Method for preparing calcined mineral binder material with reduced carbon footprint

By carbonizing and calcining the mineral binder material with carbon dioxide, calcined mineral binder material is formed, and the generated carbon dioxide recycling is reused, the problems of carbon dioxide emissions and construction waste recycling in the construction industry are solved, and environmental protection and Efficient utilization of resources.

CN119032071APending Publication Date: 2024-11-26SIKA TECH AG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380033266.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-21
Filing Date
2023-04-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The mineral binder materials used in the construction industry generate a large amount of carbon dioxide emissions during the production and demolition process, and the recycling of demolition construction waste is insufficient, resulting in environmental pollution and waste of resources.

Method used

By carbonizing and calcining the mineral binder material with carbon dioxide, a calcined mineral binder material is formed and the generated carbon dioxide is recycled to reduce environmental emissions while separating the hardened mineral binder from construction waste. Form a reusable powdered material.

Benefits of technology

Significantly reduces carbon dioxide emissions, improves the recycling rate of construction waste, reduces consumption of natural resources, and reduces the environmental negative impact of production and treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032071A_ABST
    Figure CN119032071A_ABST
Patent Text Reader

Abstract

A process for producing a calcined mineral binder material, comprising the steps of: a) providing a source material comprising a mineral binder material, carbonating the source material with carbon dioxide such that the mineral binder material is at least partially, in particular substantially completely, carbonated to produce a carbonated product; b) calcining the carbonate-containing material to produce a calcined mineral binder material and carbon dioxide as a by-product; wherein in step a) the carbon dioxide by-product of step b) is used as carbon dioxide for carbonation of the source material, optionally in combination with additional carbon dioxide from a different source; and in step b) the carbonate-containing material comprises the carbonation product of step a) and optionally further materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a calcined mineral binder material. Furthermore, the present invention relates to a method for producing a settable mineral binder composition. Background Art

[0002] In the construction industry, a large number of materials based on mineral binders are used, such as mortar or concrete. However, the production of cement and other mineral binders produces a considerable amount of carbon dioxide (CO2), which is relevant to the climate. In order to reduce carbon dioxide emissions, the cement in the binder composition can be partially replaced by potential hydraulic and / or pozzolanic cement admixtures, such as fly ash, slag or silica fume. Such admixtures are by-products of various industrial processes and are therefore advantageous in terms of carbon dioxide balance. However, in the absence of additional measures, the solidification of such cement admixtures requires much longer time than in the case of hydraulic cements.

[0003] Another problem is the disposal and recycling of demolition or construction waste containing materials based on mineral binders, such as hardened mortar or concrete.

[0004] Most of the demolition or construction waste, such as hardened concrete or mortar, is still disposed in landfills and only a small amount is partially reused as raw material for low-tech applications in the construction industry. Usually, demolition waste, such as concrete, is crushed and only the coarse fraction is reused, the smaller fraction being discarded due to the compromise effect on the properties of fresh and hardened concrete. Therefore, the current practice can only be considered as incomplete and down-cycling.

[0005] However, demolition waste often contains a large amount of useful components, such as aggregates or binder components, which can in principle be completely recycled and reused in new construction works. Moreover, in some regions and countries, the disposal of construction waste is becoming increasingly expensive and difficult due to new legislation. In Europe, for example, European directives require the reuse of at least 70% by weight of inert demolition material. Therefore, the recycling of demolition or construction waste is an important issue.

[0006] In this regard, WO 2014 / 154741 A1 (Sika Technology AG) describes an improved method for recovering aggregate and powdered mineral material from a source material, in particular waste material or demolition material, comprising hardened mineral binder and aggregate. The method comprises a step of treating the source material in a disintegration process, wherein the hardened mineral binder is at least partially, in particular substantially completely, carbonated with a gas containing carbon dioxide and removed from the surface of the aggregate, thereby producing a powdered disintegration product, which can be separated from the aggregate. The aggregate and the powdered disintegration product can be used to produce a new mineral binder composition.

[0007] However, there is still a need to develop improved solutions which reduce CO2 emissions in the construction industry. Summary of the invention

[0008] An object of the present invention is to provide an improved solution for preparing mineral binder-based materials which have as little negative impact on the environment as possible. In particular the solution should allow the production of recycled mineral binders or mineral binder-based materials with an improved carbon dioxide balance.

[0009] Surprisingly, it has been found that these objects can be achieved by a method according to claim 1. In particular, the present invention provides a method for producing a calcined mineral binder material, the method comprising the following steps:

[0010] a) providing a source material comprising a mineral binder material, carbonating the source material with carbon dioxide such that the mineral binder material is at least partially, in particular substantially completely, carbonated to obtain a carbonated product;

[0011] b) calcining the carbonate-containing material to produce a calcined mineral binder material and carbon dioxide as a by-product;

[0012] wherein in step a), the carbon dioxide by-product of step b), optionally in combination with additional carbon dioxide from a different source, is used as carbon dioxide for carbonation of the source material; and in step b), the carbonate-containing material comprises or consists of the carbonation product of step a) and optionally other materials.

[0013] The method of the invention is based on a cyclic process, in which the carbon dioxide produced in the calcination reaction is converted into a carbonate-containing material. When the material is calcined, further carbon dioxide is obtained, which is then used again to produce a carbonate-containing material. Due to this cyclic process involving the recycling of carbon dioxide, the carbon dioxide does not need to be released into the environment.

[0014] In particular, the method allows the production of calcined mineral binder materials, such as calcium oxide and / or calcium hydroxide, which can be used to produce new settable mineral binder compositions. Therefore, carbon dioxide emissions can be significantly reduced and at the same time source materials, such as waste materials or demolition materials, can be recycled. Recycling in particular allows the reduction of the amount of waste materials or demolition materials that must be deposited or landfilled. In addition, the consumption of natural resources, such as aggregates and raw materials for cement production, can be reduced.

[0015] Furthermore, the process of the invention is highly flexible. For example, in step b), other (recycled) materials to be calcined, such as excavated materials from quarries and / or mining, can be processed together with the carbonation product obtained in step a) or separately in the same manner, and any carbon dioxide produced thereby can be reused for carbonating further source materials in step a).

[0016] The present invention thus provides a very advantageous process combination which allows the preparation of mineral binder-based materials which have a much smaller negative impact on the environment than known production methods.

[0017] In addition, both methods, steps a) and b), can be carried out very well at one location, with the equipment and devices being largely available at the cement production plant. This further reduces the engineering and transport effort.

[0018] Steps a) and b) can be performed simultaneously or one after another. In the latter case, the carbonation product produced in step a) can be temporarily stored before use in step b). Similarly, the carbon dioxide by-product produced in step b) can be temporarily stored before use in step a). In the case of non-simultaneous implementation of steps a) and b), step b) can be performed, for example, immediately after step a) or at any time thereafter.

[0019] In particular, in order to start the cycle process, only carbon dioxide from different sources can be used in step a) in the first stage to produce a first amount of carbonation product. Carbon dioxide from different sources can be other carbon dioxide as described below, such as, for example, carbon dioxide as a by-product from an industrial process.

[0020] Likewise, in order to start the cyclic process, other carbonate-containing materials can be used in the first stage of step b), which do not contain the carbonation product of step a), only in order to generate a first amount of carbon dioxide.

[0021] In this document, the term "source material" represents any material comprising or consisting of a mineral binder material. In particular, the source material comprises or consists of a hardened mineral binder and / or an uncured mineral binder.

[0022] The term "hardened mineral binder" refers in particular to a mineral binder that has hardened in a chemical hydration reaction producing hydrates. Preferably, the hardened mineral binder has been hardened for at least 2 days, preferably at least 7 days, in particular at least 28 or at least 60 days.

[0023] In particular, the hardened mineral binder comprises or consists of a hardened hydraulic binder, such as a hardened cement binder. However, the hardened mineral binder may also comprise or consist of a hardened latent hydraulic and / or pozzolanic binder material.

[0024] The term "latent hydraulic and / or pozzolanic binder material" particularly denotes a type II concrete additive having latent hydraulic and / or pozzolanic properties according to EN 206-1. In particular, the latent hydraulic or pozzolanic binder material comprises or consists of slag, fly ash, silica fume, activated clay and / or natural pozzolan.

[0025] In particular, the hardening mineral binder comprises or consists of 5 to 100% by weight, in particular 50 to 100% by weight, more preferably 65 to 100% by weight, of a hardening hydraulic binder.

[0026] In particular, the hardening mineral binder comprises or consists of 5-95% by weight of a hardening hydraulic binder and 95-5% by weight of a hardening latent hydraulic and / or pozzolanic binder material. More preferably, the hardening mineral binder may comprise or consist of 30-90% by weight of a hardening hydraulic binder and 70-10% by weight of a hardening latent hydraulic and / or pozzolanic binder material.

[0027] Preferred hardened mineral binders comprise or consist of hardened cements of type CEM I, II, III, IV or V, in particular of type CEM I or II, according to standard EN 197. However, other types of cements may also be used.

[0028] In particular, the hardened hydraulic binder is hardened cement. Preferably, the hardened latent hydraulic and / or pozzolanic binder material is hardened slag and / or fly ash. A highly preferred hardened latent hydraulic binder material is hardened slag.

[0029] In particular, the source material to be processed contains or consists of a hardened mineral binder and aggregates.

[0030] In particular, the source material to be processed comprises or consists of a hardened mineral binder bonded to the surface of the aggregate. In particular, the hardened mineral binder at least partially surrounds the aggregate and / or binds some individual aggregates together.

[0031] Preferably, the calcined mineral binder material obtained in step b) of the present invention is not used as source material.

[0032] The term "aggregate" includes any type of mortar and / or concrete aggregate. In particular, the aggregate is characterized by a density of 2.2-3.0 kg / dm 3 In particular, the aggregate comprises stone, gravel, sand or a mixture thereof. However, the aggregate may comprise or consist of lightweight aggregates, in particular foamed clay and / or polystyrene, or heavy aggregates, such as barite, iron ore, etc.

[0033] In particular, the aggregate has a particle size of at least 0.125 mm or at least 0.250 mm. Preferably, the aggregate has a particle size of at most 125 mm or at most 32 mm. In particular, the aggregate has a particle size of 0.125-125 mm, in particular 0.125-32 mm, in particular 0.125-16 mm, for example 0.125-8 mm or 0.125-5 mm.

[0034] In this context, particle size is determined by sieve analysis, in particular using a sieve with square openings. In particular, particle size is expressed as the size of the openings of a test sieve which just passes the relevant particle or particles.

[0035] Preferably, the source material comprises or consists of hardened mortar and / or concrete.

[0036] In particular, the source material is a demolition material or waste material originating from a demolished building or structure. The source material may come from a demolition site and / or a landfill. In addition to the hardened mineral binder, aggregate and / or other materials may be present in the source material. Other materials are, for example, metals, plastics and / or wood. However, it may be beneficial to at least partially separate this type of material before processing the source material.

[0037] According to a preferred embodiment, the source material is comminuted before step a). This is particularly advantageous if the source material comprises a hardened mineral binder. Comminution will increase the surface of the source material, which in turn enhances the carbonation process.

[0038] "Uncured mineral binder" refers to a mineral binder that has not yet hardened in a chemical hydration reaction. In this case, therefore, the mineral binder does not contain hydrates. In particular, the uncured mineral binder comprises or consists of a hydraulic, latent hydraulic and / or pozzolanic binder material as described above, but in an uncured state.

[0039] For example, the uncured mineral binder comprises or consists of a cement of type CEM I, II, III, IV or V, in particular CEM I or II, according to standard EN 197. However, other types of cement may also be used. Preferably, the latent hydraulic and / or pozzolanic binder material is slag, fly ash, silica fume, activated clay and / or natural pozzolan.

[0040] In particular, the uncured mineral binder comprises or consists of production waste from cement production. This is cement which, for example due to temporary processing problems, does not meet certain required specifications.

[0041] As known to those skilled in the art, mineral binders, especially cement, in addition to reacting with water, can also react with carbon dioxide, thereby producing calcium carbonate in particular. Thus, the reaction of the uncured mineral binder as source material in step a) will at least partially carbonate the uncured mineral binder and produce a carbonated product, which can also be calcined in step b).

[0042] The term "carbonation" represents a process which is essentially a reversal of the chemical process of calcination which occurs, for example, in a cement kiln. In particular, "carbonation" refers to the incorporation of carbon dioxide into a compound or a chemical reaction of carbon dioxide with a source material. Thus, "carbonation" represents in particular the carbon dioxide treatment of a source material. To a certain extent, the carbonation of hardened mineral binders (e.g. mortar or concrete) occurs naturally. However, the term "carbonation" here represents a process in which carbonation is particularly enhanced or accelerated compared to the natural process. This can be achieved by providing an excess of carbon dioxide.

[0043] The progress of carbonation can be measured, for example, by measuring the CO partial pressure during step a) of the method according to the invention. If the CO partial pressure decreases, carbonation occurs. If the CO partial pressure does not decrease further during the carbonation process, it can be assumed that carbonation is substantially complete. Alternatively, the carbonation process can also be detected, for example, by measuring the pH value of the mixture during the carbonation in step a) of the method according to the invention. If the pH value decreases, carbonation occurs. If the pH does not decrease further during the carbonation process, it can be assumed that carbonation is substantially complete. This is typically the case when the pH is 7-10, preferably 7-9.

[0044] For example, a hardening mineral binder in the form of a hydraulic cementitious material consisting essentially of calcium, silicates and aluminium hydroxide may react with carbon dioxide to produce the corresponding carbonates.

[0045] Basically, the microstructure of the hardened mineral binder or binder matrix determines the rate of carbonation and the progression of the carbonation front from the exposed surface of the cementitious material towards its core. Because the ingress of gases and liquids into the hardened mineral binder material seriously impairs its durability, it is preferred to design mortars and concretes to be as impermeable as possible, i.e. to slow down the natural carbonation to a minimum rate.

[0046] The carbon dioxide used in step a) comprises the carbon dioxide by-product of step b). However, it can be mixed with other carbon dioxide or temporarily replaced with other carbon dioxide. The other carbon dioxide can, for example, be a product or by-product of any industrial process.

[0047] Preferably, substantially pure carbon dioxide is used in step a). The purity of the carbon dioxide is preferably >1 wt. %, for example >8 wt. %, preferably >50 wt. %, in particular >95 wt. %, especially >99 wt. %. With regard to the efficiency of the treatment, substantially pure carbon dioxide is most advantageous.

[0048] However, in step a), a mixture of carbon dioxide and other substances such as water vapor, nitrogen, etc. (for example air) can also be used. Such a mixture contains CO2 in an amount of >1% by weight, for example >8% by weight, preferably >10% by weight, particularly preferably >50% by weight, in particular >95% by weight, and in particular >99% by weight. The concentration of CO2 used in particular exceeds the CO2 concentration of normal air.

[0049] According to a preferred embodiment, waste gases from industrial processes and / or a mixture of carbon dioxide and other substances are used as the other carbon dioxide for carbonation in step a). Advantageously, waste gases or mixtures comprise approximately 5-25% by weight of CO , preferably 8-20% by weight of CO or 10-15% by weight of CO .

[0050] The carbon dioxide may be added in gaseous, solid or liquid form.

[0051] The additional carbon dioxide used can also be obtained from the in situ decomposition of organic or inorganic substances, in particular carbonates, or from the oxidation of carbon monoxide. Suitable carbonates are, for example, carbonates, olefin carbonates and the like.

[0052] Most preferably, the carbonation of the source material is carried out in a liquid and the carbon dioxide is added to the liquid in gaseous form. Therefore, the liquid is particularly an aqueous liquid, preferably water. This results in the carbon dioxide dissolving in the aqueous liquid or water.

[0053] Preferably, the density of solid material (particularly source material and / or carbonating product) in liquid (particularly water) is about 10 volume % to 80 volume %, especially 15 volume % to 75 volume %, especially 20 volume % to 70 volume %, more preferably 30 volume % to 65 volume % or 40 volume % to 60 volume %.This causes the effective carbonation of source material.In addition, if source material is subjected to mechanical force as further described below, then under such conditions, cause effective wear or abrasion of the mineral binder and / or carbonating material of hardening.In other words, such concentration causes high abrasiveness condition.

[0054] In particular, carbon dioxide is added to the liquid in gaseous form, thereby forming gas bubbles, which help to remove carbonation products or disintegration products from the surface of the aggregate.

[0055] Advantageously, the treatment of the source material with carbon dioxide is carried out at atmospheric pressure. However, lower or higher pressures are also possible.

[0056] The amount of carbon dioxide required for the treatment depends on the proportion of hardened binder present in the source material. The more hardened binder, the more carbon dioxide is required.

[0057] In particular, the treatment is carried out at a temperature of -10 to 100° C., in particular -5 to 75° C. or 5 to 40° C. However, the treatment can be carried out at above 100° C., for example under humid conditions.

[0058] In particular, the processing of the source material is carried out as long as new disintegration or carbonation products are formed. This means in particular that the processing is carried out as long as a significant or measurable amount of new disintegration or carbonation products is formed.

[0059] In particular, the carbonation product produced in step a) comprises or consists of calcium carbonate, silicate carbonate and / or aluminium carbonate.

[0060] Particularly preferably, in step a), the source material is carbonated under grinding conditions, in particular by mechanical grinding and / or attrition carbonation. This is particularly true if the source material comprises or consists of a hardened mineral binder material and optional aggregate. Preferably, the grinding conditions are generated by mechanical forces acting on the source material during the carbonation in step a). The mechanical forces will result in high particle friction, impact and wear or abrasion of the source material.

[0061] In this case, a combined chemical-mechanical process is performed. This results in an effective decomposition of the source material, especially if the source material comprises or consists of a hardened mineral binder material. In the process, the hardened mineral binder decomposes or degrades into fine particles or powdery decomposition products, respectively. If the source material also comprises aggregate, for example if the source material is a hardened mortar or concrete composition, the hardened mineral binder is effectively removed from the surface of the aggregate in the source material. Therefore, the surface of the aggregate can be largely cleared of the hardened binder material. Therefore, the recovered or recycled aggregate has a quality very close to that of pure aggregate.

[0062] In particular, in step a), the hardened mineral binder and / or carbonated material is removed from the aggregate surface, in particular by mechanical abrasion and / or wear. The removal is in particular achieved by mechanical forces acting on the source material. The mechanical forces will result in high particle friction, impact and abrasion or wear of the source material or hardened mineral binder and / or carbonated material, respectively.

[0063] Mechanical forces and / or wear can be caused by stirring the source material. Thus, the source material is, for example, confined in a defined volume and stirred. This will in particular cause high shear forces and wear or abrasion.

[0064] Preferably, the solid material in the treatment volume, particularly the density of source material and / or carbonation material is about 10-80 volume %, especially 15-75 volume %, particularly 20-70 volume %, more preferably 30-65 volume % or 40-60 volume %.Term " treatment volume " represents the volume in which the mechanochemical process is effectively carried out.In other words, treatment volume is defined as the space in which material to be treated, particularly source material is exposed to carbonation and / or abrasion and / or wear.

[0065] In contrast, when the density of solid material in the processing volume is below 10% by volume, mechanical forces or abrasion will generally be less effective and removal of hardened mineral binder and / or carbonated material from the aggregate surface becomes more difficult. This is due in particular to the fact that under these conditions, the solid material in the liquid is separated quite far apart. Therefore, most of the time there is hardly any mechanical contact between the solid material particles.

[0066] In particular, the material to be processed, in particular the source material, fills the processing volume according to the above-mentioned density so that when the material is stirred, abrasive contact is exerted between the particles. For stirring and / or for inducing abrasive conditions, stirring devices, mechanical mixers, rotating drums, crushers, extruders, ultrasonic treatment, vibrations, fluid flows or combinations thereof can be used.

[0067] In some embodiments, the present invention relates to the present invention to the disintegration process of the present invention. In some embodiments, the present invention relates ...

[0068] In particular, the two processes are run simultaneously and iteratively until the desired degree of carbonation and / or removal is achieved, or, if present, until a substantially clean aggregate is obtained.

[0069] In particular, due to the disintegration of the carbonation products and optionally the removal from the aggregate surface, the uncarbonated mineral binder present in the lower layer is gradually exposed and chemically reacts during the carbonation process. This interaction between chemical and mechanical processes is particularly effective and leads to a high carbonation yield and, if present, the formation of very clean aggregates.

[0070] Particularly preferably, in step a), the source material comprising hardened mineral binder and aggregate is (i) treated in a disintegration process, in particular under grinding conditions as described above, wherein the hardened mineral binder is at least partially, in particular substantially completely, carbonated and removed from the surface of the aggregate, thereby producing a powdered disintegration product; and (ii) the treated source material is separated at a predetermined cut-off size in order to recover treated aggregate having a size of at least the predetermined cut-off size and / or to recover powdered mineral material having a size below the predetermined cut-off size. Thus, the powdered mineral material having a size below the predetermined cut-off size corresponds to the carbonated product of step a).

[0071] Therefore, another advantage is that it is easy to separate clean aggregate and disintegration products when the source material containing hardened mineral binder and aggregate is carbonated. The microstructure of hardened mineral binder, especially hardened cementitious binder, consists of hydrated phases in the nanometer to micrometer range. Through the disintegration process, the disintegration products exist as fine particles or powdered products with a particle size range of several nanometers to several micrometers. Typically, the particle size of the powdered disintegration products is 0-0.250mm or 0-0.125mm. This is conducive to separating the disintegration products from the clean aggregate.

[0072] In particular, the powdered mineral material and the processed aggregate are separated at a characteristic cut size. Preferably the cut size is 0.06-1 mm, in particular 0.1-0.5 mm, preferably 0.125 mm or 0.250 mm. This means that particles below the cut size are collected as powdered mineral material or carbonation product, respectively, while particles above the cut size are collected as aggregate.

[0073] The powdered mineral material comprises or consists of a powdered disintegration product. Optionally, the powdered mineral material may comprise small aggregates having a particle size below the cut particle size and / or an untreated hardened mineral binder having a particle size below the cut particle size.

[0074] The separation of the powdered mineral material from the processed aggregate is carried out in particular by filtering, sieving, sedimentation, density separation and / or centrifugation.

[0075] In particular, if the processing of the source material is carried out under grinding conditions, it is carried out in the presence of water. The water may be present, for example, in gaseous and / or liquid form.

[0076] Preferably, the processing of the source material is carried out in a liquid, in particular in an aqueous liquid, preferably in water. This means that the source material is at least partially, in particular completely, immersed in the liquid.

[0077] However, it is also possible to carry out the treatment with moistened source materials and / or under humid conditions. Humid conditions are in particular a relative humidity of 40-100%.

[0078] In particular, when a source material comprising a hardened mineral binder and aggregates is used, the treatment in step a) is carried out until the amount of hardened mineral binder bonded to the aggregates and carbonated hardened mineral binder is 0.0001-50% by weight, in particular 0.001-25% by weight, especially 0.001-10% by weight, preferably 0.01-1% by weight, relative to the total weight of the aggregates.

[0079] In particular, the treatment in step a) is carried out until the porosity of the recycled treated aggregate measured according to standard EN 1097-6 is ≤10% by volume, in particular ≤5% by volume, especially ≤2% by volume, preferably 0.1-3% by volume or 1-3% by volume or 1.5-2% by volume.

[0080] The carbonation of the source material in step a) can be carried out in a batch process or in a continuous process.

[0081] According to a highly preferred embodiment, the source material can be, for example, immersed in an aqueous liquid (e.g., water) in a reaction vessel, such as at a concentration of 0.5-5kg of source material per liter of liquid, and treated with carbon dioxide under stirring or grinding conditions. For example, carbon dioxide can be introduced into the reaction vessel through an inlet, which allows carbon dioxide to be directly introduced into the aqueous liquid in a gaseous form. Therefore, gaseous carbon dioxide is dissolved in water, and reacts with a hardened binder material under stirring and grinding conditions to produce disintegrated products or powdered mineral materials respectively. Preferably, the reaction vessel is stirred and / or comprises a mechanical agitator for stirring a reaction mixture and realizing grinding conditions. The powdered mineral material is then particularly separated from the aggregate of processing by filtering.

[0082] According to a preferred embodiment, the carbonated product and / or aggregate obtained in step a) is dried after separation. This is particularly useful if the treatment has been carried out under wet conditions or in a liquid.

[0083] Drying can be carried out, for example, in an oven, in particular at a temperature of 30-150° C., preferably at 80-130° C. or 100-120° C. Furthermore, drying with the aid of an air stream, in particular a hot air stream, for example at a temperature of 30-150° C. is another option. This results in rapid drying of the carbonated product and / or the aggregate. However, it is also possible, for example, to dry the product under ambient conditions without further measures. This does not require any additional energy.

[0084] In particular, the carbonated product produced in step a) has a particle size of less than 250 μm, preferably less than 125 μm. The fineness of the carbonated product is in particular in the range of 0.5 to 1000 μm. 2 / g, preferably 0.5-500m 2 / g, especially 0.5-100m 2 The fineness refers to the surface area calculated by nitrogen adsorption (BET).

[0085] In particular, the carbonation product comprises or consists of carbonated hydrates of the cementitious hardening binder, optionally with residual hydrates and / or oxides, such as quartz. Optionally, aluminate products and / or sulfates may also be present.

[0086] In particular, the carbonation product has the same oxide composition as the hardened binder and the portion of the aggregate having a particle size below the cut particle size (eg, below 250 μm or below 125 μm).

[0087] In particular, at least temporarily, the carbonate-containing material used in step b) comprises a clay mineral. Thus, in this case, the further material optionally used in step b) comprises or consists of a clay mineral. In particular, before the calcination in step b) begins, the clay mineral is mixed with the carbonation product obtained in step a).

[0088] Herein, the clay mineral may be any type of clay-containing material, especially coarse clay, low temperature calcined clay or high temperature calcined clay. According to an embodiment, the clay mineral is selected from coarse clay, low temperature calcined clay and / or high temperature calcined clay.

[0089] Crude clay is a clay mineral extracted, for example, from a quarry, which is optionally purified and optionally dried. Low-temperature calcined clay is clay that has been heat-treated at a temperature of 500-1200° C. For example, low-temperature calcined clay minerals can be produced in a rotary kiln or a flash calciner. High-temperature calcined clay is a clay mineral that has been heat-treated at a temperature above 1200° C. and generally between 1300-1400° C. High-temperature calcined clay is generally crystalline or contains a large amount of crystalline phases, in particular crystalline phases of mullite.

[0090] According to an embodiment, the clay mineral of the present invention is a coarse clay, in particular a phyllosilicate. In particular, the clay mineral comprises or consists of kaolinite, montmorillonite and / or illite, in particular kaolinite. These are clays that can be calcined and have proven to be suitable as a component of a mineral binder. However, other clay minerals may also be suitable.

[0091] The clay mineral of the present invention may be pure clay or may contain other substances as impurities. According to some embodiments, the clay content of the clay mineral, in particular the crude clay, is at least 30% by weight, preferably at least 50% by weight, more preferably at least 70% by weight, and especially at least 85% by weight, relative to the dry weight of the crude clay.

[0092] According to another embodiment, the clay mineral in this article is a low-temperature calcined clay, especially a low-temperature calcined kaolinite. Suitable rapid calcination methods are described, for example, in WO 2014 / 085538. According to a particularly preferred embodiment of the present invention, the calcined clay is metakaolin. However, other clay minerals may also be suitable.

[0093] The clay mineral may be added in the form of excavated material from quarries and / or mining, or may be added in pure form.

[0094] Preferably, the weight ratio of clay mineral to carbonated product is 5:1-1:1, in particular 2.5:1-1.5:1, in particular 2:1. The weight of clay mineral is therefore relative to the pure mineral, without any possible impurities. This allows, for example, the production of a "LC 3 The mineral binder component of ” type cement comprises metakaolin, lime, cement and gypsum.

[0095] The calcination in step b) is particularly carried out at a temperature of 550-1100° C., especially 575-900° C., and particularly 650-850° C. At such temperatures, carbonates as well as crude clay can be calcined effectively.

[0096] In particular, the calcined mineral binder material produced in step b) comprises or consists of:

[0097] - calcium oxide;

[0098] - optional aggregates, in particular aggregates having a particle size below the above-mentioned cut size;

[0099] - Optionally calcined clay, especially metakaolin.

[0100] Preferably, the calcined mineral binder material produced in step b) is fully calcined. In particular, the calcined mineral binder material produced in step b) is substantially free of any carbonate material, especially calcium carbonate. Substantially free means that such carbonate material is present in an amount of no more than 5w%, preferably no more than 1w%, relative to the dry weight of the calcined mineral binder material.

[0101] If the source material in step a) is hardened mortar, hardened concrete and / or unreacted mineral binder, especially unreacted cement, then a composition with calcium oxide can be obtained, for example. Therefore, a carbonated product containing calcium carbonate is obtained in step a), which is then calcined in step b) to produce calcium oxide as a calcined mineral binder material. In addition, there may be aggregates particularly derived from hardened mortar and / or concrete. If separation is performed as described above in step a), the aggregate will particularly have a particle size below the cutting particle size.

[0102] If the carbonate-containing material used in step b) at least temporarily comprises clay minerals, in particular kaolinite, or a mixture of carbonation product and clay minerals is used as carbonate-containing material in step b), a composition further comprising calcined clay can be obtained.

[0103] Preferably, the calcined mineral binder material obtained in step b) is not introduced as source material in step a).

[0104] The composition thus obtained can be used as a mineral binder or as a component of a mineral binder composition.Thanks to the process of the invention, the composition thus produced is characterized by a significantly reduced carbon dioxide footprint.

[0105] Furthermore, the calcined mineral binder material may be subjected to a grinding procedure, in particular to obtain a Blaine fineness of at least 1000 μm measured according to DIN EN 196-6:2018. 2 / g, especially at least 2500m 2 / g, especially at least 3500m 2 / g of powder. By grinding, the solidification and hardening of the calcined mineral binder can be adjusted, and the powder can be used, for example, as a cement substitute, for example in construction works. Due to the use of the calcined mineral binder produced according to the method of the invention, the CO2 footprint of the construction work is also reduced.

[0106] According to another preferred embodiment, the calcined mineral binder material produced in step b) is partially hydrated, in particular calcium oxide is converted into calcium hydroxide. The partial hydration can be carried out before and / or after the above-mentioned grinding process. However, since the grinding process is optional, calcium hydroxide can also be produced without any grinding. Similar to calcium oxide, calcium hydroxide can be used as a mineral binder or as a component of a mineral binder composition.

[0107] Another aspect of the present invention relates to a method for producing a settable mineral binder composition, the method comprising the steps of: (i) providing a mineral binder material as described above, and (ii) mixing it with aggregate, further mineral binder, water and / or at least one additive.

[0108] The further mineral binder, if present, is in particular chemically and / or physically different from the mineral binder material provided in step (i).

[0109] Aggregates are for example selected from gravel, sand and / or rock aggregates. The corresponding compositions can be formulated, for example, as mortar or concrete compositions.

[0110] In particular, the mineral binder composition contains water, wherein the weight ratio of water to mineral binder may be in the range of 0.25-0.8, such as 0.3-0.6, such as 0.35-0.5. Such a binder composition can be directly processed into a processable mortar or concrete composition.

[0111] When the addition of water is omitted in the above-described method, for example a dry mortar or concrete composition can be prepared.

[0112] In addition, the mineral binder composition may contain at least one additive, such as a concrete additive and / or a mortar additive. The at least one additive comprises, for example, a defoamer, a dye, a preservative, a plasticizer, a retarder, a pore former, a shrinkage reducer and / or a corrosion inhibitor or a combination thereof. Typically, these additives are present in a proportion of 0.0001-10% by weight relative to the total weight of the mineral binder composition.

[0113] Further advantageous embodiments of the invention are evident from the exemplary embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0114] The accompanying drawings for explaining the embodiments are as follows:

[0115] Figure 1 is a schematic diagram of the process of the invention combining carbonation of a source material and calcination of the carbonation product so obtained to produce a calcined mineral binder material with carbon dioxide circulation;

[0116] Figure 2is comprised of ground and partially hydrated Figure 1 Schematic representation of further process steps for producing a calcined mineral binder material in the process shown.

[0117] Exemplary embodiments

[0118] exist Figure 1 In the method of the invention shown, a source material 11, for example hardened concrete from demolition waste, is subjected to a carbonation treatment 1 with gaseous carbon dioxide 12, 22 (the source of the carbon dioxide is explained in more detail below).

[0119] In the carbonation treatment 1, for example, 70 kg of crushed concrete is immersed in 30 L of water and treated in a mixing device (concrete mixer) with continuous mixing and continuous flow of gaseous carbon dioxide at a temperature of 20° C. and atmospheric pressure. Thus, pressurized carbon dioxide gas is introduced directly into liquid water, thereby generating observable carbon dioxide bubbles in the water. During the treatment, a continuous water flow is used to move the suspended carbonation product and small aggregate particles (= powdered mineral material) from the mixing device into a filtration system. In the filtration system, the turbid suspension of the carbonation product in the form of powdery fines and small aggregate particles is filtered with a filter with an opening size of 125 μm. Therefore, small aggregates with a particle size of ≥125 μm are retained in the filter, while smaller particles pass through the filter together with the water. Thereafter, the liquid suspension of the carbonation product is filtered again to remove water from the powdered mineral material. The process is stopped when the water introduced into the filter system no longer contains visible amounts of particles (clear solution, no visible turbidity) and the treated aggregate no longer contains visible amounts of hydrated cement on its surface.

[0120] Subsequently, the aggregate 14 thus obtained is removed from the concrete mixer and dried. The aggregate 14 can be used, for example, as recycled aggregate in new mineral binder compositions.

[0121] The powdered mineral material 13 (= carbonate-containing material) is subsequently subjected to a calcination process 2 in a cement kiln at a temperature of, for example, 700° C. This produces a calcined mineral binder material 23 consisting mainly of calcium oxide and small aggregates having a particle size below the cut particle size (= filter opening size, i.e. 125 μm), as well as a carbon dioxide by-product 22.

[0122] In the carbonation process 1, carbonation is carried out with the carbon dioxide by-product 22 obtained in the calcination process 2. However, for initiating the process and as a supplement, carbon dioxide 12 from external sources, for example by-products from other industrial processes, can also be used temporarily.

[0123] also, Figure 1The method shown allows optionally mixing the powdered mineral material 13 with a clay mineral 21 (e.g. kaolinite) and subjecting the mixture to a calcination treatment 2. In this case, the calcined mineral binder material 23 consists essentially of calcium oxide, calcined clay (e.g. metakaolin), and small aggregates with a particle size below the cut particle size. For example, if the calcined mineral binder material 23 is used to produce limestone calcined clay cement or LC cement, respectively 3 Type cement is interesting. 3 Portland cement is a blended Portland cement consisting of cement clinker, calcined clay, limestone and gypsum.

[0124] like Figure 2 As shown, the calcined mineral binder material 23 obtained after the calcination treatment 2 can be subjected to a grinding process 3, for example in a cement mill, to produce a finely ground calcium oxide-based binder material 31. For example, the finely ground calcium oxide-based binder material is 3500 m 2 / g Blaine fineness and can be used as a (partial) cement replacement in mortar or concrete compositions.

[0125] Furthermore, if necessary, the finely ground calcium oxide-based binder material 31 may be further subjected to a hydration treatment 4 to partially convert the calcium oxide into calcium hydroxide. Thus, water may be added to the finely ground calcium oxide-based binder material 31 in a certain proportion to hydrate the calcium oxide in a dry state to keep it as a powder (= dry aging).

[0126] The calcium hydroxide-based binder material 41 thus obtained consists essentially of calcium hydroxide, optionally calcined clay (eg metakaolin) and small aggregates having a particle size below the cut particle size.

[0127] If necessary, the calcium hydroxide-based binder material 41 is subjected to a further grinding process 5 to obtain a finely ground calcium hydroxide-based binder material 51, for example having a particle size of 4,000 m 2 / g of Blaine fineness.

[0128] The binder material 23, 31, 41, 51 produced by the method of the present invention can be used as a component of a mineral binder, which is used, for example, to produce a new mortar or concrete composition. Therefore, the carbon emissions are essentially zero, because the carbon dioxide produced during the calcination 2 can be completely consumed in the carbonation 1 of the source material 11.

[0129] Those skilled in the art will appreciate that, without departing from the spirit or essential characteristics of the present invention, the present invention can be implemented in other specific forms. Therefore, the presently disclosed embodiments are considered in all aspects to be illustrative rather than restrictive.

[0130] For example, if finely ground calcium oxide-based material 31 is used as the mineral binder component, the hydration treatment 4 and the second grinding process 5 may be omitted.

[0131] Likewise, if the calcined mineral binder material 23 obtained after the calcination process 2 is fine enough to be directly hydrated in the hydration process 4, the grinding process 3 can be omitted.

[0132] Operation Example

[0133] The carbonated mineral binder material is prepared in a wet process as described in WO 2014 / 154741 (page 18, lines 2-29; corresponding to a dry powdered mineral material of a carbonized mineral binder material). The carbonated product is mixed with kaolinite in a mass ratio of kaolinite to carbonated product of 2:1 and 5:1, respectively. The mixture of kaolinite and carbonated product is calcined for 2 hours at a predetermined temperature as shown in Table 1 below. In all cases, the target temperature is reached within 1 hour from the start of heating. The sample is then cooled to room temperature in a furnace. The composition of the material before and after calcination is determined by X-ray diffraction (XRD). Metakaolin is amorphous and therefore not visible in XRD. However, the disappearance of the peak attributable to kaolinite and the appearance of broad peaks typically observed for amorphous materials indicate that metakaolin is formed during calcination. The main components are reported in Table 1 below. Thermogravimetric analysis shows that decarbonation occurs mainly at temperatures of 600°C to 725°C.

[0134] Table 1: Overview of calcined products

[0135] Weight ratio of kaolinite to carbonated product 2:1 5:1 Starting materials, major components <![CDATA[Kaolinite, CaCO3]]> <![CDATA[Kaolinite, CaCO3]]> Calcinated at 600℃, the main components <![CDATA[Metakaolin, CaCO3]]> <![CDATA[Metakaolin, CaCO3]]> Calcinated at 700℃, the main components <![CDATA[Metakaolin, CaO, Ca(OH)2]]> <![CDATA[Metakaolin, CaCO3, CaO]]> Calcinated at 800℃, the main components <![CDATA[Metakaolin, CaO, Ca(OH)2]]> Metakaolin, CaO Calcinated at 900℃, the main components Metakaolin, CaO Metakaolin, CaO

[0136] The reactivity of the resulting calcined mineral binder was tested as follows.

[0137] The calcined mineral binder or starting material is appropriately mixed with water to achieve a water / binder ratio of 0.5. Mixing is then continued for 1 minute at 1000 rpm on a Heidolph propeller mixer. All mixing procedures are carried out at 23° C. and 50% rh. The heat flow curve of the resulting mixture is measured in an isothermal process as described in standard ASTM C1702-17. The measurement is performed using an instrument i-CAL 8000 from Calmetr ix. Table 2 below summarizes the heat released within 30 minutes to 20 hours after the start of the measurement of each sample. Positive values ​​indicate hydraulic and / or pozzolanic reactions.

[0138] Table 2: Results of heat flow measurements

[0139]

[0140] From the results in Table 2 it can be seen that a material having the properties of a mineral binder is obtained by the process of the present invention. In contrast, the starting material, ie a mixture of the carbonated product and uncalcined kaolinite, cannot be used as a mineral binder.

Claims

1. A method for producing a calcined mineral binder material, comprising the following steps: a) providing a source material comprising a mineral binder material, and carbonate the source material with carbon dioxide such that the mineral binder material is at least partially, in particular substantially completely, carbonated to produce a carbonated product; b) calcining the carbonate-containing material to produce a calcined mineral binder material and carbon dioxide as a by-product; wherein in step a), the carbon dioxide by-product of step b), optionally in combination with additional carbon dioxide from a different source, is used as carbon dioxide for carbonation of the source material; And in step b), the carbonate-containing material comprises the carbonation product of step a) and optionally other materials.

2. The method according to claim 1, wherein the carbonate-containing material further comprises clay minerals.

3. The method according to claim 2, wherein the ratio of clay mineral to carbonation product is 5:1 to 1:1, especially 2.5:1 to 1.5:1, especially 2:

1.

4. The method according to any one of claims 2-3, wherein the clay mineral is selected from crude clay, low-temperature calcined clay and / or high-temperature calcined clay.

5. The method according to any one of claims 2 to 4, wherein the clay mineral comprises kaolinite, montmorillonite and / or illite, especially kaolinite.

6. The method according to claim 1 , wherein in step a), the source material comprises a hardened mineral binder and aggregate, and wherein during carbonation, the hardened mineral binder is at least partially, in particular substantially completely, removed from the surface of the aggregate.

7. A method according to any one of claims 5-6, wherein the processed source material is separated at a predetermined cut size so as to recover processed aggregate having a particle size of at least the predetermined cut size and to recover powdered mineral material having a particle size below the predetermined cut size.

8. A method according to any one of the preceding claims, wherein the source material comprises hardened mortar and / or concrete.

9. A method according to any one of the preceding claims, wherein the source material comprises an uncured mineral binder.

10. The method according to any one of the preceding claims, wherein the carbonation product produced in step a) comprises or consists of calcium carbonate, carbonate silicate and / or aluminium carbonate.

11. The method according to any one of the preceding claims, wherein the calcination in step b) is carried out at a temperature of 550-1100°C, in particular 575-900°C, in particular 650-850°C.

12. The method according to any one of the preceding claims, wherein the calcined mineral binder material comprises or consists of: - calcium oxide; - optionally calcined clay, especially metakaolin; - Optional aggregates, especially aggregates having a particle size below the cut size.

13. A process according to any one of the preceding claims, wherein the calcined mineral binder material is partially hydrated to convert calcium oxide to calcium hydroxide.

14. A method according to any one of the preceding claims, wherein the calcined mineral binder material is subjected to a grinding procedure to obtain a granular material having a particle size of at least 1000 m 2 / g, especially at least 2500m 2 / g, especially at least 3500m 2 / g of powder with Blaine fineness measured according to DIN EN 196-6:2018.

15. A process for producing a settable mineral binder composition comprising the steps of: (i) providing a mineral binder material obtained in a process according to any one of claims 1 to 14, and (ii) mixing it with one or more representatives of the group consisting of aggregate, further mineral binder, water and additives.

Citation Information

Patent Citations

  • System for the production of fine lime

    WO2014085538A1

  • Retrieving aggregates and powdery mineral material from demolition waste

    WO2014154741A1