Secondary battery and electric device
By jointly controlling the OI value, resistance value R and mass proportion of chain carboxylic acid ester solvent of the negative electrode sheet, combined with additives in the nonaqueous electrolyte, the pole structure and electrolyte composition of the secondary battery are optimized, and the secondary battery is solved by solving the problem of the secondary battery Inadequate in fast charging, cycle and safety performance has achieved more efficient battery performance.
Patent Information
- Application Number
- CN202411114358.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-26
AI Technical Summary
The existing secondary batteries have shortcomings in fast charging performance, cycle performance and safety performance, especially the poor interface stability between the chain carboxylic acid ester and the negative electrode, resulting in the expansion of the electrode sheet and the attenuation of the battery cell capacity.
By jointly controlling the OI value, resistance value R and mass proportion of chain carboxylic acid ester solvent in the secondary battery, combining the additives in the nonaqueous electrolyte, the structure and electrolyte composition of the negative electrode sheet are optimized, and a Suitable pole orientation and interface stability to improve fast charging performance, cycle performance and safety.
The secondary battery has been comprehensively optimized in fast charging performance, cycle performance and safety performance, reducing the pole expansion rate and cell expansion, improving the low-temperature performance and cycle stability of the battery, and extending the battery life.
Smart Images

Figure CN119029322A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No.: 202380010051.X, filed on April 28, 2023, with the invention name “Secondary Battery and Electrical Device”. Technical Field
[0002] The present application relates to the technical field of secondary batteries, and in particular to secondary batteries and electrical devices. Background Art
[0003] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0004] With the development of secondary battery technology, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in electronic equipment power supplies, power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the development of science and technology and society, higher comprehensive requirements are put forward for the fast charging performance, cycle performance, safety performance and other aspects of secondary batteries.
[0005] Therefore, it is currently necessary to develop new secondary battery technologies that can take into account fast charging performance, cycle performance and safety performance. Summary of the invention
[0006] In view of the above problems, the present application provides a secondary battery and an electrical device, wherein the secondary battery includes a reasonably matched negative electrode plate and a non-aqueous electrolyte, and has excellent comprehensive functions in terms of fast charging performance, cycle performance and safety performance.
[0007] In a first aspect, the present application provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet and a non-aqueous electrolyte; wherein the negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a graphite material; the non-aqueous electrolyte includes a solvent, the solvent includes a first solvent, and the first solvent is a chain carboxylate;
[0008] The OI value of the negative electrode plate, the resistance value R of the negative electrode plate and the mass proportion W0 of the first solvent in the solvent satisfy the following relationship: 0.08 / mΩ≤W0×100 / (R×OI)≤5 / mΩ;
[0009] The OI value of the negative electrode plate refers to the ratio of the diffraction peak intensity of the 004 crystal plane of the graphite material to the diffraction peak intensity of the 110 crystal plane; the unit of R is mΩ.
[0010] The OI value of the negative electrode sheet reflects the degree of anisotropy in the grain arrangement direction in the negative electrode active material layer. By synergistically controlling the OI value of the negative electrode sheet, the resistance value R of the negative electrode sheet and the mass proportion W0 of the chain carboxylate solvent in the solvent, the fast charging performance, cycle performance and safety performance of the secondary battery can be taken into account. When the OI value, R and W0 satisfy the above relationship, on the one hand, the chain carboxylic acid ester in the non-aqueous electrolyte has the characteristics of low viscosity and conductivity, which can significantly enhance the conductivity of the battery, and can also improve the low temperature performance and cycle stability of the battery. On the other hand, the negative electrode sheet has a suitable orientation degree and has a suitable directional selectivity in the active ion (such as lithium ion) embedding process, which can disperse the active ion embedding expansion (such as lithium embedding expansion) in different directions, thereby reducing the cycle expansion of the electrode sheet and the battery cell, which can effectively alleviate the problem of the aggravated expansion of the electrode sheet itself due to the poor interface stability between the chain carboxylic acid ester and the negative electrode, improve battery safety, and reduce the concentration polarization of active ions in the transmission process of the negative electrode sheet, and achieve a significant improvement in the fast charging capability of the battery in combination with the negative electrode sheet resistance value R. Therefore, by synergistically controlling the OI value, R and W0, the secondary battery can have excellent comprehensive functions in terms of fast charging performance, cycle performance and safety performance, and can take into account a shorter fast charging time, lower cycle expansion and higher cycle capacity retention rate.
[0011] In some embodiments, 6≤OI≤25; optionally, 6≤OI≤18; further optionally, 12≤OI≤18.
[0012] By adjusting the QI value within a more appropriate range, it is more conducive to reducing the directional selectivity in the active ion embedding process, so that the active ions can be better embedded and expanded and dispersed in different directions; in addition, the active ion transport performance of the negative electrode can also be better improved.
[0013] In some embodiments, 1 mΩ≤R≤50 mΩ; optionally, 5 mΩ≤R≤30 mΩ; further optionally, 10 mΩ≤R≤20 mΩ.
[0014] By controlling the resistance value R of the negative electrode sheet within a certain range, W0×100 / (R×OI) can be controlled within a more appropriate range, thereby achieving better comprehensive effects in terms of shorter fast charging time, lower cycle expansion and higher cycle capacity retention rate, and is more conducive to improving the active ion transport performance and electronic conduction performance of the negative electrode sheet.
[0015] In some embodiments, 10%≤W0≤80%;
[0016] Optionally, 20%≤W0≤80%; further optionally, 30%≤W0≤70%; further optionally, 50%≤W0≤70%;
[0017] Alternatively, 10%≤W0≤60%; further preferably, 20%≤W0≤60%.
[0018] By controlling the content W0 of the first solvent in the solvent within a certain range, it is possible to enhance the conductivity of the battery while taking into account the fast charging performance, cycle performance and safety performance of the secondary battery, and to improve the low temperature performance and cycle stability of the secondary battery.
[0019] In some embodiments, 0.67≤W0×100 / OI≤10;
[0020] Optionally, 1≤W0×100 / OI≤10; further optionally, 1≤W0×100 / OI≤5; further optionally, 3≤W0×100 / OI≤5;
[0021] Alternatively, 0.67≤W0×100 / OI≤4; further preferably, 1≤W0×100 / OI≤4.
[0022] On the basis of controlling W0×100 / (R×OI) to conform to the above relationship, the matching of the chain carboxylic acid ester in the non-aqueous electrolyte and the grain arrangement direction in the negative electrode active material layer is further regulated by W0×100 / OI, which makes it easier to achieve the improvement of the comprehensive performance of fast charging performance, cycle performance and safety performance.
[0023] In some embodiments, 0.1 / mΩ≤W0×100 / (R×OI)≤5 / mΩ; optionally, 0.1 / mΩ≤W0×100 / (R×OI)≤2 / mΩ.
[0024] Further controlling W0×100 / (R×OI) within the above range is more beneficial for comprehensively improving fast charging performance, cycle performance and safety performance.
[0025] In some embodiments, the secondary battery satisfies the following combination of characteristics: 6≤OI≤18, 10mΩ≤R≤20mΩ, and 20%≤W0≤80%;
[0026] Optionally, 12≤OI≤18, 10mΩ≤R≤20mΩ, and 10%≤W0≤60%; further optionally, 20%≤W0≤60%;
[0027] Alternatively, 12≤OI≤18, 10 mΩ≤R≤20 mΩ, and 50%≤W0≤70%.
[0028] By finely and synergistically controlling the OI value of the negative electrode plate to be 12-18, the resistance value R of the negative electrode plate to be 10mΩ-20mΩ, and the mass proportion W0 of the chain carboxylic acid ester solvent in the solvent to be 20%-80% (further optionally 10%-60%), it is possible to better achieve a balance between fast charging performance, cycle performance and safety performance, which is more conducive to making the secondary battery have better fast charging capability, lower cycle expansion and higher cycle capacity retention rate.
[0029] By controlling the values of different parameters, it is possible to further have advantages in one or more aspects. For example, in the case of 12≤OI≤18, 10mΩ≤R≤20mΩ, and 20%≤W0≤60%, it can have significantly excellent low cycle expansion and cycle performance on the basis of better comprehensive performance. For another example, in the case of 12≤OI≤18, 10mΩ≤R≤20mΩ, and 50%≤W0≤70%, on the basis of better comprehensive performance, it can also have obvious advantages in shorter fast charging time and lower cycle expansion.
[0030] In some embodiments, the first solvent comprises a compound having a structure as shown in formula (1):
[0031]
[0032] Wherein, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Haloalkyl;
[0033] Optionally, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Fluorinated alkyl;
[0034] Further optionally, R1 and R2 are independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl;
[0035] Further optionally, R1 and R2 are independently one of methyl, ethyl, fluoromethyl and fluoroethyl;
[0036] Further optionally, the first solvent includes one or more of the following compounds: methyl acetate, ethyl acetate, methyl difluoroacetate and ethyl difluoroacetate.
[0037] A first solvent with a smaller molecular size can be selected. In this case, the first solvent has a lower viscosity, which is beneficial for the secondary battery to obtain better fast charging performance.
[0038] In some embodiments, the non-aqueous electrolyte further includes a first additive; the first additive is diisocyanate.
[0039] In some embodiments, the first additive comprises a compound having the following structure:
[0040] O==C==N-R3-N==C==O Formula (2);
[0041] Wherein R3 is unsubstituted or Ra substituted C 1-18 Alkylene; Ra includes one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC(=O)R 11 , R 12 OC(=O)-、C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 One or more of oxaalkyl; R 11 and R 12 are independently alkyl or haloalkyl;
[0042] Optionally, R3 is C 2-10 Alkylene, C 2-10 Heteroalkylene, C 6-18 Arylene, C 2-18 Heteroarylene, C 3-18 Alicyclic or C 3-18 Heteroalicyclic group, any of the aforementioned groups is unsubstituted or substituted by Ra;
[0043] Alternatively, R3 is unsubstituted or Ra substituted C 2-10 Alkylene, unsubstituted or Ra substituted C 3-18 Bivalent cycloalkyl or unsubstituted or Ra substituted C 6-18 Arylene; further optionally, R3 is C 2-10 Alkylene, C 6-18 Divalent cycloalkyl or C 6-18 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-14 Divalent cycloalkyl or C 6-14 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-10 Divalent cycloalkyl or C 6-10 Arylene; further optionally, R3 is C 4-8 Hexylene, C containing hexyl ring 6-10 A divalent cycloalkyl or C containing a benzene ring 6-10 arylene;
[0044] Alternatively, the first additive includes one or more of the following compounds: hexamethylene diisocyanate, 1,4-cyclohexanedimethyl diisocyanate, 1,3-phenylene diisocyanate and 2,4-diisocyanato-1-toluene.
[0045] In some embodiments, the mass percentage of the first additive in the non-aqueous electrolyte is 0 to 11%;
[0046] Optionally, the mass percentage of the first additive in the non-aqueous electrolyte is 0.005% to 11%;
[0047] Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.005% to 10%;
[0048] Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.01% to 10%;
[0049] Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.1% to 5%;
[0050] Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 1% to 5%.
[0051] The introduction of chain carboxylic acid ester (first solvent) is conducive to improving the fast charging ability of the battery. However, due to the compatibility factors between carboxylic acid ester and negative electrode sheet, if the amount W0 is not well matched with the OI value and resistance value R of the negative electrode sheet, it may aggravate the expansion problem of the negative electrode sheet itself, and may also affect the gas production problem at the interface, and may also cause the attenuation of the battery cell capacity and the deterioration of the battery cycle performance. By introducing the first additive into the non-aqueous electrolyte, a protective solid electrolyte interface (SEI) layer can be formed on the surface of the negative electrode sheet. The protective layer can assist the active ions to be embedded into the negative electrode active material layer of the negative electrode sheet, so that the active ion embedding expansion effect of the negative electrode sheet can be evenly conducted in all directions, thereby reducing the cycle expansion rate of the negative electrode sheet. In addition, the first additive can also significantly improve the stability of the interface between the electrolyte and the negative electrode sheet, which can reduce the consumption of the electrolyte and the damage to the negative electrode structure during the cycle of the secondary battery, thereby significantly improving the cycle performance of the secondary battery.
[0052] In some embodiments, the non-aqueous electrolyte further comprises a second additive; the second additive comprises one or more of lithium monofluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, a compound represented by formula (3), and a fluorosulfonate;
[0053]
[0054] In formula (3), a, b and c are each independently a positive integer, m is an integer selected from 1 to 3, n is an integer selected from 0 to 4, and q is 0 or 1; M a+ is a metal ion with a positive charge; any Y is independently a boron atom or a phosphorus atom; X is a halogen atom; any R is independently a substituted or unsubstituted C 1-10 Alkylene, substituted or unsubstituted C 1-10 Haloalkylene, substituted or unsubstituted C 6-20 Arylene, and substituted or unsubstituted C 6-20 One of the halogenated arylene groups;
[0055] Optionally, any one R is independently Rc substituted or unsubstituted C 1-10 Alkylene, Rc substituted or unsubstituted C 1-10 Haloalkylene, Rc substituted or unsubstituted C 6-20 Arylene, and Rc substituted or unsubstituted C 6-20 A halogenated arylene group; C substituted with Rc 1-10 Substituents in alkylene, C substituted with Rc 1-10 Substituents in haloalkylene, C substituted with Rc 6-20 Substituents in arylene and Rc substituted C 6-20 The Rc substituents in the halogenated arylene group may each independently include one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC=(O)R 41 、-C=(O)OR 42 , C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 Alkoxy; wherein R 41 and R 42 Each independently is C 1-6 alkyl;
[0056] Optionally, in the non-aqueous electrolyte, M a+ Wherein M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni;
[0057] Optionally, a, b and c are each independently selected from 1, 2 or 3.
[0058] In some embodiments, the second additive includes one or more of lithium difluorophosphate, lithium monofluorophosphate, lithium tetrafluoroborate, lithium fluorosulfonate, and sodium fluorosulfonate.
[0059] In some embodiments, the mass percentage of the second additive in the non-aqueous electrolyte is 0.005% to 11%;
[0060] Optionally, the mass percentage of the second additive in the non-aqueous electrolyte is 0.005% to 11%;
[0061] Further, the mass proportion of the second additive in the non-aqueous electrolyte is 0.005% to 10%;
[0062] Further optionally, the mass proportion of the second additive in the non-aqueous electrolyte is 0.05% to 5%.
[0063] By introducing the second additive into the non-aqueous electrolyte, an inorganic-rich SEI film can be formed at the negative electrode, which can not only improve the fast charging performance of the secondary battery, but also further improve the cycle performance of the secondary battery.
[0064] In some embodiments, the volume average particle size D of the negative electrode active material is v 50≥6μm; among which, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the substance or material reaches 50%;
[0065] Optionally, the volume average particle size D of the negative electrode active material is v 50: 6μm~20μm;
[0066] Further optionally, the volume average particle size D of the negative electrode active material is v 50 is 15μm~20μm.
[0067] By controlling the particle size of the negative electrode active material to have a relatively large particle size, the contact area between the negative electrode material and the electrolyte can be reduced, and the probability of side reactions with the solvent on the negative electrode surface can be reduced, which is more conducive to reducing the electrode expansion rate and can better improve the cycle performance of the battery cell.
[0068] In some embodiments, the BET specific surface area of the negative electrode active material is 0.5 m 2 / g~2.0m 2 / g;
[0069] Optionally, the BET specific surface area of the negative electrode active material is 0.8 m 2 / g~1.5m 2 / g.
[0070] By controlling the particle size of the negative electrode active material to have a certain specific surface area, the surface area of the negative electrode material can be reduced, thereby reducing the contact area between the negative electrode material and the electrolyte, thereby reducing the side reactions of the solvent on the negative electrode surface and better improving the cycle performance of the battery cell.
[0071] In some embodiments, the graphite material includes one or more of artificial graphite and natural graphite; alternatively, the graphite material includes artificial graphite.
[0072] In some embodiments, the weight percentage of the graphite material in the negative electrode active material is ≥50%; optionally, the weight percentage of the graphite material in the negative electrode active material is ≥80%; further optionally, the weight percentage of the graphite material in the negative electrode active material is 100%.
[0073] In some embodiments, the secondary battery is a lithium ion secondary battery.
[0074] In a second aspect, the present application provides an electrical device, which includes the secondary battery described in the first aspect of the present application.
[0075] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] In order to better describe and illustrate the embodiments or examples of those applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered as limiting the scope of any of the disclosed applications, the embodiments or examples currently described, and the best modes of these applications currently understood. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the accompanying drawings:
[0077] Figure 1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0078] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown;
[0079] Figure 3 FIG. 1 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application.
[0080] Description of reference numerals:
[0081] 5, secondary battery; 51, shell; 52, electrode assembly; 53, cover plate; 6, power-consuming device. DETAILED DESCRIPTION
[0082] Below, some embodiments of the secondary battery and the electrical device of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0083] Numerical value " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be including end value or excluding end value, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 listed, and if the maximum range value 3,4 and 5 are also listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this application, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0084] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0085] If there is no special explanation, all steps of the present application may be performed sequentially or randomly, and may preferably be performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0086] If there is no special explanation, the words "have", "include", "contain" and "include" mentioned in this application can each independently represent an open or closed form. For example, the words "include" and "include" can also mean that other members or timing characteristics that are not listed can also be included or included, or can only include or include the listed members or timing characteristics. Members include materials or components, structures, elements, instruments, etc.; non-limiting examples of timing characteristics include actions, conditions for the occurrence of actions, timing, states, etc.
[0087] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". Further, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0088] In this application, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0089] In the present application, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" means a group consisting of A, B, and "a combination of A and B". Among them, "comprising A and / or B" can mean "comprising A, comprising B, and comprising A and B", and can also mean "comprising A, comprising B, or comprising A and B", which can be properly understood according to the sentence in which it is located.
[0090] In this application, "multiple", "multiple", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two. It is understood that when "any number" of items are involved, it refers to any suitable combination of multiple items, that is, the combination of "any number" of items is performed in a manner that does not conflict and can implement this application.
[0091] The terms "combination thereof", "any combination thereof", "any combination thereof" and the like used in this application include all suitable combinations of any two or more of the listed items.
[0092] In the present application, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the technical solution that can implement the present application.
[0093] In this application, "preferred" and "better" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of this application. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.
[0094] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0095] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.
[0096] In this application, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0097] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 3~5h or 3-5h both mean that the units of the left endpoint "3" and the right endpoint "5" are both h (hours).
[0098] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Furthermore, the weight described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0099] With the development of science and technology and society, higher comprehensive requirements are put forward for the fast charging performance, cycle performance, safety performance and other aspects of secondary batteries. Among them, the electrolyte has an important influence on the realization of the above comprehensive performance of secondary batteries. Compared with other types of ester solvents, chain carboxylates have a lower freezing point and smaller viscosity, which can significantly enhance the conductivity of the battery and improve the low temperature performance and cycle stability of the battery. However, the interface stability between chain carboxylates and the negative electrode is poor, which will not only aggravate the expansion problem of the electrode itself, but also affect the gas production problem at the interface, causing the battery capacity to decay too quickly and the battery cycle performance to deteriorate. In addition, this type of electrolyte will worsen the expansion problem of the electrode after long-term circulation, especially under high temperature and high pressure, which will seriously affect the service life of the battery and even bring safety problems.
[0100] In view of the above-mentioned common technical problems, in a first aspect, the present application provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet and a non-aqueous electrolyte; wherein the negative electrode sheet includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a graphite material; the non-aqueous electrolyte includes a solvent, the solvent includes a first solvent, and the first solvent is a chain carboxylic acid ester;
[0101] The OI value of the negative electrode plate, the resistance value R of the negative electrode plate and the mass proportion W0 of the first solvent in the solvent satisfy the following relationship: 0.08 / mΩ≤W0×100 / (R×OI)≤5 / mΩ;
[0102] The OI value of the negative electrode plate refers to the ratio of the diffraction peak intensity of the 004 crystal plane of the graphite material to the diffraction peak intensity of the 110 crystal plane; the unit of R is mΩ.
[0103] In the present application, unless otherwise specified, the electrode plate can be a positive electrode plate or a negative electrode plate, and the "active material" in the electrode plate refers to a substance that can reversibly embed and release active ions. Unless otherwise specified, "negative electrode active material" refers to a substance used for negative electrode plates that can reversibly embed and release active ions; "positive electrode active material" refers to a substance used for positive electrode plates that can reversibly release and embed active ions. When the secondary battery is charged, the active ions are released from the positive electrode and embedded in the negative electrode through the electrolyte; when the secondary battery is discharged, the active ions are released from the negative electrode and embedded in the positive electrode. The active ions are not particularly limited and can be lithium ions, which corresponds to lithium-ion secondary batteries.
[0104] In this application, "active material" and "active substance" have the same meaning and can be used interchangeably; "positive electrode active substance" and "positive electrode active material" have the same meaning and can be used interchangeably; "negative electrode active substance" and "negative electrode active material" have the same meaning and can be used interchangeably.
[0105] In this application, unless otherwise specified, "active material layer" includes the positive active material layer of the positive electrode sheet and the negative active material layer of the negative electrode sheet, and may refer to the positive active material layer or the negative active material layer according to the detailed circumstances. It is understood that the positive active material layer contains positive active material, and the negative active material layer contains negative active material.
[0106] In the present application, the OI value of the negative electrode sheet has a meaning known in the art. The OI value of the negative electrode sheet refers to the ratio of the diffraction peak intensity of the 004 crystal plane of the graphite material in the negative electrode active material layer to the diffraction peak intensity of the 110 crystal plane, which can be used to characterize the orientation of the negative electrode active material layer and reflect the degree of anisotropy of the grain arrangement in the negative electrode active material layer. The 004 crystal plane corresponds to a layer structure parallel to the graphite of the electrode sheet, and the 110 crystal plane corresponds to a layer structure perpendicular to the graphite of the electrode sheet; the smaller the OI value, the more favorable it is for the diffusion of active ions (such as lithium ions) and the more favorable it is for reducing the expansion of the electrode sheet itself. The intensity of the diffraction peaks of the 004 crystal plane and the 110 crystal plane can be tested by an X-ray powder diffractometer (non-limiting example, X'pert PRO), and an X-ray diffraction spectrum can be obtained according to the general rules of X-ray diffraction analysis and the method for determining the lattice parameters of graphite JIS K0131-1996 and JB / T4220-2011, and then according to OI=I 004 / I 110 The intensity ratio of the diffraction peak of the 004 crystal plane of the negative electrode active material layer to the diffraction peak of the 110 crystal plane is obtained, wherein I 004 is the intensity of the diffraction peak of the 004 crystal plane, I 110 is the intensity of the diffraction peak of the 110 crystal plane.
[0107] In some embodiments, the OI value of the negative electrode plate can be adjusted by, but not limited to, the following methods: the OI value of the graphite particles, the particle size of the graphite particles (such as D v 50), at least one parameter of the porosity of the negative electrode sheet, the compaction density of the negative electrode sheet, the type and content of the components of the negative electrode sheet, etc. This is achievable for those skilled in the art.
[0108] In the present application, the negative electrode sheet resistance value R has a well-known meaning in the art. Unless otherwise specified, R in the present application can be obtained by testing with a resistor meter, for example, a BER1300 multi-function sheet resistance meter can be used for testing. Furthermore, the following method can be used for testing: cut the negative electrode sheet into a sample to be tested of a certain size (a small disc with a diameter of 40 mm); place the sample to be tested between two probes of a resistor meter (such as a BER1300 multi-function sheet resistance meter), and record the resistance test value; take multiple (such as at least 5) samples to be tested, and calculate the average value of the multiple samples to be tested as the test result of the negative electrode sheet resistance value R.
[0109] In the present application, "chain carboxylate" has a meaning well known in the art. Chain carboxylate refers to a class of carboxylate organic compounds having an ester group (-C(=O)-O-) structure, and the carboxylate does not contain a ring structure. In the application, the chain carboxylate acts as a solvent and is recorded as the first solvent. It can be understood that what is connected on both sides of -C(=O)-O- are chain structures, not ring structures, and -C(=O)-O- itself does not participate in the ring formation. It can be understood that the chain carboxylate is liquid in the battery cell.
[0110] By synergistically controlling the OI value of the negative electrode plate and the mass proportion W0 of the chain carboxylate solvent in the solvent, the fast charging performance, cycle performance and safety performance of the secondary battery can be taken into account. When the OI value and W0 satisfy the above relationship 0.08 / mΩ≤W0×100 / (R×OI)≤5 / mΩ, on the one hand, the chain carboxylate in the non-aqueous electrolyte has the characteristics of low viscosity and conductivity, which can significantly enhance the conductivity of the battery and improve the low temperature performance and cycle stability of the battery. On the other hand, the negative electrode plate has a suitable orientation degree and has a suitable directional selectivity in the process of active ion (such as lithium ion) embedding, which can disperse the active ion embedding expansion (such as lithium embedding expansion) in different directions, thereby reducing the cycle expansion of the plate and the battery cell, which can effectively alleviate the problem of aggravated expansion of the plate itself due to the poor interface stability between the chain carboxylate and the negative electrode, improve battery safety, and reduce the concentration polarization of active ions in the transmission process of the negative electrode plate, and achieve a significant improvement in the fast charging capability of the battery with the negative electrode plate resistance value R. Therefore, by synergistically controlling the OI value, R and W0, the secondary battery can have excellent comprehensive functions in terms of fast charging performance, cycle performance and safety performance, and can take into account a shorter fast charging time, lower cycle expansion and higher cycle capacity retention rate.
[0111] In this application, when the W0×100 / (R×OI) value is large, it is more beneficial to the fast charging capability of the battery; however, if the value is too large, it is easy to cause the pole piece itself to expand too much, seriously deteriorating the cycle and safety performance of the battery cell. When W0×100 / (R×OI) is too high, it may cause the pole piece to be demolded, causing the battery cell to fail to work.
[0112] In some embodiments, 6≤OI≤25; optionally, 6≤OI≤18; further optionally, 12≤OI≤18. The OI value of the negative electrode plate can also be any of the following values or an interval consisting of any two of the following values: 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, etc. The OI value of the negative electrode plate can be selected from any of the following ranges: 6-15, 12-25, 6-18, 14-16, etc.
[0113] By adjusting the QI value within a more appropriate range, it is more conducive to reducing the directional selectivity in the active ion embedding process, so that the active ions can be better embedded and expanded and dispersed in different directions; in addition, the active ion transport performance of the negative electrode can also be better improved.
[0114] In some embodiments, 1mΩ≤R≤50mΩ; optionally, 5mΩ≤R≤30mΩ; further optionally, 10mΩ≤R≤20mΩ. The resistance value R of the negative electrode plate can also be any of the following values or an interval consisting of any two of the following values: 1mΩ, 2mΩ, 3mΩ, 4mΩ, 5mΩ, 6mΩ, 8mΩ, 10mΩ, 12mΩ, 15mΩ, 16mΩ, 18mΩ, 20mΩ, 25mΩ, 30mΩ, 35mΩ, 40mΩ, 45mΩ, 50mΩ, etc. The resistance value R of the negative electrode plate can also be selected from any of the following ranges: 12mΩ~18mΩ, 14mΩ~16mΩ, 5mΩ~20mΩ, 5mΩ~18mΩ, 10mΩ~18mΩ, etc.
[0115] In some embodiments, the resistance value R of the negative electrode sheet can be adjusted by, but not limited to, the following methods: the compaction density of the negative electrode sheet, the porosity of the negative electrode sheet, the type and content of the components of the negative electrode sheet, etc. For example, the resistance value R of the negative electrode sheet can be adjusted by adjusting the type and / or content of the conductive agent in the negative electrode sheet.
[0116] By controlling the resistance value R of the negative electrode sheet within a certain range, W0×100 / (R×OI) can be controlled within a more appropriate range, thereby achieving better comprehensive effects in terms of shorter fast charging time, lower cycle expansion and higher cycle capacity retention rate, and is more conducive to improving the active ion transport performance and electronic conduction performance of the negative electrode sheet.
[0117] In the present application, the mass proportion of the first solvent in the solvent is denoted as W0.
[0118] In some embodiments, 10%≤W0≤80%. W0 may also be any of the following percentages: 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, etc., and may also be selected from an interval consisting of any two of the above percentages, for example, 20%≤W0≤80%, 30%≤W0≤70%, 50%≤W0≤70%, 10%≤W0≤60%, 20%≤W0≤60%, etc.
[0119] By controlling the content W0 of the chain carboxylic acid ester (first solvent) in the solvent within a certain range, it is possible to enhance the conductivity of the battery while taking into account the fast charging performance, cycle performance and safety performance of the secondary battery, and to improve the low temperature performance and cycle stability of the secondary battery.
[0120] In some embodiments, 0.67≤W0×100 / OI≤10. W0×100 / OI may also be any of the following values or an interval consisting of any two of the following values: 0.67, 0.8, 1, 1.2, 1.3, 1.33, 1.33±0.01, 1.4, 1.5, 2, 2.5, 2.67, 2.67±0.01, 3, 4, 4.5, 4.67, 4.67±0.01, 5, 5.33, 5.33±0.01, 6, 7, 8, 9, 10, etc.
[0121] In some embodiments, 1≤W0×100 / OI≤10; optionally, 1≤W0×100 / OI≤5; further optionally, 3≤W0×100 / OI≤5.
[0122] In some embodiments, 0.67≤W0×100 / OI≤4; optionally, 1≤W0×100 / OI≤4.
[0123] On the basis of controlling W0×100 / (R×OI) to conform to the above relationship, the matching of the chain carboxylic acid ester in the non-aqueous electrolyte and the grain arrangement direction in the negative electrode active material layer is further regulated by W0×100 / OI, which makes it easier to achieve the improvement of the comprehensive performance of fast charging performance, cycle performance and safety performance.
[0124] In the present application, the secondary battery has the following characteristics: 0.08 / mΩ≤W0×100 / (R×OI)≤5 / mΩ. For the secondary battery provided by the present application, W0×100 / (R×OI) can also be any of the following values or an interval consisting of any two of the following values: 0.1 / mΩ, 0.13 / mΩ, 0.15 / mΩ, 0.2mΩ, 0.3 / mΩ, 0.4 / mΩ, 0.5 / mΩ, 0.6 / mΩ, .8 / mΩ, 1 / mΩ, 1.2 / mΩ, 1.4 / mΩ, 1.5 / mΩ, 1.6 / mΩ, 1.8 / mΩ, 2 / mΩ, 2.2 / mΩ, 2.4 / mΩ, 2.5 / mΩ, 2.6 / mΩ, 2.8 / mΩ, 3 / mΩ, 3.5 / mΩ, 3.6 / mΩ, 3.8 / mΩ, 4 / mΩ, 4.5 / mΩ, 4.8 / mΩ, 5 / mΩ, etc.
[0125] In some embodiments, 0.1 / mΩ≤W0×100 / (R×OI)≤5 / mΩ.
[0126] In some embodiments, 0.1 / mΩ≤W0×100 / (R×OI)≤2 / mΩ.
[0127] On the basis of synergistically controlling the orientation degree of the negative electrode sheet and the content of the first solvent (chain carboxylate) in the solvent, the resistance value R of the negative electrode sheet is further synergistically controlled, so that W0×100 / (R×OI) can be controlled within an appropriate range, which can better take into account the comprehensive performance of the secondary battery in terms of fast charging performance, cycle performance and safety performance.
[0128] In some embodiments, the secondary battery satisfies the following characteristic combination: 6≤OI≤18, 10mΩ≤R≤20mΩ, and 20%≤W0≤80%. In some embodiments thereof, 12≤OI≤18, 10mΩ≤R≤20mΩ, and 10%≤W0≤60%.
[0129] By finely and synergistically controlling the OI value of the negative electrode plate to be 12-18, the resistance value R of the negative electrode plate to be 10mΩ-20mΩ, and the mass proportion W0 of the chain carboxylic acid ester solvent in the solvent to be 20%-80% (further optionally 10%-60%), it is possible to better achieve a balance between fast charging performance, cycle performance and safety performance, which is more conducive to making the secondary battery have better fast charging capability, lower cycle expansion and higher cycle capacity retention rate.
[0130] In some embodiments, 12≤OI≤18, 10mΩ≤R≤20mΩ, and 20%≤W0≤60%.
[0131] In some embodiments, 12≤OI≤18, 10 mΩ≤R≤20 mΩ, and 50%≤W0≤70%.
[0132] By controlling the values of different parameters, it is possible to further have advantages in one or more aspects. For example, in the case of 12≤OI≤18, 10mΩ≤R≤20mΩ, and 20%≤W0≤60%, it can have significantly excellent low cycle expansion and cycle performance on the basis of better comprehensive performance. For another example, in the case of 12≤OI≤18, 10mΩ≤R≤20mΩ, and 50%≤W0≤70%, on the basis of better comprehensive performance, it can also have obvious advantages in shorter fast charging time and lower cycle expansion.
[0133] In some embodiments, the first solvent comprises a compound having a structure as shown in formula (1):
[0134] R1 and R2 are independently alkyl or halogenated alkyl. It can be seen that R1 and R2 do not form a ring, and the compound with the structure shown in formula (1) is a chain carboxylic acid ester.
[0135] Optionally, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Halogenated alkyl.
[0136] Optionally, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Fluorinated alkyl.
[0137] Among them, C 1-3 The alkyl group may be a methyl group (which may be represented by Me, -CH3), an ethyl group (which may be represented by Et, -CH2CH3) or a propyl group, and the propyl group may be a n-propyl group (which may be represented by 1-propyl group, n-Pr, n-propyl group, -CH2CH2CH3) or an isopropyl group (which may be represented by 2-propyl group, i-Pr, i-propyl group, -CH(CH3)2). 1-3 The alkyl group may be methyl, ethyl or n-propyl. 1-3 The alkyl group may be methyl or ethyl.
[0138] Among them, C 1-3 The carbon atoms in the haloalkyl group may be 1, 2, or 3, that is, it may be a C1 haloalkyl group, a C2 haloalkyl group, or a C3 haloalkyl group. 1-3 The halogen atom in the haloalkyl group may be fluorine. 1-3 The number of halogen atoms in a haloalkyl group may be 1 or more. 1-3 When the number of halogen atoms in the haloalkyl group is plural, it may be 2 or all of the alkyl hydrogen atoms are substituted.
[0139] Among them, C 1-3 The carbon atoms in the fluoroalkyl group may be 1, 2, or 3, that is, it may be a C1 fluoroalkyl group, a C2 fluoroalkyl group, or a C3 fluoroalkyl group. 1-3 The number of fluorine atoms in the fluoroalkyl group may be 1 or more. 1-3 When the number of fluorine atoms in the fluoroalkyl group is plural, the number may be 2 to perfluoro-substituted.
[0140] In some embodiments, R1 and R2 are independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl, and optionally, R1 and R2 are independently one of methyl, ethyl, fluoromethyl and fluoroethyl. The number of fluorine atoms in the fluoromethyl group can be independently 1, 2 or 3. The number of fluorine atoms in the fluoroethyl group can be independently 1, 2, 3, 4, 5 or 6, and further can be independently 1, 2 or 3. The number of fluorine atoms in the fluoropropyl group can be independently 1, 2, 3, 4, 5, 6, 7, 8 or 9, and further can be independently 1, 2 or 3.
[0141] A first solvent with a smaller molecular size can be selected. In this case, the first solvent has a lower viscosity, which is beneficial for the secondary battery to obtain better fast charging performance.
[0142] In some embodiments, the first solvent includes one or more of the following compounds, which may be selected from one or more of the following compounds: CH3CH2-OC(=O)-CH3 (i.e., ethyl acetate), CH3-OC(=O)-CH3 (i.e., methyl acetate), CH3CH2-OC(=O)-CH2CH3 (i.e., ethyl propionate), CH3-OC(=O)-CH2CH3 (i.e., methyl propionate), CH3CH2-OC(=O)-CH2F, CH3CH2-OC(=O)-CHF2, CH3CH2-OC(=O)-CF3, CH3-OC(=O)-CH2F, CH3-OC(=O)-CHF2, CH3CH2-OC(=O)-CF3, CH3-OC(=O)-CH2F, CH3-OC(=O)-CHF2, CH3-OC(=O)-CF3, CF3-OC(=O)-CH3, and CHF2-OC(=O)-CH3;
[0143] That is, the first solvent includes one or more of the following compounds, which may be selected from one or more of the following compounds:
[0144]
[0145]
[0146] In some embodiments, the first solvent comprises one or more of the following compounds: methyl acetate, ethyl acetate, methyl difluoroacetate and ethyl difluoroacetate. In some embodiments thereof, the first solvent is selected from one or more of the following compounds: methyl acetate, ethyl acetate, methyl difluoroacetate and ethyl difluoroacetate.
[0147] In some embodiments, the nonaqueous electrolyte further includes a first additive; the first additive is diisocyanate.
[0148] In the present application, diisocyanate refers to a compound containing two isocyanate groups (—NCO).
[0149] The introduction of chain carboxylic acid ester (first solvent) is conducive to improving the fast charging ability of the battery. However, due to the compatibility factors between carboxylic acid ester and negative electrode sheet, if the amount W0 of the carboxylic acid ester does not match the OI value and resistance value R of the negative electrode sheet, it may aggravate the expansion problem of the negative electrode sheet itself, and may also affect the gas production problem at the interface, and may also cause the attenuation of the battery cell capacity and the deterioration of the battery cycle performance. By introducing the additive diisocyanate (referred to as the first additive) into the non-aqueous electrolyte, a protective solid electrolyte interface (SEI) layer can be formed on the surface of the negative electrode sheet. The protective layer can assist the active ions to be embedded in the negative electrode active material layer of the negative electrode sheet, so that the active ion embedding expansion effect of the negative electrode sheet can be evenly conducted in all directions, thereby reducing the cycle expansion rate of the negative electrode sheet. In addition, the first additive can also significantly improve the stability of the interface between the electrolyte and the negative electrode sheet, which can reduce the consumption of the electrolyte and the damage to the negative electrode structure during the cycle of the secondary battery, thereby significantly improving the cycle performance of the secondary battery.
[0150] In some embodiments, the first additive comprises a compound having the following structure:
[0151] O==C==N-R3-N==C=O Formula (2);
[0152] Wherein R3 is unsubstituted or Ra substituted C 1-18 Alkylene; Ra may include one or more of the following substituents, which may be selected from one or more of the following substituents: halogen atom (which may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine), -CN, -NCO, -OH, -COOH, -SOOH, -OC(=O)R 11 , R 12 OC(=O)-、C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 One or more of oxaalkyl; R 11 and R 12 are independently alkyl or halogenated alkyl. Unless otherwise specified, in the case of "Ra substituted", the number of Ra can be 1 or more.
[0153] In the substituent Ra, R 11 and R 12 are independently alkyl or halogenated alkyl. 11 and R 12 C 1-3 Alkyl or C 1-3 Alternatively, R 11 and R 12 C1-3 Alkyl or C 1-3 Fluorinated alkyl.
[0154] In some embodiments, R 11 and R 12 are independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl, and optionally, R 11 and R 12 Each of the fluoropropyl groups is independently selected from the group consisting of methyl, ethyl, fluoromethyl and fluoroethyl. The number of fluorine atoms in the fluoromethyl group may be independently 1, 2 or 3. The number of fluorine atoms in the fluoroethyl group may be independently 1, 2, 3, 4, 5 or 6, and further independently 1, 2 or 3. The number of fluorine atoms in the fluoropropyl group may be independently 1, 2, 3, 4, 5, 6, 7, 8 or 9, and further independently 1, 2 or 3.
[0155] In some embodiments, in "R3 is unsubstituted or Ra substituted C 1-18 "C 1-18 The number of carbon atoms in the "alkylene group" is 1 to 16. 1-18 The number of carbon atoms in the "alkylene group" can also be any of the following values or an interval consisting of any two of the following values: 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 and 16. The interval consisting of any two values is 1-16, 2-16, 4-16, 6-16, 1-14, 2-14, 4-14, 6-14, 1-10, 2-10, 4-10, 6-10, etc.
[0156] In some embodiments, in "R3 is unsubstituted or Ra substituted C 1-18 On the basis of "alkylene", the number of carbon atoms of R3 is 1 to 16. Further, the number of carbon atoms of R3 can also be any of the following values or an interval consisting of any two of the following values: 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 and 16. The interval consisting of any two values is such as 1 to 16, 2 to 16, 4 to 16, 6 to 16, 1 to 14, 2 to 14, 4 to 14, 6 to 14, 1 to 10, 2 to 10, 4 to 10, 6 to 10, etc.
[0157] In some embodiments, R3 is unsubstituted or Ra substituted C 2-10 Alkylene, unsubstituted or Ra substituted C 3-18 Bivalent cycloalkyl or unsubstituted or Ra substituted C 6-18 Arylene. Optionally, R3 is C 2-10 Alkylene, C 6-18 Divalent cycloalkyl or C6-18 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-14 Divalent cycloalkyl or C 6-14 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-10 Divalent cycloalkyl or C 6-10 Arylene; further optionally, R3 is C 4-8 Hexylene, C containing hexyl ring 6-10 A divalent cycloalkyl or C containing a benzene ring 6-10 Arylene.
[0158] In some embodiments, Ra is selected from one or more of the following substituents: a halogen atom (which may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine), -CN, -NCO, -OH, -COOH, -SOOH, -OC(=O)R 11 , R 12 OC(=O)-、C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 In some embodiments, Ra is selected from one or more of the following substituents: halogen atom (which may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine), -CN, -NCO, -OH, -COOH, -SOOH, -OC(=O)R 11 , R 12 OC(=O)- and C 2-10 One or more of oxaalkyl groups.
[0159] In some embodiments, Ra is a halogen atom, which may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine.
[0160] In R3, the number of Ra can be 0, one or more. When the number of Ra is 0, it corresponds to the "unsubstituted" situation. When the number of Ra is 1 or more, it corresponds to the "Ra substituted" situation.
[0161] In some embodiments, in R3, the number of Ra can be 0. In this case, the number of carbon atoms in R3 can be as defined above. For example, R3 is an unsubstituted C 1-18 Alkylidene, unsubstituted C 1-16 Alkylidene, unsubstituted C 2-14 Alkylene, etc.
[0162] In some embodiments, in R3, the number of Ra may be one or more.
[0163] In some embodiments, Ra is C 1-10 Alkyl, which may further be C 1-3 Alkyl may further be methyl or ethyl. In some embodiments, Ra is methyl.
[0164] In some embodiments, R3 is C 2-10 Alkylene, C 2-10 Heteroalkylene, C 6-18 Arylene, C 2-18 Heteroarylene, C 3-18 Alicyclic or C 3-18 Heteroalicyclic group, any of the above groups may be unsubstituted or substituted by Ra; if not otherwise specified, in the case of "substituted by Ra", the number of Ra may be 1 or more. 6-18 The arylene group can be C 6-14 Arylene may further be C 6-14 Arylene.
[0165] In the present application, when "substituted" is not particularly described, it means "unsubstituted".
[0166] In the present application, the term "hydrocarbon" compound refers to a compound composed of carbon atoms and hydrogen atoms. Hydrocarbon compounds can be saturated structures (i.e. saturated hydrocarbons) or unsaturated structures (i.e. unsaturated hydrocarbons), can contain ring structures (i.e. cyclic hydrocarbons) or not contain ring structures (i.e. chain hydrocarbons), can have aromaticity (i.e. aromatic hydrocarbons or aromatic hydrocarbons) or not have aromaticity (i.e. aliphatic hydrocarbons). Hydrocarbons with saturated structures, i.e. saturated hydrocarbons, can be alkanes or cycloalkanes. Alkanes do not contain ring structures, can be straight chain structures, or can contain branches. Cycloalkanes contain ring structures, and the number of ring structures can be 1 or more, such as 1, 2 or 3. Cycloalkanes are saturated hydrocarbons containing ring structures, which are non-aromatic hydrocarbons. Hydrocarbons with aromaticity, i.e. aromatic hydrocarbons, contain aromatic ring structures. Unsaturated hydrocarbons can contain carbon-carbon double bonds, carbon-carbon triple bonds, etc. Unsaturated hydrocarbons can contain ring structures or not. Unless otherwise specified, "olefin" refers to a chain hydrocarbon containing one or more carbon-carbon double bonds, "cycloolefin" refers to a cyclic hydrocarbon containing one or more carbon-carbon double bonds, "alkyne" refers to a chain hydrocarbon containing one or more carbon-carbon triple bonds, and "cycloalkyne" refers to a cyclic hydrocarbon containing one or more carbon-carbon triple bonds. "Alicyclic hydrocarbon" refers to a non-aromatic hydrocarbon containing a ring structure, which may be saturated or unsaturated, and the carbon atoms constituting the unsaturated bonds may or may not be ring-forming atoms. For example, alicyclic hydrocarbons may include, but are not limited to, cycloalkanes, cycloalkenes, cycloalkynes, etc.
[0167] In this application, the term "hydrocarbon group" refers to a monovalent residue formed by the loss of a hydrogen atom from a hydrocarbon compound containing a primary (normal) carbon atom, a secondary carbon atom, a tertiary carbon atom, a quaternary carbon atom, or a combination thereof. Phrases containing this term, for example, "C1- 10 The term "alkyl" refers to an alkyl group containing 1 to 10 carbon atoms, and each occurrence may be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl, C9 alkyl or C 10 Hydrocarbon.
[0168] In the present application, the term "alkylene" refers to a divalent hydrocarbon group having two monovalent radical centers derived from a hydrocarbon compound by removing two hydrogen atoms (or derived from a hydrocarbon group by losing another hydrogen atom), which may be a saturated branched structure or a saturated straight chain structure. For example, "C1-C 10 The term "alkylene" refers to an alkyl moiety containing 1 to 10 carbon atoms, each occurrence of which is independently C1 alkylene, C2 alkylene, C3 alkylene, C4 alkylene, C5 alkylene, C6 alkylene, C7 alkylene, C8 alkylene, C9 alkylene or C 10 Alkylene.
[0169] In the present application, the term "alkyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a saturated hydrocarbon containing a primary (normal) carbon atom, a secondary carbon atom, a tertiary carbon atom, a quaternary carbon atom, or a combination thereof. Phrases containing this term, for example, "C1- 10 "Alkyl" refers to an alkyl group containing 1 to 10 carbon atoms, each occurrence of which can be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl, C9 alkyl or C 10Alkyl. Suitable examples include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH(C H3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl (- CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH( 2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 and octyl (-(CH2)7CH3).
[0170] In the present application, the term "alkylene" refers to a divalent hydrocarbon group having two monovalent radical centers derived from an alkane by removing two hydrogen atoms (or derived from an alkyl by losing another hydrogen atom), which may be a saturated branched structure or a saturated straight chain structure. 10The term "alkylene" refers to an alkyl moiety containing 1 to 10 carbon atoms, and each occurrence can be independently C1 alkylene (i.e., methylene), C2 alkylene (i.e., ethylene), C3 alkylene (i.e., propylene), C4 alkylene (i.e., butylene), C5 alkylene (i.e., pentylene), C6 alkylene (i.e., hexylene), C7 alkylene (i.e., heptylene), C8 alkylene (i.e., octylene), C9 alkylene (i.e., nonylene) or C 10 Alkylene (i.e., decylene). Suitable examples include, but are not limited to, methylene (-CH2-), 1,1-ethyl (-CH(CH3)-), 1,2-ethyl (-CH2CH2-), 1,1-propyl (-CH(CH2CH3)-), 1,2-propyl (-CH2CH(CH3)-), 1,3-propyl (-CH2CH2CH2-), and 1,4-butyl (-CH2CH2CH2CH2-).
[0171] In this application, the term "alkenyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a chain-like olefin compound. The hydrogen atom may be located on a carbon-carbon double bond or on an alkyl substituent of the carbon-carbon double bond. Phrases containing this term, such as "C2- 10 The term "alkenyl" refers to an alkenyl group containing 2 to 10 carbon atoms, and each occurrence may be independently C2 alkenyl, C3 alkenyl, C4 alkenyl, C5 alkenyl, C6 alkenyl, C7 alkenyl, C8 alkenyl, C9 alkenyl or C 10 Suitable examples include, but are not limited to, vinyl (CH2=CH-), allyl (CH2=CH-CH2-), CH3-CH=CH-, and the like.
[0172] In this application, the term "alkynyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a chain-like alkyne compound. The hydrogen atom may be located on a carbon-carbon triple bond or on an alkyl substituent of the carbon-carbon triple bond. Phrases containing this term, such as "C2- 10 "Alkynyl" refers to an alkynyl group containing 2 to 10 carbon atoms, each occurrence of which can be independently C2 alkynyl, C3 alkynyl, C4 alkynyl, C5 alkynyl, C6 alkynyl, C7 alkynyl, C8 alkynyl, C9 alkynyl or C 10 Suitable examples include, but are not limited to, ethynyl (CH ≡ C-), propargyl (CH ≡ C-CH2-), CH3-C ≡ C-etc.
[0173] In the present application, the term "heteroalkyl" refers to that at least one carbon atom is replaced by a heteroatom on the basis of an alkyl group; a heteroatom is a non-carbon hydrogen atom, which may be, but is not limited to, an N atom, an O atom, an S atom, a P atom, etc. O, N, and S are used as examples for illustration. For example, if the carbon atom connected to an adjacent group in an alkyl group is replaced by a heteroatom O, N, or S, the resulting heteroalkyl group is an alkoxy group (e.g., -OCH3, etc.), an amino group (e.g., -NHCH3, -N(CH3)2, etc.) or a thioalkyl group (e.g., -SCH3). If the carbon atom not directly connected to an adjacent group in an alkyl group is replaced by a heteroatom O, N, or S, the resulting heteroalkyl group is an alkoxyalkyl group (e.g., -CH2CH2-O-CH3, etc.), an alkylaminoalkyl group (e.g., -CH2NHCH3, -CH2N(CH3)2, etc.) or an alkylthioalkyl group (e.g., -CH2-S-CH3). If the terminal carbon atom of an alkyl group is replaced with a heteroatom, the resulting heteroalkyl group may be a hydroxyalkyl group (e.g., -CH2CH2-OH), an aminoalkyl group (e.g., -CH2NH2), or a mercaptoamino group (e.g., -CH2CH2-SH). Phrases containing the term "heteroalkyl" such as "C 1-10 The term "heteroalkyl" refers to a heteroalkyl group containing 1 to 10 carbon atoms, each occurrence of which can be independently C1 heteroalkyl, C2 heteroalkyl, C3 heteroalkyl, C4 heteroalkyl, C5 heteroalkyl, C6 heteroalkyl, C7 heteroalkyl, C8 heteroalkyl, C9 heteroalkyl or C 10 Heteroalkyl.
[0174] In this application, the term "alkoxy" refers to a monovalent group formed by connecting an alkyl group to -O-. Phrases containing this term, such as "C 1-10 The term "oxaalkyl" refers to an alkoxy group containing 1 to 10 carbon atoms, each occurrence of which can be independently C1 alkoxy, C2 alkoxy, C3 alkoxy, C4 alkoxy, C5 alkoxy, C6 alkoxy, C7 alkoxy, C8 alkoxy, C9 alkoxy or C 10 Suitable examples may include, but are not limited to, methoxy (CH3O-), ethoxy (CH3CH2O-), and the like.
[0175] In this application, the term "oxyalkyl" means that at least one carbon atom in the alkyl group is replaced by an oxygen atom, and the oxygen atom may be located at the attachment site of the alkyl group or not. The number of oxygen atoms can be one or more. For example, one oxygen atom is hybridized, such as alkoxy, alkoxyalkyl, etc. Phrases containing this term, such as "C 1-10The term "oxaalkyl" refers to an oxaalkyl group containing 1 to 10 carbon atoms, which, at each occurrence, can be independently C1oxaalkyl, C2oxaalkyl, C3oxaalkyl, C4oxaalkyl, C5oxaalkyl, C6oxaalkyl, C7oxaalkyl, C8oxaalkyl, C9oxaalkyl or C 10 Oxaalkyl.
[0176] In the present application, the term "heteroalkylene" is also referred to as "divalent heteroalkyl", which refers to a divalent heterohydrocarbon group with two monovalent radical centers derived from a heteroalkyl group by losing a hydrogen atom (the hydrogen atom may be located on a carbon atom or a heteroatom), or refers to an alkylene group in which at least one carbon atom is replaced by a heteroatom (any heteroatom may be located at the connection site of the alkylene group or not); the heteroatom may be, but is not limited to, an N atom, an O atom, an S atom, a P atom, etc. Phrases containing this term, such as "C 1-10 The term "heteroalkylene" refers to a heteroalkylene group containing 1 to 10 carbon atoms, which, at each occurrence, can be independently C1 heteroalkylene, C2 heteroalkylene, C3 heteroalkylene, C4 heteroalkylene, C5 heteroalkylene, C6 heteroalkylene, C7 heteroalkylene, C8 heteroalkylene, C9 heteroalkylene or C 10 Heteroalkylene.
[0177] In this application, the term "cycloalkyl" refers to a monovalent residue formed by the loss of a cyclic or non-cyclic hydrogen atom from a saturated cycloalkane, which can form a monovalent attachment site directly on the ring or at the position of an alkyl substituent on the ring. Phrases containing this term, such as "C 3-10 "Cycloalkyl" refers to a cycloalkyl group containing 3 to 10 carbon atoms, each occurrence of which can be independently C3 cycloalkyl, C4 cycloalkyl, C5 cycloalkyl, C6 cycloalkyl, C7 cycloalkyl, C8 cycloalkyl, C9 cycloalkyl or C 10 Cycloalkyl. The number of ring structures in a cycloalkyl group can be 1 or more, such as 1, 2 or 3. The number of ring atoms in any ring structure in a cycloalkyl group can be 3 to 8, such as 3, 4, 5, 6, 7 or 8; for example, propylene Ding ring Pentyl ring Hexyl ring The case where a monovalent attachment site is formed directly on the ring may include, but is not limited to: cyclopropyl Cyclobutyl Cyclopentyl Cyclohexyl The formation of a monovalent attachment site from an alkyl substituent on the ring may include, but is not limited to (A C7 cycloalkyl group containing a hexyl ring).
[0178] In this application, unless otherwise specified, the terminal Indicates the site of covalent bond attachment.
[0179] In the present application, the term "alicyclic group" is also referred to as "divalent alicyclic group", which refers to a divalent residue derived from an alicyclic hydrocarbon by losing two cyclic or non-cyclic hydrogen atoms. Any of the lost hydrogen atoms may be on the ring or not on the ring, that is, a monovalent attachment site may be formed directly on the ring or at the position of a hydrocarbon substituent on the ring. Alicyclic groups may include, but are not limited to, divalent cycloalkyl groups, divalent cycloalkenyl groups, divalent cycloalkynyl groups, and the like. Phrases containing this term, such as "C 3-10 The term "alicyclic group" refers to an alicyclic group containing 3 to 10 carbon atoms, and each occurrence thereof can be independently C3 alicyclic group, C4 alicyclic group, C5 alicyclic group, C6 alicyclic group, C7 alicyclic group, C8 alicyclic group, C9 alicyclic group or C 10 Alicyclic group.
[0180] In the present application, the term "divalent cycloalkyl" is also referred to as "cycloalkylene", which refers to a divalent saturated hydrocarbon group derived from a cycloalkane by removing two hydrogen atoms (or derived from a cycloalkyl by losing another hydrogen atom), having two monovalent radical centers, and the position of any monovalent radical center can be independently located on the ring or not. Phrases containing this term, such as "C 3-10 The term "divalent cycloalkyl" refers to a divalent cycloalkyl group containing 3 to 10 carbon atoms, and each occurrence can be independently C3 divalent cycloalkyl, C4 divalent cycloalkyl, C5 divalent cycloalkyl, C6 divalent cycloalkyl, C7 divalent cycloalkyl, C8 divalent cycloalkyl, C9 divalent cycloalkyl or C 10 Divalent cycloalkyl. The number of carbon atoms in the "divalent cycloalkyl" can be 3 to 10, and can be 3, 4, 5, 6, 7, 8, 9 or 10, for example, 6 to 10. The number of ring structures in the divalent cycloalkyl can be 1 or more, for example, 1, 2 or 3. The number of ring atoms in any ring structure of the "divalent cycloalkyl" can be 3 to 8, and can be 3, 4, 5, 6, 7 or 8. Non-limiting example, "C 6-10 "Divalent cycloalkyl" refers to a divalent cycloalkyl group containing 6 to 10 carbon atoms, in which the number of ring atoms in a ring structure is not particularly limited. 6-10 "Divalent cycloalkyl" refers to a divalent cycloalkyl containing a hexyl ring and 6 to 10 carbon atoms, for example, a divalent cyclohexyl (such as a 1,4-position structure 1,3-position structure Or 1,2-position structure ), wait.
[0181] In the present application, the term "divalent cycloalkenyl" is also referred to as "cycloalkenylene", which refers to a divalent unsaturated hydrocarbon group having two monovalent radical centers derived from a cycloalkene by removing two hydrogen atoms, and the position of any monovalent radical center can be independently located on the ring or not. Phrases containing this term, such as "C 3-10 The term "divalent cycloalkenyl" refers to a divalent cycloalkenyl group containing 3 to 10 carbon atoms, which, at each occurrence, can be independently C3 divalent cycloalkenyl, C4 divalent cycloalkenyl, C5 divalent cycloalkenyl, C6 divalent cycloalkenyl, C7 divalent cycloalkenyl, C8 divalent cycloalkenyl, C9 divalent cycloalkenyl or C 10 A divalent cycloalkenyl group.
[0182] In the present application, the term "heteroalicyclic group" is also referred to as "divalent heteroalicyclic group", which means that at least one carbon atom of the hydrocarbon group is replaced by a heteroatom on the basis of the alicyclic group; the heteroatom may be located at the attachment site of the alicyclic group or not; the heteroatom may be located on the ring or not; the heteroatom may be, but is not limited to, an N atom, an O atom, an S atom, a P atom, etc. The heteroatom may be located at the attachment site of the alicyclic group (i.e., the end) or not. Phrases containing this term, such as "C 3-10 The term "heteroalicyclic group" refers to a heteroalicyclic group containing 3 to 10 carbon atoms, and each occurrence thereof can be independently C3 heteroalicyclic group, C4 heteroalicyclic group, C5 heteroalicyclic group, C6 heteroalicyclic group, C7 heteroalicyclic group, C8 heteroalicyclic group, C9 heteroalicyclic group or C 10 Heteroalicyclic.
[0183] In the present application, the term "arylene" refers to a divalent residue having two monovalent radical centers formed by losing two hydrogen atoms from an aromatic hydrocarbon (any of the lost hydrogen atoms may be independently located on the aromatic ring or may not be located on the aromatic ring). The arylene group may be a monocyclic arylene group, a condensed ring arylene group, or a polycyclic arylene group. For polycyclic rings, at least one is an aromatic ring system. For example, "C 6-14 "Arylene" refers to an arylene group containing 6 to 14 carbon atoms, and each occurrence can be independently C6 arylene, C7 arylene, C8 arylene, C9 arylene, C 10 Arylene, C 11 Arylene, C 12 Arylene, C 13 Arylene or C 14 Arylene. Suitable examples include, but are not limited to, arylene groups derived from the following aromatic rings: benzene, biphenyl, diphenylmethylene, naphthalene, anthracene, phenanthrene, perylene, triphenylene, or a hydrocarbyl substituted form of any of the foregoing, such as toluene, xylene, tetramethylbenzene, ethylbenzene, dimethylbiphenyl, and the like.
[0184] In the present application, the term "heteroarylene" is also referred to as "divalent heteroaryl", which means that at least one carbon atom on the basis of arylene is replaced by a heteroatom; any heteroatom may be located at the connection site of arylene or not; any heteroatom may be located on the aromatic ring or not; the heteroatom may be, but not limited to, N atom, O atom, S atom, P atom, etc. Phrases containing this term, such as "C 2-10 The term "heteroarylene" refers to a heteroarylene group containing 2 to 10 carbon atoms, which, at each occurrence, can be independently C2 heteroarylene, C3 heteroarylene, C4 heteroarylene, C5 heteroarylene, C6 heteroarylene, C7 heteroarylene, C8 heteroarylene, C9 heteroarylene or C 10 Heteroarylene.
[0185] In some embodiments, R3 is C 1-8 Alkylene, C 6-14 Arylene, -(Z1) p1 -C A -(Z2) p2 -and-(Z1) q1 -C A1 -(Z3) q3 -C A2 -(Z2) q2 -, or one or more hydrogen atoms in any of the aforementioned divalent groups are substituted with a substituent R a wherein Z1, Z2 and Z3 are each independently a covalent bond or C 1-3 Alkylene, C A C 4-14 Divalent alicyclic group, C A1 and C A2 Each independently is C 5-12 A divalent alicyclic group, p1, p2, q1, q2 and q3 are each independently 0 or 1.
[0186] In some embodiments, Z1, Z2 and Z3 are each independently a covalent bond or a methylene group.
[0187] In some embodiments, C A is a divalent cyclobutyl, a divalent cyclopentyl, a divalent cyclohexyl or
[0188] In some embodiments, C A1 and C A2 Each independently is C 5-12 A divalent alicyclic group; optionally, C A1 and C A2 Each independently is C 4-6 A divalent alicyclic group; further optionally, CA1 and C A2 Each is independently a divalent cyclopentyl or a divalent cyclohexyl; further optionally, C A1 and C A2 Each is independently a divalent cyclopentyl group.
[0189] In some embodiments, R3 is methylene, ethylene, propylene, butylene, pentylene, hexylene, phenylene, -CH2-Ph-CH2-, naphthylene, anthracene, -Ph-CH2-Ph-, -Ph-Ph-, divalent cyclobutyl, divalent cyclopentyl, divalent cyclohexyl, or one or more hydrogen atoms in any of the aforementioned divalent groups are substituted with a substituent R a A divalent group formed by substitution; wherein Ph is a benzene ring.
[0190] In this application, Two of It means that two single bonds are introduced from any position on the ring to form two monovalent sites. The two monovalent sites can be located in the same ring or in different rings, on different ring-forming atoms or on the same ring-forming atom. However, it is preferred that the two single bonds are introduced from different ring-forming atoms.
[0191] In some embodiments, any one of R a are independently a halogen atom or C 1-3 Alkyl; further optionally, any one of R a are independently fluorine atoms, methyl or ethyl; further optionally, any one of R a are independently a fluorine atom or a methyl group.
[0192] In some embodiments, the first additive includes one or more of the following compounds: (1,4-phenylenediisocyanate, 1,4-diisocyanatobenzene), (1,3-phenylenediisocyanate, 1,3-diisocyanatobenzene), (1,3-bis(isocyanatomethyl)benzene, m-phenylenedimethyl isocyanate), (2,3,5,6-tetrafluorophenyl diisocyanate, 1,2,4,5-tetrafluoro-3,6-diisocyanatobenzene), (1,3-diisocyanato-2-methylbenzene), (2,4-diisocyanato-1-methylbenzene), (2,5-diisocyanato-1,3-dimethylbenzene), (1,4-diisocyanato-2,5-dimethylbenzene), (1,4-diisocyanato-2,3-dimethylbenzene), (1,4-diisocyanato-2,3,5,6-tetramethylbenzene), (1-ethyl-2,3-diisocyanatobenzene), (1,5-diisocyanatonaphthalene), (9,10-diisocyanatoanthracene), (bis(4-isocyanatophenyl)methane), (3,3'-dimethyl-4,4'-biphenyl diisocyanate, 4,4'-diisocyanato-3,3'-dimethyl-1,1'-biphenyl), (3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 4,4'-diisocyanato-3,3'-dimethoxy-1,1'-biphenyl), (1,4-diisocyanatocyclohexane), (1,4-cyclohexane dimethyl diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane), (1,2-cyclohexane dimethyl diisocyanate, 1,2-bis(isocyanatomethyl)cyclohexane), (1,3-diisocyanatocyclopentane), (1,2-cyclobutane dimethyl diisocyanate, 1,2-bis(isocyanatomethyl)cyclobutane), (9,10-diisocyanatotetradecahydroanthracene), (1,3,3-trimethylcyclohexane-1,5-diisocyanate, 1,5-diisocyanato-1,3,3-trimethylcyclohexane), (2,5-diisocyanato-1,1,3-trimethylcyclohexane), (2,3,5,6-tetramethylcyclohexane-1,4-diisocyanate, 1,4-diisocyanato-2,3,5,6-tetramethylcyclohexane), (1-isocyanato-4-(isocyanatomethyl)-1-methylcyclohexane, 1-isocyanato-3-(isocyanatomethyl)-1-methylcyclohexane), (5-isocyanato-1-(isocyanatomethyl)-1,3,3-trimethylcyclohexane, Isophorone diisocyanate), (bis(4-isocyanatocyclohexyl)methane), (methyl diisocyanate), (1,4-diisocyanatobutane), (1,4-diisocyanatopentane), (hexamethylene diisocyanate, hexamethylene diisocyanate, HMDI) and so on.
[0193] In some embodiments, the first additive is one or more of the following compounds: 1,4-phenylene diisocyanate, 1,3-phenylene diisocyanate, m-phenylenedimethyl isocyanate, 2,3,5,6-tetrafluorophenylene diisocyanate, 1,3-diisocyanato-2-toluene, 2,4-diisocyanato-1-toluene, 2,5-diisocyanato-1,3-xylene, 1,4-diisocyanato-2,5-xylene, 1,4-diisocyanato-2,3-xylene, 1,4-diisocyanato-2,3,5,6-tetramethylbenzene, 2,3-diisocyanato-1-ethylbenzene, 1,5-diisocyanatonaphthalene, 9,10-diisocyanatoanthracene, diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, 3,3'-dimethoxy-4 ,4'-biphenyl diisocyanate, cyclohexane-1,4-diisocyanate, 1,4-cyclohexanedimethyl diisocyanate, 1,2-cyclohexanedimethyl diisocyanate, cyclopentane-1,3-diisocyanate, 1,2-cyclobutanedimethyl diisocyanate, 9,10-diisocyanatotetradecahydroanthracene, 1,3,3-trimethylcyclohexane-1,5-diisocyanate, 1,1,3-trimethylcyclohexane-2,5-diisocyanate, 2,3,5,6-tetramethylcyclohexane-1,4-diisocyanate, 1-isocyanato-4-(isocyanatomethyl)-1-methylcyclohexane, isophorone diisocyanate, 4,4-diisocyanatodicyclohexylmethane, methylene diisocyanate, 1,4-diisocyanatobutyl, 1,4-diisocyanatopentyl and hexamethylene diisocyanate. Furthermore, the first additive may be selected from one or more of the diisocyanates listed above.
[0194] In some embodiments, the first additive includes one or more of the following compounds: hexamethylene diisocyanate, 1,4-cyclohexane dimethyl diisocyanate, 1,3-phenylene diisocyanate, and 2,4-diisocyanate-1-toluene. In some embodiments, the first additive is selected from one or more of the following compounds: hexamethylene diisocyanate, 1,4-cyclohexane dimethyl diisocyanate, 1,3-phenylene diisocyanate, and 2,4-diisocyanate-1-toluene.
[0195] In some embodiments, the mass proportion of the first additive in the non-aqueous electrolyte (which can be recorded as W1) is 0 to 11%. When W1 is 0, that is, the first additive is not added to the non-aqueous electrolyte. The mass proportion W1 of the first additive in the non-aqueous electrolyte can also be any of the following percentages: 0, 0.005%, 0.01%, 0.015%, 0.02%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 10%, 11%, etc., and can also be selected from the interval consisting of any two of the above percentages, such as 0.005% to 11%, 0.005% to 10%, 0.1% to 5%, 1% to 5%, 0 to 1%, 0.1% to 1%, 0.01% to 10%, 1% to 10%, etc.
[0196] In some embodiments, the non-aqueous electrolyte further comprises a second additive; the second additive comprises one or more of lithium monofluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, a compound represented by formula (3), and a fluorosulfonate;
[0197]
[0198] In formula (3), a, b and c are each independently a positive integer, m is an integer selected from 1 to 3, n is an integer selected from 0 to 4, and q is 0 or 1; M a+ is a metal ion with a positive charge; any Y is independently a boron atom or a phosphorus atom; X is a halogen atom; any R is independently a substituted or unsubstituted C 1-10 Alkylene, substituted or unsubstituted C 1-10 Haloalkylene, substituted or unsubstituted C 6-20 Arylene, and substituted or unsubstituted C 6-20 A type of halogenated arylene group.
[0199] In the present application, the halogen atom in the haloalkylene group may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine. The number of halogen atoms in the haloalkylene group may be one or more.
[0200] In the present application, the halogen atom in the halogenated arylene group may be one or more of fluorine, chlorine, bromine and iodine, and may further be fluorine. The number of halogen atoms in the halogenated arylene group may be one or more.
[0201] In some embodiments, any one R is independently Rc substituted or unsubstituted C 1-10 Alkylene, Rc substituted or unsubstituted C 1-10 Haloalkylene, Rc substituted or unsubstituted C 6-20 Arylene, and Rc substituted or unsubstituted C 6-20A type of halogenated arylene group. C substituted with Rc 1-10 Substituents in alkylene, C substituted with Rc 1-10 Substituents in haloalkylene, C substituted with Rc 6-20 Substituents in arylene and Rc substituted C 6-20 The Rc substituents in the halogenated arylene group may each independently include one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC=(O)R 41 、-C=(O)OR 42 , C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 Alkoxy; wherein R 41 and R 42 Each independently is C 1-6 Alkyl, such as methyl, ethyl, etc. Among them, Rc substituted C 1-10 Substituents in alkylene, C substituted with Rc 1-10 Substituents in haloalkylene, C substituted with Rc 6-20 Substituents in arylene and Rc substituted C 6-20 The Rc substituents in the halogenated arylene group can be independently selected from one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC=(O)R 41 、-C=(O)OR 42 , C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 Alkoxy; wherein R 41 and R 42 Each independently is C 1-6 Alkyl, such as methyl, ethyl, etc. In the present application, unless otherwise specified, R contains a substituent R C When R C The number can be 1 or more.
[0202] In some embodiments, in the non-aqueous electrolyte, M a+ M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni.
[0203] In some embodiments, a, b, and c are each independently selected from 1, 2, or 3.
[0204] In some embodiments, m is 1, 2, or 3.
[0205] In some embodiments, n is 0 or 1-4, and further can be 0, 1, 2, 3 or 4.
[0206] In some embodiments, the second additive includes one or more of lithium difluorophosphate, lithium monofluorophosphate, lithium tetrafluoroborate, lithium fluorosulfonate, and sodium fluorosulfonate. Further, it can be one or more of lithium difluorophosphate, lithium monofluorophosphate, lithium tetrafluoroborate, lithium fluorosulfonate, and sodium fluorosulfonate.
[0207] In some embodiments, the mass proportion of the second additive in the non-aqueous electrolyte (which can be recorded as W2) is 0 to 11%. The mass proportion of the second additive in the non-aqueous electrolyte W2 is any of the following percentages: 0, 0.005%, 0.01%, 0.015%, 0.02%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 10%, 11%, etc., and can also be selected from the interval consisting of any two of the above percentages, such as 0.005% to 11%, 0.01% to 11%, 0 to 10%, 0.005% to 10%, 0.01% to 10%, 0.05% to 10%, 0.05% to 5%, etc. When W2 is 0, that is, the second additive is not added to the non-aqueous electrolyte.
[0208] The introduction of the first additive diisocyanate may increase the impedance of the formed SEI film. By introducing the second additive into the non-aqueous electrolyte, an inorganic-rich SEI film can be formed at the negative electrode, which can improve the fast charging performance of the secondary battery and further improve the cycle performance of the secondary battery.
[0209] In some embodiments, the volume average particle size D of the negative electrode active material is v 50≥6μm; among which, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the substance or material reaches 50%; Optionally, the volume average particle size D of the negative electrode active material v 50 is 6 μm to 20 μm; further optionally, the volume average particle size D of the negative electrode active material v 50 is 15 μm to 20 μm. The D v 50 can also be any of the following sizes: 6μm, 8μm, 10μm, 12μm, 15μm, 16μm, 18μm, 20μm, etc., or a range consisting of any two of the above sizes.
[0210] In the context of this application, the volume cumulative distribution particle size D vN (where N represents any value selected from 0 to 100) is used to characterize the particle size of a substance or material, which refers to the particle size corresponding to when the cumulative volume distribution percentage of the substance or material reaches N%, and the particle size is less than or equal to D v The volume percentage of N is N%. v N can be obtained from the volume cumulative distribution curve of the particle size of the substance or material. If there is no other explanation, the volume cumulative distribution curve starts from zero from the small particle size side. v 50 as an example, D v 50 refers to the particle size corresponding to when the cumulative volume distribution percentage of a substance or material reaches 50%. v 50, for example, means that 50% of the volume of the substance or material has a particle size less than or equal to D v 50, and 50% of the volume of the substance or material has a particle size larger than D v 50. Those skilled in the art will appreciate that v 50, and can be measured by instruments and methods known in the art. For example, it can be conveniently measured by a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer and LS-909 laser particle size analyzer (OMEC) of Malvern Instruments Ltd., UK, with reference to the particle size distribution laser diffraction method of GB / T19077-2016.
[0211] By controlling the particle size of the negative electrode active material to have a relatively large particle size, the contact area between the negative electrode material and the electrolyte can be reduced, and the probability of side reactions with the solvent on the negative electrode surface can be reduced, which is more conducive to reducing the electrode expansion rate and can better improve the cycle performance of the battery cell.
[0212] In some embodiments, the BET specific surface area of the negative electrode active material is 0.5 m 2 / g~2.0m 2 / g; Optionally, the BET specific surface area of the negative electrode active material is 0.8m 2 / g~1.5m 2 The BET specific surface area of the negative electrode active material can also be any of the following values or a range consisting of any two of the following values: 0.5 m 2 / g, 0.6m 2 / g, 0.8m 2 / g, 1m 2 / g, 1.5m 2 / g, 1.8m 2 / g, 2m 2 / g, etc.
[0213] In the present application, the BET specific surface area of the negative electrode active material can be obtained by testing (but not limited to) the following method: testing by nitrogen adsorption specific surface area analysis test method, and calculated by BET (Brunauer Emmett Teller) method, wherein the nitrogen adsorption specific surface area analysis test can be performed by the Tri Star II specific surface and pore analyzer of Micromeritics Company of the United States, and the test steps can refer to GB / T 19587-2004. The sample to be tested: the raw material of the negative electrode active material; it can also be the negative electrode active material sampled from the negative electrode active material layer of the negative electrode sheet. The test analysis method is as follows: the sample to be tested is dried in a vacuum drying oven at 200°C for 2 hours; then argon is used as the adsorption gas, and the adsorption and desorption curve with a relative pressure P / P0 of 0 to 0.99 is measured by the specific surface and pore analyzer, P is the equilibrium adsorption pressure, P0 is the saturated vapor pressure, and the specific surface area of the negative electrode active material is calculated by the BET method.
[0214] By controlling the particle size of the negative electrode active material to have a certain specific surface area, the surface area of the negative electrode material can be reduced, thereby reducing the contact area between the negative electrode material and the electrolyte, thereby reducing the side reactions of the solvent on the negative electrode surface and better improving the cycle performance of the battery cell.
[0215] Negative electrode
[0216] In the present application, the negative electrode sheet in the secondary battery includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a graphite material.
[0217] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active substance, and the negative electrode active substance includes a graphite material.
[0218] In some embodiments, the weight percentage of graphite material in the negative electrode active material is ≥50%. The weight percentage of graphite material in the negative electrode active material can also be any of the following percentages, or greater than or equal to any of the following percentages, or an interval from any of the following percentages to 100%, or an interval consisting of any two of the following percentages: 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, etc. In some embodiments, the weight percentage of graphite material in the negative electrode active material is ≥80%. In some embodiments, the weight percentage of graphite material in the negative electrode active material is 100%.
[0219] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0220] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the negative electrode current collector, non-limiting examples of the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the negative electrode current collector, non-limiting examples of the polymer material substrate may include one or more of substrates such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0221] In some embodiments, the graphite material in the negative electrode active material may include one or more of artificial graphite and natural graphite. The negative electrode active material may also include other negative electrode active materials for batteries known in the art. As a non-limiting example, the negative electrode active material may also include one or more of the following materials: soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used, as long as they contain graphite materials. These negative electrode active materials may use only one type of graphite material alone, or may use two or more in combination (at this time at least including graphite materials).
[0222] In some embodiments, the negative electrode active material includes artificial graphite.
[0223] In some embodiments, the negative electrode film layer may further optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0224] In some embodiments, the negative electrode film layer may further include a conductive agent, which may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0225] In some embodiments, the negative electrode film layer may further include other auxiliary agents, such as a thickener, etc. Non-limiting examples of thickeners may include sodium carboxymethyl cellulose (CMC-Na) and the like.
[0226] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on at least one side of the surface of the negative electrode collector, and after drying, compaction (compacting can be performed by cold pressing), etc., the negative electrode sheet can be obtained. The surface of the negative electrode collector coated with the negative electrode slurry can be on a single surface of the negative electrode collector or on both surfaces of the negative electrode collector. The solid content of the negative electrode slurry can be 40wt% to 60wt%. The compacted density of the negative electrode sheet can be 1.4g / cm 3 ~1.95g / cm 3 , further optional to 1.5g / cm 3 ~1.8g / cm 3 .
[0227] In the present application, wt% means weight percentage.
[0228] Positive electrode
[0229] In the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer includes a positive electrode active material layer, and further, the positive electrode active material layer includes a positive electrode active substance.
[0230] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0231] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material on a polymer material substrate; the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy; non-limiting examples of polymer material substrates include substrates made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and the like.
[0232] In some embodiments of the present application, the positive electrode active material includes a lithium ion material; further, the secondary battery is a lithium ion secondary battery.
[0233] In some embodiments of the present application, the secondary battery is a lithium-ion secondary battery. A lithium-ion secondary battery utilizes the embedding and de-embedding of lithium ions in electrodes and the transmission in electrolytes to achieve the charging and discharging process. Generally speaking, the active ions in a lithium-ion secondary battery are lithium ions, but are not limited thereto.
[0234] The positive electrode active material may adopt the positive electrode active material for the battery known in the art. As a non-limiting example, the positive electrode active material may include one or more of the following materials or substances: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials or substances, and other traditional materials or substances that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, non-limiting examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and their modified compounds. Non-limiting examples of lithium cobalt oxide include LiCoO2; non-limiting examples of lithium nickel oxide include LiNiO2; non-limiting examples of lithium manganese oxide include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxide include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxides include LiNi 0.85 Co 0.15 Al 0.05O2. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. Non-limiting examples of lithium iron phosphate include LiFePO4 (also referred to as LFP); non-limiting examples of lithium manganese phosphate include LiMnPO4.
[0235] In some embodiments, the positive electrode active material may include but is not limited to one or more of the following materials: lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, sodium oxide and potassium oxide, and materials consisting of any of the foregoing substances and doping elements; further, the doping elements in any one of the positive electrode active materials independently include one or more of transition metal elements and non-transition metal elements.
[0236] In some embodiments, the positive electrode film layer may also optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0237] In some embodiments, the positive electrode film layer may further include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0238] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on at least one side of the positive electrode collector, and after drying, compaction (compacting can be performed by cold pressing), etc., the positive electrode sheet can be obtained. The type of solvent may include but is not limited to any one of the aforementioned embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode collector coated with the positive electrode slurry may be on a single surface of the positive electrode collector or on both surfaces of the positive electrode collector. The solid content of the positive electrode slurry may be 40wt% to 80wt%. The compacted density of the positive electrode sheet may be 3.0 to 3.6g / cm 3 , can be selected as 3.3~3.5g / cm 3 .
[0239] Electrolytes
[0240] The electrolyte has the function of conducting active ions between the positive electrode sheet and the negative electrode sheet. The electrolyte in the present application includes an electrolyte solution.
[0241] In some embodiments, the electrolyte is a non-aqueous electrolyte. The non-aqueous electrolyte may include an electrolyte salt and a solvent. In a lithium-ion secondary battery, the electrolyte salt may include an electrolyte lithium salt.
[0242] In some embodiments, the electrolyte lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorobis(oxalatophosphate), and lithium tetrafluorooxalatophosphate.
[0243] In some embodiments, the solvent is an organic solvent.
[0244] In the present application, the solvent in the non-aqueous electrolyte includes a chain carboxylic acid ester (referred to as a first solvent). The definition of the first solvent is as described above.
[0245] In some embodiments, in addition to including the first solvent, the solvent may also include one or more of an ether solvent and a carbonate solvent. The carbonate solvent may include one or more of carbonates and halogenated carbonates, such as, for example, ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) and one or more of any of the fluorochemicals described above.
[0246] In other embodiments, the solvent, in addition to the first solvent, may also include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, ethyl methyl sulfone and diethyl sulfone.
[0247] In some embodiments, the solvent includes one or more of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in addition to the first solvent. In some embodiments, the solvent includes ethylene carbonate. In some embodiments, the solvent includes ethyl methyl carbonate. In some embodiments, the solvent includes ethylene carbonate and ethyl methyl carbonate, and further, the volume ratio of ethylene carbonate and ethyl methyl carbonate can be 3:7, but is not limited thereto.
[0248] In some embodiments, the solvent is a combination of the first solvent, ethylene carbonate, and ethyl methyl carbonate.
[0249] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0250] In some embodiments, the additive may include one or more of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), methylene methanedisulfonate (MMDS), 1-propylene-1,3-sultone (PST), vinyl sulfite (ES), propylene sulfite (PS), vinyl sulfate (DTD), succinonitrile (SN), adiponitrile (AND), sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB) and anisole.
[0251] In some embodiments, the additive includes one or more of a first additive and a second additive.
[0252] In some embodiments, the additive includes a first additive.
[0253] In some embodiments, the additive includes a second additive.
[0254] In some embodiments, the additive includes a first additive and a second additive.
[0255] The definitions of the first additive and the second additive are as described above, including but not limited to the types and amounts.
[0256] Isolation film
[0257] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0258] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0259] Electrode assembly, electrochemical energy storage device, secondary battery
[0260] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0261] In some embodiments, the electrochemical energy storage device may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0262] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0263] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0264] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.
[0265] In some embodiments, reference Figure 2 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to actual needs.
[0266] In some embodiments, the secondary battery has one or more of the following effects:
[0267] Fast charging time: fast charging time ≤35min, further can be ≤33min, further can be ≤32min, further can be ≤30min, further can be ≤28min;
[0268] Negative electrode sheet expansion: When cycled at 45°C to 80% SOH, the negative electrode sheet expansion rate is ≤36%, further ≤35.5%, further ≤33%, further ≤32%, further ≤30%, further ≤258%;
[0269] Cycle performance: The number of cycles at 45°C to 80% SOH is ≥800, further ≥900, further ≥950, further ≥1000, further ≥1100, further ≥1150, further ≥1200;
[0270] Gas production performance: The expansion rate of 30D battery cells stored at 60℃ is ≤9%, further ≤8%, further ≤7.5%, further ≤7%.
[0271] In some embodiments, the secondary battery has excellent storage performance based on the comprehensive performance of excellent fast charging capability, cycle performance and safety performance. In some embodiments, the capacity retention rate of 30D storage at 60°C is ≥85%, further ≥88%, further ≥90%, and further ≥95%.
[0272] In some embodiments, the fast charging time is ≤35min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤33%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥900, the expansion rate of the battery cell when stored at 60°C for 30D is ≤8%, and further, the capacity retention rate when stored at 60°C for 30D is ≥88%.
[0273] In some embodiments, the fast charging time is ≤33min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤32%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥1000, the expansion rate of the battery cell when stored at 60°C for 30D is ≤8%, and further, the capacity retention rate when stored at 60°C for 30D is ≥90%.
[0274] In some embodiments, the fast charging time is ≤30min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤30%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥950, the expansion rate of the battery cell when stored at 60°C for 30D is ≤8%, and further, the capacity retention rate when stored at 60°C for 30D is ≥90%.
[0275] In some embodiments, the fast charging time is ≤35min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤32%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥900, the expansion rate of the battery cell when stored at 60°C for 30D is ≤7%, and further, the capacity retention rate when stored at 60°C for 30D is ≥88%.
[0276] In some embodiments, the fast charging time is ≤30min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤30%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥1000, the expansion rate of the battery cell when stored at 60°C for 30D is ≤7%, and further, the capacity retention rate when stored at 60°C for 30D is ≥90%.
[0277] In some embodiments, the fast charging time is ≤32 min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤33%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥1100, the expansion rate of the battery cell when stored at 60°C for 30D is ≤7.5%, and further, the capacity retention rate when stored at 60°C for 30D is ≥90%.
[0278] In some embodiments, the fast charging time is ≤28min, the expansion rate of the negative electrode plate when cycled at 45°C to 80% SOH is ≤28%, the number of cycles corresponding to the cycle at 45°C to 80% SOH is ≥1200, the expansion rate of the battery cell when stored at 60°C for 30D is ≤7.5%, and further, the capacity retention rate when stored at 60°C for 30D is ≥95%.
[0279] In a second aspect, the present application provides an electrical device, which includes the secondary battery described in the first aspect of the present application.
[0280] The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.
[0281] As the electrical device, a secondary battery can be selected according to its usage requirements.
[0282] Figure 3 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.
[0283] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0284] Below, some embodiments of the present application are described. The embodiments described below are exemplary, are only used to explain the present application, and cannot be construed as limiting the present application. In the embodiments, if the technology or conditions are not indicated, they are carried out according to the description above, or according to the technology or conditions described in the document in this area or according to the product specification. The reagents used or the instruments that do not indicate the manufacturer are conventional products that can be obtained commercially, or can be synthesized in a conventional manner by commercially available products.
[0285] Example 1.
[0286] 1. Preparation of negative electrode
[0287] 1.1. The type of negative electrode active material is selected according to Table 1, and a certain volume average particle size D is selected. v 50 and BET specific surface area of negative electrode active material.
[0288] (1) Particle size test
[0289] Sample preparation: negative electrode active material raw material; it can also be the negative electrode active material sampled from the negative electrode active material layer of the negative electrode sheet. In order to avoid the agglomeration during the drying process affecting the particle size test, the washed and wetted sample is taken for dispersion test.
[0290] Particle size type: volume average particle size D v 50 tests.
[0291] Equipment model: Malvern 3000 (MasterSizer 3000) laser particle size analyzer, reference standard process: GB / T19077-2016 / ISO 13320:2009.
[0292] Test process: Take an appropriate amount of the sample to be tested (the sample concentration can meet the 8% to 12% shading degree), add 20mL of anhydrous ethanol, and ultrasonically treat for 5 minutes (53KHz / 120W) to completely disperse the sample, and then measure the sample according to GB / T19077-2016 / ISO13320:2009 standard.
[0293] (2) BET specific surface area test of negative electrode active material
[0294] Sample preparation: negative electrode active material raw material; it can also be the negative electrode active material sampled from the negative electrode active material layer of the negative electrode sheet.
[0295] Test method: The nitrogen adsorption specific surface area analysis test method is used for testing, and the result is calculated by the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed by the Tri Star II specific surface and pore analyzer of Micromeritics Company of the United States. The test steps can refer to GB / T 19587-2004.
[0296] The detailed steps are as follows: dry the sample to be tested in a vacuum drying oven at 200°C for 2 hours; then use argon as the adsorption gas, and use a specific surface and pore analyzer to map the adsorption-desorption curve with a relative pressure P / P0 of 0 to 0.99, where P is the equilibrium adsorption pressure and P0 is the saturated vapor pressure. The specific surface area of the negative electrode active material is calculated using the BET method.
[0297] 1.2. Preparation of negative electrode
[0298] The negative electrode active material artificial graphite, conductive agent carbon black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in solvent deionized water at a weight ratio of 90:4:4:2, and mixed evenly to prepare a negative electrode slurry (solid content of 48%); the negative electrode slurry is evenly coated on the double-sided surface of the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting. The compacted density of the negative electrode sheet is 1.65g / cm 3 .
[0299] Among them, the OI value of graphite particles, the D v 50. The OI value of the negative electrode sheet is regulated by at least one parameter selected from the group consisting of the porosity of the negative electrode sheet, the compaction density of the negative electrode sheet, the type and content of the components of the negative electrode sheet, etc.
[0300] The OI value of the negative electrode is tested by using an X-ray powder diffractometer (X'pert PRO) to test the intensity of the diffraction peaks of the 004 crystal plane and the 110 crystal plane. According to the general rules of X-ray diffraction analysis and the lattice parameter determination method of graphite JIS K0131-1996 and JB / T4220-2011, the X-ray diffraction spectrum is obtained, and then according to OI=I 004 / I 110 The intensity ratio of the diffraction peak of the 004 crystal plane of the negative electrode active material layer to the diffraction peak of the 110 crystal plane is obtained, wherein I 004 is the intensity of the diffraction peak of the 004 crystal plane, I 110 is the intensity of the diffraction peak of the 110 crystal plane.
[0301] Test of negative electrode sheet resistance R: Use BER1300 multi-function electrode sheet resistance meter for testing. First, cut the negative electrode sheet into a sample of a certain size (a small disc with a diameter of 40mm); place the sample between two probes and record the test results. Take multiple (≥5) samples to be tested and calculate the average value of the multiple samples to be tested as the test result.
[0302] 2. Preparation of electrolyte (non-aqueous electrolyte)
[0303] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3:7. 60wt% of methyl acetate based on the total weight of the solvent was added thereto. Subsequently, lithium hexafluorophosphate (LiPF6) was added and dissolved in an organic solvent to make the concentration of LiPF6 12.5wt%, and stirred uniformly to obtain an electrolyte.
[0304] 3. Preparation of positive electrode
[0305] The lithium iron phosphate positive electrode material, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were added to the solvent N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, and the positive electrode slurry (solid content of 67%) was obtained after being fully stirred and mixed. Then, the positive electrode slurry was evenly coated on the double-side surface of the positive electrode current collector, and the single-side coating weight was about 22.7 mg / cm 2 (e.g. 350mg / 1540.25mm 2 ); and then through drying, cold pressing and slitting, the positive electrode sheet is obtained.
[0306] 4. Diaphragm
[0307] A conventional commercially available polypropylene film was used as the isolation film.
[0308] 5. Assembly of secondary batteries
[0309] The positive electrode sheet (width 87mm×length 605mm), the separator (width 98mm×length 1896mm), and the negative electrode sheet (width 93mm×length 735mm) are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain an electrode assembly; the electrode assembly is placed in a battery casing, and after drying, 12.0g of electrolyte (3Ah, injection coefficient 4.0g / Ah) is injected, and then a lithium-ion battery is obtained through processes such as formation and standing.
[0310] Examples 2 to 41 and Comparative Examples 1 to 9 adopt the same method as Example 1, except that the type of negative electrode active material, the negative electrode OI value, the resistance value R of the negative electrode sheet, the type and amount of the first solvent (chain carboxylic acid ester), the type and amount of the first additive, the type and amount of the second additive, the D of the negative electrode active material v 50 and one or more parameters of specific surface area (BET), please refer to Table 1 and Table 2.
[0311] Table 1.
[0312]
[0313]
[0314] In Table 1, W0 is the mass proportion of the first solvent in the electrolyte solvent.
[0315] Table 2.
[0316]
[0317]
[0318]
[0319] In Table 1, W1 is the mass proportion of the first additive in the electrolyte (non-aqueous electrolyte); W2 is the mass proportion of the second additive in the electrolyte (non-aqueous electrolyte).
[0320] Test analysis method
[0321] 1. Fast charging performance test
[0322] At 25℃, the divided battery was subjected to 2.5V~3.65V charge and discharge test. The test steps are: first 3C constant current charge to 30% SOC, 2C constant current charge to 60% SOC, 1C constant current constant voltage charge to 80% SOC, cut-off current is 0.01C, stand for 5min; 1C constant current discharge to 2.0V, stand for 5min. Determine the time it takes for the battery to charge to 80% SOC.
[0323] Among them, SOC represents the remaining capacity of the battery, and its value range is 0-100%. When SOC=0, it means that the battery is fully discharged, and when SOC=100%, it means that the battery is fully charged.
[0324] 2. Pole expansion rate test (45℃ cycle to 80% SOH pole expansion rate)
[0325] At 45°C, the lithium-ion battery is charged to 3.65V at a constant current of 0.5C, then charged at a constant voltage of 3.65 until the current is less than 0.05C, and then the lithium-ion battery is discharged to 2.5V at a constant current of 0.5C. This is a charge and discharge process (i.e., 1 cycle). The thickness L0 of the negative electrode plate is measured using a micrometer (Mitutoyo293-100, with an accuracy of 0.01mm). Repeat the charging and discharging in this way, and record the thickness L1 of the negative electrode plate when the capacity retention rate is 80%; the expansion rate of the negative electrode plate after cycling at 45°C to 80% SOH = (L1 / L0-1)×100%.
[0326] 3. Cycle performance test
[0327] At 45°C, charge the lithium-ion battery at a constant current of 0.5C to 3.65V, then charge at a constant voltage of 3.65 until the current is less than 0.05C, and then discharge the lithium-ion battery at a constant current of 0.5C to 2.5V. This is one charge and discharge process (i.e., 1 cycle). Repeat the charging and discharging process, and record the number of cycles when the capacity retention rate is 80%. Record it as "the number of cycles corresponding to 80% SOH at 45°C".
[0328] 4. Gas production performance test
[0329] The lithium-ion secondary battery is charged to 3.65V at a constant current of 0.33C, and then charged to a current of 0.05C at a constant voltage of 3.65V to fully charge the lithium-ion battery. The volume of the battery is tested by the water displacement method, and the volume at this time is recorded as the volume before storage. The lithium-ion battery is then stored at 60°C for 30 days. After the storage is completed, the lithium-ion secondary battery is placed in an environment of 25°C and the volume of the battery is tested by the water displacement method, and the volume at this time is recorded as the volume after storage. The volume expansion rate of the battery is calculated according to the following formula:
[0330] Battery volume expansion rate = (volume after storage / volume before storage-1) × 100%.
[0331] It is recorded as "30D battery cell expansion rate stored at 60℃". The lower the value, the lower the gas production, and the lower the value, the better the gas production performance.
[0332] 5. Storage performance test
[0333] At 25°C, the lithium-ion battery is charged to 3.65V at a constant current of 0.33C, then charged at a constant voltage of 3.65 until the current is less than 0.05C, and then the lithium-ion battery is discharged to 2.5V at a constant current of 0.33C (the battery discharge capacity is recorded as C0). The fully charged battery is placed in a 60°C oven for 30 days, the battery is taken out, and the battery is placed in a 25°C environment for 0.33C discharge, and the discharge capacity is recorded as C1; the capacity retention rate = (C1 / C0) × 100%, recorded as "60°C storage 30D capacity retention rate".
[0334] Test analysis results
[0335] The test results can be found in Table 3.
[0336] The secondary batteries prepared in Examples 1 to 41 have achieved excellent comprehensive performance in terms of fast charging capability, low negative electrode plate expansion, and battery cycle performance. Among them, the battery cell expansion rate in the high-temperature gas production test also reflects the gas production performance, which can be referred to the fast charging time, the expansion rate of the negative electrode plate when cycled to 80% SOH at 45°C, the number of cycles corresponding to 80% SOH at 45°C, and the battery cell expansion rate data stored at 60°C for 30D. In addition, the secondary batteries prepared in Examples 1 to 41 also have excellent storage performance (refer to the capacity retention rate data stored at 60°C for 30D).
[0337] The W0×100 / (R×OI) of Comparative Examples 1 to 9 is either less than 0.08 or greater than 5, resulting in that the comprehensive performance of the secondary battery in terms of fast charging capability, cycle performance and safety performance is significantly inferior to that of Examples 1 to 41.
[0338] Although the OI value, negative electrode sheet resistance R and W0 in Comparative Examples 1 to 5 can be used for the technical solution of the present application, their combined relationship does not meet 0.08≤W0×100 / (R×OI)≤5, which makes it difficult to take into account the better fast charging capability, low electrode sheet expansion, low gas production battery cell expansion and better cycle performance. At least one performance parameter is obviously poor or has not improved in the fast charging capability, low electrode sheet expansion, low battery cell expansion and better cycle performance. Among them, in Comparative Example 1, W0×100 / (R×OI) is greater than 5, the negative electrode sheet is demolded, and the battery cell cannot work. The negative electrode sheet of Comparative Example 2 expands significantly more, the battery cell of Comparative Example 3 expands significantly more, and the fast charging capability of Comparative Examples 4-5 deteriorates significantly.
[0339] In Comparative Example 6, the OI value is slightly large, but W0×100 / (R×OI) is too small; in Comparative Example 7, the negative electrode sheet resistance R value is slightly low, but W0×100 / (R×OI) is too large; in Comparative Example 8, the R value is slightly high, but W0×100 / (R×OI) is too small; in Comparative Example 9, the content of chain carboxylic acid ester (first solvent) is slightly high, but W0×100 / (R×OI) is too large. As a result, Comparative Examples 6-9 failed to achieve excellent comprehensive effects in terms of fast charging capability, cycle performance and safety performance.
[0340] Although Comparative Examples 7 and 9 have shorter fast charging times, the cost is increased electrode expansion, significantly deteriorated cycle performance, significantly increased cell expansion after high-temperature gas production, and poor storage performance.
[0341] Although the expansion of the electrode is suppressed in Comparative Example 8, the fast charging capability is sacrificed, and the cycle performance is significantly deteriorated, and the expansion of the battery cell after gas production is still large.
[0342] Table 3.
[0343]
[0344]
[0345] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0346] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples. Within the scope of the technical solution of the present application, the embodiments that have the same structure as the technical idea and play the same effect are all included in the technical scope of the present application. The above-mentioned embodiments only express several embodiments of the present application, and the description is relatively detailed, but it cannot be understood as a limitation on the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various deformations that can be thought of by those skilled in the art and other methods of combining and constructing some of the constituent elements in the embodiments are also included in the scope of the present application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several deformations and improvements can be made, which all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the attached claims, and the description and drawings can be used to explain the content of the claims.
Claims
1. A secondary battery comprising a positive electrode sheet, a negative electrode sheet and a non-aqueous electrolyte; in, The negative electrode plate includes a negative electrode active material, the negative electrode active material includes a graphite material, the OI value of the negative electrode plate satisfies 6≤OI≤18, and the resistance value R of the negative electrode plate satisfies 2mΩ≤R≤16mΩ; The non-aqueous electrolyte includes a solvent, the solvent includes a first solvent, the first solvent is a chain carboxylate, and a mass proportion W0 of the first solvent in the solvent satisfies 20%≤W0≤60%; The OI value of the negative electrode plate refers to the ratio of the diffraction peak intensity of the 004 crystal plane of the graphite material to the diffraction peak intensity of the 110 crystal plane; the unit of R is mΩ.
2. The secondary battery according to claim 1, wherein 12≤OI≤18.
3. The secondary battery according to claim 1 or 2, wherein: 2mΩ≤R≤15mΩ; Optionally, 5mΩ≤R≤15mΩ.
4. The secondary battery according to any one of claims 1 to 3, wherein 1≤W0×100 / OI≤10; further optionally, 1≤W0×100 / OI≤5; further optionally, 3≤W0×100 / OI≤5; Alternatively, 1≤W0×100 / OI≤4.
5. The secondary battery according to any one of claims 1 to 4, wherein 0.07 / mΩ≤W0×100 / (R×OI)≤5 / mΩ; Optionally, 0.08 / mΩ≤W0×100 / (R×OI)≤5 / mΩ; Further optionally, 0.1 / mΩ≤W0×100 / (R×OI)≤5 / mΩ; Further optionally, 0.1 / mΩ≤W0×100 / (R×OI)≤2 / mΩ; further optionally, 0.1 / mΩ≤W0×100 / (R×OI)≤1 / mΩ.
6. The secondary battery according to any one of claims 1 to 5, wherein 6≤OI≤18, 2mΩ≤R≤15mΩ, and 20%≤W0≤60%; Alternatively, 12≤OI≤18, 5mΩ≤R≤15mΩ, and 20%≤W0≤60%.
7. The secondary battery according to any one of claims 1 to 6, wherein The first solvent comprises a compound having a structure as shown in formula (1): Wherein, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Haloalkyl; Optionally, R1 and R2 are independently C 1-3 Alkyl or C 1-3 Fluorinated alkyl; Further optionally, R1 and R2 are independently one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl and fluoropropyl; Further optionally, R1 and R2 are independently one of methyl, ethyl, fluoromethyl and fluoroethyl; Further optionally, the first solvent includes one or more of the following compounds: methyl acetate, ethyl acetate, methyl difluoroacetate and ethyl difluoroacetate.
8. The secondary battery according to claim 7, wherein The first solvent is methyl acetate, and the mass proportion W0 of methyl acetate in the solvent is 20%-40%; or the first solvent is ethyl acetate, and the mass proportion W0 of ethyl acetate in the solvent is 40%-60%.
9. The secondary battery according to any one of claims 1 to 8, wherein The non-aqueous electrolyte further includes a first additive; the first additive is diisocyanate.
10. The secondary battery according to claim 9, wherein The first additive includes a compound having the following structure: Wherein R3 is unsubstituted or Ra substituted CC 1-18 Alkylene; Ra includes one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC(=O)R 11 , R 12 OC(=O)-、C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 One or more of oxaalkyl; R 11 and R 12 are independently alkyl or haloalkyl; Optionally, R3 is C 2-10 Alkylene, C 2-10 Heteroalkylene, C 6-18 Arylene, C 2-18 Heteroarylene, C 3-18 Alicyclic or C 3-18 Heteroalicyclic group, any of the aforementioned groups is unsubstituted or substituted by Ra; Alternatively, R3 is unsubstituted or Ra substituted C 2-10 Alkylene, unsubstituted or Ra substituted C 3-18 Bivalent cycloalkyl or unsubstituted or Ra substituted C 6-18 Arylene; further optionally, R3 is C 2-10 Alkylene, C 6-18 Divalent cycloalkyl or C 6-18 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-14 Divalent cycloalkyl or C 6-14 Arylene; further optionally, R3 is C 4-10 Alkylene, C 6-10 Divalent cycloalkyl or C 6-10 Arylene; further optionally, R3 is C 4-8 Hexylene, C containing hexyl ring 6-10 A divalent cycloalkyl group or a C 6-10 arylene; Alternatively, the first additive includes one or more of the following compounds: hexamethylene diisocyanate, 1,4-cyclohexanedimethyl diisocyanate, 1,3-phenylene diisocyanate and 2,4-diisocyanato-1-toluene.
11. The secondary battery according to claim 9 or 10, wherein: The mass percentage of the first additive in the non-aqueous electrolyte is 0.005% to 11%; Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.005% to 10%; Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.01% to 10%; Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 0.1% to 5%; Further optionally, the mass proportion of the first additive in the non-aqueous electrolyte is 1% to 5%.
12. The secondary battery according to any one of claims 1 to 11, wherein The non-aqueous electrolyte further includes a second additive; the second additive includes one or more of lithium monofluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, a compound represented by formula (3) and a fluorosulfonate; In formula (3), a, b and c are each independently a positive integer, m is an integer selected from 1 to 3, n is an integer selected from 0 to 4, and q is 0 or 1; M a+ is a metal ion with a positive charge; any Y is independently a boron atom or a phosphorus atom; X is a halogen atom; any R is independently a substituted or unsubstituted C 1-10 Alkylene, substituted or unsubstituted C 1-10 Haloalkylene, substituted or unsubstituted C 6-20 Arylene, and substituted or unsubstituted C 6-20 One of the halogenated arylene groups; Optionally, any one R is independently Rc substituted or unsubstituted C 1-10 Alkylene, Rc substituted or unsubstituted C 1-10 Haloalkylene, Rc substituted or unsubstituted C 6-20 Arylene, and Rc substituted or unsubstituted C 6-20 A halogenated arylene group; C substituted with Rc 1-10 Substituents in alkylene, C substituted with Rc 1-10 Substituents in haloalkylene, C substituted with Rc 6-20 Substituents in arylene and Rc substituted C 6-20 The Rc substituents in the halogenated arylene group may each independently include one or more of the following substituents: halogen atoms, -CN, -NCO, -OH, -COOH, -SOOH, -OC=(O)R 41 、-C=(O)OR 42 , C 1-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl and C 2-10 Alkoxy; wherein R 41 and R 42 Each independently is C 1-6 alkyl; Optionally, in the non-aqueous electrolyte, M a+ Wherein M includes one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni; Optionally, a, b and c are each independently selected from 1, 2 or 3.
13. The secondary battery according to claim 12, wherein: The second additive includes one or more of lithium difluorophosphate, lithium monofluorophosphate, lithium tetrafluoroborate, lithium fluorosulfonate and sodium fluorosulfonate; optionally, includes lithium difluorophosphate and / or lithium fluorosulfonate.
14. The secondary battery according to claim 12 or 13, wherein: The mass percentage of the second additive in the non-aqueous electrolyte is 0.005% to 11%; Optionally, the mass percentage of the second additive in the non-aqueous electrolyte is 0.005% to 11%; Further, the mass proportion of the second additive in the non-aqueous electrolyte is 0.005% to 10%; Further optionally, the mass proportion of the second additive in the non-aqueous electrolyte is 0.05% to 5%.
15. The secondary battery according to any one of claims 1 to 14, wherein The solvent of the non-aqueous electrolyte further comprises one or more of an ether solvent, a halogenated carbonate solvent and a carbonate solvent; Optionally, the solvent of the non-aqueous electrolyte further includes one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone; Optionally, the solvent of the non-aqueous electrolyte further includes ethylene carbonate and / or ethyl methyl carbonate.
16. The secondary battery according to any one of claims 1 to 15, wherein The non-aqueous electrolyte further includes an electrolyte, and the electrolyte includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate.
17. The secondary battery according to any one of claims 1 to 16, wherein The non-aqueous electrolyte further includes a third additive, and the third additive includes one or more of vinylene carbonate, ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, trifluoromethylethylene carbonate, methylene disulfonate, 1-propylene-1,3-sultone, vinyl sulfite, propylene sulfite, vinyl sulfate, succinonitrile, adiponitrile, sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate and anisole.
18. The secondary battery according to any one of claims 1 to 17, wherein The volume average particle size D of the negative electrode active material v 50≥6μm; among which, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the substance or material reaches 50%; Optionally, the volume average particle size D of the negative electrode active material is v 50: 6μm~20μm; Further optionally, the volume average particle size D of the negative electrode active material is v 50 is 15μm~20μm.
19. The secondary battery according to any one of claims 1 to 18, wherein The BET specific surface area of the negative electrode active material is 0.5 m 2 / g~2.0m 2 / g; Optionally, the BET specific surface area of the negative electrode active material is 0.8 m 2 / g~1.5m 2 / g.
20. The secondary battery according to any one of claims 1 to 19, wherein The graphite material includes one or more of artificial graphite and natural graphite; Optionally, the graphite material includes artificial graphite.
21. The secondary battery according to any one of claims 1 to 20, wherein The weight percentage of the graphite material in the negative electrode active material is ≥50%; Optionally, the weight percentage of the graphite material in the negative electrode active material is ≥80%; Further optionally, the weight percentage of the graphite material in the negative electrode active material is 100%.
22. The secondary battery according to any one of claims 1 to 21, wherein The secondary battery is a lithium ion secondary battery; Optionally, the positive electrode plate includes a positive electrode active material, and the positive electrode active material includes lithium iron phosphate or lithium nickel cobalt manganese oxide; Optionally, the secondary battery includes an outer package, and an electrode assembly and the electrolyte encapsulated in the outer package, and the electrode assembly is made of the positive electrode sheet, the negative electrode sheet and a separator through a winding process or a lamination process.
23. The secondary battery according to claim 22, wherein: The fast charging time of the secondary battery is ≤35 min, further ≤33 min, further ≤32 min, further ≤30 min, further ≤28 min; Optionally, the expansion rate of the negative electrode plate when cycled to 80% SOH at 45° C. is ≤36%, further ≤35.5%, further ≤33%, further ≤32%, further ≤30%; Optionally, under the condition of storage at 60° C. for 30 days, the expansion rate of the battery cell is ≤9%, further ≤8%, further ≤7.5%, further ≤7%.