Electrolyte containing composite additive for zinc powder negative electrode, preparation method and aqueous zinc ion battery
By using composite electrolyte additives of amino acids and sugar compounds in aqueous zinc ion batteries, the problem of poor stability of zinc powder negative electrodes is solved, the growth and side reactions of zinc dendrites are inhibited, the battery performance and life are improved, and the zinc powder negative electrodes are promoted. commercial application.
Patent Information
- Application Number
- CN202411145863.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The poor stability of the zinc powder negative electrode in aqueous zinc ion batteries leads to zinc dendrites, passivation phenomenon on the electrode surface and hydrogen evolution reaction, which affects the cycle life and energy efficiency of the battery. It is difficult for existing electrolyte additives to fully solve these problems.
Using the synergistic effect of amino acids and sugar compounds, a composite electrolyte additive is prepared for aqueous zinc ion batteries. By regulating the solvation structure of zinc ions, blocking side-reactivity sites, inhibiting zinc dendrites' growth and reducing electrodes Surface side reactions.
It significantly improves the cycle stability and corrosion resistance of zinc powder negative electrodes, extends the service life of the battery, improves battery performance and Coulomb efficiency, and promotes the widespread application of zinc powder negative electrodes in aqueous zinc ion batteries.
Smart Images

Figure CN119029356A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy storage, and in particular to an electrolyte containing a composite additive for a zinc powder negative electrode, a preparation method thereof, and an aqueous zinc ion battery. Background Art
[0002] With the rapid development of renewable energy, there is an increasing demand for efficient, safe and environmentally friendly energy storage systems. Aqueous zinc-ion batteries are regarded as a promising energy storage technology due to their high safety, cost-effectiveness and environmental friendliness. However, despite their many theoretical advantages, aqueous zinc-ion batteries still face a series of technical challenges in practical applications, especially the stability of the zinc anode, including the formation of zinc dendrites, passivation of the electrode surface and hydrogen evolution reaction, which seriously affect the cycle life and energy efficiency of the battery.
[0003] At present, the methods to improve the stability of zinc negative electrode mainly include surface coating modification, internal structure optimization, electrolyte regulation and diaphragm modification. Among them, electrolyte additives are considered to be an efficient, economical and simple strategy to improve the stability of zinc negative electrode in aqueous zinc ion batteries. By introducing specific additives, the double layer near the negative electrode surface is adjusted or the solvation structure is improved, thereby improving the cycle stability and coulombic efficiency of the zinc negative electrode.
[0004] However, although these additives can improve battery performance to a certain extent, they often have a single effect and can only improve the occurrence of some problems, and it is difficult to fully solve the multiple problems faced by the electrolyte and the zinc negative electrode. In addition, from the perspective of cost-effectiveness and adjustability, the negative electrode made of zinc powder has obvious advantages in commercial applications, but compared with zinc foil, the zinc powder negative electrode is more susceptible to corrosion and side reactions.
[0005] At present, the research on electrolyte additives is mainly focused on zinc foil negative electrodes, and there is relatively little research on electrolyte additives for zinc powder negative electrodes, which limits the wide application of zinc powder negative electrodes in aqueous zinc ion batteries. Therefore, it is necessary to develop a composite electrolyte additive for zinc powder negative electrodes to comprehensively solve the problems of zinc powder negative electrodes in aqueous zinc ion batteries, thereby achieving comprehensive improvement of battery performance and long-term stability. Summary of the invention
[0006] The present invention aims to solve the problem of poor stability of zinc powder negative electrode in aqueous zinc ion battery in the prior art, and aims to provide an electrolyte containing composite additive for zinc powder negative electrode, a preparation method and aqueous zinc ion battery, and solve the stability problem of zinc powder negative electrode in aqueous zinc ion battery through the synergistic effect of amino acid and sugar compound. The composite additive can not only effectively inhibit the growth of zinc dendrites, but also reduce the side reaction on the negative electrode surface, thereby significantly improving the cycle stability of zinc powder negative electrode, achieving comprehensive improvement of battery performance, and having the characteristics of cost-effectiveness and easy implementation.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] An electrolyte containing a composite additive for a zinc powder negative electrode comprises a solvent, an electrolyte and an electrolyte additive, wherein the electrolyte additive is a mixture of an amino acid compound and a sugar compound.
[0009] Furthermore, the solvent is water, and the electrolyte is a soluble zinc salt.
[0010] Furthermore, the electrolyte is one or more of zinc sulfate, zinc acetate, zinc chloride and zinc trifluoromethanesulfonate.
[0011] Furthermore, the concentration of the electrolyte additive in the mixture of the solvent, the electrolyte and the electrolyte additive is 0.001 to 1 mol / L.
[0012] Furthermore, the amino acid compound is one or more of amino acids, L-glutamine, sodium L-glutamate, zinc aspartate, histidine and glycine.
[0013] Furthermore, the molar ratio of the amino acid compound to the sugar compound is 1:1-4:1.
[0014] Furthermore, the carbohydrate compound is one or more of glucose, trehalose, maltose, sucrose and fructose.
[0015] Furthermore, the concentration of the electrolyte in the mixture of the solvent, the electrolyte and the electrolyte additive is 0.1 to 3 mol / L.
[0016] A method for preparing an electrolyte containing a composite additive for a zinc powder negative electrode comprises adding an electrolyte additive to a mixture of a solvent and an electrolyte, and mixing them uniformly to obtain an electrolyte containing a composite additive for a zinc powder negative electrode.
[0017] An aqueous zinc ion battery comprises a positive electrode, a negative electrode, a diaphragm between the positive electrode and the negative electrode, and an electrolyte containing a composite additive for the zinc powder negative electrode.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention uses a mixture of amino acid compounds and saccharide compounds as a composite electrolyte additive, which can adjust the solvation structure of zinc ions, block the active sites of side reactions, and achieve uniform zinc deposition, which not only effectively inhibits the growth of zinc dendrites, but also reduces the passivation phenomenon and side reactions on the electrode surface, significantly improves the cycle stability of the zinc powder negative electrode, and solves the problem of insufficient stability of the zinc negative electrode in the prior art. The present invention is particularly aimed at the characteristics of the zinc powder negative electrode, and through the use of a mixture of amino acid compounds and saccharide compounds as a composite additive, the corrosion resistance and stability of the zinc powder negative electrode are significantly improved, the influence of corrosion and side reactions is reduced, and the research and development of zinc powder negative electrode electrolyte additives are promoted, thereby promoting the wide application of zinc powder negative electrodes in aqueous zinc ion batteries, and achieving comprehensive improvement and long-term stability of battery performance. The composite electrolyte additive of the present invention is applied to aqueous zinc ion battery electrolytes and has the characteristics of being easy to implement, can be obtained by a simple dissolution method, and the zinc salts and additives used in the present invention have the advantages of low cost and wide sources. At the same time, this additive has a wide range of applicability to zinc powder negative electrodes, which is conducive to promoting the commercial application of zinc powder negative electrodes in aqueous zinc ion batteries and promoting the further development of energy storage technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The Zn|Zn symmetric battery using the electrolytes of Comparative Example 1 and Example 1 at 2 mA cm -2 The current density and 2 mAh cm -2 SEM images of the zinc negative electrode surface after 80 cycles at a surface capacity of ; wherein (a) is comparative example 1, and (b) is example 1;
[0021] Figure 2 The Zn|Zn symmetric battery using the electrolytes of Comparative Example 1 and Example 1 at 2 mA cm -2 The current density and 2 mAh cm -2 XRD pattern of zinc negative electrode after 80 cycles at the surface capacity;
[0022] Figure 3 The Zn|Zn symmetric battery using the electrolytes of Comparative Examples 1-3 and Example 1 at 2 mA cm -2 The current density and 2 mAh cm -2 Cyclic charge and discharge curves under the surface capacity of ; wherein (a) is comparative example 1, (b) is comparative example 2, (c) is comparative example 3, and (d) is embodiment 1;
[0023] Figure 4 The Zn|Cu asymmetric battery using the electrolytes of Comparative Example 1 and Example 1 at 2 mA cm -2The current density and 2 mAh cm -2 Coulombic efficiency at surface capacity. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. These embodiments are only to further illustrate the features and advantages of the present invention, and are not intended to limit the scope of the present invention.
[0025] The present invention provides an electrolyte additive containing a composite additive for a zinc powder negative electrode, wherein the composite electrolyte additive is a combination of amino acids and their derivatives and sugar compounds. The amino acid derivative is one or more of L-glutamine, sodium L-glutamate, zinc aspartate, histidine and glycine, and the sugar compound is one or more of glucose, trehalose, maltose, sucrose and fructose. The concentration of the electrolyte additive in the electrolyte is 0.001-1 mol / L.
[0026] On the other hand, the present invention provides an electrolyte containing a composite additive for a zinc powder negative electrode, wherein the aqueous zinc ion battery electrolyte is composed of a solvent, an electrolyte and an electrolyte additive, wherein the solvent is deionized water, and the electrolyte is a soluble zinc salt, including one or more of zinc sulfate, zinc acetate, zinc chloride and zinc trifluoromethanesulfonate, and the concentration of the soluble zinc salt is 0.1 to 3 mol / L. The electrolyte additive is a combination of amino acids and their derivatives and carbohydrate compounds. The amino acid derivative is one or more of L-glutamine, sodium L-glutamate, zinc aspartate, histidine and glycine, and the carbohydrate compound is one or more of glucose, trehalose, maltose, sucrose and fructose, and the concentration of the additive in the electrolyte is 0.001 to 1 mol / L.
[0027] On the other hand, the present invention provides an aqueous zinc ion battery, comprising a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and the electrolyte of the present invention. The negative electrode is made of zinc powder coated on a current collector, the positive electrode is made of zinc powder or copper foil coated on a current collector, the separator is made of glass fiber or filter paper, and the electrolyte is added to assemble into a Zn|Zn symmetric battery or a Zn|Cu asymmetric battery, i.e., a half-cell.
[0028] Example 1
[0029] (1) Preparation of electrolyte containing composite additives
[0030] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution.
[0031] 0.567 g of trehalose and 0.28 g of sodium L-glutamate were weighed and added to the above zinc sulfate solution, and ultrasonicated at 25°C for 10 min. After complete dissolution, an electrolyte containing a composite additive was obtained, wherein the concentration of the additive trehalose was 0.1 mol / L, and the concentration of the additive sodium L-glutamate was 0.1 mol / L, recorded as 2 mol / L ZSO+0.1 mol / L THL+0.1 mol / L MSG.
[0032] (2) Assembly of aqueous zinc ion batteries
[0033] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.1 mol / L THL+0.1 mol / L MSG was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. The current density was 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0034] Example 2
[0035] (1) Preparation of electrolyte containing composite additives
[0036] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution.
[0037] 0.2835 g of trehalose and 0.14 g of sodium L-glutamate were weighed and added to the above zinc sulfate solution, and ultrasonicated at 25°C for 10 min. After complete dissolution, an electrolyte containing a composite additive was obtained, wherein the concentration of the additive trehalose was 0.05 mol / L, and the concentration of the additive sodium L-glutamate was 0.05 mol / L, recorded as 2 mol / L ZSO+0.05 mol / L THL+0.05 mol / LMSG.
[0038] (2) Assembly of aqueous zinc ion batteries
[0039] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.05 mol / L THL+0.05 mol / L MSG was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. The current density was 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0040] Example 3
[0041] (1) Preparation of electrolyte containing composite additives
[0042] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution.
[0043] 1.134 g of trehalose and 0.56 g of sodium L-glutamate were weighed and added to the above zinc sulfate solution, and ultrasonicated at 25°C for 10 min. After complete dissolution, an electrolyte containing a composite additive was obtained, wherein the concentration of the additive trehalose was 0.2 mol / L, and the concentration of the additive sodium L-glutamate was 0.2 mol / L, recorded as 2 mol / L ZSO+0.2 mol / LM THL+0.2 mol / L MSG.
[0044] (2) Assembly of aqueous zinc ion batteries
[0045] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.2 mol / L THL+0.2 mol / L MSG was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. The current density was 2 mA cm -2 The dough capacity is 2 mAh cm -2The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0046] Example 4
[0047] (1) Preparation of electrolyte containing composite additives
[0048] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution.
[0049] Weigh 0.27 g of glucose and 0.219 g of L-glutamine and add them to the above zinc sulfate solution, ultrasonicate at 25°C for 10 min, and obtain an electrolyte containing a composite additive after complete dissolution, wherein the concentration of the additive glucose is 0.1 mol / L, and the concentration of the additive L-glutamine is 0.1 mol / L, recorded as 2 mol / L ZSO+0.1 mol / L GLC+0.1 mol / L GIn.
[0050] (2) Assembly of aqueous zinc ion batteries
[0051] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.1 mol / L GLC+0.1 mol / L GIn was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. At a current density of 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0052] Example 5
[0053] (1) Preparation of electrolyte containing composite additives
[0054] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution.
[0055] Weigh 0.135g glucose and 0.1095g L-glutamine and add them to the above zinc sulfate solution, ultrasonicate at 25°C for 10min, and obtain an electrolyte containing composite additives after complete dissolution, wherein the concentration of the additive glucose is 0.05mol / L, and the concentration of the additive L-glutamine is 0.05mol / L, recorded as 2mol / L ZSO+0.05mol / L GLC+0.05mol / LGIn.
[0056] (2) Assembly of aqueous zinc ion batteries
[0057] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.05 mol / L GLC+0.05 mol / L GIn was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. At a current density of 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0058] Example 6
[0059] (1) Preparation of electrolyte containing composite additives
[0060] Weigh zinc acetate and add it to deionized water. Ultrasonicate at 25°C for 10 min, and adjust the volume after it is completely dissolved to obtain a 0.1 mol / L zinc acetate solution.
[0061] Weigh glucose and amino acid and add them to the zinc acetate solution, ultrasonicate them at 25°C for 10 min, and obtain an electrolyte containing composite additives after they are completely dissolved, wherein the concentration of glucose is 0.0005 mol / L, and the concentration of amino acid is 0.0005 mol / L.
[0062] (2) Assembly of aqueous zinc ion batteries
[0063] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form a pole piece. The dried pole piece was punched into a circular pole piece with a diameter of 12 mm, and the prepared zinc powder pole piece was used as the positive and negative electrodes, the electrolyte containing the composite additive was used as the electrolyte, and the glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery.
[0064] Example 7
[0065] (1) Preparation of electrolyte containing composite additives
[0066] Weigh zinc chloride and add it to deionized water. Ultrasonicate at 25°C for 10 min, and adjust the volume after it is completely dissolved to obtain a 1 mol / L zinc chloride solution.
[0067] Weigh maltose and zinc aspartate and add them to the zinc chloride solution, ultrasonicate them at 25°C for 10 minutes, and obtain an electrolyte containing the composite additive after they are completely dissolved, wherein the concentration of aspartate is 0.8 mol / L and the concentration of maltose is 0.2 mol / L.
[0068] (2) Assembly of aqueous zinc ion batteries
[0069] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form a pole piece. The dried pole piece was punched into a circular pole piece with a diameter of 12 mm, and the prepared zinc powder pole piece was used as the positive and negative electrodes, the electrolyte containing the composite additive was used as the electrolyte, and the glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery.
[0070] Example 8
[0071] (1) Preparation of electrolyte containing composite additives
[0072] Weigh zinc trifluoromethanesulfonate and add it to deionized water. Ultrasonicate was performed at 25° C. for 10 min. After the solution was completely dissolved, the volume was fixed to obtain a 3 mol / L zinc trifluoromethanesulfonate solution.
[0073] Sucrose and histidine were weighed and added to the above zinc trifluoromethanesulfonate solution, and ultrasonicated at 25° C. for 10 min. After the mixture was completely dissolved, an electrolyte containing the composite additive was obtained, wherein the concentration of histidine was 0.015 mol / L, and the concentration of sucrose was 0.005 mol / L.
[0074] (2) Assembly of aqueous zinc ion batteries
[0075] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form a pole piece. The dried pole piece was punched into a circular pole piece with a diameter of 12 mm, and the prepared zinc powder pole piece was used as the positive and negative electrodes, the electrolyte containing the composite additive was used as the electrolyte, and the glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery.
[0076] Example 9
[0077] (1) Preparation of electrolyte containing composite additives
[0078] A mixture of zinc acetate and zinc chloride (the molar ratio of zinc acetate to zinc chloride is 1:1) was weighed and added into deionized water, and ultrasonicated at 25°C for 10 min. After complete dissolution, the volume was fixed to obtain a 0.5 mol / L mixed solution of zinc acetate and zinc chloride.
[0079] A mixture of sucrose and fructose (the molar ratio of sucrose to fructose is 1:1) and a mixture of histidine and glycine (the molar ratio of histidine to glycine is 1:1) are weighed and added to the mixed solution of zinc acetate and zinc chloride, and ultrasonicated at 25°C for 10 min. After complete dissolution, an electrolyte containing a composite additive is obtained, wherein the total concentration of sucrose and fructose is 0.2 mol / L, and the total concentration of histidine and glycine is 0.4 mol / L.
[0080] (2) Assembly of aqueous zinc ion batteries
[0081] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form a pole piece. The dried pole piece was punched into a circular pole piece with a diameter of 12 mm, and the prepared zinc powder pole piece was used as the positive and negative electrodes, the electrolyte containing the composite additive was used as the electrolyte, and the glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery.
[0082] Example 10
[0083] (1) Preparation of electrolyte containing composite additives
[0084] Weigh zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min, and adjust the volume after it is completely dissolved to obtain a 2.5 mol / L zinc sulfate solution.
[0085] Weigh trehalose and zinc aspartate and add them to the zinc sulfate solution, ultrasonicate at 25° C. for 10 min, and obtain an electrolyte containing the composite additive after complete dissolution, wherein the concentration of trehalose is 0.5 mol / L, and the concentration of zinc aspartate is 0.5 mol / L.
[0086] (2) Assembly of aqueous zinc ion batteries
[0087] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form a pole piece. The dried pole piece was punched into a circular pole piece with a diameter of 12 mm, and the prepared zinc powder pole piece was used as the positive and negative electrodes, the electrolyte containing the composite additive was used as the electrolyte, and the glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery.
[0088] Comparative Example 1
[0089] (1) Preparation of electrolyte
[0090] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution, recorded as 2 mol / L ZSO.
[0091] (2) Assembly of aqueous zinc ion batteries
[0092] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. The current density was 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0093] Comparative Example 2
[0094] (1) Preparation of electrolyte
[0095] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution, recorded as 2 mol / L ZSO.
[0096] 0.567 g of trehalose was weighed and added to the above solution. The solution was ultrasonicated at 25° C. for 10 min. After the solution was completely dissolved, an electrolyte containing the composite additive was obtained. The concentration of the additive trehalose was 0.1 mol / L, recorded as 2 mol / L ZSO+0.1M THL.
[0097] (2) Assembly of aqueous zinc ion batteries
[0098] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / LM ZSO + 0.1 mol / L THL was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. At a current density of 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode. -2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0099] Comparative Example 3
[0100] (1) Preparation of electrolyte
[0101] Weigh 8.6268 g of zinc sulfate heptahydrate and add it to deionized water. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, adjust the volume to 15 ml to obtain a 2 mol / L zinc sulfate solution, recorded as 2 mol / L ZSO.
[0102] Weigh 0.28 g of sodium glutamate and add it to the above solution. Ultrasonicate at 25°C for 10 min. After it is completely dissolved, an electrolyte containing the composite additive is obtained, wherein the concentration of the additive sodium glutamate is 0.1 mol / L, recorded as 2 mol / L ZSO+0.1 mol / LMSG.
[0103] (2) Assembly of aqueous zinc ion batteries
[0104] Zinc powder, conductive agent carbon black, and binder PVDF were added to the organic solvent NMP in a mass ratio of 8:1:1 to prepare a slurry, which was then scraped onto a copper foil and dried to form an electrode. The dried electrode was punched into a circular electrode with a diameter of 12 mm. The prepared zinc powder electrode was used as the positive and negative electrodes, 2 mol / L ZSO+0.1 mol / L MSG was used as the electrolyte, and glass fiber filter paper was used as the diaphragm to assemble a Zn|Zn symmetrical battery. The current density was 2 mA cm -2 The dough capacity is 2 mAh cm -2 The cycling performance of the symmetrical battery was tested under the condition of . The Zn|Cu asymmetric battery was assembled with copper foil as the positive electrode and the prepared zinc powder electrode as the negative electrode.-2 The dough capacity is 2 mAh cm -2 The cycling performance and Coulombic efficiency of the asymmetric battery were tested under the conditions.
[0105] The Zn|Zn symmetric battery assembled from Example 1 and Comparative Example 1 was heated to 2 mA cm -2 and 2mAh cm -2 After 80 cycles under the condition of , the battery was disassembled and the morphology of the zinc powder negative electrode was observed by SEM. Figure 1 As shown in (a) and (b). The morphology of zinc deposits in the electrolyte of comparative example 1 is uneven, with flaky dendrites, and agglomerates and is relatively rough. In contrast, the zinc deposits in the electrolyte of example 1 show a dense, uniform and flat morphology, indicating that the composite additive can inhibit the growth of zinc dendrites. The Zn|Zn symmetrical battery assembled from example 1 and comparative example 1 was subjected to a 2 mA cm -2 and 2mAh cm -2 After 80 cycles under the condition of , the battery was disassembled and the zinc powder negative electrode was subjected to XRD test. Figure 2 As shown, compared with Example 1, the XRD spectrum of zinc in the electrolyte of Comparative Example 1 shows a strong diffraction peak of the by-product basic zinc sulfate, indicating that the composite additive can inhibit the corrosion side reaction.
[0106] like Figure 3 As shown in (a), (b), (c) and (d), the Zn|Zn symmetric battery using the electrolyte of Comparative Example 1 short-circuited after 80 hours, the Zn|Zn symmetric battery of Comparative Example 2 short-circuited after 130 hours, and the Zn|Zn symmetric battery of Comparative Example 3 short-circuited after 250 hours, while the Zn|Zn symmetric battery using the electrolyte of Example 1 can operate stably for 480 hours.
[0107] like Figure 4 As shown, the Zn|Cu asymmetric battery using the electrolyte of Comparative Example 1 failed after 80 cycles, and the average coulombic efficiency was only 97.8%, while the Zn|Cu asymmetric battery using the electrolyte of Example 2 could cycle 240 cycles, showing a coulombic efficiency of 99.6%. This shows that the composite additive improves the reversibility and stability of zinc ion deposition / stripping.
[0108] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0109] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. An electrolyte containing a composite additive for a zinc powder negative electrode, characterized in that: The invention comprises a solvent, an electrolyte and an electrolyte additive, wherein the electrolyte additive is a mixture of an amino acid compound and a sugar compound.
2. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The solvent is water, and the electrolyte is a soluble zinc salt.
3. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The electrolyte is one or more of zinc sulfate, zinc acetate, zinc chloride and zinc trifluoromethanesulfonate.
4. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The concentration of the electrolyte additive in the mixture of the solvent, the electrolyte and the electrolyte additive is 0.001 to 1 mol / L.
5. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The amino acid compound is one or more of amino acids, L-glutamine, sodium L-glutamate, zinc aspartate, histidine and glycine.
6. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The molar ratio of the amino acid compound to the sugar compound is 1:1-4:
1.
7. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The sugar compound is one or more of glucose, trehalose, maltose, sucrose and fructose.
8. The electrolyte containing composite additives for zinc powder negative electrode according to claim 1, characterized in that: The concentration of the electrolyte in the mixture of the solvent, the electrolyte and the electrolyte additive is 0.1 to 3 mol / L.
9. A method for preparing an electrolyte containing a composite additive for a zinc powder negative electrode as claimed in any one of claims 1 to 8, characterized in that: An electrolyte additive is added to a mixture of a solvent and an electrolyte, and the mixture is mixed evenly to obtain an electrolyte containing a composite additive for a zinc powder negative electrode.
10. An aqueous zinc ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, and an electrolyte containing a composite additive for the zinc powder negative electrode prepared by the method according to any one of claims 1 to 8.
Citation Information
Cited By
Preparation method and application of metal interface layer coated zinc powder negative electrode