Method for recovering lithium from waste lithium ion battery
By using sodium hydroxide and potassium hydroxide for neutralization and membrane electrolysis during the recovery process of lithium-ion battery, the problems of low lithium ion recovery and reuse of inorganic acid and alkali sources are solved, and efficient lithium ion recovery and process circulation are achieved use.
Patent Information
- Application Number
- CN202380030036.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-27
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing wet process has a low recovery rate of lithium ions during the lithium-ion battery recycling process, and the recycling technology of inorganic acid and alkaline sources has not been effectively solved.
By adding sodium hydroxide and potassium hydroxide to the solution of active substance powder, neutralizing and alkali metal hydroxide re-adding, the lithium salt is separated and membrane electrolysis is performed, the process is optimized to improve the recovery rate of lithium, and in the process The generated salt is reused as an inorganic acid and a base.
It realizes high recovery of lithium ion, and effectively utilizes the salts generated in the process, reducing the external demand for inorganic acids and alkalis, and improving the environmental protection and economicality of the process.
Smart Images

Figure HDA0005057430090000011 
Figure HDA0005057430090000021 
Figure HDA0005057430090000031
Abstract
Description
[Technical field]
[0001] The invention relates to a method for recovering lithium from waste lithium-ion batteries. [Background Technology]
[0002] In recent years, as lithium-ion batteries have become more common, research has been conducted on methods for recovering valuable metals such as cobalt, nickel, manganese, and lithium from waste lithium-ion batteries and reusing them as materials for the lithium-ion batteries.
[0003] In the past, when the above-mentioned valuable metals were recovered from the above-mentioned waste lithium-ion batteries, cobalt, nickel, manganese and lithium were separated and refined from the powder containing the above-mentioned valuable metals by a wet process. The above-mentioned powder was obtained by heating (roasting) the waste lithium-ion batteries or crushing and classifying them without heating (for example, refer to Patent Documents 1 and 2).
[0004] In addition, in the present invention, waste lithium ion batteries refer to used lithium ion batteries whose life span as battery products has been exhausted, lithium ion batteries discarded as defective products in the manufacturing process, and the remaining positive electrode materials and negative electrode materials used for productization in the manufacturing process. In addition, the powder containing the positive electrode and the negative electrode obtained from the above-mentioned waste lithium ion batteries is used as active material powder. In addition, impurities refer to metals that do not need to be recovered in the metals contained in the active material powder. [Prior art literature] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 6835820 Patent Document 2: Japanese Patent No. 6869444 [Summary of the invention] Problems to be solved by the invention
[0006] However, in the existing wet process, a compound other than the lithium compound as the recovery target is used as an alkali source, so the concentration of cations other than lithium increases, while the concentration of lithium ions decreases. As a result, in the previous wet process, the recovery rate of lithium as the target is significantly reduced. In addition, in the previous wet process, the inorganic acid used in the dissolution of the active material powder and the compound used as the alkali source are discharged in the form of salt, and there is the following disadvantage: there is no technology for recycling the inorganic acid and the compound used as the alkali source.
[0007] In recent years, a method for recovering lithium from waste lithium-ion batteries has been sought, which can eliminate such undesirable conditions, recover lithium at a high recovery rate, and preferably can reuse salts generated in the recovery process as inorganic acids and alkalis in the process, but such a method has not yet been provided. The problem to be solved by the present invention is to provide a method for recovering lithium from waste lithium-ion batteries, which can recover lithium at a high recovery rate, and preferably can reuse salts generated in the recovery process as inorganic acids and alkalis in the process. Means for solving problems
[0008] The present inventors have repeatedly studied in view of the above-mentioned problems and found that: adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to a solution obtained by dissolving active material powder with an inorganic acid, thereby separating a lithium salt aqueous solution from a salt solution of at least one selected from the group consisting of sodium and potassium, and preferably reusing the inorganic acid obtained by membrane electrolysis of the separated salt solution of at least one selected from the group consisting of sodium and potassium and at least one selected from the group consisting of sodium hydroxide and potassium hydroxide. The present invention was completed based on these findings.
[0009] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 1 of the present invention"), which comprises: a dissolution step, using an inorganic acid to dissolve active material powder obtained by pre-treating waste lithium-ion batteries; a neutralization step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolution step; an alkali metal hydroxide re-addition step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the neutralization step again; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the alkali metal hydroxide re-addition step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0010] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 2 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution A to extract and separate manganese, and obtain solution B; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution B to extract and separate cobalt, and obtain solution C; a nickel extraction step, adding an organic phosphorus compound extraction solvent to the solution C to extract and separate nickel; a separation step, respectively separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the nickel extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0011] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 3 of the present invention"), which comprises: a dissolving step, using an inorganic acid to dissolve active material powder obtained by pre-treating waste lithium-ion batteries; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution A to extract and separate manganese, and obtain a solution D; a nickel extraction step, adding a hydroxamate extraction solvent to the solution D to extract and separate nickel, and obtain a solution E; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution E to extract and separate cobalt; a separation step, respectively separating lithium salt and at least one salt selected from sodium and potassium from the alkaline mixed salt aqueous solution obtained in the cobalt extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0012] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 4 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a cobalt extraction step, adding an organic amine compound extraction solvent to the solution A to extract and separate cobalt, and obtain a solution F; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution F to extract and separate manganese, and obtain a solution G; a nickel extraction step, adding an organic phosphorus compound extraction solvent to the solution G to extract and separate nickel, and obtain a first lithium salt aqueous solution; a separation step, respectively separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the nickel extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0013] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 5 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a cobalt extraction step, adding an organic amine compound extraction solvent to the solution A to extract and separate cobalt, and obtain a solution H; a nickel extraction step, adding a hydroxamate extraction solvent to the solution H to extract and separate nickel, and obtain a solution I; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution I to extract and separate manganese, and obtain a first lithium salt aqueous solution; a separation step, respectively separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the manganese extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0014] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 6 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a nickel extraction step, adding a hydroxamic extraction solvent to the solution A to extract and separate nickel, and obtain a solution J; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution J to extract and separate manganese, and obtain a solution K; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution K to extract and separate cobalt, and obtain a first lithium salt aqueous solution; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the cobalt extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0015] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 7 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step, performing solid-liquid separation on the insoluble matter obtained in the neutralizing step and solution A; a nickel extraction step, adding a hydroxamic extraction solvent to the solution A to extract and separate nickel, and obtain a solution L; a cobalt extraction step, adding an organic amine compound extraction solvent to the solution L to extract and separate cobalt, and obtain a solution M; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution M to extract and separate manganese, and obtain a first lithium salt aqueous solution; a separation step, respectively separating lithium salt and at least one salt selected from sodium and potassium from the alkaline mixed salt aqueous solution obtained in the manganese extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0016] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 8 of the present invention"), which comprises: a dissolution step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralization step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolution step; a solvent extraction step, separating at least one metal other than lithium from the metals contained in the active material powder from the solution obtained in the neutralization step by organic solvent extraction to obtain an alkaline mixed salt solution as the residual liquid of the solvent extraction; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution; and a lithium recovery step, recovering lithium from the first lithium salt solution obtained in the separation step.
[0017] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 9 of the present invention"), which comprises: a dissolving step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step, using an organic solvent to extract at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the solvent extraction step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step, in which an aqueous solution containing at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is mixed with the organic solvent and then subjected to oil-water separation to obtain an alkali-containing organic solvent, and the solution obtained in the neutralization step.
[0018] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 10 of the present invention"), which comprises: a dissolving step, dissolving active material powder obtained by pre-treating waste lithium-ion batteries with an inorganic acid; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a metal sulfide removing step, mixing the solution obtained in the neutralizing step with a sulfide in a pH range of 2 to 6 to generate a sulfide of at least one metal selected from the group consisting of copper, cadmium, lead, and mercury, and removing the metal sulfide; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the metal sulfide removing step; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step.
[0019] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 11 of the present invention"), which comprises: a dissolving step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step, using an organic solvent to extract at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction; a separation step, respectively separating lithium salts and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; a second A membrane electrolysis step, using an ion exchange membrane to perform membrane electrolysis on at least one salt solution selected from the group consisting of sodium and potassium obtained in the separation step to obtain an alkali metal hydroxide aqueous solution; a carbonation step, carbonating a portion of the alkali metal hydroxide aqueous solution; and a lithium recovery step, recovering lithium from the first lithium salt aqueous solution obtained in the separation step, reusing the alkali metal hydroxide aqueous solution obtained in the second membrane electrolysis step in at least one step selected from the group consisting of the neutralization step, the solvent extraction step and the separation step, and reusing at least one selected from the group consisting of an inorganic acid obtained by recovering the gas generated in the second membrane electrolysis step and an inorganic acid obtained in the anode chamber of the second membrane electrolysis step in the dissolution step.
[0020] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 12 of the present invention"), which comprises: a dissolving step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralizing step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step, using an organic solvent to extract at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction; a nickel removing step, mixing the first alkaline mixed salt solution obtained in the solvent extraction step with an alkali, removing the nickel contained in the first alkaline mixed salt solution, and obtaining a second alkaline mixed salt solution; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the second alkaline mixed salt solution; and a lithium recovery step, recovering lithium from the first lithium salt solution obtained in the separation step.
[0021] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter, sometimes referred to as "lithium recovery method 13 of the present invention"), which comprises: a dissolution step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralization step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolution step; a solvent extraction step, using an organic solvent to extract at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction; a separation step, separating lithium salts and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the solvent extraction step; and a carbonation step, carbonating the first lithium salt aqueous solution obtained in the separation step to obtain lithium carbonate.
[0022] The present invention relates to a method for recovering lithium from waste lithium-ion batteries (hereinafter sometimes referred to as "lithium recovery method 14 of the present invention"), which comprises: a dissolution step, using an inorganic acid to dissolve an active material powder obtained by pre-treating the waste lithium-ion batteries; a neutralization step, adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolution step; a solvent extraction step, using an organic solvent to extract at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction; a separation step, separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; and a first membrane electrolysis step, using an ion exchange membrane to perform membrane electrolysis on the first lithium salt aqueous solution obtained in the separation step to obtain a lithium hydroxide aqueous solution.
[0023] Preferably, the lithium recovery methods 1 to 10 and 12 to 14 of the present invention further include a second membrane electrolysis step, in which the brine solution of at least one selected from the group consisting of sodium and potassium obtained from the separation step is subjected to membrane electrolysis using an ion exchange membrane to obtain an alkali metal hydroxide aqueous solution. Preferably, the alkali metal hydroxide aqueous solution obtained in the second membrane electrolysis step is reused in at least one step selected from the group consisting of the neutralization step, the solvent extraction step, and the separation step.
[0024] Preferably, in the lithium recovery methods 1 to 12 and 14 of the present invention, the lithium recovery step includes a carbonation step, in which the first lithium salt aqueous solution obtained in the separation step is carbonated to obtain lithium carbonate. The lithium recovery process also includes a first membrane electrolysis process, in which the first lithium salt aqueous solution obtained in the separation process is subjected to membrane electrolysis using an ion exchange membrane to obtain a lithium hydroxide aqueous solution, an acid, and a second lithium salt aqueous solution that is more diluted than the first lithium salt aqueous solution. Preferably, the second lithium salt aqueous solution is concentrated and added to the first lithium salt aqueous solution.
[0025] Preferably, the inorganic acid includes at least one selected from the group consisting of hydrochloric acid, sulfuric acid and nitric acid, and more preferably includes hydrochloric acid. Preferably, hydrochloric acid produced by reacting chlorine and hydrogen obtained by membrane electrolysis of the first lithium salt aqueous solution using an ion exchange membrane is used as the inorganic acid. Preferably, the electricity used in the first membrane electrolysis step includes electricity obtained from renewable energy, and more preferably includes electricity obtained from at least one selected from the group consisting of solar power generation, wind power generation, and hydropower generation.
[0026] Preferably, in the lithium recovery methods 13 and 14 of the present invention, the separation step is performed by at least one method selected from the group consisting of a lithium phosphate method, an evaporation concentration method and a solvent extraction method. Preferably, the lithium recovery methods 13 and 14 of the present invention further include: a second membrane electrolysis step, in which the brine solution of at least one selected from the group consisting of sodium and potassium obtained from the separation step is subjected to membrane electrolysis using an ion exchange membrane to obtain an alkali metal hydroxide aqueous solution; the brine solution of at least one selected from the group consisting of sodium and potassium is concentrated, and the concentrated brine solution of at least one selected from the group consisting of sodium and potassium is electrolyzed in the second membrane electrolysis step. Effects of the Invention
[0027] The lithium recovery methods 1 to 14 of the present invention provide a method capable of recovering lithium at a high recovery rate and preferably capable of reusing the salt generated in the recovery process as an inorganic acid and base in the process. [Brief Description of the Drawings]
[0028] Figure 1 This is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 1 of the present invention. Figure 2 This is an explanatory diagram showing the structure of another embodiment of the lithium recovery method 1 of the present invention. Figure 3 It is an explanatory diagram showing the structure of one embodiment of lithium recovery method 2 to 9 of the present invention. Figure 4 It is an explanatory diagram showing the structure of another embodiment of the lithium recovery method 2 to 9 of the present invention. Figure 5 It is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 10 of the present invention. Figure 6 This is an explanatory diagram showing the structure of another embodiment of the lithium recovery method 10 of the present invention. Figure 7 It is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 11 of the present invention. Figure 8 This is an explanatory diagram showing the structure of another embodiment of the lithium recovery method 11 of the present invention. Fig. 9 It is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 12 of the present invention. Fig.10 This is an explanatory diagram showing the structure of another embodiment of the lithium recovery method 12 of the present invention. Fig.11 It is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 13 of the present invention. Fig.12 It is an explanatory diagram showing the structure of one embodiment of the lithium recovery method 14 of the present invention. Fig.13 This is an explanatory diagram showing the structure of one embodiment using the lithium phosphate method. Fig.14 This is an explanatory diagram showing the structure of another embodiment using the lithium phosphate method. Fig.15 This is an explanatory diagram showing the structure of still another embodiment using the lithium phosphate method. Fig.16 This is an explanatory cross-sectional view showing the structure of an ion exchange membrane electrolytic cell used in the first membrane electrolysis step of lithium recovery methods 1 to 12 and 14 of the present invention. Fig.17 This is an explanatory cross-sectional view showing the structure of the ion exchange membrane electrolytic cell used in the second membrane electrolysis step of the lithium recovery methods 1 to 14 of the present invention. [Specific implementation method]
[0029] The present invention will be described in more detail with reference to the accompanying drawings. In addition, unless otherwise specified, the "to" in a numerical range means above to below, and both ends of the numerical value are included. In addition, when expressing a numerical range, the upper limit and the lower limit can be appropriately combined, and the numerical range thus obtained is also disclosed. In the description of the drawings, the same elements are denoted by the same reference numerals, and duplicate descriptions are omitted. In addition, the dimensional ratios of the drawings are exaggerated for convenience of description and may be different from the actual ratios.
[0030] like Figures 1 to 12 As shown, the lithium recovery methods 1 to 14 of the present invention use active material powder 1 as the starting material.
[0031] <Dissolving process> Lithium recovery methods 1 to 14 of the present invention ( Figures 1 to 12 ) includes a dissolving step (step 1), wherein the active material powder 1 is obtained by pre-treatment by dissolving with an inorganic acid. The inorganic acid preferably includes at least one selected from the group consisting of hydrochloric acid, sulfuric acid and nitric acid, more preferably at least one selected from the group consisting of hydrochloric acid, sulfuric acid and nitric acid, further preferably hydrochloric acid, sulfuric acid or nitric acid, and particularly preferably hydrochloric acid. The active material powder 1 includes valuable metals such as lithium, iron, aluminum, cobalt, nickel, and manganese. Therefore, by dissolving the active material powder 1 with the inorganic acid, a solution of the valuable metals contained in the active material powder 1 can be obtained.
[0032] <Neutralization process> The lithium recovery methods 1 to 14 of the present invention include a neutralization step (step 2), in which at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is added to the solution of the valuable metal obtained in the dissolution step. Figures 1 to 17 , only sodium hydroxide is added as the alkali metal hydroxide. The addition of at least one selected from the group consisting of sodium hydroxide and potassium hydroxide may be at least one solid selected from the group consisting of sodium hydroxide and potassium hydroxide, at least one selected from the group consisting of sodium hydroxide aqueous solution and potassium hydroxide aqueous solution, or at least one of a mixture thereof. The above-mentioned solution of the valuable metal is neutralized in the above-mentioned neutralization step. Furthermore, iron hydroxide and aluminum hydroxide are sequentially precipitated by adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the above-mentioned valuable metal solution, and iron and aluminum may be separated from the above-mentioned valuable metal solution.
[0033] In the lithium recovery method 1 ( Figure 1 and 2 ), in the neutralized valuable metal solution, at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is then added again in step 3 (alkali metal hydroxide re-addition process). The valuable metals in the solution, for example, at least one selected from the group consisting of manganese, cobalt and nickel, are removed as precipitate 2, and an alkaline mixed salt solution containing lithium and at least one selected from the group consisting of sodium and potassium can be obtained as a filtrate. In the case where the solution contains two or more metals as the valuable metals, the precipitate 2 can be a mixture of hydroxides of the two or more metals, or a hydroxide of a mixture of the two or more metals.
[0034] <Extraction process> Lithium recovery method 2 to 9 of the present invention ( Figure 3 and Figure 4 ) includes a solvent extraction step (step 3), in which the valuable metals contained in the above-mentioned active material powder 1 are extracted from the solution obtained in the above-mentioned neutralization step by solvent extraction using an organic solvent.
[0035] In the lithium recovery method 2 of the present invention, the insoluble matter generated by the neutralized solution of the valuable metal is subjected to solid-liquid separation from the solution A. An organic phosphorus compound extraction solvent is added to the solution A to extract and separate manganese, and a solution B is obtained (manganese extraction step 2). An organic phosphorus compound extraction solvent is added to the solution B to extract and separate cobalt, and a solution C is obtained (cobalt extraction step 2). An organic phosphorus compound extraction solvent is added to the solution C to extract and separate nickel, and a first lithium salt aqueous solution is obtained (nickel extraction step 2). These extraction steps can be simply managed by pH.
[0036] The solvent used in the above-mentioned manganese extraction step 2, cobalt extraction step 2 and nickel extraction step 2 is an organic phosphorus compound such as a phosphate ester, a phosphonate ester, a phosphinic acid, and a phosphine oxide. These organic phosphorus compounds are commercially available, and examples thereof include D2EHPA (diisooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by Daichika Kogyo Co., Ltd. as a phosphonate ester, CYANEX272 manufactured by Solvay Co., Ltd. as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide.
[0037] For example, D2EHPA is used as an extraction solvent in the manganese extraction step 2, and CYANEX272 is used as an extraction solvent in the cobalt extraction step 2 and the nickel extraction step 2. The pH of CYANEX272 used in the cobalt extraction step 2 and the nickel extraction step 2 is different.
[0038] In the lithium recovery method 2 of the present invention, in the extraction step, manganese, cobalt, and nickel are subjected to solvent extraction in the order of the valuable metals except lithium, and are removed as respective metal sulfate aqueous solutions to obtain a first lithium salt aqueous solution. The lithium salt contained in the first lithium salt aqueous solution becomes lithium chloride when hydrochloric acid is used in the acid dissolution in step 1.
[0039] In the lithium recovery method 3 of the present invention, the insoluble matter generated from the neutralized solution of the valuable metal is subjected to solid-liquid separation from the solution A. An organic phosphorus compound extraction solvent is added to the solution A to extract and separate manganese, and obtain a solution D (manganese extraction step 3). A hydroxime extraction solvent is added to the solution D to extract and separate nickel, and obtain a solution E (nickel extraction step 3). An organic phosphorus compound extraction solvent is added to the solution E to extract and separate cobalt, and obtain a first lithium salt aqueous solution (cobalt extraction step 3).
[0040] The solvent used in the above-mentioned manganese extraction step 3 and cobalt extraction step 3 is an organic phosphorus compound such as a phosphate ester, a phosphonate ester, a phosphinic acid, and a phosphine oxide. These organic phosphorus compounds are commercially available, and examples thereof include D2EHPA (diisooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by the Eighth Chemical Industry Co., Ltd. as a phosphonate ester, CYANEX272 manufactured by Solvay as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide. The solvent used in the nickel extraction step 3 is hydroxamate. Examples of the hydroxyoxime include 5,8-diethyl-7-hydroxy-6-dodecyl oxime (LIX-63), 5-dodecyl-2-hydroxybenzaldehyde oxime (LIX 860), 2-hydroxy-5-nonylbenzophenone oxime (LIX 65N), 2-hydroxy-5-nonylacetophenone oxime (SME 529), and 2-hydroxy-5-nonylphenylbenzyl ketone oxime (Acorga P-17).
[0041] For example, D2EHPA is used as the extraction solvent in the manganese extraction step 3, LIX 860 is used as the extraction solvent in the nickel extraction step 3, and CYANEX272 is used as the extraction solvent in the cobalt extraction step 3.
[0042] In the lithium recovery method 4 of the present invention, the insoluble matter generated from the neutralized solution of the valuable metal is subjected to solid-liquid separation from the solution A. An organic amine compound extraction solvent is added to the solution A to extract and separate cobalt, and obtain a solution F (cobalt extraction step 4). An organic phosphorus compound extraction solvent is added to the solution F to extract and separate manganese, and obtain a solution G (manganese extraction step 4). An organic phosphorus compound extraction solvent is added to the solution G to extract and separate nickel, and obtain a first lithium salt aqueous solution (nickel extraction step 4). In the above cobalt extraction step 4, when a cobalt chloride complex of appropriate concentration is formed, a cobalt salt solution with high purity can be separated. In this case, since the above solution F contains no cobalt or almost no cobalt, the purity of the metal salt solutions obtained in the above manganese extraction step 4 and the nickel extraction step 4 is also high.
[0043] The solvent used in the above-mentioned cobalt extraction step 4 is an organic amine compound. Examples of the organic amine compound include Primene (registered trademark) JM-T manufactured by Dow Chemical Company as a primary amine, Amberlite (registered trademark) LA-2 manufactured by Sigma-Aldrich Company as a secondary amine, Alamine 336 (trioctylamine) manufactured by Sigma-Aldrich Company as a tertiary amine, and Aliquat (registered trademark) 336 manufactured by Sigma-Aldrich Company as a quaternary ammonium salt. The solvent used in the above-mentioned manganese extraction step 4 and nickel extraction step 4 is an organic phosphorus compound such as a phosphate ester, a phosphonate ester, a phosphinic acid, and a phosphine oxide. These organic phosphorus compounds are commercially available, and examples thereof include D2EHPA (diisooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by Daichika Kogyo Co., Ltd. as a phosphonate ester, CYANEX 272 manufactured by Solvay Company as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide.
[0044] For example, trioctylamine is used as the extraction solvent in the cobalt extraction step 4 , D2EHPA is used as the extraction solvent in the manganese extraction step 4 , and CYANEX272 is used as the extraction solvent in the nickel extraction step 4 .
[0045] In the lithium recovery method 5 of the present invention, the insoluble matter generated from the neutralized solution of the valuable metal is subjected to solid-liquid separation from the solution A. An organic amine compound extraction solvent is added to the solution A to extract and separate cobalt, and obtain a solution H (cobalt extraction step 5). A hydroxime extraction solvent is added to the solution H to extract and separate nickel, and obtain a solution I (nickel extraction step 5). An organic phosphorus compound extraction solvent is added to the solution I to extract and separate manganese, and obtain a first lithium salt aqueous solution (manganese extraction step 5). In the above-mentioned cobalt extraction step 5, when a cobalt chloride complex of appropriate concentration is formed, a cobalt salt solution with high purity can be separated. In this case, since the above-mentioned solution H contains no cobalt or hardly contains cobalt, the purity of the metal salt solutions obtained in the above-mentioned nickel extraction step 5 and manganese extraction step 5 is also high.
[0046] The solvent used in the above-mentioned cobalt extraction step 5 is an organic amine compound. Examples of the above-mentioned organic amine compound include Primene (registered trademark) JM-T manufactured by Dow Chemical Company as a primary amine, Amberlite (registered trademark) LA-2 manufactured by Sigma-Aldrich Company as a secondary amine, Alamine 336 (trioctylamine) manufactured by Sigma-Aldrich Company as a tertiary amine, and Aliquat (registered trademark) 336 manufactured by Sigma-Aldrich Company as a quaternary ammonium salt. The solvent used in the above-mentioned nickel extraction step 5 is hydroxamate. Examples of the hydroxyoxime include 5,8-diethyl-7-hydroxy-6-dodecyl oxime (LIX-63), 5-dodecyl-2-hydroxybenzaldehyde oxime (LIX 860), 2-hydroxy-5-nonylbenzophenone oxime (LIX 65N), 2-hydroxy-5-nonylacetophenone oxime (SME529), 2-hydroxy-5-nonylphenylbenzyl ketone oxime (Acorga P-17), etc. The solvent used in the manganese extraction step 5 is an organic phosphorus compound such as a phosphate ester, a phosphonate ester, a phosphinic acid, or a phosphine oxide. These organophosphorus compounds are commercially available, and examples thereof include D2EHPA (di-isooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by the Daichika Kogyo Co., Ltd. as a phosphonic acid ester, CYANEX272 manufactured by Solvay as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide.
[0047] For example, trioctylamine is used as the extraction solvent in the cobalt extraction step 5, LIX 860 is used as the extraction solvent in the nickel extraction step 5, and D2EHPA is used as the extraction solvent in the manganese extraction step.
[0048] In the lithium recovery method 6 of the present invention, the insoluble matter generated from the neutralized solution of the valuable metal is subjected to solid-liquid separation from the solution A. A hydroxime extraction solvent is added to the solution A to extract and separate nickel, and a solution J is obtained (nickel extraction step 6). An organic phosphorus compound extraction solvent is added to the solution J to extract and separate manganese, and a solution K is obtained (manganese extraction step 6). An organic phosphorus compound extraction solvent is added to the solution K to extract and separate cobalt, and a first lithium salt aqueous solution is obtained (cobalt extraction step 6).
[0049] The solvent used in the nickel extraction step 6 is a hydroxime. Examples of the hydroxime include 5,8-diethyl-7-hydroxy-6-dodecyl oxime (LIX-63), 5-dodecyl-2-hydroxybenzaldehyde oxime (LIX 860), 2-hydroxy-5-nonylbenzophenone oxime (LIX 65N), 2-hydroxy-5-nonylacetophenone oxime (SME 529), and 2-hydroxy-5-nonylphenylbenzyl ketone oxime (Acorga P-17). The solvent used in the manganese extraction step 6 and the cobalt extraction step 6 is an organic phosphorus compound such as a phosphate, a phosphonate, a phosphinic acid, and a phosphine oxide. These organophosphorus compounds are commercially available, and examples thereof include D2EHPA (di-isooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by the Daichika Kogyo Co., Ltd. as a phosphonic acid ester, CYANEX272 manufactured by Solvay as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide.
[0050] For example, LIX 860 is used as the extraction solvent in the nickel extraction step 6 , D2EHPA is used as the extraction solvent in the manganese extraction step 6 , and CYANEX 272 is used as the extraction solvent in the cobalt extraction step 6 .
[0051] In the lithium recovery method 7 of the present invention, the acid solution is neutralized with lithium hydroxide, and the generated insoluble matter is subjected to solid-liquid separation from the solution A. A hydroxime extraction solvent is added to the solution A to extract and separate nickel, and a solution L is obtained (nickel extraction step 7). An organic amine extraction solvent is added to the solution L to extract and separate cobalt, and a solution M is obtained (cobalt extraction step 7). An organic phosphorus compound extraction solvent is added to the solution M to extract and separate manganese, and a first lithium salt aqueous solution is obtained (manganese extraction step 7).
[0052] The solvent used in the nickel extraction step 7 is a hydroxime. Examples of the hydroxime include 5,8-diethyl-7-hydroxy-6-dodecyl oxime (LIX-63), 5-dodecyl-2-hydroxybenzaldehyde oxime (LIX 860), 2-hydroxy-5-nonylbenzophenone oxime (LIX 65N), 2-hydroxy-5-nonylacetophenone oxime (SME 529), and 2-hydroxy-5-nonylphenylbenzyl ketone oxime (Acorga P-17). The solvent used in the cobalt extraction step 7 is an organic amine compound. As the organic amine compound, for example, Primene (registered trademark) JM-T manufactured by Dow Chemical Company as a primary amine, Amberlite (registered trademark) LA-2 manufactured by Sigma-Aldrich Company as a secondary amine, Alamine 336 (trioctylamine) manufactured by Sigma-Aldrich Company as a tertiary amine, Aliquat (registered trademark) 336 manufactured by Sigma-Aldrich Company as a quaternary ammonium salt, etc. The solvent used in the above-mentioned manganese extraction step 7 is an organic phosphorus compound such as a phosphate ester, a phosphonate ester, a phosphinic acid, and a phosphine oxide. These organic phosphorus compounds are commercially available, and for example, D2EHPA (diisooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by Daichika Kogyo Co., Ltd. as a phosphonate ester, CYANEX272 manufactured by Solvay Company as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide can be mentioned.
[0053] For example, LIX 860 is used as the extraction solvent in the nickel extraction step 7 , trioctylamine is used as the extraction solvent in the cobalt extraction step 7 , and CYANEX 272 is used as the extraction solvent in the manganese extraction step 7 .
[0054] In the lithium recovery method 8 of the present invention, the extraction process includes a first extraction process, in which iron, aluminum, manganese, cobalt or nickel is extracted from the solution of the valuable metals using a first organic solvent. The pH of the uniform mixture of the solution of the valuable metals and the first organic solvent is adjusted by adding at least one alkali selected from the group consisting of sodium hydroxide and potassium hydroxide, and a first metal-containing organic phase and a first extraction residue are obtained in the first extraction process.
[0055] The extraction step may further include a second extraction step, in which the valuable metals not extracted in the first extraction step are extracted from the first raffinate using a second organic solvent. The pH of the uniform mixture of the first raffinate and the second organic solvent is adjusted by adding at least one alkali selected from the group consisting of sodium hydroxide and potassium hydroxide, and a second metal-containing organic phase and a second raffinate are obtained in the second extraction step.
[0056] The extraction step may further include third to fifth extraction steps for sequentially extracting the valuable metals that have not been extracted in the first and second extraction steps from the second residual extract.
[0057] Examples of the organic solvent used in the extraction step include at least one selected from the group consisting of organic phosphorus compounds such as phosphoric acid esters, phosphonic acid esters, phosphinic acid, phosphine oxides, hydroxyoximes, and organic amine compounds. The organic solvent preferably does not contain a reducing agent or an oxidizing agent. When the organic solvent does not contain an oxidant, the metals, especially manganese, contained in the neutralized acid solution are precipitated, and clogging of the pipes does not occur. Furthermore, the organic solvent does not deteriorate due to the oxidant.
[0058] Organic phosphorus compounds are commercially available, and examples thereof include D2EHPA (di-isooctyl phosphate) as an acidic phosphate ester, PC-88A manufactured by Daichaku Kogyo Co., Ltd. as a phosphonate, CYANEX272 manufactured by Solvay Co., Ltd. as a phosphinic acid, TBP (tributyl phosphate) as a neutral phosphate ester, and tri-n-octylphosphine (TOPO) as a phosphine oxide. Examples of hydroxyoximes include 5,8-diethyl-7-hydroxy-6-dodecyl oxime (LIX-63), 5-dodecyl-2-hydroxybenzaldehyde oxime (LIX 860), 2-hydroxy-5-nonylbenzophenone oxime (LIX 65N), 2-hydroxy-5-nonylacetophenone oxime (SME 529), and 2-hydroxy-5-nonylphenylbenzyl ketone oxime (Acorga P-17). Examples of the organic amine compound include Primene (registered trademark) JM-T manufactured by The Dow Chemical Company as a primary amine, Amberlite (registered trademark) LA-2 manufactured by Sigma-Aldrich Company as a secondary amine, Alamine 336 (trioctylamine) manufactured by Sigma-Aldrich Company as a tertiary amine, and Aliquat (registered trademark) 336 manufactured by Sigma-Aldrich Company as a quaternary ammonium salt.
[0059] The iron-containing organic phase, aluminum-containing organic phase, manganese-containing organic phase, cobalt-containing organic phase and nickel-containing organic phase are respectively subjected to back extraction using sulfuric acid to recover an aqueous solution 2 of metal sulfates (iron sulfate, aluminum sulfate, manganese sulfate, cobalt sulfate and nickel sulfate).
[0060] In the lithium recovery method 9 of the present invention, in the solvent extraction process, the alkali-containing organic solvent obtained by mixing an aqueous solution containing at least one selected from the group consisting of sodium hydroxide and potassium hydroxide with the organic solvent and then performing oil-water separation is mixed with the dissolved solution obtained in the neutralization process. The alkali concentration in the aqueous solution containing at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is low, and even if a large amount of alkali aqueous solution is mixed with the above-mentioned organic solvent, the aqueous phase will be separated from the above-mentioned alkali-containing organic solvent by oil-water separation, so the amount of the above-mentioned alkali-containing organic solvent used in the above-mentioned extraction process will not increase. As a result, it is possible to prevent the dilution of the above-mentioned valuable metal dissolved solution by the liquid from the above-mentioned alkali metal hydroxide aqueous solution.
[0061] Examples of the organic solvent used in the extraction step include di(2-ethylhexyl)phosphate, 2-ethylhexyl(2-ethylhexyl)phosphate, and bis(2,4,4-trimethylpentyl)phosphinic acid. The organic solvent may be diluted with a hydrocarbon such as kerosene.
[0062] The organic phases containing each valuable metal obtained in the above extraction step are subjected to back extraction with sulfuric acid to recover an aqueous solution 2 of each metal sulfate (iron sulfate, aluminum sulfate, manganese sulfate, cobalt sulfate and nickel sulfate).
[0063] The lithium recovery method 10 of the present invention includes a neutralization step (step 2A), in which at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is added to the solution of the valuable metal obtained in the dissolution step. Figure 5 and Figure 6 , which shows the case where only sodium hydroxide is added as the alkali metal hydroxide. The addition of at least one selected from the group consisting of sodium hydroxide and potassium hydroxide may be at least one solid selected from the group consisting of sodium hydroxide and potassium hydroxide, at least one selected from the group consisting of sodium hydroxide aqueous solution and potassium hydroxide aqueous solution, or at least one of a mixture thereof. The above-mentioned valuable metal solution is neutralized in the neutralization step. Furthermore, iron hydroxide and aluminum hydroxide are sequentially precipitated by adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the above-mentioned valuable metal solution, and iron and aluminum may be separated from the above-mentioned valuable metal solution. The solution of the valuable metal is then mixed with a sulfide in the pH range of 2 to 6 in step 2B to generate a sulfide of at least one metal selected from the group consisting of copper, cadmium, lead, and mercury, and the metal sulfide is removed. Examples of the sulfide mixed with the solution of the valuable metal include hydrogen sulfide gas, sodium hydrosulfide, sodium sulfide, and the like.
[0064] The solution of the valuable metals from which the metal sulfides have been removed is used for solvent extraction in step 3. In the solvent extraction, manganese, cobalt, and nickel other than lithium in the valuable metals are respectively extracted by solvent, or iron and aluminum are separated and removed as respective metal sulfate aqueous solutions 2, thereby obtaining a first lithium salt aqueous solution. The lithium salt contained in the first lithium salt aqueous solution is lithium chloride when hydrochloric acid is used in the acid dissolution in step 1.
[0065] Examples of the organic solvent used in the extraction step include di(2-ethylhexyl)phosphate, 2-ethylhexyl(2-ethylhexyl)phosphate, and bis(2,4,4-trimethylpentyl)phosphinic acid. The organic solvent may be diluted with a hydrocarbon such as kerosene.
[0066] The iron-containing organic phase, aluminum-containing organic phase, manganese-containing organic phase, cobalt-containing organic phase and nickel-containing organic phase are respectively subjected to back extraction using sulfuric acid to recover an aqueous solution 2 of metal sulfates (iron sulfate, aluminum sulfate, manganese sulfate, cobalt sulfate and nickel sulfate).
[0067] In the lithium recovery method 11 to 14 of the present invention ( Figures 7 to 12 ), the extraction step includes a first extraction step, in which iron, aluminum, manganese, cobalt or nickel is extracted from the solution of the valuable metals using a first organic solvent. The pH of the uniform mixture of the solution of the valuable metals and the first organic solvent is adjusted by adding at least one alkali selected from the group consisting of sodium hydroxide and potassium hydroxide, and a first metal-containing organic phase and a first raffinate are obtained in the first extraction step.
[0068] The extraction step may further include a second extraction step, in which the valuable metals not extracted in the first extraction step are extracted from the first raffinate using a second organic solvent. The pH of the uniform mixture of the first raffinate and the second organic solvent is adjusted by adding at least one alkali selected from the group consisting of sodium hydroxide and potassium hydroxide, and a second metal-containing organic phase and a second raffinate are obtained in the second extraction step.
[0069] The extraction step may further include third to fifth extraction steps for sequentially extracting the valuable metals that have not been extracted in the first and second extraction steps from the second residual extract.
[0070] Examples of the organic solvent used in the extraction step include di(2-ethylhexyl)phosphate, 2-ethylhexyl(2-ethylhexyl)phosphate, and bis(2,4,4-trimethylpentyl)phosphinic acid. The organic solvent may be diluted with a hydrocarbon such as kerosene.
[0071] The iron-containing organic phase, aluminum-containing organic phase, manganese-containing organic phase, cobalt-containing organic phase and nickel-containing organic phase are respectively subjected to back extraction using sulfuric acid to recover an aqueous solution 2 of metal sulfates (iron sulfate, aluminum sulfate, manganese sulfate, cobalt sulfate and nickel sulfate).
[0072] In the lithium recovery method 12 ( Fig. 9 and 10 ), the first lithium salt aqueous solution is mixed with a base, the pH of the aqueous solution is preferably adjusted to 8 to 14, more preferably to 10 to 12, and the trace amount of nickel contained in the first lithium salt aqueous solution is removed as nickel hydroxide to obtain a second alkaline mixed salt aqueous solution (step 3-1). The base mixed with the first lithium salt aqueous solution preferably includes at least one selected from the group consisting of lithium, sodium, potassium, rubidium, cesium, and francium, more preferably includes at least one selected from the group consisting of lithium, sodium, and potassium, and further preferably includes at least one selected from the group consisting of lithium, sodium, and potassium. The base can be a solid or an aqueous solution. The nickel hydroxide is separated from the second alkaline mixed salt aqueous solution in a solid-liquid separation step such as filtration. A coagulant can also be used in the solid-liquid separation step of nickel hydroxide.
[0073] <Separation process> The lithium recovery methods 1 to 14 of the present invention include a separation step (step 4) for separating lithium salt and at least one salt selected from the group consisting of sodium and potassium from the lithium obtained in the above-mentioned extraction step and an alkali metal mixed salt aqueous solution containing at least one salt selected from the group consisting of sodium and potassium. The separation step is not limited to a specific method, but is preferably performed by at least one of a lithium phosphate method, an evaporation concentration method, and a solvent extraction method.
[0074] (Lithium phosphate method) use Figures 13-15 The lithium phosphate method is described. The lithium phosphate method includes a phosphating step (step A), wherein aluminum phosphate and an aqueous solution of at least one alkali metal hydroxide (MOH) selected from the group consisting of sodium hydroxide and potassium hydroxide are added to the above-mentioned alkali metal mixed salt aqueous solution to generate a solid substance including lithium phosphate and aluminum hydroxide. Alkali metal chloride (MCl) is dissolved in the above-mentioned aqueous liquid in which the above-mentioned solid substance is generated. The above-mentioned alkali metal hydroxide is preferably sodium hydroxide. Figures 13-15 2 shows the case where only sodium hydroxide is used as the alkali metal.
[0075] The lithium phosphate method includes a first solid-liquid separation (step B) in which the solid matter generated in the phosphating step is subjected to solid-liquid separation. Examples of the first solid-liquid separation step include filtration.
[0076] In the lithium phosphate method, the solid separated in the first solid-liquid separation step may also be washed. It includes a pH adjustment step (step C), adding an inorganic acid to the suspension obtained by suspending the solid in water, and adjusting the pH of the suspension to 2-3. The inorganic acid is not limited to a specific inorganic acid. The inorganic acid preferably includes at least one selected from the group consisting of hydrochloric acid, sulfuric acid and nitric acid. The inorganic acid is more preferably at least one of hydrochloric acid, sulfuric acid and nitric acid, further preferably hydrochloric acid, sulfuric acid or nitric acid, and particularly preferably hydrochloric acid. In the case where the inorganic acid is hydrochloric acid, the lithium salt is lithium chloride, Figures 13-15 This situation is recorded in.
[0077] The lithium phosphate method includes a second solid-liquid separation step (step D) for solid-liquid separation of the aluminum phosphate and the lithium salt aqueous solution obtained in the pH adjustment step. As the second solid-liquid separation step, for example, filtration can be cited. The aluminum phosphate obtained in the second solid-liquid separation step can be solid-liquid separated in a short time, and the aluminum phosphate after solid-liquid separation is reused in the phosphorylation step.
[0078] The pH of the aqueous lithium salt solution obtained in the second solid-liquid separation step is preferably adjusted in the pH adjustment step (step 5). Since the pH of the suspension is adjusted to 2 to 3 in the pH adjustment step (step C), the pH of the aqueous lithium salt solution is 2 to 3, but the pH is preferably adjusted to 6 to 14, more preferably 6 to 8 in the pH adjustment step (step 5). At this time, unreacted aluminum and phosphorus are precipitated, and the purity of the aqueous lithium salt solution becomes higher.
[0079] Preferably, a carbonation step (step 6a) described later is performed to carbonate the first lithium salt aqueous solution whose pH is adjusted in the pH adjustment step (step 5) to obtain lithium carbonate ( Fig.13 ). In the brine solution of at least one selected from the group consisting of sodium chloride and potassium chloride, a trace amount of lithium chloride, and at least one selected from the group consisting of sodium carbonate and potassium carbonate are dissolved in the brine solution of at least one selected from the group consisting of sodium and potassium generated in the above-mentioned carbonation step. Preferably, the pH of the brine solution of at least one selected from the group consisting of sodium and potassium is about 12. When hydrochloric acid is added to the brine solution of at least one selected from the group consisting of sodium and potassium to adjust its pH to 5 or less, at least one selected from the group consisting of sodium carbonate and potassium carbonate is decomposed to generate carbon dioxide and water, becoming an aqueous solution in which at least one selected from the group consisting of sodium chloride and potassium chloride is dissolved. The above-mentioned aqueous solution can be concentrated in the concentration step (step 9) described later. Fig.13 The implementation of this concentration step is described in.
[0080] It is preferred to implement the first membrane electrolysis step (step 6, step 6b) described later, wherein the lithium salt aqueous solution whose pH is adjusted in the pH adjustment step (step 5) is subjected to membrane electrolysis using an ion exchange membrane to obtain a lithium hydroxide aqueous solution ( Fig.14 and Fig.15 ). The lithium salt aqueous solution may be concentrated in a first concentration step (step E) before the first membrane electrolysis step. The first concentration step may be performed using, for example, evaporation concentration, reverse osmosis membrane (RO membrane), or the like.
[0081] In the lithium phosphate method, the filtrate in which the alkali metal chloride is dissolved and separated in the first solid-liquid separation step may be concentrated in the second concentration step (step 9) described later.
[0082] (Evaporation Concentration Method) Lithium and at least one alkali metal mixed salt solution selected from the group consisting of sodium and potassium are evaporated and concentrated, and at least one selected from the group consisting of sodium chloride and potassium chloride and at least one selected from the group consisting of sodium salt and potassium salt are sequentially crystallized and separated from the alkali metal mixed salt solution. The second membrane electrolysis step (step 7) described later is implemented, and at least one selected from the group consisting of sodium chloride and potassium chloride and at least one selected from the group consisting of sodium salt and potassium salt separated are dissolved in water, and the salt solution of at least one selected from the group consisting of sodium and potassium is subjected to membrane electrolysis using an ion exchange membrane. The above-mentioned first lithium salt aqueous solution from which at least one selected from the group consisting of sodium salt and potassium salt has been separated is preferably subjected to the above-mentioned pH adjustment step (step 5) and then the above-mentioned carbonation step (step 6a) in the same manner as the above-mentioned first lithium salt aqueous solution obtained by the above-mentioned lithium phosphate method. In the case where the salt solution of at least one selected from the group consisting of sodium and potassium generated in the above-mentioned carbonation step becomes an aqueous solution in which at least one selected from the group consisting of sodium chloride and potassium chloride is dissolved as described above, the aqueous solution can be concentrated in the concentration step (step 9) described later.
[0083] In addition, the first lithium salt aqueous solution is preferably subjected to the pH adjustment step (step 5) and the first concentration step (step E) similarly to the first lithium salt aqueous solution obtained by the lithium phosphate method, and is subjected to the first membrane electrolysis step (step 6, step 6b) described later.
[0084] (Solvent Extraction Method) By adding at least one alkali selected from the group consisting of sodium hydroxide and potassium hydroxide, the pH of the uniform mixed solution of the above-mentioned lithium, and the mixed salt solution of at least one selected from the group consisting of sodium and potassium and the organic solvent for lithium extraction is preferably adjusted to the range of 5 to 9, and a lithium-containing organic phase and a salt solution of at least one selected from the group consisting of sodium and potassium as an extract residue are obtained. As an organic solvent for lithium extraction, for example, di(2-ethylhexyl)phosphate can be cited. The above-mentioned lithium-containing organic phase is washed with an inorganic acid to recover the first lithium salt aqueous solution. The above-mentioned first lithium salt aqueous solution is preferably subjected to the above-mentioned pH adjustment step (step 5) and then the above-mentioned carbonation step (step 6a) in the same manner as the first lithium salt aqueous solution obtained by the above-mentioned lithium phosphate method. In the case where the salt solution of at least one selected from the group consisting of sodium and potassium generated in the above-mentioned carbonation step becomes an aqueous solution in which at least one selected from the group consisting of sodium chloride and potassium chloride is dissolved as described above, the above-mentioned aqueous solution can be concentrated in the concentration step (step 9) described later. In addition, the first lithium salt aqueous solution may be subjected to the pH adjustment step (step 5) and the first concentration step (step E) as in the case of the lithium salt aqueous solution obtained by the lithium phosphate method, and then subjected to the first membrane electrolysis step (step 6, step 6b) described later.
[0085] The second membrane electrolysis step (step 7) described later is carried out, and the brine solution containing at least one selected from the group consisting of sodium and potassium, such as at least one selected from the group consisting of sodium chloride and potassium chloride, from which lithium has been separated by extraction, is subjected to membrane electrolysis using an ion exchange membrane. The brine solution containing at least one selected from the group consisting of sodium and potassium is concentrated in the concentration step (step 9) described later using evaporation concentration, a reverse osmosis membrane (RO membrane), or the like.
[0086] The lithium recovery methods 1 to 14 of the present invention may include a pH adjustment step (step 5), wherein at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is added to the first lithium salt aqueous solution obtained in the separation step using the solvent extraction method to adjust the pH of the first lithium salt aqueous solution. The pH of the first lithium salt aqueous solution is preferably adjusted to 8 to 14, more preferably to 10 to 11.
[0087] <Lithium Recovery> (Carbonation of the First Lithium Salt Aqueous Solution) In the lithium recovery methods 1 to 12 of the present invention, as a lithium recovery process, for example, a carbonation process (step 6a) may be included, in which the first lithium salt aqueous solution obtained in the separation process is carbonated to obtain lithium carbonate. The lithium recovery method 13 of the present invention includes the carbonation process ( Fig.13In the carbonation step, at least one alkali metal carbonate (excluding lithium carbonate) selected from the group consisting of sodium carbonate and potassium carbonate obtained in the carbon dioxide absorption step (step 8) may be added to the first lithium salt aqueous solution. The carbon dioxide absorption step is to allow the aqueous solution 4 obtained in the second membrane electrolysis step described later and containing at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to absorb carbon dioxide.
[0088] The alkali metal of the alkali metal carbonate preferably includes at least one selected from the group consisting of sodium, potassium, rubidium, cesium and francium. The alkali metal more preferably includes at least one selected from the group consisting of sodium and potassium, further preferably at least one selected from the group consisting of sodium and potassium, and particularly preferably sodium.
[0089] (First membrane electrolysis step) In the lithium recovery method 1 to 12 of the present invention ( Fig.14 ) and 14( Figure 1 5), as another lithium recovery process, for example, including a first membrane electrolysis process ( Fig.14 Step 6b Fig.15 In step 6), the first lithium salt aqueous solution obtained in the above separation step and subjected to at least one of the group consisting of the above pH adjustment step (step 5) and the above first concentration step (step E) as needed is subjected to membrane electrolysis using an ion exchange membrane to obtain a lithium hydroxide aqueous solution.
[0090] You can use, for example Fig.16 The membrane electrolysis cell 11 shown performs the above-mentioned first membrane electrolysis step. The membrane electrolyzer 11 has an anode plate 12 on one inner side surface and a cathode plate 13 on the inner side surface opposite to the anode plate 12. The anode plate 12 is connected to an anode 14 of a power source, and the cathode plate 13 is connected to a cathode 15 of a power source. In addition, the membrane electrolyzer 11 is divided into an anode chamber 17 having the anode plate 12 and a cathode chamber 18 having the cathode plate 13 by an ion exchange membrane 16.
[0091] In the membrane electrolyzer 11, when the lithium salt aqueous solution containing lithium chloride is supplied to the anode chamber 17 for electrolysis, chloride ions generate chlorine gas (C12) on the anode plate 12. Meanwhile, lithium ions move to the cathode chamber 18 via the ion exchange membrane 16.
[0092] In the cathode chamber 18, water (H2O) is ionized into hydroxide ions (OH-) and hydrogen ions (H+), and the hydrogen ions generate hydrogen gas (H2) on the cathode plate 13. On the other hand, lithium hydroxide aqueous solution is generated from the hydroxide ions and lithium ions.
[0093] The electricity required for the above-mentioned first membrane electrolysis process preferably includes electricity obtained from renewable energy, more preferably includes at least one selected from the group consisting of solar power generation, wind power generation and hydropower generation, further preferably includes electricity obtained from renewable energy, and particularly preferably includes at least one selected from the group consisting of solar power generation, wind power generation and hydropower generation.
[0094] Hydrogen (H2) generated in the first membrane electrolysis step can be reacted with chlorine (C12) to produce hydrochloric acid. Fig.16 Although not shown, when the lithium chloride aqueous solution contains sulfate ions, sulfuric acid can be obtained in the anode chamber 17. When the lithium chloride aqueous solution contains nitrate ions, nitric acid can be obtained in the anode chamber 17. That is, the inorganic acid 5 can be obtained in the first membrane electrolysis step, and the inorganic acid 5 can be used for at least one of the dissolution of the active material powder 1 in step 1 and the pH adjustment in step C.
[0095] (Separation of lithium hydroxide monohydrate) The lithium recovery methods 1 to 12 and 14 of the present invention may include a crystallization step (step F), wherein the lithium hydroxide aqueous solution obtained in the first membrane electrolysis step is evaporated and concentrated to crystallize lithium hydroxide monohydrate 3. (Separation of lithium carbonate) The lithium recovery methods 1 to 12 and 14 of the present invention may also include a carbonation step (step G), in which carbon dioxide is blown into the lithium hydroxide aqueous solution obtained in the first membrane electrolysis step to generate lithium carbonate 6.
[0096] <Second membrane electrolysis step> The lithium recovery methods 1 to 10 and 12 to 14 of the present invention may include a second membrane electrolysis step (step 7), using an ion exchange membrane to electrolyze the brine solution obtained from the above separation step, which contains at least one selected from the group consisting of sodium chloride and potassium chloride, to obtain an alkali metal hydroxide aqueous solution. The lithium recovery method 11 of the present invention includes the above second membrane electrolysis step. For example, Fig.17 The membrane electrolysis cell 21 shown carries out the above-mentioned second membrane electrolysis step.
[0097] The membrane electrolyzer 21 has an anode plate 22 on one inner side surface and a cathode plate 23 on the inner side surface opposite to the anode plate 22. The anode plate 22 is connected to an anode 24 of a power source, and the cathode plate 23 is connected to a cathode 25 of a power source. In addition, the membrane electrolyzer 21 is divided into an anode chamber 27 having the anode plate 22 and a cathode chamber 28 having the cathode plate 23 by an ion exchange membrane 26.
[0098] In the membrane electrolyzer 21, when a brine solution of at least one selected from the group consisting of sodium and potassium is supplied to the anode chamber 27 to perform membrane electrolysis, chloride ions generate chlorine gas (C12) on the anode plate 22. On the other hand, at least one alkali metal ion selected from the group consisting of sodium ions and potassium ions moves to the cathode chamber 28 via the ion exchange membrane 26.
[0099] In the cathode chamber 28, water (H2O) is ionized into hydroxide ions (OH - ) and hydrogen ions (H + ), hydrogen ions generate hydrogen gas (H2) on the cathode plate 23, and on the other hand, an alkali metal aqueous solution 4 in which at least one selected from the group consisting of sodium hydroxide and potassium hydroxide is dissolved is generated by hydroxide ions and at least one selected from the group consisting of sodium ions and potassium ions.
[0100] The electricity required for the above-mentioned second membrane electrolysis process preferably includes electricity obtained from renewable energy, more preferably includes at least one selected from the group consisting of solar power generation, wind power generation and hydropower generation, further preferably includes electricity obtained from renewable energy, and particularly preferably includes at least one selected from the group consisting of solar power generation, wind power generation and hydropower generation.
[0101] In the case where the salt solution of at least one selected from the group consisting of sodium and potassium contains chloride ions, the hydrogen (H2) generated in the second membrane electrolysis step can be reacted with chlorine (Cl2) to obtain hydrochloric acid. In the case where the salt solution of at least one selected from the group consisting of sodium and potassium contains sulfate ions, sulfuric acid can be obtained in the anode chamber 27. In the case where the salt solution of at least one selected from the group consisting of sodium and potassium contains nitrate ions, nitric acid can be obtained in the anode chamber 27. That is, the inorganic acid 5 can be obtained in the second membrane electrolysis step, and the inorganic acid 5 is used for at least one selected from the group consisting of dissolving the active material powder 1 in step 1 and adjusting the pH in step C.
[0102] The lithium recovery methods 1 to 10 and 12 to 14 of the present invention may include a carbon dioxide absorption step (step 8), wherein the alkali metal hydroxide aqueous solution 4 obtained by the second membrane electrolysis step and dissolved with at least one selected from the group consisting of sodium hydroxide and potassium hydroxide absorbs carbon dioxide. In addition, the lithium recovery method 11 of the present invention includes the carbon dioxide absorption step (step 8). At least one alkali metal carbonate 6 selected from the group consisting of sodium carbonate and potassium carbonate generated in the carbon dioxide absorption step can be used in the carbonation step (step 6a).
[0103] The alkali metal hydroxide aqueous solution 4 generated in the second membrane electrolysis step may be reused in at least one step selected from the group consisting of the alkali metal hydroxide adding step, the extraction step, the separation step using the lithium phosphate method, and the separation step using the solvent extraction method.
[0104] In the second membrane electrolysis step, the brine solution of at least one selected from the group consisting of sodium and potassium is subjected to membrane electrolysis, resulting in a brine solution of at least one selected from the group consisting of sodium and potassium that is more dilute than the brine solution of at least one selected from the group consisting of sodium and potassium. Therefore, the lithium recovery methods 1 to 14 of the present invention may include a concentration step (step 9), concentrating the dilute brine solution of at least one selected from the group consisting of sodium and potassium, and adding it to the brine solution of at least one selected from the group consisting of sodium and potassium obtained in the separation step. The concentration step can be performed using, for example, evaporation concentration, reverse osmosis membrane (RO membrane), etc. Example
[0105] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited thereto.
[0106] In the Examples, various physical properties were measured or calculated as follows. <Metal Content in Mixed Salt Solution of Lithium and Sodium, Impurity Content in Lithium Carbonate> The metal content in the mixed salt solution of lithium and sodium and the impurity content in lithium carbonate were measured by inductively coupled plasma optical emission spectroscopy (ICP-OES) using Optima 8300 manufactured by PerkinElmer.
[0107] Example 1 A used lithium-ion battery whose life as a battery product has been exhausted is subjected to a discharge treatment to discharge all the residual charge. Then, the waste lithium-ion battery is subjected to a heat treatment (roasting), crushed with a hammer mill, and the shell, collector, etc. constituting the waste lithium-ion battery are sieved to obtain an active material powder. 500g of the active material powder is dissolved in 3L6mol / L hydrochloric acid, and 2.8L 2mol / L sodium hydroxide aqueous solution is added to the obtained solution to neutralize the solution. 5.8L of the neutralized solution is mixed with 5.8L of bis(2,4,4-trimethylpentyl)phosphinic acid (Cyanex272, the diluent is kerosene) as an extractant to perform solvent extraction on cobalt. 5mol / L sodium hydroxide aqueous solution is added to the mixed solution, and the pH is adjusted to 4 to obtain a cobalt-containing organic phase and a first extraction residue. After washing the cobalt-containing organic phase with dilute sulfuric acid, 1.5mol / L sulfuric acid is used to strip to obtain a cobalt sulfate solution. Nickel was extracted from the first raffinate using the same organic solvent as that used in the cobalt extraction step, to obtain a mixed salt solution of lithium and sodium as the raffinate. The aqueous solution contained 3.5 g / L of lithium and 38.2 g / L of sodium.
[0108] 187g of aluminum phosphate was added to 8.3L of the above aqueous solution, followed by sodium hydroxide, and the pH of the above aqueous solution was adjusted to 10.5, and the reaction was carried out for 2 hours to obtain white slurry A. Then, the white slurry A was filtered and washed to obtain 614g of white filter cake A with a water content of 55%. The white filter cake A was suspended in 300mL of pure water, 35% by mass of hydrochloric acid was added, the pH of the suspension was adjusted to 2.5, the suspension was heated to 60°C and reacted for 6 hours to obtain white slurry B. The white slurry B was filtered and washed to obtain 467g of white filter cake B with a water content of 60%, and a total of 1060mL of filtrate and washing water. To the filtrate obtained by adding sodium hydroxide to the above 1060mL filtrate and washing water and adjusting the pH to 7 and filtering, 680g of 35% by mass of sodium carbonate aqueous solution was added, heated to 60°C, and reacted for 1 hour. The obtained solid component was filtered and washed to obtain hydrous lithium carbonate. The aqueous lithium carbonate was dried at 500° C. for 4 hours to obtain 129 g of lithium carbonate. The recovery rate of lithium was 83.5%. The sodium content in the lithium carbonate was less than 200 ppm, the aluminum content was less than 10 ppm, the phosphorus content was less than 10 ppm, and the water content was less than 0.1 mass %.
[0109] 10.5 L of the filtrate and washing water (sodium chloride concentration: 98 g / L) obtained by filtering and washing the white slurry A were concentrated by evaporation and then heated at a current density of 40 A / dm using an ion exchange membrane (Nafiion N324 manufactured by Chemours). 2 、Electrode area 1.75dm 2The obtained sodium chloride aqueous solution (sodium chloride concentration of 300 g / L) was subjected to membrane electrolysis under the conditions of 1.6 kg of 21.2% by mass sodium hydroxide and 1.04 kg of 30% by mass hydrochloric acid by absorbing the generated chlorine and hydrogen in water. The sodium hydroxide generated in the membrane electrolysis step can be reused in the sodium hydroxide addition step (step 2), the extraction step (step 3) and the separation step (step 4). In addition, the hydrochloric acid synthesized in the membrane electrolysis step can be reused in the dissolution step (step 1). The current efficiency in the membrane electrolysis step is 81.5%.
[0110] Example 2 A used lithium-ion battery whose life as a battery product has been exhausted is subjected to a discharge treatment to discharge all the residual charge. Then, the waste lithium-ion battery is subjected to a heat treatment (roasting), crushed with a hammer mill, and the shell, collector, etc. constituting the waste lithium-ion battery are sieved to obtain an active material powder. 500g of the active material powder is dissolved in 3L6mol / L hydrochloric acid, and 2.8L 2mol / L sodium hydroxide aqueous solution is added to the obtained solution to neutralize the solution. 5.8L of the neutralized solution is mixed with 5.8L of bis(2,4,4-trimethylpentyl)phosphinic acid (Cyanex272, the diluent is kerosene) as an extractant to perform solvent extraction on cobalt. 5mol / L sodium hydroxide aqueous solution is added to the mixed solution, and the pH is adjusted to 4 to obtain a cobalt-containing organic phase and a first extraction residue. After washing the cobalt-containing organic phase with dilute sulfuric acid, 1.5mol / L sulfuric acid is used to strip to obtain a cobalt sulfate solution. Nickel was extracted from the first raffinate using the same organic solvent as that used in the cobalt extraction step, to obtain a mixed salt solution of lithium and sodium as the raffinate. The aqueous solution contained 3.5 g / L of lithium and 38.2 g / L of sodium.
[0111] 187 g of aluminum phosphate was added to 8.3 L of the aqueous solution, followed by sodium hydroxide, and the pH of the aqueous solution was adjusted to 10.5, and the reaction was carried out for 2 hours to obtain white slurry A. Then, the white slurry A was filtered and washed to obtain 614 g of a white filter cake A with a water content of 55%. The white filter cake A was suspended in 300 mL of pure water, 35% by mass of hydrochloric acid was added, the pH of the suspension was adjusted to 2.5, the suspension was heated to 60° C. and reacted for 6 hours to obtain white slurry B. The white slurry B was filtered and washed to obtain 467 g of a white filter cake B with a water content of 60%, and a total of 1060 mL of filtrate and washing water. The 1060 mL filtrate (filtrate 1) (lithium chloride concentration: 92 g / L) obtained by adding lithium hydroxide to the 1060 mL filtrate and washing water and adjusting the pH to 7 was concentrated using the RO membrane and then filtered. The ion exchange membrane (Nafion N324 manufactured by Chemours) was used to carry out the filtration at a current density of 40 A / dm 2 、Electrode area 0.7dm 2 The obtained lithium chloride aqueous solution (lithium chloride concentration is 200g / L) was subjected to membrane electrolysis (first membrane electrolysis step) under the conditions of , and 1100g of 6.2% by mass lithium hydroxide aqueous solution was obtained. Furthermore, the reaction product of the generated chlorine and hydrogen was absorbed by water, and 350g of 30% by mass hydrochloric acid was also obtained. The recovery rate of lithium in the above-mentioned first membrane electrolysis step was 70.3%.
[0112] 380 g of the 6.2 mass % lithium hydroxide aqueous solution was taken and 80 mass % of the aqueous solution was crystallized to obtain 19.3 g of lithium hydroxide monohydrate crystals (mass after drying). The sodium content of the lithium hydroxide monohydrate was less than 50 ppm, the aluminum content was less than 10 ppm, and the phosphorus content was less than 10 ppm.
[0113] 10.5 L of the filtrate and washing water (sodium chloride concentration: 98 g / L) obtained by filtering and washing the white slurry A were concentrated using the RO membrane and then concentrated using an ion exchange membrane (Nafion N324 manufactured by Chemours) at a current density of 40 A / dm 2 、Electrode area 1.75dm 2 The obtained sodium chloride aqueous solution (sodium chloride concentration of 300 g / L) was subjected to membrane electrolysis under the conditions of 1.6 kg of 21.2% by mass sodium hydroxide and 1.04 kg of 30% by mass hydrochloric acid was obtained by absorbing the generated chlorine and hydrogen reactants into water. The sodium hydroxide generated in the membrane electrolysis step can be reused in the sodium hydroxide addition step (step 2), the extraction step (step 3) and the separation step (step 4). In addition, the hydrochloric acid synthesized in the membrane electrolysis step can be reused in the dissolution step (step 1). The current efficiency in the membrane electrolysis step is 81.5%.
[0114] In Examples 1 and 2, it is known that the inorganic acid and alkali used can be regenerated and reused. In addition, it is also known that the purity of lithium carbonate and the recovery rate of lithium obtained in the final stage of recovering lithium from waste lithium-ion batteries are very high.
[0115] In the lithium recovery methods 1 to 14 of the present invention, at least one of sodium hydroxide and potassium hydroxide can be directly obtained in the second membrane electrolysis step using the ion exchange membrane of the alkali mixed salt solution. The inorganic acid and alkali generated in the second membrane electrolysis step can be recycled in the recovery method of the present invention, so a closed-loop recycling process can be achieved. In addition, the lithium recovery methods 1 to 14 of the present invention can recycle inorganic acids and alkalis, so compared with the previous situation of purchasing inorganic acids and alkalis from outside, the emission of carbon dioxide generated in the logistics process of inorganic acids and alkalis can be reduced. [Explanation of symbols]
[0116] 1: active material powder; 2: precipitate or metal sulfate aqueous solution; 3: lithium carbonate or lithium hydroxide monohydrate; 4: sodium hydroxide aqueous solution; 5: inorganic acid; 6: sodium carbonate or lithium carbonate; 11, 21: membrane electrolyzer; 12, 22: anode plate; 13, 23: cathode plate; 14, 24: anode; 15, 25: cathode; 16, 26: ion exchange membrane; 17, 27: anode chamber; 18, 28: cathode chamber.
Claims
1. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; an alkali metal hydroxide re-addition step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the neutralization step; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt aqueous solution obtained in the alkali metal hydroxide re-addition step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
2. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; A manganese extraction step, in which an organic phosphorus compound extraction solvent is added to the solution A to extract and separate manganese, and obtain a solution B; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution B to extract and separate cobalt, and obtain a solution C; A nickel extraction step, adding an organic phosphorus compound extraction solvent to the solution C to extract and separate nickel; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the nickel extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
3. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution A to extract and separate manganese, and obtain a solution D; A nickel extraction step, adding a hydroxamic extraction solvent to the solution D to extract and separate nickel, and obtaining a solution E; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution E to extract and separate cobalt; A separation step of separating a lithium salt and at least one salt selected from sodium and potassium from the alkaline mixed salt solution obtained in the cobalt extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
4. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; a cobalt extraction step, adding an organic amine compound extraction solvent to the solution A to extract and separate cobalt, and obtain a solution F; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution F to extract and separate manganese, and obtain a solution G; A nickel extraction step, adding an organic phosphorus compound extraction solvent to the solution G to extract and separate nickel, and obtain a first lithium salt aqueous solution; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the nickel extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
5. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; a cobalt extraction step, adding an organic amine compound extraction solvent to the solution A to extract and separate cobalt, and obtaining a solution H; A nickel extraction step, adding a hydroxamic extraction solvent to the solution H to extract and separate nickel, and obtaining a solution I; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution I to extract and separate manganese, and obtain a first lithium salt aqueous solution; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the manganese extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
6. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; A nickel extraction step, adding a hydroxamic extraction solvent to the solution A to extract and separate nickel, and obtaining a solution J; a manganese extraction step, in which an organic phosphorus compound extraction solvent is added to the solution J to extract and separate manganese, thereby obtaining a solution K; a cobalt extraction step, adding an organic phosphorus compound extraction solvent to the solution K to extract and separate cobalt, and obtain a first lithium salt aqueous solution; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the cobalt extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
7. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solid-liquid separation step of separating the insoluble matter obtained in the neutralization step from the solution A; A nickel extraction step, adding a hydroxamic extraction solvent to the solution A to extract and separate nickel, and obtaining a solution L; a cobalt extraction step, in which an organic amine compound extraction solvent is added to the solution L to extract and separate cobalt, and obtain a solution M; a manganese extraction step, adding an organic phosphorus compound extraction solvent to the solution M to extract and separate manganese, and obtain a first lithium salt aqueous solution; A separation step of separating the lithium salt and at least one salt selected from sodium and potassium from the alkaline mixed salt solution obtained in the manganese extraction step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
8. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of separating at least one metal other than lithium from the metals contained in the active material powder from the solution obtained in the neutralization step by extraction with an organic solvent, and obtaining an alkaline mixed salt solution as a residual liquid of the solvent extraction; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
9. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of extracting at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction using an organic solvent; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; as well as a lithium recovery step of recovering lithium from the first lithium salt aqueous solution obtained in the separation step, In the solvent extraction step, an alkali-containing organic solvent obtained by mixing an aqueous solution containing at least one selected from the group consisting of sodium hydroxide and potassium hydroxide with the organic solvent and then subjecting the mixture to oil-water separation is mixed with the solution obtained in the neutralization step.
10. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a metal sulfide removal step of mixing the solution obtained in the neutralization step with a sulfide in a pH range of 2 to 6 to generate a sulfide of at least one metal selected from the group consisting of copper, cadmium, lead, and mercury, and removing the metal sulfide; a separation step of separating a lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the metal sulfide removal step; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
11. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of extracting at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction using an organic solvent; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; a second membrane electrolysis step of performing membrane electrolysis on the aqueous salt solution of at least one selected from the group consisting of sodium and potassium obtained in the separation step using an ion exchange membrane to obtain an aqueous alkali metal hydroxide solution; a carbonation step of carbonating a portion of the alkali metal hydroxide aqueous solution; and a lithium recovery step of recovering lithium from the first lithium salt aqueous solution obtained in the separation step, The alkali metal hydroxide aqueous solution obtained in the second membrane electrolysis step is reused in at least one step selected from the group consisting of the neutralization step, the solvent extraction step and the separation step, At least one selected from the group consisting of an inorganic acid obtained by recovering the gas generated in the second membrane electrolysis step and an inorganic acid obtained in the anode chamber of the second membrane electrolysis step is reused in the dissolution step.
12. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of extracting at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction using an organic solvent; a nickel removal step of mixing the first alkaline mixed salt solution obtained in the solvent extraction step with an alkali to remove nickel contained in the first alkaline mixed salt solution to obtain a second alkaline mixed salt solution; A separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the second alkaline mixed salt solution; as well as The lithium recovery step recovers lithium from the first lithium salt aqueous solution obtained in the separation step.
13. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of extracting at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction using an organic solvent; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; as well as The carbonation step is to carbonate the first lithium salt aqueous solution obtained in the separation step to obtain lithium carbonate.
14. A method for recovering lithium from waste lithium-ion batteries, comprising: A dissolution step, in which active material powder obtained by pre-treating waste lithium-ion batteries is dissolved using an inorganic acid; a neutralization step of adding at least one selected from the group consisting of sodium hydroxide and potassium hydroxide to the solution obtained in the dissolving step; a solvent extraction step of extracting at least one selected from the group consisting of iron, aluminum, manganese, cobalt and nickel contained in the active material powder from the solution obtained in the neutralization step by solvent extraction using an organic solvent; a separation step of separating the lithium salt and at least one salt selected from the group consisting of sodium and potassium from the alkaline mixed salt solution obtained in the solvent extraction step; as well as In the first membrane electrolysis step, the first lithium salt aqueous solution obtained in the separation step is subjected to membrane electrolysis using an ion exchange membrane to obtain a lithium hydroxide aqueous solution.
15. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 10 and 12 to 14, further comprising a second membrane electrolysis step, in which the brine solution of at least one selected from the group consisting of sodium and potassium obtained in the separation step is subjected to membrane electrolysis using an ion exchange membrane to obtain an alkali metal hydroxide aqueous solution.
16. The method for recovering lithium from waste lithium-ion batteries according to claim 15, wherein: The alkali metal hydroxide aqueous solution obtained in the second membrane electrolysis step is reused in at least one step selected from the group consisting of the neutralization step, the solvent extraction step, and the separation step.
17. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 12, wherein: The lithium recovery step includes a carbonation step, in which the first lithium salt aqueous solution obtained in the separation step is carbonated to obtain lithium carbonate.
18. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 12, wherein: The lithium recovery process also includes a first membrane electrolysis process, in which the first lithium salt aqueous solution obtained in the separation process is subjected to membrane electrolysis using an ion exchange membrane to obtain a lithium hydroxide aqueous solution, an acid, and a second lithium salt aqueous solution that is more diluted than the first lithium salt aqueous solution.
19. The method for recovering lithium from waste lithium-ion batteries according to claim 18, wherein: The second lithium salt aqueous solution is concentrated and added to the first lithium salt aqueous solution.
20. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 14, wherein: The inorganic acid includes at least one selected from the group consisting of hydrochloric acid, sulfuric acid, and nitric acid.
21. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 14, wherein: The inorganic acid includes hydrochloric acid.
22. The method for recovering lithium from waste lithium-ion batteries according to any one of claims 1 to 14, wherein: Chlorine and hydrogen obtained by membrane electrolysis of the first lithium salt aqueous solution using an ion exchange membrane are reacted, and the generated hydrochloric acid is used as the inorganic acid.
23. The method for recovering lithium from waste lithium-ion batteries according to claim 14, wherein: The electric power used in the first membrane electrolysis step includes electric power obtained from renewable energy.
24. The method for recovering lithium from waste lithium-ion batteries according to claim 18, wherein: The electric power used in the first membrane electrolysis step includes electric power obtained from renewable energy.
25. The method for recovering lithium from waste lithium-ion batteries according to claim 11, wherein: The electric power used in the second membrane electrolysis step includes electric power obtained from renewable energy.
26. The method for recovering lithium from waste lithium-ion batteries according to claim 15, wherein: The electric power used in the second membrane electrolysis step includes electric power obtained from renewable energy.
27. The method for recovering lithium from waste lithium-ion batteries according to claim 23, wherein: The electric power obtained from renewable energy includes electric power obtained from at least one selected from the group consisting of solar power generation, wind power generation and hydroelectric power generation.
28. The method for recovering lithium from waste lithium-ion batteries according to claim 24, wherein: The electric power obtained from renewable energy includes electric power obtained from at least one selected from the group consisting of solar power generation, wind power generation and hydroelectric power generation.
29. The method for recovering lithium from waste lithium-ion batteries according to claim 25, wherein: The electric power obtained from renewable energy includes electric power obtained from at least one selected from the group consisting of solar power generation, wind power generation and hydropower generation.
30. The method for recovering lithium from waste lithium-ion batteries according to claim 26, wherein: The electric power obtained from renewable energy includes electric power obtained from at least one selected from the group consisting of solar power generation, wind power generation and hydroelectric power generation.
31. The method for recovering lithium from waste lithium-ion batteries according to claim 13 or 14, wherein: The separation step is performed by at least one method selected from the group consisting of a lithium phosphate method, an evaporation concentration method, and a solvent extraction method.
32. The method for recovering lithium from waste lithium-ion batteries according to claim 13 or 14, further comprising: A second membrane electrolysis step, in which the brine solution of at least one selected from the group consisting of sodium and potassium obtained from the separation step is subjected to membrane electrolysis using an ion exchange membrane to obtain an alkali metal hydroxide aqueous solution; the brine solution of at least one selected from the group consisting of sodium and potassium is concentrated, and in the second electrolysis step, the concentrated brine solution of at least one selected from the group consisting of sodium and potassium is electrolyzed.