in high resistivity and stability are solved, and the performance improvement of RF devices and the uniformity of resistivity are achieved. .

CN119028993APending Publication Date: 2024-11-26GLOBALWAFERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149823.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-07-13
Filing Date
2019-06-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, when preparing semiconductor wafers on insulating layers, it is difficult to maintain high resistivity and stability, resulting in parasitic power loss and harmonic distortion problems of radio frequency devices.

Method used

Adopting the integrated structure of floating-region silicon-based wafers and well-rich layers, the formation of parasitic conductive layers is suppressed by forming high-resistance floating-region silicon and well-rich layers on the single crystal silicon wafer treatment substrate, thereby improving the performance of the radio frequency device. .

Benefits of technology

The superior performance and stability of the radio frequency device are achieved, the conductive coupling and junction capacitance are reduced, the resistivity uniformity and stability are improved, the formation of thermal and excessive dosages is reduced, and the resistivity deviation is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028993A_ABST
    Figure CN119028993A_ABST
Patent Text Reader

Abstract

The invention relates to radio frequency silicon on an insulator wafer platform. A semiconductor-on-insulator (e.g., silicon-on-insulator) structure with superior radio frequency device performance and a method of making the structure are provided by utilizing a monocrystalline silicon handling wafer sliced from a floating region growing monocrystalline silicon ingot.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Information about divisional applications

[0002] This application is a divisional application of the Chinese invention patent application with application number 201980044763.7, application date June 28, 2019, and invention name “RF Silicon on Insulator Wafer Platform”.

[0003] CROSS REFERENCE TO RELATED APPLICATIONS

[0004] This application claims the benefit of priority to U.S. Provisional Application Serial No. 62 / 697,474, filed on July 13, 2019, the disclosure of which is incorporated herein by reference as if fully set forth. Technical Field

[0005] The present invention relates generally to the field of semiconductor wafer fabrication. More particularly, the present invention relates to a method of fabricating semiconductor-on-insulator (eg, silicon-on-insulator) structures and semiconductor-on-insulator structures having superior radio frequency device performance. Background Art

[0006] Semiconductor wafers are typically prepared from a single crystal ingot (e.g., a silicon ingot) that is trimmed and ground to have one or more flat edges or indentations for proper orientation of the wafer in subsequent processes. The ingot is then sliced ​​into individual wafers. Although reference will be made herein to semiconductor wafers constructed of silicon, other materials may be used to prepare semiconductor wafers, such as germanium, silicon carbide, silicon germanium, gallium arsenide, and other alloys of Group III and Group V elements (e.g., gallium nitride or indium phosphide), or alloys of Group II and Group VI elements (e.g., cadmium sulfide or zinc oxide).

[0007] Semiconductor wafers (e.g., silicon wafers) can be used in the preparation of composite layer structures. Composite layer structures (e.g., semiconductor on insulator, and more specifically, silicon on insulator (SOI) structures) typically include a handle wafer or layer, a device layer, and an insulating (i.e., dielectric) film (typically an oxide layer) between the handle layer and the device layer. Typically, the device layer has a thickness between 0.01 and 20 microns, such as a thickness between 0.05 and 20 microns. A thick film device layer may have a device layer thickness between about 1.5 microns and about 20 microns. A thin film device layer may have a thickness between about 0.01 microns and about 0.20 microns. In general, composite layer structures such as silicon on insulator (SOI), silicon on sapphire (SOS), and silicon on quartz are produced by placing two wafers in intimate contact, thereby initiating bonding through van der Waals forces, hydrogen bonding, or both, followed by heat treatment to strengthen bonding. Annealing can convert terminal silanol groups into siloxane bonds between the two interfaces, thereby strengthening bonding.

[0008] After thermal annealing, the bonded structure undergoes further processing to remove a large portion of the donor wafer to achieve layer transfer. For example, a wafer thinning technique such as etching or grinding may be used, which is often referred to as bonded and etched SOI (i.e., BESOI) or bonded and ground SOI (i.e., BGSOI), in which a silicon wafer is tethered to a handle wafer and then slowly etched away until only a thin layer of silicon on the handle wafer remains. See, for example, U.S. Pat. No. 5,189,500, the disclosure of which is incorporated herein by reference as if fully set forth. This method is time consuming and expensive, wastes one of the substrates, and generally does not have suitable thickness uniformity for layers thinner than a few microns.

[0009] Another common method of achieving layer transfer utilizes hydrogen implantation followed by thermally induced layer splitting. Particles (atoms or ionized atoms, such as hydrogen atoms or a combination of hydrogen and helium atoms) are implanted at a specified depth below the front surface of the donor wafer. The implanted particles form a cleave plane in the donor wafer at the specified depth at which the particles were implanted. The surface of the donor wafer is cleaned to remove organic compounds or other contaminants, such as boron compounds and any other particulate matter, that were deposited on the wafer during the implantation process.

[0010] Next, the front surface of the donor wafer is bonded to the handle wafer by a hydrophilic bonding process to form a bonded wafer. Prior to bonding, the donor wafer and / or the handle wafer are activated by exposing the surfaces of the wafers to a plasma containing, for example, oxygen or nitrogen. Exposure to the plasma modifies the structure of the surfaces in a process generally referred to as surface activation, which renders the surface of one or both of the donor water and the handle wafer hydrophilic. The surface of the wafer may additionally be chemically activated by a wet treatment, such as an SCI clean. The wet treatment and plasma activation may occur in either order, or the wafer may be subjected to only one treatment. Next, the wafers are pressed together, and a bond is formed therebetween. Due to van der Waals forces, this bond is relatively weak, and must be strengthened before further processing can occur.

[0011] In some processes, the hydrophilic bond between the donor wafer and the handle wafer (i.e., the bonded wafer) is strengthened by heating or annealing the bonded wafer pair. In some processes, wafer bonding may occur at a low temperature, such as between approximately 300° C. and 500° C. The lower bonding temperature reduces the bridging layer of adsorbed water vapor on the surface and increases the density of hydrogen bonds between silanol groups on the surface of each wafer. In some processes, wafer bonding may occur at a high temperature, such as between approximately 800° C. and 1100° C. The higher temperature results in the formation of covalent bonds between the adjacent surfaces of the donor wafer and the handle wafer (e.g., converting silanol hydrogen bonds to covalent siloxane bonds), thereby strengthening the bond between the donor wafer and the handle wafer. While the bonded wafer is heated or annealed, the particles previously implanted in the donor wafer weaken the cleavage plane.

[0012] Next, a portion of the donor wafer is separated from the bonded wafer along the cleavage plane (i.e., cleaved) to form an SOI wafer. The cleaving can be performed by placing the bonded wafer in a fixture, wherein a mechanical force is applied perpendicular to the opposite side of the bonded wafer so as to pull a portion of the donor wafer away from the bonded wafer. According to some methods, the mechanical force is applied using a suction cup. The separation of the portion of the donor wafer is initiated by applying a mechanical force at the edge of the bonded wafer at the cleavage plane so as to initiate the propagation of a crack along the cleavage plane. Next, the portion of the donor wafer is pulled from the bonded wafer by the mechanical force applied by the suction cup, thereby forming an SOI wafer.

[0013] According to other methods, the bonded pair may instead be subjected to high temperatures for a period of time to separate a portion of the donor wafer from the bonded wafer. Exposure to high temperatures results in the initiation and propagation of cracks along the cleavage plane, thereby separating a portion of the donor wafer. The cracks are formed due to the formation of voids from the implanted ions grown by Oswald ripening. The voids are filled with hydrogen and helium. The voids become thin plates. The pressurized gas in the thin plate propagates microcavities and microcracks, which weaken the silicon on the implanted face. If the annealing is stopped at the appropriate time, the weakened bonded wafer can be split by a mechanical process. However, if the heat treatment is continued for a longer duration and / or at a higher temperature, the microcracks propagate to the point where all cracks merge along the cleavage plane, thereby separating a portion of the donor wafer. This method allows for better uniformity of the transferred layer and allows for recycling of the donor wafer, but generally requires heating the implanted and bonded pair to a temperature close to 500°C.

[0014] The use of high resistivity semiconductor-on-insulator (e.g., silicon-on-insulator) wafers for RF-related devices (e.g., antenna switches) provides cost and integration benefits over conventional substrates. To reduce parasitic power losses and minimize inherent harmonic distortion when using conductive substrates for high frequency applications, it is necessary but not sufficient to use substrate wafers with high resistivity. Accordingly, the resistivity of handle wafers used for RF devices is typically greater than about 500 ohm-cm. Referring now to FIG. Figure 1 , a silicon-on-insulator structure 2 includes a very high resistivity silicon wafer 4, a dielectric layer 6 (e.g., a buried oxide (BOX) layer), and a silicon device layer 10. This substrate tends to form a high conductivity charge inversion or accumulation layer 12 at the BOX / handle interface, resulting in the generation of free carriers (electrons or holes), which reduces the effective resistivity of the substrate and causes parasitic power losses and device nonlinearities when the device is operated at RF frequencies. These inversion / accumulation layers can be attributed to BOX fixed charge, oxide trapped charge, interface trapped charge, and even DC bias applied to the device itself.

[0015] Therefore, a method is needed to suppress any induced inversion or accumulation layer formation so that the high resistivity of the substrate is maintained even in very near surface regions. It is known that high resistivity treatment of the well-rich layer between the substrate and the buried oxide (BOX) can improve the performance of RF devices manufactured using SOI wafers. Several methods have been proposed to form such high interface trapping layers. For example, reference is now made to Figure 2 One of the methods of producing a semiconductor on insulator 20 (e.g., silicon on insulator, or SOI) with a well-rich layer 28 for RF device applications is based on depositing an undoped polysilicon film on a silicon substrate 22 having a high resistivity and then forming a dielectric layer 24 (e.g., an oxide stack or a buried oxide layer) and a top silicon layer 26 thereon. The polysilicon layer acts as a high defectivity layer between the silicon substrate 22 and the dielectric layer 24. See Figure 2 , which depicts a polysilicon film used as a well-rich layer 28 between a high resistivity substrate 22 and a dielectric layer 24 in a silicon-on-insulator structure 20. An alternative approach is to implant heavy ions to create a near-surface damage layer. Devices such as radio frequency devices are built into the top silicon layer 26.

[0016] The polysilicon layer between the oxide and the substrate has been shown in academic studies to improve device isolation, reduce transmission line losses and reduce harmonic distortion. See, for example, H. S. Gamble et al., “Low-loss CPW lines on surface stabilized high resistivity silicon,” Microwave Guided Wave Lett., 9(10), pp. 395-397, 1999; D. Lederer, R. Lobet, and J.-P. Raskin, “Enhanced high resistivity SOI wafers for RF applications,” IEEE Intl. SOI Conf., pp. 46-47, 2004; D. Lederer and J.-P. Raskin, “New substrate passivation method dedicated to high resistivity SOI wafer fabrication with increased substrate resistivity,” IEEE Intl. SOI Conf., pp. 46-47, 2004. resistivity,” IEEE Electron Device Letters, Vol. 26, Chapter 11, pp. 805-807, 2005; D. Lederer, B. Aspar, C. Laghaé, and J.-P. Raskin, “Performance of RF passive structures and SOI MOSFETs transferred on a passivated HR SOI substrate,” IEEE International SOI Conference, pp. 29-30, 2006; and Daniel C. Kreiter, J.-P.Kerret et al., “Identification of RF harmonic distortion on Si substrates and its reduction using a trap-rich layer”, Silicon Monolithic Integrated Circuits in RF Systems, 2008. SiRF 2008 (EEE Topical Meeting), pp. 151-154, 2008. Summary of the invention

[0017] Briefly, the present invention relates to a multilayer structure comprising: a single crystal silicon wafer handling substrate comprising two major, substantially parallel surfaces (one of the surfaces being a front surface of the single crystal silicon wafer handling substrate and the other of the surfaces being a rear surface of the single crystal silicon wafer handling substrate), a circumferential edge joining the front and rear surfaces of the single crystal silicon wafer handling substrate, and a central plane of the single crystal silicon wafer handling substrate between the front and rear surfaces of the single crystal silicon wafer handling substrate, wherein the single crystal silicon wafer handling substrate has a bulk resistivity of at least about 5000 ohm-cm, a resistivity of less than about 1×10 16 Atom / cm 3 interstitial oxygen concentration of at least about 1×10 13 Atom / cm 3 a nitrogen concentration; a well-rich layer in interface contact with the front surface of the single crystal silicon wafer processing substrate; a dielectric layer in interface contact with the well-rich layer; and a single crystal semiconductor device layer in interface contact with the dielectric layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A depiction of a silicon wafer on an insulating layer including a high resistivity substrate and a buried oxide layer.

[0019] Figure 2 A depiction of a silicon-on-insulator wafer according to the prior art, the SOI wafer includes a polysilicon well-rich layer between a high-resistivity substrate and a buried oxide layer.

[0020] Figure 3 is a graph depicting harmonic distortion depending on substrate resistivity in a HR-SOI structure employing a well-rich layer.

[0021] Figure 4 is a graph depicting resistivity depth profiles of a float zone growth treated wafer and a Czochralski growth treated wafer after SOI processing with a well rich layer.

[0022] Figure 5 is a graph depicting the average resistivity of the first 90 microns below the BOX / treat interface of a float zone growth treat wafer after SOI processing with a well rich layer. DETAILED DESCRIPTION

[0023] According to the present invention, a method for producing a semiconductor-on-insulator (e.g., silicon-on-insulator) structure that achieves superior radio frequency (RF) device performance, device stability, and device fabrication manufacturability is provided and a structure is provided. The present invention integrates a high-resistivity (e.g., very high-resistivity or ultra-high-resistivity) floating zone (FZ) silicon-based wafer (handle wafer) and a well-rich layer into a semiconductor-on-insulator (e.g., silicon-on-insulator) structure.

[0024] Radio frequency (RF) chip designs benefit significantly from higher substrate resistivity levels. Utilizing higher resistivity silicon substrates enables improvements in quality factor of passive components (e.g., inductors and capacitors), reduced attenuation of transmission lines, and substrate electrical isolation between integrated digital, RF, and analog components. The industry standard is a handled substrate resistivity above 1,000 ohm-cm, with higher resistivities being preferred. Integrating high resistivity substrates into semiconductor-on-insulator (e.g., silicon-on-insulator) structures (HRSOI) further improves RF capabilities by providing preferred device isolation, reduced conductive coupling to the substrate wafer, and lower junction capacitance.

[0025] Growing ultra-high resistivity Czochralski (CZ) crystals to resistivity values ​​greater than 7,500 ohm-cm presents a severe challenge. As the concentration of added electrically active dopants is significantly reduced, additional emphasis must be placed on the control of dopants (e.g., boron and phosphorus) introduced from all raw materials and components used in the CZ crystal puller. These materials and components include the polysilicon source material and the quartz crucible. In addition, the very low dopant levels in the melt make it important to control the mass transfer of dopants to the boundary layer at the melt-solid interface and then through the boundary layer to achieve acceptable radial resistivity variations. Another key challenge in the growth of higher resistivity Czochralski silicon ingots is to control the behavior of interstitial oxygen incorporated during crystal growth. Interstitial oxygen concentrations in Czochralski grown silicon are typically greater than 5×10 17 atoms / cm 3 (10PPMA new-ASTM), for example up to about 1×10 18 atoms / cm 3 (20 PPMA new-ASTM). The source of this interstitial oxygen is dissolution of the SiO2 crucible during crystal growth. In high resistivity CZ silicon, oxygen can be controlled to about 5 PPMA (2.5×10 17 atoms / cm 3 ) range and lower, for example, about 2PPMA (1×10 17atoms / cm 3 ), about 3PPMA (1.5×10 17 atoms / cm 3 ), and about 4PPMA (2×10 17 atoms / cm 3 ). However, even at low concentrations, interstitial oxygen can aggregate into electrically active thermal donors that depend strongly on both interstitial oxygen concentration and annealing time / temperature in the range of 350°C to 500°C. At aggregation levels greater than 4 oxygen atoms, the thermal donors become electrically active, acting as dual donors. The formation of such donors is maximized at about 450°C and decays thereafter, and they can dissociate upon annealing treatments above about 550°C and return to an electrically inactive state. However, at longer annealing times and higher annealing temperatures (e.g., in the range of 550°C to 850°C), so-called new thermal donors can form. Peak new thermal donor formation occurs at temperatures from 750°C to 800°C. We have recently discovered another class of excess donors in high resistivity silicon subjected to high temperature heat treatment. Fast diffusing species that have not yet been identified are introduced into the silicon wafer during the very high T anneal and quenched during wafer cooling. Upon subsequent heating to a range of 450°C to 650°C, these species rapidly recombine with interstitial oxygen in the wafer to form electrically active "excess donors". These excess donors will dissociate upon heating above about 1050°C to 1100°C. The oxygen-thermal dual donors, new donors, and excess hot donors enable electron conduction, which can alter the resistivity and type of the wafer depending on the number of donors generated relative to the background carrier concentration of the wafer. In p-type silicon, the hot donors increase the resistivity of the wafer until the hot donor concentration exceeds the p-type carrier concentration, at which point the wafer will convert to n-type. Further hot donor generation will then result in n-type wafers with lower and lower resistivity. Changes in resistivity during or at the end of a device process can disrupt resistivity-sensitive processes and lead to degradation of device performance. While hot donors can in principle be annihilated by high T anneals (greater than about 550°C for hot dual donors, between about 1050°C and about 1100°C for new and excess donors), in practice most of these donors are formed by low temperature annealing steps that occur later in the integrated circuit manufacturing process (in the "back end of line, BEOL") after metallization, which can occur at temperatures of about 450°C. Once the metal is deposited, the wafer cannot be heated above a T of about 500°C, so none of the hot donor species formed in the BEOL can be annihilated. While hot donors formed in the 350°C to 500°C range can be eliminated by short duration, high temperature anneals, the presence of excess hot donors becomes particularly noticeable for high resistivity silicon with resistivities greater than 4000 ohm-cm, and is significant for materials with resistivities greater than 7500 ohm-cm. In such materials, dopant concentrations can be as high as 1.8×10 12 / cm 3(p-type) or Nd<5×10 11 / cm 3 For comparison, the excess thermal donor concentration for a material annealed at a temperature between about 1100°C and 1125°C may be about 1×10 12 / cm 3 The excess donor drops to as low as 1×10 11 / cm 3 Given comparable concentrations of dopant materials (eg, boron, arsenic, phosphorus) and concentrations of excess thermal donors, materials designated as high resistivity may suffer from resistivity variability, and even significant switching from p-type to n-type.

[0026] Float zone (FZ) silicon is an ultra-high purity alternative to CZ silicon. FZ can be fabricated at resistivity levels greater than 5,000 ohm-cm, greater than 7,500 ohm-cm, even greater than 10,000 ohm-cm, or even greater than 20,000 ohm-cm. The float zone process minimizes the introduction of oxygen into the growing single crystal and can advantageously minimize oxygen thermal double donor formation, new thermal donor formation, and excess thermal donor formation. The concomitant reduction in thermal donor formation axially and radially minimizes resistivity variability in the ingot and wafers sliced ​​therefrom. This can improve both device performance and resistivity stability.

[0027] HRSOI wafers also experience parasitic conduction at the interface between the buried oxide layer (BOX) and the high-resistivity substrate which can extend more than 10 microns into the underlying high-resistivity substrate. It is caused by a combination of normal oxide charge in the BOX and the very low doping concentration of the substrate. Figure 1 The parasitic surface conduction 12 effect (referred to as PSC in the literature) shown in FIG. 1 results in a lower effective substrate resistivity and increased RF losses, substrate nonlinearity, and crosstalk. Figure 2 ) is placed between the dielectric layer 24 and the high resistivity substrate 22 to prevent the parasitic conductive layer 12 (reference Figure 1 ) is formed by trapping free carriers attracted to the BOX / substrate interface, thereby inhibiting the formation of an accumulation or inversion layer. When the well-rich layer is combined with a stable float zone silicon handle wafer having a resistivity greater than 5,000 ohm-cm, greater than 7,500 ohm-cm, even greater than 10,000 ohm-cm, or even greater than 20,000 ohm-cm, the formation of an accumulation or inversion layer can be achieved. Figure 3 Excellent RF performance, such as second harmonic distortion or HD2 values ​​better than -90dB, is achieved as shown in the .

[0028] The use of float zone treated wafers is expected to solve multiple problems; 1) the FZ provides a manufacturable crystal growth path for resistivity target levels greater than 5,000 ohm-cm, greater than 7,500 ohm-cm, even greater than 10,000 ohm-cm, or even greater than 20,000 ohm-cm, which when coupled with a well-rich layer achieves improved RF performance, and 2) the FZ has an oxygen content below the detection limit, which reduces and can eliminate electrically active thermal donors and excess thermal donor formation and thus prevents resistivity excursions that can degrade RF electrical performance and interfere with the processing of wafers in the device manufacturing line. Float zone silicon is grown by vertical zone melting / refining of a high purity polycrystalline rod. A single crystal is placed at one end of the rod to initiate single crystal growth. The process avoids the use of a containment vessel, which greatly reduces the introduction of impurities including oxygen. Eliminating oxygen effects such as thermal donor formation is essential in ultra-high resistivity silicon. Nitrogen is often intentionally added during FZ growth to control point defect formation and improve its mechanical strength. The doping level and dopant type of the ultra-high resistivity FZ depends on the purity of the polycrystalline source rod.

[0029] I. Float Zone Treatment Wafer

[0030] According to the present invention, a wafer sliced ​​from a single crystal silicon ingot grown by a floating zone method is integrated as a high resistivity treatment structure having Figure 2 2. The structure shown in FIG. 2 is a semiconductor-on-insulator (e.g., silicon-on-insulator) structure 20. That is, the SOI structure 20 includes a floating region high-resistivity handle structure (e.g., semiconductor handle substrate 22) (e.g., wafer), a well-rich layer 28, a dielectric layer 24, and a device layer 26.

[0031] The substrate used in the present invention includes a semiconductor handling substrate (e.g., a single crystal semiconductor handling wafer) and a semiconductor donor substrate (e.g., a single crystal semiconductor donor wafer). The semiconductor device layer 26 in the semiconductor-on-insulator (composite) structure 20 is derived from the single crystal semiconductor donor wafer. The semiconductor device layer 26 can be transferred to the semiconductor handling substrate 22 by wafer thinning techniques (e.g., etching the semiconductor donor substrate) or by cleaving the semiconductor donor substrate including the damaged plane.

[0032] In general, single crystal semiconductor handling wafers and single crystal semiconductor donor wafers include two main, substantially parallel surfaces. One of the parallel surfaces is the front surface of the substrate, and the other parallel surface is the rear surface of the substrate. The substrate includes a circumferential edge joining the front surface and the rear surface, a main body region between the front surface and the rear surface, and a center plane between the front surface and the rear surface. The substrate additionally includes an imaginary center axis perpendicular to the center plane and a radial length extending from the center axis to the circumferential edge. In addition, because semiconductor substrates (e.g., silicon wafers) typically have some total thickness variation (TTV), warpage, and bow, the midpoint between each point on the front surface and each point on the rear surface may not fall exactly within the plane. However, as a practical matter, the TTV, warpage, and bow are typically so small that approximately the midpoint can be said to fall within an imaginary center plane approximately equidistant between the front surface and the rear surface.

[0033] Prior to any operation as described herein, the front surface and the back surface of the substrate may be substantially the same. A surface is referred to as the "front surface" or the "back surface" for convenience only and is generally used to distinguish the surface on which the operation of the method of the present invention is performed. In the context of the present invention, the "front surface" of a single crystal semiconductor handling substrate (e.g., a single crystal silicon handling wafer) refers to the main surface of the substrate, which becomes the inner surface of the bonding structure. A well-rich layer is formed on this front surface. Accordingly, the "back surface" of a single crystal semiconductor handling substrate (e.g., a handling wafer) refers to the main surface that becomes the outer surface of the bonding structure. Similarly, the "front surface" of a single crystal semiconductor donor substrate (e.g., a single crystal silicon donor wafer) refers to the main surface of the single crystal semiconductor donor substrate, which becomes the inner surface of the bonding structure. The front surface of the single crystal semiconductor donor substrate typically includes a dielectric layer, such as a silicon dioxide layer, which forms part or all of a buried oxide (BOX) layer in the final structure. The "back surface" of a single crystal semiconductor donor substrate (e.g., a single crystal silicon donor wafer) refers to the main surface that becomes the outer surface of the bonding structure. After completing conventional bonding and wafer thinning steps, the single crystal semiconductor donor substrate is then used to form a semiconductor device layer of a semiconductor-on-insulator (eg, silicon-on-insulator) composite structure.

[0034] The handling wafer includes a material (e.g., silicon) derived from an ingot grown by a floating zone method. A single crystal silicon handling wafer sliced ​​from an ingot grown by a floating zone method typically has a nominal diameter of at least about 20 mm, at least about 50 mm, at least about 100 mm, at least about 150 mm, at least about 200 mm, such as about 150 mm, or about 200 mm. Surface tension limitations during the growth process typically result in a diameter of no more than 250 mm or about 200 mm. The handling wafer thickness may vary between about 100 microns and about 5000 microns, such as between about 100 microns and about 1500 microns, such as between about 250 microns and about 1500 microns, such as between about 300 microns and about 1000 microns, suitably in the range of about 500 microns to about 1000 microns. In some specific embodiments, the wafer thickness may be about 725 microns. In some embodiments, the wafer thickness may be about 775 microns.

[0035] In some embodiments, the float zone crystal ingot and the single crystal semiconductor handling substrates sliced ​​therefrom have a bulk resistivity of at least about 5,000 ohm-cm, at least about 7,500 ohm-cm, such as at least about 10,000 ohm-cm, at least about 15,000 ohm-cm, or at least about 20,000 ohm-cm. In some embodiments, the single crystal semiconductor handling substrate has a bulk resistivity of less than about 100,000 ohm-cm. High resistivity wafers may include typically very low concentrations (e.g., less than 1×10 12 atoms / cm 3 , or even less than 1×10 11 atoms / cm 3 ) electrically active dopants such as boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type). Methods for preparing high resistivity wafers from float zone single crystal silicon ingots are known in the art, and such high resistivity wafers are available from commercial suppliers.

[0036] Silicon processed wafers derived from float zone grown ingots can be more reliably calibrated to ultra-high resistivity values ​​with a minimum to maximum variation of about 2X. For example, unlike in UHRCz wafers where the specification is typically single sided (e.g., >= 7500 ohm-cm), a double sided minimum-maximum specification for wafer resistivity, such as 10,000-20,000 ohm-cm or tighter, may be acceptable. A tolerance of + / - 30% to 50% around the target value may be acceptable. This will enable the end user to have not only improved RF electrical performance levels (such as Figure 3The underlying reason for this solution is that the float zone grown silicon handle wafer has an oxygen concentration below the detectable limit and thereby avoids hot donor formation and excessive hot donor formation, which leads to the variability of ultra-high resistivity Czochralski grown silicon. In some embodiments, the float zone grown silicon handle wafer has an oxygen level that is below the detection limit of the metrology method (e.g., less than about 2.5×10 16 atoms / cm 3 (0.5PPMA, new ASTM standard), less than about 2×10 16 atoms / cm 3 (0.4PPMA, new ASTM standard), less than about 1×10 16 atoms / cm 3 (0.2PPMA, new ASTM standard), or even less than about 1×10 15 atoms / cm 3 (0.02 PPMA, new ASTM standard)) and eliminates the presence of oxygen thermal donors and excess donors formed in Czochralski grown silicon wafers, including detectable oxygen concentrations. In some embodiments, the silicon treated wafer has less than 1×10 11 Donor body / cm 3 , or even less than 5×10 10 Donor body / cm 3 In some embodiments, the oxygen concentration is so low that the dual donor thermal donor concentration, the new thermal donor concentration and / or the excess thermal donor concentration are below the detectable limit, and a first approximation would be that the concentration of such donors may be at least one order of magnitude less than the p-type acceptor or n-type donor concentration. In other words, the concentration of any one of the dual donor thermal donor concentration, the new thermal donor concentration and / or the excess thermal donor concentration or the sum of the dual donor thermal donor concentration, the new thermal donor concentration and / or the excess thermal donor concentration is at least one order of magnitude less than the p-type acceptor or n-type donor concentration, i.e., 1 / 10 less than the concentration of the p-type or n-type dopant. In CZ, the thermal donor and excess may be lower, equal to or higher than the background doping concentration, depending on the oxygen concentration and the thermal cycle details. The thermal dual donor concentration in CZ Si will remain at about 450°C and increase with annealing time to considerable values. The concentration will eventually saturate at a certain value depending on Oi. For a large Oi of about 15 nppma, the saturation concentration may be about 1×10 16 / cm 3or greater. The saturated (maximum) TDD concentration will decrease with decreasing Oi, but I have no information on how low it will be at 2 to 5 nppma. It will be much greater than the actual dopant concentrations involved in HR Si. The low donor concentration in FZ wafers reduces variability in RF performance, reduces the impact of resistivity variability on device processes that are sensitive to wafer resistivity (electrostatic adsorption), and eliminates sensitivity to new hot donor formation, which is another source of variability in ultra-high resistivity / low-oxygen Czochralski-grown silicon wafers.

[0037] In addition, for example, after annealing at 450°C, the spread resistance profile (SRP) of Czochralski-grown silicon handle wafers is rarely flat over the first tens of microns below the BOX / handle interface. The SRP of Czochralski-grown silicon handle wafers is often affected by the formation of TD and excess donor, resulting in significant changes in the profile, such as Figure 4 However, the SRP of the float zone grown silicon treated wafer is very flat and shows a complete lack of hot donor and excess donor in the 450°C and 600°C tests. Figure 4 .exist Figure 4 On the graph in , the line with diamonds (◆) is the resistivity at each depth of the floating zone treated wafer before 450°C donor generation annealing (DGA), and the line with X is the resistivity at each depth of the floating zone treated wafer after 450°C DGA annealing. In addition, on the graph, the line with squares (■) is the resistivity at each depth of the p-type Czochralski growth treated wafer after 450°C DGA annealing. Finally, on the graph, the line with triangles (▲) is the resistivity at each depth of the n-type Czochralski growth treated wafer after 450°C DGA annealing. See also Figure 5 , which depicts the average resistivity of the first 90 microns below the BOX / treat interface of a float zone growth treat wafer after SOI processing with a well-rich layer, the wafer has a resistivity greater than 5000 ohm-cm and a resistivity greater than 10,000 ohm-cm. The distribution is very flat and shows a complete lack of heat donors in the 450°C and 600°C tests.

[0038] Since float zone grown silicon handle wafers have oxygen below the detectable limit, such wafers may be more susceptible to slipping during thermal processes. However, nitrogen can be added during the growth of the float zone crystal to control point defect formation and increase the strength against slipping. Specialized doping techniques such as core doping, pellet doping, gas doping with nitrogen or ammonia can be used to incorporate uniform concentrations of impurities. In some embodiments, the nitrogen concentration in the float zone grown silicon handle wafer can be at least about 1×10 13 atoms / cm 3 , for example at least about 1×10 14 atoms / cm 3In some embodiments, the nitrogen concentration in the floating zone grown silicon handle wafer may be less than about 3×10 15 atoms / cm 3 , or less than about 1×10 15 atoms / cm 3 , or less than about 7×10 14 atoms / cm 3 It was demonstrated in an SOI manufacturing line that nitrogen doped floating region grown silicon handle wafers exhibited acceptable sliding performance nearly equal to that of Czochralski grown silicon handle wafers.

[0039] In this regard, the floating zone grown silicon handle wafers and the Czochralski grown silicon handle wafers were subjected to oxidation at 800°C, followed by a 2-hour annealing cycle at 1100°C, and then a slip test. The result was that no slip was found in either wafer type. Accordingly, the nitrogen doped floating zone handle wafers can continue to exist in the thermal cycles associated with the deposition of the well-rich layer and subsequent SOI wafer manufacturing without slip. In another furnace push test, the furnace was heated to 1000°C, and the floating zone grown silicon handle wafers and the Czochralski grown silicon handle wafers were quickly pushed through the furnace. Both wafer types performed similarly under this slip test.

[0040] In some embodiments, the front surface, the back surface, or both the front surface and the back surface of the single crystal semiconductor handling substrate may be subjected to a process (e.g., an oxidation process) to thereby grow a dielectric layer, such as a semiconductor oxide layer, a semiconductor nitride layer, or a semiconductor oxynitride layer. In some embodiments, the dielectric layer includes silicon dioxide, which may be formed by oxidizing the front surface of the silicon handling substrate. This may be achieved by thermal oxidation (wherein some portion of the deposited semiconductor material film will be consumed) and / or CVD oxide deposition and / or atomic layer deposition. In some embodiments, the semiconductor handling substrate may be thermally oxidized in a furnace such as an ASM A400. In an oxidizing environment, the temperature may range from 750° C. to 1100° C. The oxidizing ambient atmosphere may be a mixture of an inert gas (e.g., Ar or N2) and O2. The oxygen content may vary from 1% to 10% or more. In some embodiments, the oxidizing ambient atmosphere may be up to 100% oxygen (“dry oxidation”). In some embodiments, the oxidizing ambient atmosphere may be oxygen and ammonia, which is suitable for depositing silicon oxynitride. In some embodiments, the ambient atmosphere may include a mixture of an inert gas (e.g., Ar or N2) and an oxidizing gas (e.g., O2 and water vapor) ("wet oxidation"). In some embodiments, the ambient atmosphere may include a mixture of an inert gas (e.g., Ar or N2) and an oxidizing gas (e.g., O2 and water vapor) ("wet oxidation") and a nitriding gas (e.g., ammonia). In some embodiments, the ambient atmosphere may include a mixture of an inert gas (e.g., Ar or N2) and a nitriding gas (e.g., ammonia), which is suitable for depositing silicon nitride. In an exemplary embodiment, a semiconductor processing wafer may be loaded into a vertical furnace (e.g., A400). The temperature is ramped up to an oxidation temperature using a mixture of N2 and O2. At the desired temperature, water vapor is introduced into the gas flow. After the desired oxide thickness has been obtained, the water vapor and O2 are turned off, the furnace temperature is reduced, and the wafer is unloaded from the furnace. The oxide layer on the front surface, the back surface, or both may be between about 100 angstroms and about 100,000 angstroms, between about 100 angstroms and about 10,000 angstroms, between about 100 angstroms and about 1000 angstroms, for example, between about 100 angstroms and about 700 angstroms, or between about 100 angstroms and about 500 angstroms, or between about 100 angstroms and about 250 angstroms.

[0041] In some embodiments, the oxide layer is relatively thin, such as between about 5 angstroms to about 25 angstroms, such as between about 10 angstroms to about 15 angstroms. The thin oxide layer can be obtained on both sides of the semiconductor wafer by exposure to a standard cleaning solution (e.g., SC1 / SC2 cleaning solution). In some embodiments, the SC1 solution includes 5 parts by weight of deionized water, 1 part by weight of aqueous NH4OH (ammonium hydroxide, 29 weight % NH3), and 1 part by weight of aqueous H2O2 (hydrogen peroxide, 30%). In some embodiments, the treated substrate can be oxidized by exposure to an aqueous solution including an oxidant (e.g., SC2 solution). In some embodiments, the SC2 solution includes 5 parts by weight of deionized water, 1 part by weight of aqueous HCl (hydrogen acid, 39 weight %), and 1 part by weight of aqueous H2O2 (hydrogen peroxide, 30%).

[0042] II. Well-Rich Layer

[0043] According to the method of the present invention, a well-rich layer including a polycrystalline or amorphous semiconductor material is deposited onto the exposed front surface of a single crystal semiconductor processing wafer. Semiconductor materials suitable for forming a well-rich layer in a semiconductor device on an insulating layer are suitably capable of forming a highly defective layer in a manufacturing device. Such materials include polycrystalline semiconductor materials and amorphous semiconductor materials. Materials that can be polycrystalline or amorphous include silicon (Si), silicon germanium (SiGe), carbon-doped silicon (SiC) and germanium (Ge). Polycrystalline silicon refers to a material including small silicon crystals with random crystal orientation. The size of a polycrystalline silicon die can be as small as about 20 nanometers. According to the method of the present invention, the smaller the crystal die size of the deposited polycrystalline silicon, the higher the defect rate in the well-rich layer. Amorphous silicon includes non-crystalline allotropic silicon, which lacks short-range and long processes. Silicon dies with a crystallinity of no more than about 10 nanometers can also be considered to be substantially amorphous. Silicon germanium includes alloys of silicon germanium in any molar ratio of silicon and germanium. Carbon-doped silicon includes compounds of silicon and carbon, which can vary in molar ratios of silicon and carbon. The resistivity of the polysilicon well-rich layer may be at least 100 ohm-cm, at least about 500 ohm-cm, at least about 1000 ohm-cm, or even at least about 3000 ohm-cm, such as between about 100 ohm-cm and about 100,000 ohm-cm, or between about 500 ohm-cm and about 100,000 ohm-cm, or between about 1000 ohm-cm and about 100,000 ohm-cm, or between about 500 ohm-cm and about 100,000 ohm-cm. ohm-cm to about 10,000 ohm-cm, or between about 750 ohm-cm to about 10,000 ohm-cm, between about 1000 ohm-cm to about 10,000 ohm-cm, between about 2000 ohm-cm to about 10,000 ohm-cm, between about 3000 ohm-cm to about 10,000 ohm-cm, or between about 3000 ohm-cm to about 8,000 ohm-cm.

[0044] The material for deposition onto the optional oxidized front surface of the single crystal semiconductor handle wafer may be deposited by means known in the art. For example, the semiconductor material may be deposited using metal organic chemical vapor deposition (MOCVD), physical vapor deposition (PVD), chemical vapor deposition (CVD), low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), or molecular beam epitaxy (MBE). Silicon precursors for LPCVD or PECVD include methylsilane, tetrahydrosilane (silane), trisilane, disilane, pentasilane, neopentasilane, tetrasilane, dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), and other silicon precursors. For example, polycrystalline silicon may be deposited onto the surface oxide layer by pyrolyzing silane (SiH4) in a temperature range between about 550°C to about 690°C, such as between about 580°C to about 650°C. The chamber pressure may range from about 70 mTorr to about 400 mTorr. Amorphous silicon can be deposited by plasma enhanced chemical vapor deposition (PECVD) at a temperature generally ranging between about 75°C to about 300°C. Silicon germanium (especially amorphous silicon germanium) can be deposited by chemical vapor deposition comprising an organic germanium compound (e.g., isobutylgermane, alkylgermanium trichloride, and dimethylaminogermanium trichloride) at a temperature up to about 300°C. Carbon-doped silicon can be deposited by thermal plasma chemical vapor deposition in an epitaxial reactor using precursors such as silicon tetrachloride and methane. Suitable carbon precursors for CVD or PECVD include methylsilane, methane, ethane, ethylene, and other carbon precursors. For LPCVD deposition, methylsilane is a particularly preferred precursor because it provides both carbon and silicon. For PECVD deposition, the preferred precursors include silane and methane. In some embodiments, the silicon layer may include a carbon concentration of at least about 1% based on atoms, for example, between about 1% based on atoms and about 10% based on atoms.

[0045] In some embodiments, the deposition of the semiconductor material of the well-rich layer may be temporarily interrupted at least once and preferably more than once in order to prepare multiple layers of well-rich material. The intermediate surface of the semiconductor material film may be exposed to an inert, oxidizing, nitriding or passivating atmosphere to thereby damage or passivate the deposited semiconductor material. In other words, the method of the present invention may include depositing multiple layers of well-rich semiconductor material through a cyclic process in which semiconductor material is deposited, the deposition is interrupted, the semiconductor material layer is damaged or passivated, and the next layer of semiconductor material is deposited. In some embodiments, a multilayer including a passivating semiconductor layer may be formed and an additional semiconductor layer may be deposited to form a well-rich layer. In some embodiments, the multilayer includes more than one passivating semiconductor layer and an additional semiconductor layer in the well-rich layer. By depositing the well-rich layer in this manner, a multilayer comprising, for example, one or more passivation layers, or two or more passivation layers (e.g., three or more passivation layers, such as at least 4 passivation layers, or between 4 and about 100 passivation layers, or between 4 and about 60 passivation layers, or between 4 and about 50 passivation layers, or between 4 and about 25 passivation layers, or between 6 and about 20 passivation layers) of semiconductor material is deposited onto a handling substrate. A large number of semiconductor layers can be deposited, limited in part by throughput requirements and by the minimum practical layer thickness that can be deposited, which is currently about 20 nanometers. Each of such layers of semiconductor material is damaged or passivated so that during the high temperature process of semiconductor fabrication on insulating layers, die growth in each layer of the multilayer is limited by the thickness of the passivating multilayer, rather than by the thickness of the entire well-rich layer as in prior art processes. In some embodiments, the semiconductor layer may be passivated by exposing the first semiconductor layer to an atmosphere including a nitrogen-containing gas, such as nitrogen, nitrous oxide, ammonia (NH3), nitrogen plasma, and any combination thereof. In this regard, the atmosphere in which the semiconductor layer is deposited may include a nitrogen-containing gas, such as nitrogen, and termination of the deposition process followed by exposure to the gas may be sufficient to form a thin passivation layer over the semiconductor layer. In some embodiments, the chamber may be evacuated of the deposition gas and flushed with a nitrogen-containing gas in order to achieve passivation of the previously deposited semiconductor layer. Exposure to nitrogen may nitridate the deposited semiconductor layer, for example, resulting in the formation of a thin silicon nitride layer of only a few angstroms thick. Alternative passivation methods may be used. For example, the semiconductor layer may be passivated by exposing the first semiconductor layer to an atmosphere including an oxygen-containing gas, such as oxygen, ozone, water vapor, or any combination thereof. According to such embodiments, a thin layer of semiconductor oxide may be formed on the semiconductor layer, the semiconductor oxide being sufficient to passivate the layer. For example, a thin layer of silicon oxide may be formed between each layer of the multilayer. The oxide layer may be only a few angstroms thick, such as between about 1 angstrom to about 20 angstroms, or between about 1 angstrom to about 10 angstroms. In some embodiments, air including both nitrogen and oxygen may be used as the passivation gas.In some embodiments, the semiconductor layer may be passivated by exposing the first semiconductor layer to a liquid selected from the group consisting of water, a peroxide (eg, a hydrogen peroxide solution), or a SCl solution (NH 3 :H 2 O 2 :H 2 O).

[0046] The total thickness of the well-rich layer may be between about 0.3 microns and about 5 microns, such as between about 0.3 microns and about 3 microns, such as between about 0.3 microns and about 2 microns or between about 2 microns and about 3 microns.

[0047] In some embodiments, the deposition of the well-rich layer is followed by the formation of a dielectric layer on the surface of the well-rich layer. In some embodiments, a single semiconductor handling substrate (e.g., a single crystal silicon handling substrate) is oxidized to form a semiconductor oxide (e.g., silicon dioxide) film on the well-rich layer. In some embodiments, the well-rich layer (e.g., a polycrystalline film) may be thermally oxidized (wherein some portion of the deposited semiconductor material film will be consumed) or the semiconductor oxide (e.g., silicon dioxide) film may be grown by CVD oxide deposition. The oxide layer (e.g., silicon dioxide layer) in contact with the polycrystalline or amorphous well-rich layer (e.g., a polycrystalline or amorphous silicon well-rich layer) may have a thickness between about 0.1 microns to about 10 microns, such as between about 0.1 microns to about 4 microns, such as between about 0.1 microns to about 2 microns, or between about 0.1 microns to about 1 micron. The oxidation process additionally oxidizes the back surface of the single crystal semiconductor handling wafer, which advantageously reduces warping and bowing potentially caused by the different thermal expansion coefficients of silicon and silicon dioxide.

[0048] III. Preparation of the Bonding Structure

[0049] A single crystal semiconductor handle wafer (e.g., a single crystal silicon handle wafer) prepared according to a floating zone method is then bonded to a single crystal semiconductor donor wafer prepared according to a conventional layer transfer method. In a preferred embodiment, the single crystal semiconductor donor wafer comprises a material selected from the group consisting of silicon, silicon carbide, silicon germanium, gallium arsenide, gallium nitride, indium phosphide, indium gallium arsenide, germanium, and combinations thereof. The donor wafer may be sliced ​​from an ingot prepared by a floating zone or Czochralski method. The wafer thickness may vary from about 100 microns to about 5000 microns, such as between about 100 microns to about 1500 microns, such as between about 250 microns to about 1500 microns, such as between about 300 microns to about 1000 microns, suitably in the range of about 500 microns to about 1000 microns. In some specific embodiments, the wafer thickness may be about 725 microns. In some embodiments, the wafer thickness may be about 775 microns. Depending on the desired properties of the final integrated circuit device, the single crystal semiconductor (e.g., silicon) donor wafer may include electrically active dopants such as boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type). The resistivity of the single crystal semiconductor (e.g., silicon) donor wafer may range from 1 ohm-cm to 100 ohm-cm, 1 ohm-cm to 50 ohm-cm, or 5 ohm-cm to 25 ohm-cm. The single crystal semiconductor donor wafer may be subjected to standard process steps including oxidation, implantation, and post-implantation cleaning. Accordingly, the single crystal semiconductor donor wafer, which has been etched and polished and optionally oxidized, is subjected to ion implantation to form a damage layer in the donor substrate.

[0050] In some embodiments, the single crystal semiconductor donor wafer includes a dielectric layer. The dielectric layer may include one or more insulating layers formed on the front surface of the single crystal semiconductor donor wafer. The insulating layer may include a material selected from the group consisting of silicon dioxide, silicon nitride, and silicon oxynitride. In some embodiments, the insulating layer may include a material selected from the group consisting of Al2O3, AlN, or a combination thereof. In some embodiments, the dielectric layer includes multiple layers of insulating material, but other configurations are within the scope of the present invention. Each insulating layer may include a material selected from the group consisting of silicon dioxide, silicon nitride, and silicon oxynitride. In some embodiments, the dielectric layer includes three layers of insulating material in the order of silicon dioxide, silicon nitride, and silicon dioxide. Each insulating layer may have a thickness of at least about 10 nanometers thick, such as between about 10 nanometers to about 10,000 nanometers, between about 10 nanometers to about 5,000 nanometers, between 50 nanometers to about 400 nanometers, or between about 100 nanometers to about 400 nanometers, such as about 50 nanometers, 100 nanometers, or 200 nanometers.

[0051] Ion implantation can be performed in commercially available instruments such as Applied Materials Quantum II, Quantum H, Quantum LEAP, or Quantum X. The implanted ions include He, H, H2, or a combination thereof. The ion implantation is performed at a density and duration sufficient to form a damaged layer in the semiconductor donor substrate. The implantation density can range from about 10 12 ions / cm 2 To about 10 17 ions / cm 2 , for example from about 10 14 ions / cm 2 To about 10 17 ions / cm 2 , for example from about 10 15 ions / cm 2 To about 10 17 ions / cm 2 , or from about 10 16 ions / cm 2 To about 10 17 ions / cm 2 . The implantation energy may range from about 1 keV to about 3,000 keV, such as from about 10 keV to about 3,000 keV. The implantation energy may range from about 1 keV to about 3,000 keV, such as from about 5 keV to about 1,000 keV, or from about 5 keV to about 200 keV, or from 5 keV to about 100 keV, or from 5 keV to about 80 keV. The implantation depth determines the thickness of the single crystal semiconductor device layer transferred to the treatment in the SOI process. The ions may be implanted to a depth of between about 100 angstroms to about 30,000 angstroms, such as between about 200 angstroms to about 20,000 angstroms, such as between about 2000 angstroms to about 15,000 angstroms, or between about 15,000 angstroms to about 30,000 angstroms. In some embodiments, it may be desirable to subject the single crystal semiconductor donor wafer (e.g., a single crystal silicon donor wafer) to cleaning after implantation. In some preferred embodiments, cleaning may include a Piranha clean followed by a DI water rinse and a SC1 / SC2 clean.

[0052] In some embodiments of the present invention, wherein there is a He + , H + 、H2 +A single crystal semiconductor donor wafer having an ion implanted region formed by any combination of ion implantation and ion implantation thereof is annealed at a temperature sufficient to form a thermally activated cleavage plane in the single crystal semiconductor donor substrate. An example of a suitable tool may be a simple box furnace, such as a Blue M model. In some preferred embodiments, the ion-implanted single crystal semiconductor donor substrate is annealed at a temperature from about 200° C. to about 350° C., from about 225° C. to about 325° C., preferably about 300° C. The thermal annealing may occur for a duration of from about 2 hours to about 10 hours, such as from about 2 hours to about 8 hours. Thermal annealing within these temperature ranges is sufficient to form a thermally activated cleavage plane. After the thermal annealing to activate the cleavage plane, the surface of the single crystal semiconductor donor substrate is optionally cleaned.

[0053] In some embodiments, the ion implanted and optionally cleaned and optionally annealed single crystal semiconductor donor wafer is subjected to oxygen plasma and / or nitrogen plasma surface activation. In some embodiments, the oxygen plasma surface activation tool is a commercially available tool, such as a tool available from EV Group, such as Low temperature plasma activation system. An ion implanted and optionally cleaned single crystal semiconductor donor wafer is loaded into a chamber. The chamber is evacuated and backfilled with O2 to a pressure less than atmospheric pressure to thereby generate a plasma. The single crystal semiconductor donor wafer is exposed to such plasma for a desired time, which may range from about 1 second to about 120 seconds. Oxygen plasma surface oxidation is performed so as to render the front surface of the single crystal semiconductor donor substrate hydrophilic and capable of being bonded to a single crystal semiconductor handle substrate prepared according to the method described above.

[0054] The hydrophilic front surface of the single crystal semiconductor donor wafer and the front surface of the single crystal semiconductor handle wafer are then brought into close contact to thereby form a bonded structure. According to the method of the present invention, each of the front surface of the single crystal semiconductor donor wafer and the front surface of the single crystal semiconductor handle wafer may include one or more insulating layers. The insulating layer forms a dielectric layer of the bonded structure.

[0055] Since the mechanical bond may be relatively weak, the bonded structure may be further annealed to strengthen the bond between the single crystal semiconductor donor wafer and the single crystal semiconductor handle wafer. In some embodiments of the present invention, the bonded structure is annealed at a temperature sufficient to form a thermally activated cleavage plane in the single crystal semiconductor donor substrate. An example of a suitable tool may be a simple box furnace, such as the Blue M model. In some embodiments, the bonded structure is annealed at a temperature from about 200° C. to about 400° C., from about 300° C. to about 400° C., such as from about 350° C. to about 400° C.

[0056] In some embodiments, annealing may occur at a relatively high pressure, such as between about 0.5 MPa and about 200 MPa, such as between about 0.5 MPa and about 100 MPa, such as between about 0.5 MPa and about 50 MPa, or between about 0.5 MPa and about 10 MPa, or between about 0.5 MPa and about 5 MPa. In conventional bonding methods, the temperature may be limited by thermal cleavage. This occurs when the pressure of the thin plate at the implant surface exceeds the external equalizing pressure. Accordingly, conventional annealing may be limited to a bonding temperature between about 350° C. and about 400° C. due to thermal cleavage. After implantation and bonding, the wafers are weakly held together. However, the gap between the wafers is sufficient to prevent gas infiltration or escape. The weak bond can be strengthened by thermal treatment, but the cavity formed during implantation is filled with gas. When heated, the gas in the cavity is pressurized. It is estimated that the pressure can reach 0.2 to 1 GPa depending on the dose (Cherkashin et al., J. Appl. Phys. 118, 245301 (2015)). When the pressure exceeds a critical value, the layers delaminate. This is called thermal cleavage. It prevents higher temperatures or longer times in annealing. According to some embodiments of the present invention, bonding occurs at high pressure, for example, between about 0.5 MPa and about 200 MPa, for example, between about 0.5 MPa and about 100 MPa, for example, between about 0.5 MPa and about 50 MPa, or between about 0.5 MPa and about 10 MPa, or between about 0.5 MPa and about 5 MPa, thereby achieving bonding at high temperature. In some embodiments, the bonded structure is annealed at a temperature from about 300°C to about 700°C, from about 400°C to about 600°C, such as between about 400°C to about 450°C, or even between about 450°C to about 600°C, or between about 350°C to about 450°C. Increasing the thermal budget will have a positive effect on the bond strength. The thermal annealing may occur for a duration of from about 0.5 hours to about 10 hours, such as between about 0.5 hours to about 3 hours, preferably about 2 hours. The thermal annealing within such a temperature range is sufficient to form a thermally activated cleavage plane. In conventional bond annealing, the edges of both the handling wafer and the donor wafer may become far apart due to edge drop. In this region, there is no layer transfer. It is referred to as a step. It is expected that pressurized bonding reduces this step, extending the SOI layer further outward toward the edge. The mechanism is based on the capture air bag being compressed and "zipping" outward. After the thermal annealing to activate the cleavage plane, the bonded structure can be cleaved.

[0057] After thermal annealing, the bond between the single crystal semiconductor donor wafer and the single crystal semiconductor handle wafer is strong enough to initiate layer transfer by cleaving the bonded structure at the cleavage plane. The cleaving can occur according to techniques known in the art. In some embodiments, the bonded structure can be placed on a conventional cleaving table, which is attached to a fixed suction cup on one side and to an articulated arm on the other side through an additional suction cup. The crack is initiated near the suction cup attachment and the movable arm is pivoted about the hinge, thereby cleaving the wafer. The cleaving removes a portion of the semiconductor donor wafer, thereby leaving a single crystal semiconductor device layer 26 (preferably a silicon device layer) on the semiconductor-on-insulator (composite) structure 20. See. Figure 2 .

[0058] After cleaving, the cleaved structure may be subjected to a high temperature anneal in order to further strengthen the bond between the transferred device layer 26 and the single crystal semiconductor handle wafer 20. An example of a suitable tool may be a vertical furnace, such as an ASM A400. In some preferred embodiments, the bonded structure is annealed at a temperature from about 1000° C. to about 1200° C., preferably at about 1000° C. The thermal annealing may occur for a duration from about 0.5 hours to about 8 hours, preferably for a duration of about 4 hours. Thermal annealing within these temperature ranges is sufficient to strengthen the bond between the transferred device layer and the single crystal semiconductor handle substrate.

[0059] After cleaving and high temperature annealing, the bonded structure may be subjected to a cleaning process designed to remove thin thermal oxides and clean particles from the surface. In some embodiments, the single crystalline semiconductor device layer may achieve a desired thickness and smoothness by being subjected to a vapor phase HCl etching process in a horizontal flow single wafer epitaxial reactor using H2 as a carrier gas. In some embodiments, the semiconductor device layer 26 may have a thickness between about 20 nanometers to about 3 micrometers, such as between about 20 nanometers to about 2 micrometers, such as between about 20 nanometers to about 1.5 micrometers or between about 1.5 micrometers to about 3 micrometers.

[0060] In some embodiments, an epitaxial layer may be deposited on the transferred single crystalline semiconductor device layer 26. The deposited epitaxial layer may include substantially the same electrical characteristics as the underlying single crystalline semiconductor device layer 26. Alternatively, the epitaxial layer may include different electrical characteristics than the underlying single crystalline semiconductor device layer 26. The epitaxial layer may include a material selected from the group consisting of silicon, silicon carbide, silicon germanium, gallium arsenide, gallium nitride, indium phosphide, indium gallium arsenide, germanium, and combinations thereof. Depending on the desired properties of the final integrated circuit device, the epitaxial layer may include electrically active dopants such as boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type). The resistivity of the epitaxial layer may range from 1 ohm-cm to 1050 ohm-cm, from 1 ohm-cm to 50 ohm-cm, and typically from 5 ohm-cm to 25 ohm-cm. In some embodiments, the epitaxial layer can have a thickness between about 20 nanometers and about 3 micrometers, such as between about 20 nanometers and about 2 micrometers, such as between about 20 nanometers and about 1.5 micrometers or between about 1.5 micrometers and about 3 micrometers.

[0061] Next, the completed SOI wafer including the single crystal semiconductor handle wafer 22, well-rich layer 28, dielectric layer 24, and semiconductor device layer 26 may be subjected to end-of-line metrology inspection and a final cleaning using a typical SC1-SC2 process.

[0062] When introducing elements of the present invention or embodiments thereof, the articles "a," "an," "the," and "said" are intended to mean that there are one or more elements. The terms "comprising," "including," and "having" are intended to be inclusive and mean that there may be additional elements other than the listed elements.

[0063] As various changes could be made in the above without departing from the scope of the invention, it is intended that all matter contained in the above description and shown in the accompanying drawings shall be interpreted as illustrative and not in a limiting sense.

Claims

1. A multilayer structure comprising: A single crystal silicon wafer handling substrate comprising two major, substantially parallel surfaces, one of which is a front surface of the single crystal silicon wafer handling substrate and the other of which is a rear surface of the single crystal silicon wafer handling substrate, a circumferential edge joining the front surface and the rear surface of the single crystal silicon wafer handling substrate, and a central plane of the single crystal silicon wafer handling substrate between the front surface and the rear surface of the single crystal silicon wafer handling substrate, wherein the single crystal silicon wafer handling substrate has a bulk resistivity of at least about 5000 ohm-cm, a resistivity of less than about 1×10 16 atoms / cm 3 The interstitial oxygen concentration is at least about 1×10 13 atoms / cm 3 The nitrogen concentration of the single crystal silicon wafer handling substrate comprises less than 1×10 12 atoms / cm 3 A p-type dopant having a concentration of , and further wherein the concentration of the oxygen-thermal dual donor, the new donor, and the excess thermal donor or any combination thereof is at least one order of magnitude less than the concentration of the p-type dopant; a well-rich layer in interfacial contact with the front surface of the single crystal silicon wafer handle substrate; a dielectric layer in interface contact with the well-rich layer; and A single crystal semiconductor device layer is in interface contact with the dielectric layer.

2. The multilayer structure of claim 1, wherein the single crystal silicon wafer handling substrate comprises a silicon wafer sliced ​​from a single crystal silicon ingot grown by a floating zone method, and further wherein the silicon wafer has a diameter of at least about 150 mm.

3. The multilayer structure of claim 1, wherein the single crystal silicon wafer handling substrate comprises a silicon wafer sliced ​​from a single crystal silicon ingot grown by a floating zone method, and further wherein the silicon wafer has a diameter of at least about 200 mm.

4. The multilayer structure of claim 1 wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 7,500 ohm-cm.

5. The multi-layer structure of claim 1 wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 10,000 ohm-cm.

6. The multi-layer structure of claim 1 wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 15,000 ohm-cm.

7. The multi-layer structure of claim 1 wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 20,000 ohm-cm.

8. The multi-layer structure of claim 1 wherein the single crystal silicon wafer handle substrate has a bulk resistivity of less than about 100,000 ohm-cm.

9. The multilayer structure according to claim 1, wherein the single crystal silicon wafer handling substrate has a thickness of less than 1×10 11 Donor body / cm 3 Excess heat donor concentration.

10. The multilayer structure according to claim 1, wherein the single crystal silicon wafer handling substrate has a thickness of less than 5×10 10 Donor body / cm 3 Excess heat donor concentration.

11. The multilayer structure of claim 1, wherein the single crystal silicon wafer handling substrate comprises less than 1×10 11 atoms / cm 3 The p-type dopant has a concentration of, and further wherein the concentration of the oxygen-thermal dual donor, the new donor and the excess thermal donor or any combination thereof is at least one order of magnitude less than the concentration of the p-type dopant.

12. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 1×10 15 atoms / cm 3 interstitial oxygen concentration.

13. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness of at least about 1×10 14 atoms / cm 3 of the nitrogen concentration.

14. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 3×10 15 atoms / cm 3 of the nitrogen concentration.

15. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 1×10 15 atoms / cm 3 of the nitrogen concentration.

16. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 7×10 14 atoms / cm 3 of the nitrogen concentration.

17. The multilayer structure of claim 1, wherein the single crystal silicon wafer handle substrate has a thickness between about 5×10 14 atoms / cm 3 To about 2×10 15 atoms / cm 3 of the nitrogen concentration.

18. The multi-layer structure of claim 1, wherein the well-rich layer comprises one or more polycrystalline semiconductor layers, wherein each of the one or more polycrystalline semiconductor layers comprises a material selected from the group consisting of silicon, SiGe, SiC, and Ge.

19. The multilayer structure of claim 1, wherein the well-rich layer comprises one or more amorphous semiconductor layers, wherein each of the one or more amorphous semiconductor layers comprises a material selected from the group consisting of silicon, SiGe, SiC, and Ge.

20. The multi-layer structure of claim 1, wherein the well rich layer has a resistivity greater than about 1000 Ohm-cm.

21. The multi-layer structure of claim 1, wherein the well-rich layer has a resistivity greater than about 3000 Ohm-cm.

22. The multi-layer structure of claim 1, wherein the well-rich layer has a resistivity between about 2000 ohm-cm and about 10,000 ohm-cm.

23. The multi-layer structure of claim 1, wherein the well-rich layer has a resistivity between about 3000 ohm-cm and about 10,000 ohm-cm.

24. The multi-layer structure of claim 1, wherein the well-rich layer has a resistivity between about 3000 ohm-cm and about 5000 ohm-cm.

25. The multi-layer structure of claim 1, wherein the well-rich layer has a thickness between about 0.1 microns and about 50 microns.

26. The multilayer structure of claim 1, wherein the dielectric layer comprises a material selected from silicon dioxide, silicon nitride, silicon oxynitride, hafnium oxide, titanium oxide, zirconium oxide, lanthanum oxide, barium oxide, aluminum oxide, aluminum nitride, and any combination thereof.

27. A multilayer structure comprising: A single crystal silicon wafer handling substrate comprising two major, substantially parallel surfaces, one of which is a front surface of the single crystal silicon wafer handling substrate and the other of which is a rear surface of the single crystal silicon wafer handling substrate, a circumferential edge joining the front surface and the rear surface of the single crystal silicon wafer handling substrate, and a central plane of the single crystal silicon wafer handling substrate between the front surface and the rear surface of the single crystal silicon wafer handling substrate, wherein the single crystal silicon wafer handling substrate has a bulk resistivity of at least about 5000 ohm-cm, a resistivity of less than about 1×10 16 atoms / cm 3 The interstitial oxygen concentration is at least about 1×10 13 atoms / cm 3 The nitrogen concentration of the single crystal silicon wafer handling substrate comprises less than 1×10 12 atoms / cm 3 and further wherein the concentration of the oxygen-thermal dual donor, the new donor, and the excess thermal donor or any combination thereof is at least one order of magnitude less than the concentration of the n-type dopant; a well-rich layer in interfacial contact with the front surface of the single crystal silicon wafer handle substrate; a dielectric layer in interface contact with the well-rich layer; and A single crystal semiconductor device layer is in interface contact with the dielectric layer.

28. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handling substrate comprises a silicon wafer sliced ​​from a single crystal silicon ingot grown by a floating zone method, and further wherein the silicon wafer has a diameter of at least about 150 mm.

29. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handling substrate comprises a silicon wafer sliced ​​from a single crystal silicon ingot grown by a floating zone method, and further wherein the silicon wafer has a diameter of at least about 200 mm.

30. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 7,500 ohm-cm.

31. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 10,000 ohm-cm.

32. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 15,000 ohm-cm.

33. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a bulk resistivity of at least about 20,000 ohm-cm.

34. The multi-layer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a bulk resistivity of less than about 100,000 ohm-cm.

35. The multilayer structure of claim 27, wherein the single crystal silicon wafer handling substrate has a thickness of less than 1×10 11 Donor body / cm 3 Excess heat donor concentration.

36. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of less than 5×10 10 Donor body / cm 3 Excess heat donor concentration.

37. The multilayer structure of claim 27, wherein the single crystal silicon wafer handling substrate comprises less than 1×10 11 atoms / cm 3 and further wherein the concentration of the oxygen-thermal dual donor, the new donor, and the excess thermal donor, or any combination thereof, is at least one order of magnitude less than the concentration of the n-type dopant.

38. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 1×10 15 atoms / cm 3 interstitial oxygen concentration.

39. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of at least about 1×10 14 atoms / cm 3 of nitrogen concentration.

40. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 3×10 15 atoms / cm 3 of nitrogen concentration.

41. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 1×10 15 atoms / cm 3 of nitrogen concentration.

42. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness of less than about 7×10 14 atoms / cm 3 of nitrogen concentration.

43. The multilayer structure of claim 27, wherein the single crystal silicon wafer handle substrate has a thickness between about 5×10 14 atoms / cm 3 To about 2×10 15 atoms / cm 3 The nitrogen concentration between 44. The multi-layer structure of claim 27, wherein the well-rich layer comprises one or more polycrystalline semiconductor layers, wherein each of the one or more polycrystalline semiconductor layers comprises a material selected from the group consisting of silicon, SiGe, SiC, and Ge.

45. The multi-layer structure of claim 27, wherein the well-rich layer comprises one or more amorphous semiconductor layers, wherein each of the one or more amorphous semiconductor layers comprises a material selected from the group consisting of silicon, SiGe, SiC, and Ge.

46. ​​The multi-layer structure of claim 27, wherein the well rich layer has a resistivity greater than about 1000 Ohm-cm.

47. The multi-layer structure of claim 27, wherein the well-rich layer has a resistivity greater than about 3000 Ohm-cm.

48. The multi-layer structure of claim 27, wherein the well rich layer has a resistivity between about 2000 ohm-cm and about 10,000 ohm-cm.

49. The multi-layer structure of claim 27, wherein the well rich layer has a resistivity between about 3000 ohm-cm and about 10,000 ohm-cm.

50. The multi-layer structure of claim 27, wherein the well rich layer has a resistivity between about 3000 ohm-cm and about 5,000 ohm-cm.

51. The multi-layer structure of claim 27, wherein the well-rich layer has a thickness between about 0.1 microns and about 50 microns.

52. The multilayer structure of claim 27, wherein the dielectric layer comprises a material selected from silicon dioxide, silicon nitride, silicon oxynitride, hafnium oxide, titanium oxide, zirconium oxide, lanthanum oxide, barium oxide, aluminum oxide, aluminum nitride, and any combination thereof.