Prism sheet and active energy ray-curable composition for prism sheet
By using an active energy ray curable composition containing high content of inorganic nanoparticles in a liquid crystal display device, combining a transparent base material layer and a fine concave and concave structure layer, the problem of reducing the softness of the high refractive index is solved, and the prism sheet is realized Taking into account both wear resistance and high refractive index.
Patent Information
- Application Number
- CN202380033211.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-26
AI Technical Summary
In the liquid crystal display device, existing materials with high refractive index tend to reduce the flexibility of the resin cured substance, which in turn leads to defects in concave and convex shapes, making it difficult to take into account both wear resistance and high refractive index.
Using an active energy ray curable composition containing more than 40% of inorganic nanoparticles, the indentation depth of the maximum test force is more than 8 μm and the elastic deformation power is more than 50%, combined with a transparent substrate layer and a fine concave convexity. A structural layer was used to prepare a prism sheet that was resistant to wear and high refractive index.
It achieves good wear resistance and high refractive index, ensuring that the prism sheet is not prone to defects during use, and maintains high refractive index performance.
Smart Images

Figure CN119032302A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a prism sheet used in displays such as liquid crystal display devices and an active energy ray-curable composition for the prism sheet.
[0002] This case claims priority based on Japanese Tokugan Application No. 2022-073693 filed in Japan on April 27, 2022, and its contents are cited herein. Background Art
[0003] In recent years, optical sheets with functions such as improving brightness and expanding viewing angles have been used in displays such as liquid crystal display devices. Such optical sheets usually have a substrate and an optical functional layer having a fine concave-convex structure on the substrate, and modulate light through geometric optical effects such as refraction in the concave-convex shape to exhibit the desired function. Such concave-convex shapes are mainly manufactured by a method of shaping a resin material using a mold, so the material used in the optical functional layer is required to be solvent-free and low-viscosity.
[0004] In addition, among the above optical sheets, for example, a prism sheet has a sharp convex shape, and thus is easily damaged by friction with adjacent members, etc. In the case of such a prism sheet, abrasion resistance is particularly required.
[0005] On the other hand, with the thinning of displays and the reduction of power consumption, the materials used in the optical functional layer are required to have a high refractive index. In order to cope with this, some people have proposed using a high refractive index resin or adding organic or inorganic high refractive index particles (for example, Patent Documents 1 and 2).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2020 / 250721
[0009] Patent Document 2: Japanese Patent Application Publication No. 2013-249439 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] However, materials with a high refractive index generally reduce the flexibility of the cured resin, which makes it easy to cause defects in the concavo-convex shape. Therefore, a material with good wear resistance and a high refractive index is required.
[0012] The present invention is completed to solve the above-mentioned problems, and its purpose is to use a flat indenter to evaluate the mechanical properties of the convex portion of a prism sheet, and as a result, achieve a balance between good wear resistance and high refractive index through a material with certain parameters.
[0013] Solutions for solving problems
[0014] The present disclosure includes the following embodiments.
[0015] [1] A prism sheet comprising a fine concavo-convex structure layer and a transparent base layer, wherein the fine concavo-convex structure layer is a cured product of an active energy ray-curable composition,
[0016] The active energy ray-curable composition contains 40% by mass or more of inorganic nanoparticles,
[0017] The fine concavo-convex structure layer has a fine concavo-convex structure with a period of 10 to 100 μm on the surface.
[0018] The indentation depth (hmax) of the maximum test force of the fine concavo-convex structure layer is 8 μm or more, and the elastic deformation power (nIT) is 50% or more.
[0019] The indentation depth (hmax) and elastic deformation power (nIT) at the maximum test force described above were obtained under the following measurement conditions.
[0020] Indenter: 100μm×100μm flat indenter
[0021] Compressive force of flat indenter per second: 20~60mN
[0022] Maximum compression force: 500mN
[0023] Stop time of maximum compression force: 5 to 10 seconds
[0024] [2] The prism sheet according to [1], wherein the maximum point displacement in a tear test of a test piece composed of a cured product of the active energy ray-curable composition is 2.1% or more.
[0025] In addition, the above-mentioned tear test was performed in accordance with JIS-K-7128-3 under the following measurement conditions.
[0026] Test piece shape: Right-angle tear test piece described in JIS-K-7128-3
[0027] Thickness of the test piece: 200±50μm (measured value of each test piece)
[0028] Preparation of the above test piece: Made by punching
[0029] Distance between fixtures: 56mm
[0030] Test environment: 23℃×50%RH
[0031] Test speed: 500mm / min
[0032] [3] The prism sheet according to [1] or [2], wherein the inorganic nanoparticles are zirconium oxide.
[0033] [4] The prism sheet according to any one of [1] to [3], wherein the active energy ray-curable composition contains a (meth)acrylate compound.
[0034] [5] The prism sheet according to any one of [1] to [4], wherein the active energy ray-curable composition contains a surface conditioner in a range of 0.1 to 1.5 parts by mass.
[0035] [6] The prism sheet according to [5], wherein the surface conditioning agent contains silicon.
[0036] [7] An active energy ray-curable composition for a prism sheet, comprising inorganic nanoparticles and a (meth)acrylate compound,
[0037] The active energy ray-curable composition for a prism sheet contains 40% by mass or more of the inorganic nanoparticles.
[0038] The standard prism sheet produced using the cured product of the active energy ray-curable composition for a prism sheet has an indentation depth (hmax) of 8 μm or more at the maximum test force and an elastic deformation power (nIT) of 50% or more.
[0039] In addition, the standard prism sheet has a transparent substrate layer and a fine concavo-convex structure layer.
[0040] The transparent substrate layer is polyethylene terephthalate with a thickness of 125 μm.
[0041] The fine concavoconvex structure layer has a fine concavoconvex structure with a period of 50 μm on the surface of the transparent substrate layer, the unit structure of the fine concavoconvex structure constitutes a unit prism, and the shape of the unit prism is set to be a triangular prism shape of an isosceles triangle with a height of 25 μm, a base of 50 μm, and a vertex angle of 90° in the cross-section in the thickness direction,
[0042] The unit prisms are arranged adjacent to each other at an arrangement period of 50 μm in a direction perpendicular to the ridge lines so that the ridge lines of the unit prisms are balanced with each other in a plan view of the prism sheet.
[0043] The indentation depth (hmax) and elastic deformation power (nIT) at the maximum test force described above were obtained under the following measurement conditions.
[0044] Indenter: 100μm×100μm flat indenter
[0045] Compressive force of flat indenter per second: 20~60mN
[0046] Maximum compression force: 500mN
[0047] Stop time of maximum compression force: 5 to 10 seconds
[0048] [8] The active energy ray-curable composition for a prism sheet according to [7], wherein the maximum point displacement in a tear test of a test piece composed of a cured product of the active energy ray-curable composition for a prism sheet is 2.1% or more.
[0049] In addition, the above-mentioned tear test was performed in accordance with JIS-K-7128-3 under the following measurement conditions.
[0050] Test piece shape: Right-angle tear test piece described in JIS-K-7128-3
[0051] Thickness of the test piece: 200±50μm (measured value of each test piece)
[0052] Preparation of the above test piece: Made by punching
[0053] Distance between fixtures: 56mm
[0054] Test environment: 23℃×50%RH
[0055] Test speed: 500mm / min
[0056] [9] The active energy ray-curable composition for a prism sheet according to [7] or [8], wherein the inorganic nanoparticles are zirconium oxide.
[0057]
[10] The active energy ray-curable composition for a prism sheet according to any one of [7] to [9], comprising 0.1 to 1.5 parts by mass of a surface conditioner.
[0058] Effects of the Invention
[0059] According to the present invention, a plane indenter was used to evaluate the mechanical properties of the convex portion of the prism sheet, and it was found that a material having certain parameters can achieve both good wear resistance and a high refractive index. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a schematic perspective view of an example of a prism sheet according to the present embodiment.
[0061] Figure 2 This is a schematic cross-sectional view of an example of a prism sheet according to the present embodiment.
[0062] Figure 3 This is a schematic cross-sectional view of the surface of an example of the prism sheet according to the present embodiment.
[0063] Figure 4 It is a cross-sectional view of a flat indenter used in the indentation test method of this embodiment.
[0064] Figure 5 It is a schematic diagram showing an indentation test method using a flat indenter according to the present embodiment.
[0065] Figure 6 It is a schematic diagram for explaining the measurement position of the flat indenter in the indentation test of this embodiment. DETAILED DESCRIPTION
[0066] Hereinafter, the present invention will be described in further detail. In addition, the present invention is not limited to the embodiments described below.
[0067] “~” means a value greater than or equal to the value preceding the “~” and less than or equal to the value following the “~”. “(Meth)acrylic acid” is a general term for acrylic acid and methacrylic acid, and “(meth)acrylate compound” is a general term for acrylic resin and methacrylic resin.
[0068] (Prism Sheet)
[0069] Figure 1 It is a schematic perspective view showing an example of the prism sheet 10 according to the present embodiment. Figure 2 Schematic cross-sectional view of an example of the prism sheet 10 of the present embodiment. The prism sheet 10 of the present embodiment has a fine concavo-convex structure layer and a transparent substrate layer, wherein the fine concavo-convex structure layer is a cured product of an active energy ray-curable composition. The active energy ray-curable composition contains more than 40% by mass of inorganic nanoparticles. In addition, the fine concavo-convex structure layer has a fine concavo-convex structure 2a with a period P of 10 to 100 μm on its surface.
[0070] In the indentation test using a flat indenter on the surface having the fine concave-convex structure 2a of the prism sheet 10 of the present embodiment, the indentation depth (hmax) of the maximum test force is greater than 8μm, preferably greater than 8.5μm and less than 15μm, and more preferably greater than 9μm and less than 12μm. In addition, the elastic deformation power (nIT) is greater than 50%, preferably greater than 51%, and more preferably greater than 55%. In addition, the upper limit value of the elastic deformation power (nIT) is not particularly limited, and the higher the value, the more preferred. If we have to say, from the perspective of balance with the refractive index, it is preferably greater than 51% and less than 70%, and more preferably greater than 55% and less than 65%.
[0071] The indentation depth (hmax) and elastic deformation power (nIT) at the maximum test force described above were obtained under the following measurement conditions.
[0072] Indenter: 100μm×100μm flat indenter
[0073] Compressive force of flat indenter per second: 20~60mN
[0074] Maximum compression force: 500mN
[0075] Stop time of maximum compression force: 5 to 10 seconds
[0076] The indentation test is described in detail in the examples.
[0077] The prism sheet 10 preferably includes a fine concavo-convex structure layer 2 and a transparent base material layer 4 .
[0078] 〔Micro-concave-convex structure layer〕
[0079] For the fine concavo-convex structure layer 2 of this embodiment, as an example, Figure 1 and 2 As shown, examples include, but are not limited to, a structure in which triangular pyramidal unit concave-convex structures 2a are two-dimensionally arranged on the surface of the transparent substrate layer 4. For example, with respect to the fine concave-convex structure layer 2 of the present embodiment, examples include a structure in which cones, truncated cones, or triangular, quadrangular, pentagonal, or hexagonal pyramidal or truncated pyramidal unit concave-convex structures 2a are two-dimensionally arranged on the surface of the transparent substrate layer.
[0080] The cross-sectional shape of the unit prism in the normal direction of the transparent substrate layer plane (hereinafter referred to as the "thickness direction") can be as follows: Figure 3 As shown, it is an isosceles triangle, although not shown, it can also be made into an unequal-sided triangle.
[0081] The value of the vertex angle 24a of the triangular unit prism in the cross section in the thickness direction can be expressed as Figure 3 As shown in the figure, it is 90°, but it can also be an angle other than that, and can be adjusted in the range of 40 to 120°. In addition, the value of its bottom angle 24b can be as follows: Figure 3 As shown, it is 90°, but it may be any other angle, and can be adjusted within the range of 40 to 120°.
[0082] The thickness of the fine concavo-convex structure layer 2 of the present embodiment is preferably 5 μm to 100 μm, more preferably 5 μm to 60 μm, and further preferably 10 μm to 40 μm.
[0083] <Active Energy Ray-Curable Composition>
[0084] In the tear test of the test piece composed of the cured product of the active energy ray-curable composition of the present embodiment, the maximum point displacement is preferably 2.1% or more, more preferably 2.5% or more, and further preferably 3.1% or more. In addition, it is preferably 20% or less. When the maximum point displacement is 2.1% or more, the wear resistance is excellent. When it is 20% or less, a sufficient effect can be obtained in practical use.
[0085] In addition, the above-mentioned tear test was performed in accordance with JIS-K-7128-3 under the following measurement conditions.
[0086] Test piece shape: Right-angle tear test piece described in JIS-K-7128-3
[0087] Thickness of the test piece: 200±50μm (measured value of each test piece)
[0088] Preparation of the above test piece: Made by punching
[0089] Distance between fixtures: 56mm
[0090] Test environment: 23℃×50%RH
[0091] Test speed: 500mm / min
[0092] The test is described in detail in Examples.
[0093] The active energy ray-curable composition of the present embodiment preferably contains a (meth)acrylate compound. The inorganic nanoparticles contained in the active energy ray-curable composition of the present embodiment are more preferably zirconium oxide fine particles (hereinafter, simply referred to as zirconium oxide).
[0094] The aforementioned active energy ray-curable composition containing the aforementioned zirconium oxide and the aforementioned (meth)acrylate compound is recorded as "active energy ray-curable composition for prism sheet". At this time, the indentation depth (hmax) of the maximum test force of the standard prism sheet made of the cured product of the aforementioned active energy ray-curable composition for prism sheet is 8 μm or more, preferably 8.5 μm or more and 15 μm or less, and more preferably 9 μm or more and 12 μm or less. In addition, the elastic deformation power (nIT) is 50% or more, preferably 51% or more and 70% or less, and more preferably 55% or more and 65% or less.
[0095] In addition, the standard prism sheet used to evaluate the indentation depth has a transparent substrate layer and a fine concavo-convex structure layer.
[0096] The transparent substrate layer is polyethylene terephthalate with a thickness of 125 μm.
[0097] The fine concavo-convex structure layer has a fine concavo-convex structure with a period of 50 μm on the surface of the transparent base material layer portion,
[0098] The unit structure of the fine concavoconvex structure constitutes a unit prism, and the unit prism is shaped like a triangular prism having a cross section in the thickness direction and an isosceles triangle with a height of 25 μm, a base of 50 μm, and a vertex angle of 90°.
[0099] The unit prisms are arranged adjacent to each other at an arrangement period of 50 μm in a direction perpendicular to the ridge lines so that the ridge lines of the unit prisms are balanced with each other in a plan view of the prism sheet.
[0100] The measurement conditions of the indentation depth (hmax) and elastic deformation power (nIT) of the maximum test force are the same as the measurement conditions described in the prism sheet of the present embodiment.
[0101] The method of curing the active energy ray-curable composition for a prism sheet to produce a standard prism sheet is the same as the method of producing the active energy ray-curable composition P1 obtained in the preparation example in Example 1 described later.
[0102] In this embodiment, the so-called "active energy ray" is not only an electromagnetic wave with a wavelength in the non-visible light region such as visible light, ultraviolet rays and X-rays, but also includes electron beams and particle beams such as α rays, which are collectively referred to as radiation. The aforementioned radiation has an energy quantum sufficient to cause a crosslinking reaction and / or a polymerization reaction in a molecule having an active energy ray curable group. As for the active energy ray, ultraviolet rays are preferred.
[0103] [Zirconium oxide]
[0104] As the zirconium oxide of the present embodiment, generally known ones can be used, and the shape of the particles is not particularly limited. Examples thereof include spherical, hollow, porous, rod-like, and fibrous shapes. Among these, spherical shapes are preferred.
[0105] The average primary particle size of the zirconium oxide of the present embodiment is preferably 1 to 50 nm, more preferably 1 to 30 nm. Furthermore, the crystal structure is not particularly limited, but is preferably a monoclinic system.
[0106] In addition, the average primary particle size of the present invention can be measured using a TEM (transmission electron microscope) to measure the size of the primary particles directly from an electron microscope photograph. As for the measuring method, for example, the minor axis diameter and the major axis diameter of the primary particles of each inorganic fine particle can be cited, and the average is used as the method of the average primary particle size of the primary particles.
[0107] Specific examples of the zirconium oxide according to the present embodiment include UEP-100 (manufactured by Daiichi Kisen Kogyo Co., Ltd., average primary particle size: 11 nm) and PCS (manufactured by Nippon Denko KK, average primary particle size: 20 nm).
[0108] The content of the zirconium oxide of the present embodiment in the active energy ray-curable composition is preferably 40% by mass to 90% by mass, more preferably 40% by mass to 80% by mass, and even more preferably 40% by mass to 70% by mass.
[0109] [(Meth)acrylate compound]
[0110] The (meth)acrylate compound of the present embodiment may be a monofunctional (meth)acrylate or a polyfunctional (meth)acrylate having a (meth)acryloyl group or a (meth)acryloyloxy group, which is conventionally known for forming a prism sheet. An oligomer or a prepolymer may be used as required.
[0111] Examples of the monofunctional (meth)acrylate include vinyl monomers, (meth)acrylate monomers, and (meth)acrylamide derivatives described in Patent Literature (Japanese Unexamined Patent Application Publication No. 2009-37204).
[0112] Examples of the multifunctional (meth)acrylate include difunctional (meth)acrylates and trifunctional (meth)acrylates, and examples thereof include ethylene glycol di(meth)acrylate, bisphenol A polyethoxy glycol di(meth)acrylate, and pentaerythritol tri(meth)acrylate described in the patent document (Japanese Patent Application Laid-Open No. 2009-37204).
[0113] Examples of the reactive prepolymer include epoxy (meth)acrylate, urethane (meth)acrylate, and polyester (meth)acrylate described in Patent Literature (Japanese Patent Application Laid-Open No. 2009-37204).
[0114] In a suitable form of the prism sheet of the present embodiment, the aforementioned (meth) acrylate compound preferably contains (A) a monofunctional (meth) acrylate having one active energy ray curable group (hereinafter, sometimes referred to as "(A) component".) and (B) a difunctional (meth) acrylate and / or a trifunctional (meth) acrylate having two active energy ray curable groups (hereinafter, sometimes referred to as "(B) component".). It is more preferred to contain the aforementioned (A) component, the aforementioned (B) component and the (C) initiator (hereinafter, sometimes referred to as "(C) component".). It is further preferred to contain the aforementioned (A) component, the aforementioned (B) component, the aforementioned (C) component and the (D) surface adjuster (hereinafter, sometimes referred to as "(D) component".). The total mass of (A) and (B) is preferably 50% by mass or less relative to the total solid content mass of the active energy ray curable resin composition. This is because: in this case, the fine concave-convex structure layer can exhibit the above-mentioned specific range of indentation depth and the above-mentioned specific resilience, while becoming a high refractive index.
[0115] Hereinafter, the components (A) to (D) will be described in order.
[0116] ((A) ingredient)
[0117] Component (A) is a monofunctional (meth)acrylate having one active energy ray-curable group. The monofunctional (meth)acrylate may also contain heteroatoms such as halogen atoms, sulfur atoms, oxygen atoms or nitrogen atoms. The monofunctional (meth)acrylate may also be a chain aliphatic (meth)acrylate or a cyclic alicyclic (meth)acrylate or an aromatic (meth)acrylate. For example, the monofunctional (meth)acrylate described in Patent Document 1 may be used.
[0118] (A) Component includes: n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenylphenol (EO)n (meth)acrylate, phenol (EO)n (meth)acrylate, phenoxybenzyl (meth)acrylate, biphenyl methyl (meth)acrylate, phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, morpholine (meth)acrylate, (meth)acrylate) Monofunctional (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, cyclohexylmethyl (meth)acrylate, cyclohexylethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentyloxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate.
[0119] (A) Specific examples of the component include the following monofunctional (meth)acrylate-1 to monofunctional (meth)acrylate-6 used in Examples.
[0120] Monofunctional (meth)acrylate-1: KOMERATE A011 (manufactured by Green Chemical Co., Ltd.)
[0121] Structural formula or compound name: o-phenylphenol (EO) acrylate
[0122] Monofunctional (meth)acrylate-2: Photomer 4035 (manufactured by IGM Resins Inc.)
[0123] Structural formula or compound name: Phenol (EO) acrylate
[0124] Monofunctional (meth)acrylate-3: MOMERATE A008 (manufactured by Green Chemical Co., Ltd.)
[0125] Structural formula or compound name: 3-phenoxybenzyl acrylate
[0126] Monofunctional (meth)acrylate-4: MIRAMER M1192 (manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.)
[0127] Structural formula or compound name: Biphenyl methyl acrylate
[0128] Monofunctional (meth)acrylate-5: MIRAMER M142 (manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.)
[0129] Structural formula or compound name: Phenol (EO) 2 acrylate
[0130] Monofunctional (meth)acrylate-6: MIRAMER M144 (manufactured by MIWON SPECIALTY CHEMICAL Co., LTD.)
[0131] Structural formula or compound name: Phenol (EO) 4 acrylate
[0132] The component (A) may be used alone or in combination of two or more.
[0133] The content of component (A) is preferably 20 to 50% by mass relative to the total solid content of the composition. Furthermore, the content of the aromatic ring-containing acrylate is preferably 15 to 30% by mass, more preferably 22 to 27% by mass relative to the total solid content of the composition.
[0134] The content of the compound represented by the general formula (2) is preferably 5 to 20% by mass, more preferably 5 to 15% by mass, based on the total solid content of the composition.
[0135] The total mass ((A) + (B)) of the above-mentioned component (A) and the component (B) described later is preferably 50% by mass or less, more preferably 10 to 40% by mass, relative to the total solid content mass of the composition. By making the total mass 50% by mass or less relative to the total solid content mass of the composition, the fine concavo-convex structure layer can exhibit the indentation depth within the above-mentioned specific range and the above-mentioned specific resilience, while having a high refractive index.
[0136] ((B) ingredient)
[0137] Component (B) is a multifunctional (meth)acrylate having two or more active energy ray-curable groups. It may also be a chain aliphatic or cyclic alicyclic or aromatic (meth)acrylate containing heteroatoms such as halogen atoms, sulfur atoms, oxygen atoms or nitrogen atoms, for example, the multifunctional (meth)acrylate described in Patent Document 1 may be used.
[0138] Examples of the component (B) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, tetrabutanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, glycerol di(meth)acrylate, neopentyl glycol hydroxypivalate di(meth)acrylate, caprolactone-modified hydroxypivalate neopentyl glycol di(meth)acrylate, tetrabromobisphenol A di(meth)acrylate, hydroxypivalaldehyde-modified trimethylolpropane di(meth)acrylate, bisphenol fluorene di(meth)acrylate, bisphenol fluorene (EO) n Di(meth)acrylate, bisphenol A (EO) n Di(meth)acrylate, trimethylolpropane (EO) n Polyfunctional (meth)acrylates such as tri(meth)acrylate, 1,4-cyclohexanedimethanol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerol tri(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, epoxy (meth)acrylate, urethane (meth)acrylate and polyester (meth)acrylate.
[0139] Specific examples of the component (B) include the difunctional (meth)acrylate, trifunctional (meth)acrylate-1, and trifunctional (meth)acrylate-2 used in the examples.
[0140] Difunctional (meth)acrylate: MIRAMER M2100 (manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.)
[0141] Structural formula or compound name: Bisphenol A (EO) 10 Diacrylate
[0142] Trifunctional (meth)acrylate-1: MIRAMER M3130 (manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.)
[0143] Structural formula or compound name: Trimethylolpropane (EO) 3 triacrylate
[0144] Trifunctional (meth)acrylate-2: MIRAMER M3160 (manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.)
[0145] Structural formula or compound name: Trimethylolpropane (EO) 6 triacrylate
[0146] The content of the component (B) is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, and particularly preferably 3 to 15% by mass, based on the total solid content of the composition.
[0147] From the viewpoint of sufficiently exhibiting the above-mentioned specific indentation depth (hmax) and elastic deformation power (nIT) of the maximum test force, the content of component (B) is preferably 0 to 20% by mass, more preferably 3 to 15% by mass, relative to the total solid mass of the composition.
[0148] ((C) ingredient)
[0149] The component (C) is an initiator, and is preferably a photopolymerization initiator.
[0150] Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propane-1-one, thioxanthone and thioxanthone derivatives, 2,2′-dimethoxy-1,2-diphenylethane-1-one, diphenyl(2,4,6-trimethoxybenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone.
[0151] (C) As a specific example of a component, an initiator-1 - an initiator-3 are mentioned, for example.
[0152] Initiator-1: Runtecure 1108 (manufactured by Runtec Chemical Co., Ltd.)
[0153] Structural formula or compound name: 2,4,6-trimethylbenzoyldiphenylphosphine oxide
[0154] Initiator-2: Runtecure 1104 (manufactured by Runtec Chemical Co., Ltd.)
[0155] Structural formula or compound name: 1-Hydroxycyclohexyl phenyl ketone
[0156] Initiator-3: Benzophenone (manufactured by IGM Resins Inc.)
[0157] Structural formula or compound name: Benzophenone
[0158] The content of the component (C) is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass, based on the total solid content of the composition.
[0159] ((D) ingredient)
[0160] The component (D) is a surface conditioner, preferably a silicon-based surface conditioner.
[0161] The component (D) has a function of imparting slip properties.
[0162] Specific examples of the component (D) include silicone-based surface conditioners: BYK series such as BYK-333 (manufactured by BYK Japan KK).
[0163] From the viewpoint of anti-bleeding property, the content of the component (D) is preferably 0.01 to 3% by mass, more preferably 0.2 to 1.5% by mass, based on the total solid content mass of the composition.
[0164] In the composition of the present embodiment, in addition to the above-mentioned components, phosphate esters, silane coupling agents, plasticizers, antioxidants, polymerization inhibitors, thickeners, mold release agents, antistatic agents, ultraviolet stabilizers, defoaming agents, solvents, non-reactive urethane resins such as non-reactive urethane polymers, non-reactive acrylic resins, non-reactive polyester resins, pigments, dyes, or diffusing agents may also be used in combination as needed.
[0165] The composition of the present embodiment is usually appropriately prepared so that the total amount of the essential components and components other than the essential components that form a matrix of the prism sheet after curing contained in the composition is usually 90% by mass or more relative to the total mass of the composition.
[0166] <Phosphate ester>
[0167] The phosphoric acid ester of the present embodiment is not particularly limited, and examples thereof include those having a polyester chain and those having a (meth)acryloyl group.
[0168] As those having a polyester chain, for example, DISPERBYK-110 and DISPERBYK-111 (manufactured by BYK Japan KK) can be mentioned.
[0169] In addition, as for those having a (meth)acryloyl group, for example, those represented by the following structural formula (1) can be cited. When the one represented by the following structural formula (1) is used, the obtained inorganic fine particle dispersion has excellent dispersion stability, and the curable composition containing it has a low viscosity and can form a cured coating film having high refractive index performance and excellent anti-bleeding property.
[0170]
[0171] (R 1 is a hydrogen atom or a methyl group, R 2 is an alkylene chain having 2 to 4 carbon atoms. In addition, x is an integer of 4 to 10, y is an integer greater than 1, and n is an integer of 1 to 3.
[0172] For the phosphate compound represented by the above structural formula (1), x in the formula is preferably 4 or 5, and y is preferably an integer of 2 to 7. When such a phosphate compound is used, the obtained active energy ray-curable composition has a low viscosity and can form a cured coating film having a high refractive index performance and excellent anti-bleeding properties. In addition, the dispersant represented by the above structural formula (1) may also be a mixture in which n in the formula is 1, 2 and / or 3.
[0173] The content of the phosphate compound in the active energy ray-curable composition is more preferably in the range of 5 to 40 parts by mass, and further preferably in the range of 10 to 25 parts by mass, relative to 100 parts by mass of zirconium oxide. When the content of the phosphate compound is in the range of 5 to 40 parts by mass relative to 100 parts by mass of zirconium oxide, a cured coating film having high refractive index performance and excellent bleed resistance can be formed.
[0174] <Silane coupling agent>
[0175] Examples of the silane coupling agent of the present embodiment include (meth)acryloxy-based silane coupling agents such as 3-(meth)acryloxypropyltrimethylsilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane; vinyl-based silane coupling agents such as allyltrichlorosilane, allyltriethoxysilane, allyltrimethoxysilane, diethoxymethylvinylsilane, trichlorovinylsilane, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltri(2-methoxyethoxy)silane;
[0176] Epoxy silane coupling agents such as diethoxy(glycidoxypropyl)methylsilane, 2-(3,4-ethoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane;
[0177] Styrene-based silane coupling agents such as p-phenylenedimethoxysilane;
[0178] Amino silane coupling agents such as N-2(aminoethyl)3-aminopropylmethyldimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane;
[0179] Urea-based silane coupling agents such as 3-ureidopropyltriethoxysilane;
[0180] Chloropropyl-based silane coupling agents such as 3-chloropropyltrimethoxysilane; mercapto-based silane coupling agents such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane;
[0181] Sulfide-based silane coupling agents such as bis(triethoxysilylpropyl)tetrasulfide;
[0182] Isocyanate silane coupling agents such as 3-isocyanatopropyltriethoxysilane;
[0183] Aluminum-based silane coupling agents such as acetyl alkoxy diisopropyl aluminum, etc. These silane coupling agents can be used alone or in combination of two or more. Among these, 3-(meth)acryloyloxypropyltrimethoxysilane is preferred from the perspective of good compatibility with the (meth)acryloyl-containing compound (C) described later.
[0184] The amount of the silane coupling agent used in this embodiment is preferably in the range of 10 to 30 parts by mass relative to 100 parts by mass of zirconium oxide, because the obtained active energy ray-curable composition has excellent dispersion stability, has low viscosity, and can form a cured coating film having high refractive index performance and excellent bleed resistance.
[0185] [Transparent substrate layer]
[0186] The transparent base material layer 4 of the present embodiment is a base material of the prism sheet 10 and is not particularly limited, and any transparent base material used in a conventionally known prism sheet can be used. For example, the transparent base material layer described in Patent Document 2 can be used.
[0187] The transparent base material layer 4 of the present embodiment may be appropriately selected in terms of material and thickness in consideration of required suitability such as desired transparency and mechanical strength.
[0188] The transparent base material layer 4 of the present embodiment may be a resin base material or a glass base material.
[0189] The resin material of the transparent film is preferably a (meth)acrylate compound, polycarbonate resin, vinyl chloride resin, polymethacrylimide resin, polyimide resin, polyester resin, cycloolefin polymer (COP) resin, cycloolefin copolymer (COC) resin, triacetyl cellulose (TAC) resin, or the like.
[0190] The transparent base material layer 4 of the present embodiment may be in a long strip shape or in a single sheet shape having a predetermined size.
[0191] The thickness of the transparent base material layer 4 in the present embodiment is usually preferably 50 to 500 μm, but is not limited thereto.
[0192] The light transmittance of the transparent base material layer 4 of the present embodiment is desirably 100% for installation on the front surface of a display, and preferably 85% or more.
[0193] The transparent substrate layer 4 of the present embodiment may also be subjected to conventionally known matte treatment (formation of light diffusive micro-concave and convex), antistatic treatment or antireflection treatment on its surface as required. In addition, matte treatment, antistatic treatment or antireflection treatment may be applied between the transparent resin and the substrate, and these may be freely combined for use.
[0194] [Method for manufacturing prism sheet]
[0195] The method for manufacturing the prism sheet 10 of the present embodiment is not particularly limited as long as it is a method that can obtain the above-mentioned specific indentation depth or the above-mentioned elastic deformation power, and a conventionally known method can be used.
[0196] For example, as described in the patent document (Japanese Patent Application Laid-Open No. 2009-37204), Figure 2 As shown, the composition is placed in a mold of a desired unit concave-convex shape, a transparent substrate layer is superimposed thereon, the transparent substrate layer is pressed onto the composition using a laminator or the like, and the composition is cured using ultraviolet rays or the like to form a unit concave-convex shape. Next, by peeling or removing the mold of the unit concave-convex shape, a prism sheet having an optical function display portion having a desired concave-convex shape on the transparent substrate layer can be obtained.
[0197] (Active energy ray-curable composition for prism sheet)
[0198] The active energy ray-curable composition for a prism sheet according to the present embodiment contains zirconium oxide and a (meth)acrylate compound, and is an active energy ray-curable composition for producing the prism sheet according to the present embodiment described above.
[0199] The standard prism sheet produced using the cured product of the active energy ray-curable composition for a prism sheet of the present embodiment has an indentation depth (hmax) of 8 μm or more at the maximum test force and an elastic deformation power (nIT) of 50% or more.
[0200] In addition, the standard prism sheet of this embodiment is the same as the standard prism sheet described in the prism sheet of this embodiment.
[0201] The measurement conditions of the indentation depth (hmax) and the elastic deformation power (nIT) of the maximum test force of the present embodiment are the same as the measurement conditions described in the prism sheet of the present embodiment.
[0202] In the tear test of the test piece composed of the cured product of the active energy ray-curable composition for a prism sheet of the present embodiment, the maximum point displacement is preferably 2.1% or more.
[0203] In addition, the measurement conditions of the tear test of this embodiment are the same as the measurement conditions described in the prism sheet of this embodiment.
[0204] The active energy ray-curable composition for a prism sheet of this embodiment preferably contains a surface conditioning agent, more preferably contains a surface conditioning agent in the range of 0.01 to 3 parts by mass, and further preferably contains a surface conditioning agent in the range of 0.2 to 1.5 parts by mass. The surface conditioning agent of this embodiment is the same as the surface conditioning agent described in the prism sheet of this embodiment.
[0205] Example
[0206] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited thereto.
[0207] (raw material)
[0208] Zirconia: UEP-100, manufactured by First Rare Earth Chemical Industry Co., Ltd.
[0209] Titanium oxide: P25, manufactured by NIPPON AEROSIL CO., LTD.
[0210] Phosphate ester: DISPERBYK-111, manufactured by BYK Japan KK.
[0211] Silane coupling agent: KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.
[0212] Monofunctional (meth)acrylate-1: KOMERATE A011, manufactured by Green Chemical Co., Ltd.
[0213] Monofunctional (meth)acrylate-2: Photomer 4035, manufactured by IGM Resins Inc.
[0214] Monofunctional (meth)acrylate-3: KOMERATE A008, manufactured by Green Chemical Co., Ltd.
[0215] Monofunctional (meth)acrylate-4: MIRAMER M1192, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0216] Monofunctional (meth)acrylate-5: MIRAMER M142, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0217] Monofunctional (meth)acrylate-6: MIRAMER M144, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0218] Difunctional (meth)acrylate: MIRAMER M2100, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0219] Trifunctional (meth)acrylate-1: MIRAMER M3130, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0220] Trifunctional (meth)acrylate-2: MIRAMER M3160, manufactured by MIWON SPECIALTY CHEMICAL CO., LTD.
[0221] Phthalate plasticizer: Diethylene glycol dibenzoate, manufactured by Tokyo Chemical Industry Co., Ltd.
[0222] Initiator-1: Runtecure 1108, manufactured by Runtec Chemical Co., Ltd.
[0223] Initiator-2: Runtecure 1104, manufactured by Runtec Chemical Co., Ltd.
[0224] Initiator-3: Benzophenone, manufactured by IGM Resins Inc.
[0225] Silicone surface conditioner: BYK-333, manufactured by BYK Japan KK.
[0226] HALS: TINUVIN 292, manufactured by BASF Japan
[0227] <Indentation test>
[0228] The test pieces for the indentation test were prism sheets obtained in the examples and comparative examples described later.
[0229] Figure 3 The schematic diagram of the cross section of the plane indenter used in the present embodiment is shown (the upper side is the measurement surface). In addition to using a diamond plane indenter instead of a diamond quadrangular pyramid, the indenter uses a micro hardness tester (trade name HM2000) made by FischerInstruments Co., Ltd. according to ISO 14577-1 to measure the indentation depth (hmax) and elastic deformation power (nIT) of the maximum test force.
[0230] Test conditions:
[0231] Plane size of the flat indenter: 100μm×100μm
[0232] 20~60mN per 1 second
[0233] Maximum compression force 500mN
[0234] Stop time of maximum compression force 5 to 10 seconds
[0235] F 500 / mN / 10s
[0236] C 5.0s
[0237] R 0.1mN / 10s
[0238] C2 10.0s
[0239] <Abrasion resistance>
[0240] The wear resistance of each prism sheet of the aforementioned embodiments and comparative examples was evaluated. The prism sheet was attached to a movable plate manufactured by Imoto Manufacturing in such a manner that the top of the prism sheet was facing the load-bearing part side. A PET-based diffusion film was attached to a retaining member with a diameter of 1 cm as a wear part on the load-bearing part side, and was arranged in such a manner that the base material layer of the diffusion film rubbed against the top of the prism sheet. The evaluation was carried out indoors at 23°C (humidity: 50%). A load of 300g was applied to the load-bearing part and the wear resistance tester was operated. After the movable plate was moved in one direction (moving speed: 4m / min, moving distance: 10cm, number of reciprocating times: 40 times), the degree of band damage was visually evaluated. The criteria are as follows.
[0241] The judgment criteria are shown below.
[0242] A: No obvious damage could be confirmed.
[0243] B: Thin and fine damage is visible.
[0244] C: Moderate damage is visible.
[0245] D: Deep and thick lesions are seen.
[0246] <Liquid Refractive Index>
[0247] The refractive index of the liquid was evaluated by measuring the refractive index at a temperature of 25° C. and a wavelength of 589 nm using a multi-wavelength Abbe refractometer DR-M4 (manufactured by ATAGO Co., Ltd.).
[0248] <Viscosity>
[0249] The viscosity was evaluated by measuring the viscosity at a temperature of 25° C. using an E-type rotational viscometer (“TVE-25H” manufactured by Toki Sangyo Co., Ltd.).
[0250] (evaluate)
[0251] <Tear test>
[0252] The test piece for the tear test is a cured product of the active energy ray-curable composition of the present embodiment. The curing conditions are the same as those of Example 1 described below.
[0253] The tear test was performed in accordance with JIS-K-7128-3 under the following measurement conditions.
[0254] Test piece shape: Right-angle tear test piece described in JIS-K-7128-3
[0255] Thickness of the test piece: 200±50μm (measured value of each test piece)
[0256] Preparation of the above test piece: Made by punching
[0257] Distance between fixtures: 56mm
[0258] Test environment: 23℃×50%RH
[0259] Test speed: 500mm / min
[0260] (Preparation Example 1)
[0261] Mix 51.2 parts by mass of UEP-100 as zirconium oxide, 7.7 parts by mass of DISPERBYK-111 as phosphate, 5.1 parts by mass of KBM-503 as a silane coupling agent, and 110.1 parts by mass of methyl ethyl ketone (hereinafter referred to as "MEK"). Stir for 30 minutes using a dispersing mixer to perform coarse dispersion. Then, the obtained mixed solution is dispersed using a medium-type wet disperser ("STARMILL LMZ-015" manufactured by Ashizawa Finetech Co., Ltd.) and zirconium oxide beads with a particle size of 100 μm. While confirming the particle size midway, a dispersion treatment with a residence time of 100 minutes is performed to obtain an inorganic fine particle dispersion.
[0262] In this inorganic particle dispersion, 24.0 parts by mass of Photomer 4035 as a monofunctional (meth) acrylate and 10.0 parts by mass of MIRAMER M2100 as a difunctional (meth) acrylate were added, and the volatile components were removed by decompression while heating with an evaporator. Further, 0.7 parts by mass of Runtecure 1108 as an initiator and 0.7 parts by mass of Runtecure 1104 and 0.5 parts by mass of BYK-333 as a silicon-based surface adjuster were added to prepare the active energy ray-curable composition P1 (composition P1) of the present embodiment. The liquid refractive index and viscosity of composition P1 were evaluated. In addition, a tear test of the cured product of composition P1 was performed. These results are shown in Table 1.
[0263] (Preparation Examples 2 to 6, Comparative Preparation Examples 1 to 11)
[0264] In each preparation example, except for using the components and composition ratios shown in Table 1, the same method as Preparation Example 1 was used to prepare compositions P2 to P6 and cP1 to cP11 of Preparation Examples 2 to 6 and Comparative Preparation Examples 1 to 11, respectively. The liquid refractive index and viscosity of each composition were evaluated. In addition, the tear test of the cured product of each composition was performed. The results are shown in Table 1.
[0265] [Table 1]
[0266]
[0267] (Example 1)
[0268] In being able to form Figure 1The composition P1 prepared in the above-mentioned Preparation Example 1 was dripped into a prism mold (not shown) having a concave-convex shape with linear arrangement of unit prisms as shown. Then, a polyethylene terephthalate (PET) (trade name "A4300" manufactured by Toyobo Co., Ltd.) with a thickness of 125 μm was stacked as a transparent substrate layer, and the entire surface of the PET substrate was pressed onto the composition P1 using a laminator.
[0269] Next, the prism portion having a plurality of unit prisms was cured under the following curing conditions to be integrated with the PET substrate.
[0270] Curing conditions:
[0271] Light source: UV light
[0272] Irradiation device: High-pressure mercury lamp (manufactured by GS Yuasa Lighting Service Co., Ltd.)
[0273] Irradiation light: 780mJ / cm 2 .
[0274] Thereafter, the prism sheet S1 is obtained by peeling off the prism mold.
[0275] Here, the shape of the unit prism is a triangular prism whose cross section in the thickness direction is an isosceles triangle with a height of 25 μm, a base of 50 μm, and a vertex angle of 90°. In addition, in the fine concave-convex structure layer, a plurality of unit prisms are arranged adjacent to each other at an arrangement period of 50 μm in a direction orthogonal to the ridge line in such a way that the ridge lines of the unit prisms are balanced with each other.
[0276] The prism sheet S1 was subjected to an indentation test and an abrasion resistance test.
[0277] (Examples 2 to 6 and Comparative Examples 1 to 11)
[0278] In Example 1, except that composition P1 was replaced with compositions P2 to P6 and cP1 to cP11 as shown in Table 1, the same procedure as in Example 1 was carried out to obtain prism sheets S1 to S6 and cS1 to cS11.
[0279] The results are shown in Table 2.
[0280] [Table 2]
[0281]
[0282] (Research)
[0283] As shown in Tables 1 and 2, for a prism sheet containing 40% or more of zirconium oxide in the form of inorganic nanoparticles, having an nIT of 50% or more and an hmax of 8μm or more, it is possible to achieve both high refractive index and wear resistance. Generally, if inorganic nanoparticles are added, the flexibility will decrease, and the crosslinking density of the resin will decrease, so the wear resistance will deteriorate. However, by making the nIT more than 50% and the hmax more than 8μm, a good result of wear resistance can be obtained. It is believed that this is because in a prism sheet with a large hmax, the top of the prism will be deformed due to the load during the wear test, and the contact area with the wear cloth will increase, thereby dispersing the load. In addition, in a composition with a large nIT, the power of elastic deformation is greater than the power of plastic deformation, so even if a load is applied to cause it to deform, it will still return to its original shape when the load is removed.
[0284] In addition, the prism made from the composition with a maximum point displacement of 2.1% or more in the tear test of the cured product showed good abrasion resistance. It is believed that this is because if the maximum point displacement of the tear test is large, even if the top of the prism is stretched due to friction during the abrasion test, it will still deform without causing defects or breaks.
[0285] The wear resistance of these prism sheets can be further improved by adding a silicon-based surface conditioning agent to impart sliding properties.
[0286] Description of Reference Numerals
[0287] 2: Micro-concave-convex structure layer (prism layer)
[0288] 2a: Unit concave-convex structure (unit prism)
[0289] 4: Transparent substrate layer
[0290] 10: Prism
[0291] 24a: Top Angle
[0292] 24b: Bottom Corner
[0293] 24: concave part
[0294] 50: Flat pressure head
[0295] 52: Measurement surface
Claims
1. A prism sheet comprising a fine concavo-convex structure layer and a transparent base layer, wherein the fine concavo-convex structure layer is a cured product of an active energy ray-curable composition. The active energy ray-curable composition contains 40% by mass or more of inorganic nanoparticles, The fine concavo-convex structure layer has a fine concavo-convex structure with a period of 10 to 100 μm on the surface. The indentation depth (hmax) of the maximum test force of the fine concavo-convex structure layer is greater than 8 μm, and the elastic deformation power (nIT) is greater than 50%. In addition, the indentation depth (hmax) and elastic deformation power (nIT) of the maximum test force are obtained under the following measurement conditions: Indenter: 100μm×100μm flat indenter Compression force of flat indenter per second: 20-60 mN Maximum compression force: 500mN Stop time of maximum compression force: 5 to 10 seconds.
2. The prism sheet according to claim 1, wherein the maximum point displacement in a tear test of a test piece composed of a cured product of the active energy ray-curable composition is 2.1% or more, The tear test was conducted in accordance with JIS-K-7128-3 under the following measurement conditions: Test piece shape: Right-angle tear test piece described in JIS-K-7128-3 Thickness of the test piece: 200±50μm (measured value of each test piece) Preparation of the test piece: Made by punching Distance between fixtures: 56mm Test environment: 23°C × 50% RH Test speed: 500mm / min.
3. The prism sheet according to claim 1 or 2, wherein: The inorganic nanoparticles are zirconium oxide.
4. The prism sheet according to claim 1 or 2, wherein: The active energy ray-curable composition contains a (meth)acrylate compound.
5. The prism sheet according to claim 1 or 2, wherein: The active energy ray-curable composition contains a surface conditioner in the range of 0.1 to 1.5 parts by mass.
6. The prism sheet according to claim 5, wherein The surface conditioner contains silicon.
7. An active energy ray-curable composition for a prism sheet, comprising inorganic nanoparticles and a (meth)acrylate compound. The active energy ray-curable composition for a prism sheet contains 40% by mass or more of the inorganic nanoparticles. The standard prism sheet produced by using the cured product of the active energy ray-curable composition for a prism sheet has an indentation depth (hmax) of 8 μm or more under the maximum test force and an elastic deformation power (nIT) of 50% or more. In addition, the standard prism sheet has a transparent base material layer and a fine concavo-convex structure layer. The transparent substrate layer is polyethylene terephthalate with a thickness of 125 μm. The fine concavo-convex structure layer has a fine concavo-convex structure with a period of 50 μm on the surface of the transparent base material layer, and the unit structure of the fine concavo-convex structure constitutes a unit prism, and the unit prism is shaped into a triangular prism with a height of 25 μm, a base of 50 μm, and a vertex angle of 90° in the cross section in the thickness direction. The unit prisms are arranged adjacent to each other in a direction perpendicular to the ridge lines with an arrangement period of 50 μm in a manner such that the ridge lines of the unit prisms are balanced with each other in a plan view of the prism sheet. The indentation depth (hmax) and elastic deformation power (nIT) of the maximum test force are obtained under the following test conditions: Indenter: 100μm×100μm flat indenter Compression force of flat indenter per second: 20-60 mN Maximum compression force: 500mN Stop time of maximum compression force: 5 to 10 seconds.
8. The active energy ray-curable composition for a prism sheet according to claim 7, wherein a maximum point displacement in a tear test of a test piece composed of a cured product of the active energy ray-curable composition for a prism sheet is 2.1% or more, The tear test was conducted in accordance with JIS-K-7128-3 under the following measurement conditions: Test piece shape: Right-angle tear test piece described in JIS-K-7128-3 Thickness of the test piece: 200±50μm (measured value of each test piece) Preparation of the test piece: Made by punching Distance between fixtures: 56mm Test environment: 23°C × 50% RH Test speed: 500mm / min.