By using a high-tensile-strength negative electrode current collector and a base coating containing conductive agents and binders, the problems of electrode shrinkage and film delamination caused by the expansion of silicon-based materials are solved, thereby improving the cycle performance and stability of the battery.
Patent Information
- Application Number
- CN202310594306.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The expansion of silicon-based materials during battery charging can cause wrinkling of the electrode sheets and delamination of the active layer, affecting the battery's cycle performance.
The negative electrode current collector with high tensile strength is used with a base coating containing conductive agent and first binder to enhance the adhesion between the negative electrode film layer and the current collector, buffer the expansion of silicon-based material, and reduce the risk of electrode wrinkling and film delamination.
It improves the cycle performance of the battery, reduces the risk of electrode shrinkage and delamination during charging, and enhances the stability and lifespan of the battery.
Smart Images

Figure CN119029344A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate, a battery and an electrical device. Background Art
[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0003] Silicon-based materials have a high gram capacity, and using them as active materials in batteries can increase the energy density of batteries. However, silicon-based materials usually have a large expansion rate. At this time, during the charging process of the battery, the expansion of silicon-based materials may cause wrinkles on the pole piece and delamination of the active layer, which in turn has an adverse effect on the cycle performance of the battery. Summary of the invention
[0004] In order to achieve the above-mentioned object, the present application provides a negative electrode plate. The negative electrode plate comprises a negative electrode current collector and a negative electrode film layer located on the negative electrode current collector, the negative electrode film layer comprises an undercoat layer and a negative electrode active layer, the undercoat layer is located between the negative electrode current collector and the negative electrode active layer, the undercoat layer comprises a conductive agent and a first binder, the active material of the negative electrode active layer comprises a silicon-based material, the tensile strength of the negative electrode current collector is ≥800MPa, and the peel strength of the negative electrode film layer is ≥30N / m.
[0005] In the above-mentioned negative electrode plate, the risk of wrinkling of the plate during charging can be reduced by adapting the negative electrode collector with greater tensile strength to the active layer containing silicon-based materials. At the same time, the base coating layer containing a conductive agent and a first binder can improve the bonding force between the negative electrode film layer and the negative electrode collector while maintaining conductivity, thereby reducing the risk of the negative electrode film layer falling off in the plate, thereby improving the cycle performance of the battery.
[0006] In some embodiments, the Young's modulus of the negative electrode current collector is ≥80 GPa.
[0007] In some embodiments, the primer layer further comprises graphite.
[0008] In some embodiments, the graphite includes lamellar graphite.
[0009] In some embodiments, the mass percentage of the graphite in the primer layer is 20% to 35%.
[0010] In some embodiments, the primer layer has a thickness of 2 μm to 6 μm.
[0011] In some embodiments, the mass percentage of the first binder in the primer layer is 25% to 40%.
[0012] In some embodiments, the first binder has a glass transition temperature of 10°C to 50°C.
[0013] In some embodiments, the conductive agent accounts for 30% to 50% by mass of the primer layer;
[0014] In some embodiments, the conductive agent includes at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0015] In some embodiments, the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥50%.
[0016] In some embodiments, the silicon-based material includes at least one of a silicon-oxygen material and a silicon-carbon material.
[0017] In some embodiments, the negative electrode active layer further includes a second binder.
[0018] In some embodiments, the Dv50 of the second binder is 100 nm to 600 nm.
[0019] In some embodiments, the second binder has a glass transition temperature of 10°C to 50°C.
[0020] In some embodiments, the compaction density of the negative electrode active layer is 1.1 g / cm 3 ~1.8g / cm 3 .
[0021] In some embodiments, the compaction density of the negative electrode active layer is 1.15 g / cm 3 ~1.65g / cm 3 .
[0022] In some embodiments, the material of the negative electrode current collector includes at least one of a copper alloy, stainless steel, and an iron-nickel alloy.
[0023] In some embodiments, the thickness of the negative electrode current collector is 4 μm to 20 μm.
[0024] In some embodiments, the thickness of the negative electrode current collector is 5 μm to 10 μm.
[0025] In some embodiments, the elongation at break of the negative electrode current collector is ≤4%.
[0026] A battery comprises the negative electrode plate.
[0027] An electrical device comprises the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0029] Figure 1 It is a schematic diagram of a secondary battery according to one embodiment of the present application.
[0030] Figure 2 for Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.
[0031] Figure 3 FIG. 1 is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source.
[0032] Description of reference numerals:
[0033] 1. Secondary battery; 11. Shell; 12. Electrode assembly; 13. Top cover assembly; 2. Electrical device.
[0034] In order to better describe and illustrate the embodiments and / or examples of the inventions disclosed herein, reference may be made to one or more drawings. The additional details or examples used to describe the drawings should not be considered to limit the scope of the disclosed inventions, the embodiments and / or examples currently described, and any of the best modes of these inventions currently understood. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0037] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0038] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0040] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0041] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0042] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true or exists, and B is false or does not exist; A is false or does not exist, and B is true or exists; or both A and B are true, or both A and B exist.
[0043] Unless otherwise stated, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise stated, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art. For example, the test can be performed according to the method provided in the examples of this application.
[0044] An embodiment of the present application provides a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer located on the negative electrode current collector, the negative electrode film layer includes a primer layer and a negative electrode active layer, the primer layer is located between the negative electrode current collector and the negative electrode active layer, the primer layer includes a conductive agent and a first binder, the active material of the negative electrode active layer includes a silicon-based material, the tensile strength of the negative electrode current collector is ≥800MPa, and the peel strength of the negative electrode film layer is ≥28N / m.
[0045] In the negative electrode sheet of the above embodiment, the risk of wrinkling of the electrode sheet during charging can be reduced by adapting the negative electrode current collector with greater tensile strength to the active layer comprising silicon-based materials. At the same time, the bottom coating layer comprising a conductive agent and a first binder can improve the bonding force between the negative electrode film layer and the negative electrode current collector while maintaining conductivity, thereby reducing the risk of the negative electrode film layer falling off in the electrode sheet.
[0046] It is understood that the negative electrode film layer is located on at least one surface of the negative electrode current collector.
[0047] It can also be understood that the undercoat layer is located between the negative electrode current collector and the negative electrode active layer, and the negative electrode current collector and the negative electrode active layer may be connected through the undercoat layer. In this case, the connection between the undercoat layer and the negative electrode current collector and the negative electrode active layer can have a certain buffering effect on the expansion of the silicon-based material, further reducing the risk of wrinkling of the electrode sheet.
[0048] Optionally, the tensile strength of the negative electrode current collector is ≥800 MPa, or the tensile strength of the negative electrode current collector is ≥850 MPa, or the tensile strength of the negative electrode current collector is ≥900 MPa, or the tensile strength of the negative electrode current collector is ≥950 MPa, or the tensile strength of the negative electrode current collector is ≥1000 MPa.
[0049] Optionally, the peel strength of the negative electrode film layer is ≥28N / m, or the peel strength of the negative electrode film layer is ≥30N / m, or the peel strength of the negative electrode film layer is ≥32N / m, or the peel strength of the negative electrode film layer is ≥35N / m, or the peel strength of the negative electrode film layer is ≥38N / m, or the peel strength of the negative electrode film layer is ≥40N / m, or the peel strength of the negative electrode film layer is ≥45N / m, or the peel strength of the negative electrode film layer is ≥50N / m.
[0050] In the present application, the tensile strength can be tested as follows: cut the negative electrode current collector sample with a length of 100 mm and a width of 15 mm with an accuracy of 0.05 mm, clamp it on the upper and lower clamps of the tensile testing machine, with a distance of 50 mm between the upper and lower clamps, start the clamps and keep loading at 5 mm / min at a stable speed, and record the maximum load of the sample shear failure.
[0051] In the present application, the peel strength of the negative electrode film layer can be tested as follows: a 20 mm wide standard tape (31B) is attached to one surface of the negative electrode film layer using a roller press with a fixed stress (2 kg, 300 mm / min), and a 180 degree peel test is performed using a tensile tester at a speed of 300 mm / min, and 50 peel force values are obtained at a test distance of 50 mm to 120 mm and the average value is calculated. The peel strength is used to indicate the degree of bonding between the negative electrode film layer and the negative electrode current collector. The greater the peel strength, the better the bonding between the negative electrode film layer and the negative electrode current collector.
[0052] In some embodiments, the Young's modulus of the negative electrode current collector is ≥80 GPa. The Young's modulus of the negative electrode current collector within this range can make the negative electrode current collector have a lower extension under stress, which can have a certain restraining effect on the extension of the negative electrode pole piece during the charge and discharge process, and further reduce the risk of wrinkling of the negative electrode pole piece. Optionally, the Young's modulus of the negative electrode current collector is ≥83 GPa, or the Young's modulus of the negative electrode current collector is ≥85 GPa, or the Young's modulus of the negative electrode current collector is ≥90 GPa.
[0053] In the present application, the Young's modulus of the negative electrode current collector can be measured by the static method in accordance with the national standard "Test method for elastic modulus and Poisson's ratio of metallic materials" (GB / T 22315-2008).
[0054] As some selected examples of the negative electrode current collector, the material of the negative electrode current collector includes at least one of a copper alloy, stainless steel, and an iron-nickel alloy.
[0055] In some embodiments, the thickness of the negative electrode current collector is 4 μm to 20 μm. If the thickness of the negative electrode current collector is too small, the structural stability of the negative electrode plate may be low. If the thickness of the negative electrode current collector is too large, the volume of the negative electrode plate may be too large, which may reduce the amount of active material used and reduce the energy density of the battery. Optionally, the thickness of the negative electrode current collector is 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm. Further optionally, the thickness of the negative electrode current collector is 5 μm to 10 μm.
[0056] In some embodiments, the elongation at break of the negative electrode current collector is ≤4%. For example, the elongation at break of the negative electrode current collector is 4%, 3.8%, 3.5%, 3.2%, 3%, etc.
[0057] In some embodiments, the base coating further comprises graphite. It is understood that the graphite may include at least one of natural graphite and artificial graphite. Adding graphite to the base coating can prevent the silicon-based active material from crushing the current collector during the compaction of the pole piece, and can also work together with the conductive agent in the base coating to form a better conductive network.
[0058] Optionally, the graphite includes lamellar graphite. Lamellar graphite has certain slip properties, which can reduce the elongation of silicon-based materials during expansion, release the stress generated during the expansion of active materials, and further reduce the risk of pole film shedding and wrinkling. Further optionally, the graphite includes at least one of KS series graphite and SFG series graphite. Further optionally, the graphite includes KS-6, KS-10, KS-16, SFG-6, SFG-10, and SFG-15. It can be understood that KS and SFG respectively represent the types of graphite, which can be purchased from commercial channels.
[0059] Optionally, the mass percentage of graphite in the primer layer is 20% to 35%. Further optionally, the mass percentage of graphite in the primer layer is 20%, 22%, 25%, 28%, 30%, 32%, 35%, etc. If the mass percentage of graphite in the primer layer is too low, it is difficult to achieve a good effect, and if the mass percentage of graphite in the primer layer is too high, it may have a certain adverse effect on the bonding performance of the primer layer.
[0060] As some examples of the thickness of the primer layer, the thickness of the primer layer is 2 μm to 6 μm. Optionally, the thickness of the primer layer is 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, etc. Too thick a primer layer may increase the overall thickness and volume of the negative electrode sheet, and may also reduce the thickness of the active layer accordingly, reduce the amount of active material used, and reduce the energy density of the battery.
[0061] In some embodiments, the mass percentage of the first binder in the primer layer is 25% to 40%. The mass percentage of the first binder in the primer layer within this range can provide suitable bonding properties for the primer layer and improve the peel strength of the negative electrode film layer. Optionally, the mass percentage of the first binder in the primer layer is 25%, 28%, 30%, 32%, 35%, 38%, 40%, etc.
[0062] In some embodiments, the glass transition temperature of the first binder is 10°C to 50°C. If the glass transition temperature of the first binder is too low, the pole piece may have the problem of sticking to the roller during the subsequent processing, which will have an adverse effect on the subsequent processing of the pole piece. If the glass transition temperature of the first binder is too high, the pole piece may have high brittleness and poor flexibility, and problems such as powder loss and demolding may occur during the subsequent processing, which may also have an adverse effect on the subsequent processing of the pole piece. When the glass transition temperature of the first binder is 10°C to 50°C, the first binder can have a certain viscoelasticity, reduce the risk of cracking of the pole piece due to stress concentration when the silicon-based material expands, and further improve the cycle performance of the battery. Optionally, the glass transition temperature of the first binder is 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc.
[0063] It is understandable that the first binder can be selected from commonly used binders for electrode plates. Optionally, the first binder includes at least one of styrene butadiene and its derivatives, styrene acrylate and its derivatives, polyurethane and its derivatives, polyvinylidene fluoride and its derivatives, and acrylate and its derivatives.
[0064] In some embodiments, in the primer layer, the mass percentage of the conductive agent in the primer layer is 30% to 50%. Optionally, the mass percentage of the conductive agent in the primer layer is 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48% and 50%, etc. Further optionally, the conductive agent includes at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0065] It is understandable that the base coating layer also contains a dispersant, and the use of the dispersant can improve the dispersion uniformity of the materials in the base coating layer.
[0066] In some embodiments, the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥50%. Optionally, the mass percentage of the silicon-based material in the active material of the negative electrode active layer is 50% to 100%. Further optionally, the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥55%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥60%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥65%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥70%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥75%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥80%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥85%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥90%, or the mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥95%.
[0067] In some embodiments, the silicon-based material includes at least one of elemental silicon, silicon-oxygen material, and silicon-carbon material.
[0068] Optionally, when the silicon-based material includes a silicon-oxygen material, since the silicon-oxygen material has a higher expansion rate, a thicker primer layer can be used to buffer the expansion of the silicon-oxygen material, further reducing the risk of wrinkling and delamination of the negative electrode sheet. For example, when the silicon-based material includes a silicon-oxygen material, the thickness of the primer layer is 3 μm to 6 μm, and the mass percentage of the first binder to the primer layer is 25% to 40%.
[0069] Optionally, when the silicon-based material includes a silicon-carbon material, since the silicon-carbon material has a higher hardness and is more difficult to calender, the flexibility of the base coating layer can be improved by using a first binder with a larger mass percentage. For example, when the silicon-based material includes a silicon-carbon material, the mass percentage of the first binder in the base coating layer is 30% to 40%, and the thickness of the base coating layer is 2 μm to 6 μm.
[0070] It is understandable that the negative electrode active layer also includes a second binder. Optionally, the Dv50 of the second binder is 100nm to 600nm. When the negative electrode active layer includes a silicon-based material, the pore size inside the particles of the silicon-based material will be larger after expansion. Using a second binder with a larger particle size, such as a second binder with a Dv50 of 100nm to 600nm, can make the binder more distributed between the particles of the silicon-based material, and can better bond the silicon-based material particles. Optionally, the Dv50 of the second binder is 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, etc.
[0071] Optionally, when the silicon-based material includes a silicon-oxygen material, the Dv50 of the second binder is 100 nm to 600 nm. When the silicon-based material includes a silicon-carbon material, the Dv50 of the second binder is 300 nm to 600 nm.
[0072] In some embodiments, the glass transition temperature of the second binder is 10°C to 50°C. If the glass transition temperature of the second binder is too low, the pole piece may have a problem of sticking to the roller during the subsequent processing, which will have an adverse effect on the subsequent processing of the pole piece. If the glass transition temperature of the second binder is too high, the pole piece may have high brittleness and poor flexibility, and problems such as powder loss and demolding may occur during the subsequent processing, which may also have an adverse effect on the subsequent processing of the pole piece. When the glass transition temperature of the second binder is 10°C to 50°C, the second binder can have a certain viscoelasticity, reduce the risk of cracking of the pole piece due to stress concentration when the silicon-based material expands, and further improve the cycle performance of the battery. Optionally, the glass transition temperature of the second binder is 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc.
[0073] It is understandable that the second binder can be selected from commonly used binders for electrode plates. Optionally, the second binder includes at least one of styrene butadiene and its derivatives, styrene acrylate and its derivatives, polyurethane and its derivatives, polyvinylidene fluoride and its derivatives, and acrylate and its derivatives.
[0074] In some embodiments, the compaction density of the negative electrode active layer is 1.1 g / cm 3 ~1.8g / cm 3 If the compaction density of the negative electrode active layer is too small, the energy density of the battery may be reduced. If the compaction density is too large, the particles of the negative electrode active layer may be pulverized, which may deteriorate the cycle performance. Optionally, the compaction density of the negative electrode active layer is 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 Optionally, the compaction density of the negative electrode active layer is 1.15 g / cm 3 ~1.65g / cm 3 .
[0075] In some embodiments, since the silicon-carbon material has a higher hardness, it is easier to pulverize during the tableting process. Therefore, when the silicon-based material includes the silicon-carbon material, a smaller compaction density can be used. For example, when the silicon-based material includes the silicon-carbon material, the compaction density of the negative electrode active layer is 1.15 g / cm 3 ~1.5g / cm 3 When the silicon-based material includes silicon-oxygen material, the compaction density of the negative electrode active layer is 1.3 g / cm 3 ~1.65g / cm 3 .
[0076] It is understandable that the negative electrode active layer may further include at least one of a conductive agent and a dispersant. The conductive agent and the dispersant may be selected from the conductive agents and dispersants commonly used in electrode plates.
[0077] It is understood that the active material of the negative electrode active layer may include a silicon-based material. Alternatively, the active material of the negative electrode active layer may include a silicon-based material and a carbon-based material. Further optionally, the carbon-based material includes at least one of graphite, soft carbon and hard carbon. Further optionally, the active material of the negative electrode active layer includes graphite and a silicon-based material.
[0078] In some embodiments, the negative electrode active layer includes an active material, a conductive agent, a dispersant, and a second binder. Optionally, the mass ratio of the active material, the conductive agent, the dispersant, and the second binder is (80-95):(4-10):(4-10):(4-10).
[0079] Another embodiment of the present application provides a battery. The battery includes the above-mentioned negative electrode plate.
[0080] Another embodiment of the present application provides an electric device, which includes the above-mentioned battery.
[0081] The secondary battery and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0082] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0083] Positive electrode
[0084] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0085] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two facing surfaces of the positive electrode current collector.
[0086] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum foil may be used. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material on a polymer material substrate. Optionally, the metal material may include but is not limited to one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. Optionally, the polymer material substrate may include but is not limited to one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0087] As an example, the positive electrode active material may include positive electrode active materials for batteries that are well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Optionally, lithium cobalt oxide includes LiCoO2. Lithium nickel oxide includes LiNiO2. Lithium manganese oxide includes at least one of LiMnO2 and LiMn2O4. Lithium nickel cobalt manganese oxide includes LiNi 1 / 3 Co 1 / 3Mn 1 / 3 O2(NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 ) and LiNi 0.8 Co 0.1 Mn 0.1O2(NCM 811 ) at least one of the following. Lithium nickel cobalt aluminum oxide includes LiNi 0.85 Co 0.15 Al 0.05 O2. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. Optionally, the lithium iron phosphate includes LiFePO4 (LFP). The lithium manganese phosphate includes LiMnPO4. The weight ratio of the positive electrode active material in the positive electrode film layer is 80 to 100 weight %, based on the total weight of the positive electrode film layer.
[0088] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0 to 20 weight%, based on the total weight of the positive electrode film layer.
[0089] In some embodiments, the positive electrode film layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0 to 20 weight %, based on the total weight of the positive electrode film layer.
[0090] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent to form a positive electrode slurry. Optionally, the solvent includes N-methylpyrrolidone. The positive electrode slurry has a solid content of 40 to 80 wt%, and the viscosity at room temperature is adjusted to 5000 to 25000 mPa·s. The positive electrode slurry is coated on the surface of the positive electrode collector, and after drying, it is cold-pressed by a cold rolling mill to form a positive electrode sheet; the positive electrode powder coating unit surface density is 25 to 40 mg / cm 2 The compaction density of the positive electrode is 3.0-3.6g / cm 3 , optional: 3.3-3.6g / cm 3 The calculation formula of the compaction density is: compaction density = coating surface density / (thickness of the electrode sheet after extrusion - thickness of the current collector).
[0091] Negative electrode
[0092] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0093] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0094] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Optionally, the metal material includes at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. The polymer material includes at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0095] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more. The weight ratio of the negative electrode active material in the negative electrode film layer is 70 to 100% by weight, based on the total weight of the negative electrode film layer.
[0096] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the negative electrode film layer is 0 to 30% by weight, based on the total weight of the negative electrode film layer.
[0097] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0 to 20 weight %, based on the total weight of the negative electrode film layer.
[0098] In some embodiments, the negative electrode film layer may further include other additives, such as thickeners, etc. The weight ratio of the other additives in the negative electrode film layer is 0 to 15 weight %, based on the total weight of the negative electrode film layer. Optionally, the thickener includes sodium carboxymethyl cellulose (CMC-Na).
[0099] In some embodiments, the negative electrode sheet can be prepared by the following method: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent to form a negative electrode slurry. Optionally, the solvent includes deionized water. The solid content of the negative electrode slurry is 30-70wt%, and the viscosity at room temperature is adjusted to 2000-10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode collector, and after a drying process, cold pressing such as a roller is performed to obtain a negative electrode sheet. The negative electrode powder coating unit surface density is 6-10mg / cm 2 , the compaction density of the negative electrode is 1.1~1.8g / cm 3 .
[0100] Electrolytes
[0101] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0102] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0103] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP). The concentration of the electrolyte salt is generally 0.5 to 5 mol / L.
[0104] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0105] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0106] Isolation film
[0107] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0108] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0109] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0110] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0111] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate. The present application has no particular restrictions on the shape of the secondary battery, which can be cylindrical, square, or any other shape. For example, Figure 1 The secondary battery 1 is a square structure as an example.
[0112] In some embodiments, reference Figure 2 , the outer packaging may include a shell 11 and a top cover assembly 13. Among them, the shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the top cover assembly 13 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 12 through a winding process or a lamination process. The electrode assembly 12 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 12. The number of electrode assemblies 12 contained in the secondary battery 1 can be one or more, and those skilled in the art can select according to specific actual needs.
[0113] In addition, the present application also provides an electric device, which includes a secondary battery provided in the present application. The secondary battery can be used as a power source for the electric device, or as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0114] As the electrical device, a secondary battery can be selected according to its usage requirements.
[0115] Figure 3 The power consumption device 2 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.
[0116] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a secondary battery may be used as a power source.
[0117] Example
[0118] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the present application will be further described in detail below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its applications. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0119] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0120] Example 1
[0121] In this embodiment, a coating method is adopted to prepare a negative electrode film layer on the negative electrode current collector. Among them, the negative electrode film layer includes an undercoat layer and a negative electrode active layer, and the undercoat layer is located between the negative electrode current collector and the negative electrode active layer. The material of the negative electrode current collector is an iron-nickel alloy foil. The undercoat layer contains super P conductive agent, sodium carboxymethyl cellulose dispersant and modified styrene-butadiene rubber binder (mass ratio is 50:10:40). The negative electrode active layer contains graphite, silicon-carbon material, sodium carboxymethyl cellulose dispersant and modified styrene-butadiene rubber binder (mass ratio is 46.5:46.5:2:5), and the compaction density of the negative electrode active layer is 1.6g / cm 3 The tensile strength and Young's modulus of the negative electrode current collector, the thickness of the primer layer, the mass percentage of the binder in the primer layer, the peel strength of the negative electrode film layer, and the Dv50 of the conductive agent in the negative electrode active layer are shown in Table 1.
[0122] Embodiment 2 to Embodiment 3
[0123] Compared with Example 1, the differences between Examples 2 and 3 are that the silicon-based material in Example 2 is a silicon-oxygen material, and the silicon-based material in Example 3 is a single-element nano-silicon particle.
[0124] Embodiment 4 to Embodiment 6
[0125] Compared with Example 1, the differences between Examples 4 to 6 are that the tensile strength and Young's modulus of the negative electrode current collector, the thickness of the primer layer, the mass percentage of the binder in the primer layer, the peel strength of the negative electrode film layer, etc. are different, as shown in Table 1.
[0126] Example 7
[0127] Compared with Example 1, Example 7 is different in that the primer layer further comprises KS-6 flake graphite.
[0128] Embodiment 8-embodiment 9
[0129] Compared with Example 1, the difference between Examples 8 and 9 is that the Dv50 of the binder in the negative electrode active layer is as shown in Table 1.
[0130] Comparative Example 1
[0131] Compared with Example 1, Comparative Example 1 is different in that the negative electrode plate does not include a primer layer.
[0132] Comparative Example 2
[0133] Compared with Example 1, the difference of Comparative Example 2 is that the negative electrode plate does not include a primer layer, and the negative electrode collector is a copper foil, and the tensile strength is as shown in Table 1.
[0134] Comparative Example 3
[0135] Compared with Example 1, Comparative Example 3 is different in that the negative electrode current collector is copper foil, and the tensile strength is as shown in Table 1.
[0136] Table 1
[0137]
[0138] Test Case
[0139] (1) The negative electrode film peel strength test was performed on the negative electrode sheets in the embodiment and the comparative example. The test method was to use a roller press to stick a 20 mm wide standard tape (31B) to one surface of the negative electrode film at a fixed stress (2 kg, 300 mm / min), and use a tensile tester to perform a 180 degree peel test at a speed of 300 mm / min. The peel strength values of 50 points were obtained at a test distance of 50 mm to 120 mm and the average value was calculated. The results are shown in Table 1.
[0140] (2) The negative electrode sheets in the embodiment and the comparative example were tested for wrinkling after full charge. The test method was to charge the battery cell at a rate of 0.33C to a cut-off voltage of 4.25V, switch to constant voltage charging, and stop charging when the current drops to a rate of 0.05C to obtain a fully charged cell. The fully charged battery cell was then disassembled to obtain the fully charged negative electrode sheet, so that it can be observed whether the sheet is wrinkled. The results are shown in Table 1.
[0141] (3) The negative electrode sheets in the embodiment and the comparative example were tested for whether the fully charged sheets were detached. The test method was to charge the battery cell at a rate of 0.33C to a cut-off voltage of 4.25V, switch to constant voltage charging, and stop charging when the current drops to a rate of 0.05C to obtain a fully charged cell. The fully charged battery cell was then disassembled to obtain the fully charged negative electrode sheet, so that it can be observed whether the active material film layer on the sheet is detached from the current collector surface. The results are shown in Table 1.
[0142] (4) Battery cycle performance test.
[0143] The negative electrode sheet and the positive electrode sheet, the separator and the electrolyte in the embodiment and the comparative example are assembled into a battery.
[0144] Preparation of positive electrode sheet: The positive electrode active material lithium nickel cobalt manganese oxide NCM811, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 94:3:3, and the solvent N-methylpyrrolidone (NMP) was added. The mixture was stirred under the action of a vacuum mixer until the system was uniform to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on the two surfaces of a positive electrode current collector aluminum foil with a thickness of 13 μm, dried at 115°C for 15 minutes, and cold pressed to obtain a positive electrode sheet. The single-side density of the positive electrode active layer was 30 mg / cm 2 , compacted density is 3.3g / cm 3 .
[0145] Preparation of electrolyte: The organic solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), wherein the volume ratio of EC, EMC and DEC is 20:20:60. In an argon atmosphere glove box with a water content of <10ppm, fully dried LiPF6 is dissolved in the organic solvent and mixed evenly to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0146] Isolation membrane: A polyethylene microporous film is used as the porous isolation membrane substrate, and inorganic alumina powder, polyvinylpyrrolidone, and acetone solvent are evenly mixed in a weight ratio of 3:1.5:5.5 to form a slurry, which is then coated on one side of the substrate and dried to obtain an isolation membrane.
[0147] The battery cycle performance was tested. The test method was to charge the battery at 0.33C constant current to 4.25V at 25°C, then switch to constant voltage charging, stop charging when the current drops to 0.05C current, then discharge the battery at 0.33C constant current to 2.5V, and then stop discharging. At this time, the number of cycles is 1.
[0148] The above charge and discharge cycles were repeated until the battery capacity dropped to 80% of the initial capacity, and the test was stopped. The cycle number m of the lithium ion battery at this time was recorded. The results are shown in Table 1.
[0149] It can be seen from Table 1 that when the negative electrode sheet includes a silicon-based material, a primer layer, and a current collector with greater tensile strength, the wrinkling and demolding problems of the negative electrode sheet are well improved, and the battery cycle performance is higher.
[0150] Furthermore, when the flake graphite contained in the undercoat layer and / or the Dv50 of the binder in the active layer is appropriate, the battery exhibits better cycle performance.
[0151] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0152] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A negative electrode sheet, It is characterized in that It includes a negative electrode current collector and a negative electrode film layer located on the negative electrode current collector, the negative electrode film layer includes a primer layer and a negative electrode active layer, the primer layer is located between the negative electrode current collector and the negative electrode active layer, the primer layer contains a conductive agent and a first binder, the active material of the negative electrode active layer contains a silicon-based material, the tensile strength of the negative electrode current collector is ≥800MPa, and the peel strength of the negative electrode film layer is ≥28N / m.
2. The negative electrode sheet according to claim 1, It is characterized in that The Young's modulus of the negative electrode current collector is ≥80 GPa.
3. The negative electrode sheet according to claim 1 or 2, It is characterized in that The basecoat layer further comprises graphite; Optionally, the graphite includes lamellar graphite; Optionally, the mass percentage of the graphite in the primer layer is 20% to 35%.
4. The negative electrode sheet according to any one of claims 1 to 3, It is characterized in that The thickness of the primer layer is 2 μm to 6 μm.
5. The negative electrode sheet according to any one of claims 1 to 4, It is characterized in that The first binder satisfies at least one of the following characteristics (1) to (2): (1) The mass percentage of the first binder in the primer layer is 25% to 40%; (2) The glass transition temperature of the first binder is 10°C to 50°C.
6. The negative electrode sheet according to any one of claims 1 to 5, It is characterized in that The conductive agent satisfies at least one of the following characteristics (1) to (2): (1) The mass percentage of the conductive agent in the primer layer is 30% to 50%; (2) The conductive agent includes at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
7. The negative electrode sheet according to any one of claims 1 to 6, It is characterized in that The silicon-based material satisfies at least one of the following characteristics (1) to (2): (1) The mass percentage of the silicon-based material in the active material of the negative electrode active layer is ≥50%; (2) The silicon-based material includes at least one of a silicon-oxygen material and a silicon-carbon material.
8. The negative electrode sheet according to any one of claims 1 to 7, It is characterized in that The negative electrode active layer further comprises a second binder; Optionally, the Dv50 of the second binder is 100nm to 600nm; Optionally, the second binder has a glass transition temperature of 10°C to 50°C.
9. The negative electrode sheet according to any one of claims 1 to 8, It is characterized in that The compaction density of the negative electrode active layer is 1.1 g / cm 3 ~1.8g / cm 3 ; Optionally, the compaction density of the negative electrode active layer is 1.15 g / cm 3 ~1.65g / cm 3 .
10. The negative electrode sheet according to any one of claims 1 to 9, It is characterized in that The negative electrode current collector satisfies at least one of the following characteristics (1) to (3): (1) The material of the negative electrode current collector includes at least one of copper alloy, stainless steel and iron-nickel alloy; (2) The thickness of the negative electrode current collector is 4 μm to 20 μm; Optionally, the thickness of the negative electrode current collector is 5 μm to 10 μm; (3) The elongation at break of the negative electrode current collector is ≤4%.
11. A battery, It is characterized in that The invention comprises the negative electrode sheet according to any one of claims 1 to 10.
12. An electrical device, It is characterized in that Comprising the battery of claim 11.
Citation Information
Cited By
A battery cell, a battery device, and an electrical device.
CN122677557A
Anode piece, battery, and electric apparatus
EP4648156A1
Battery cell, negative electrode sheet, battery apparatus and electrical apparatus
WO2026118604A1
Secondary battery and electric device
WO2026157374A1
Secondary battery and electrical device
WO2026157480A1