Polar-solvent-resistant nanofiltration membrane as well as preparation method and application thereof
Through the interfacial polymerization technology of potassium permanganate permanganate oxidation and hexachlorocyclotriphosphazene polyphenols, combined with polar solvent activation, the problem of poor solvent resistance in organic solvent environment is solved, and high solvent resistance and long-term stability are achieved , avoid swelling and plasticization, significantly improve separation performance and flux.
Patent Information
- Application Number
- CN202411286447.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-29
AI Technical Summary
The existing nanofiltration membranes are susceptible to erosion when exposed to organic solvents, resulting in swelling and plasticization, and are insufficient solvent resistance, making it difficult to maintain high separation performance and flux stably for a long time.
Potassium permanganate oxidation modified polyethylene film is adopted, and the polymerization of hexachlorocyclotriphosphazene and polyphenol compounds is formed into a polymer separation layer. Combined with polar solvent activation treatment, the solvent resistance and flux of the film are enhanced. .
A high-solvent-resistant nanofiltration membrane that works in an organic solvent environment for a long time is achieved, avoiding swelling and plasticization problems, maintaining high separation performance and flux, and significantly improving the polarity and stability of the membrane.
Smart Images

Figure CN119034485A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanofiltration membranes, and in particular to a polar solvent-resistant nanofiltration membrane and a preparation method and application thereof. Background Art
[0002] At present, a large number of organic solvents are used in industrial production, such as methanol, ethanol, acetone, ethyl acetate, toluene, tetrahydrofuran, DMAC, DMF and NMP. On the one hand, most organic solvents are toxic substances, and the recovery of organic solvents is of great significance to resource conservation and environmental protection; on the other hand, in the production process, the extraction of products requires the removal of organic solvents, and the extraction method needs to take into account the influence of organic solvents. At present, the methods of organic solvent recovery and product extraction mainly include distillation, extraction, absorption and membrane separation. The distillation operation has a large processing scale, high operating temperature and energy consumption, which is suitable for the industrial production of ordinary compounds and difficult to handle heat-sensitive substances; extraction requires the introduction of new solvents as extractants, which consumes raw materials and increases costs, and the subsequent mixture needs secondary separation, which is not effective; the volatility of organic solvents is used to dissolve or react organic waste gas with absorbents to achieve the purpose of recovery, but the absorbent is generally also an organic solvent, which will cause secondary pollution. Therefore, in order to meet the requirements of green energy conservation and environmental protection, the treatment of related solvents through organic solvent separation membranes has received more and more attention.
[0003] Organic solvent nanofiltration (OSN) technology has shown great application potential in processes such as material separation, drug concentration and refining. Solvent-resistant nanofiltration membrane materials are the core of OSN technology. Nanofiltration membrane is a new type of membrane separation technology between reverse osmosis membrane and ultrafiltration membrane. Nanofiltration membrane has high filtration accuracy and flux, and can achieve separation, purification and concentration of substances at the molecular level. It is widely used in water treatment, chemical industry and medicine. However, traditional nanofiltration membranes are insufficient in solvent resistance. When in contact with organic solvents, they are easily corroded by solvents and swell and plasticize. When processing solutions containing organic solvents, problems such as decreased membrane flux and reduced filtration accuracy often occur. Therefore, it is of great practical significance to develop a nanofiltration membrane with high solvent resistance.
[0004] Prior art CN116078160A discloses a polyethylene-based solvent-resistant and acid-base-resistant reverse osmosis membrane and a preparation method thereof. The polyethylene membrane is placed in a polymer solution with a hydroxyl group for hydrophilic modification, and then the surface is coated with a PES-type polymer. Then, interfacial polymerization is performed on the PES coating to prepare the reverse osmosis membrane. This method immerses the polyethylene membrane in a hydrophilic agent for modification, and the binding between the hydrophilic agent and the polyethylene membrane is weak. At the same time, since a PES small-pore membrane layer is coated on the polyethylene surface, the advantage brought by the large-pore flux of the polyethylene will be reduced to a certain extent, and its separation layer is polyamide, which has limited tolerance to polar solvents.
[0005] The prior art CN103933881A discloses that an ultrafiltration membrane is used as a porous support layer, cyanuric chloride and / or hexachlorocyclotriphosphazene are selected as oil phase solutes to undergo polymerization reaction with amine water phase solutes at the interface between the two phases, the reaction temperature is controlled to activate various groups in the reaction monomers, and different active nucleophilic reagents are introduced step by step to connect specific groups, thereby synthesizing a loosely structured membrane selection layer on the surface of the porous support layer; however, the reagent used in the water phase of this method is amines, and is prepared on an ultrafiltration membrane, resulting in a low flux of the obtained membrane product and limited solvent resistance.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] One of the purposes of the present invention is to provide a method for preparing a polar solvent-resistant nanofiltration membrane, which can solve the technical problem of poor solvent resistance of the nanofiltration membrane in the prior art.
[0008] The second object of the present invention is to provide a polar solvent resistant nanofiltration membrane, which can not only effectively filter and separate different components in a solution, but also has high solvent resistance and long-term stability, can work stably in a solvent for a long time, and maintain high separation performance and flux.
[0009] The third object of the present invention is to provide an application of a polar solvent-resistant nanofiltration membrane, which can avoid the problem of the nanofiltration membrane being easily corroded, swollen and plasticized when contacting an organic solvent, and can achieve outstanding application effects.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] In a first aspect, a method for preparing a polar solvent resistant nanofiltration membrane comprises the following steps:
[0012] (a) a polyethylene film is oxidized and modified by potassium permanganate to obtain a modified polyethylene film;
[0013] (b) interfacial polymerization and thermal curing of hexachlorocyclotriphosphazene and polyphenol compounds on the surface of the modified polyethylene membrane to form a polymer separation layer, and then activating the polymer separation layer to obtain the polar solvent resistant nanofiltration membrane.
[0014] Furthermore, the oxidation modification method comprises the following steps:
[0015] The polyethylene film is immersed in a potassium permanganate solution to obtain a modified polyethylene film.
[0016] Furthermore, the concentration of the potassium permanganate solution is 0.1-0.2 mol / L;
[0017] The soaking temperature is 50-60° C., and the soaking time is 36-60 hours.
[0018] Furthermore, the polyphenol compound includes at least one of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, bisphenol S, 4,4'-dihydroxydiphenyl disulfide, 4,4'-dihydroxydiphenyl propane, 3,5,4'-trihydroxystilbene and derivatives thereof.
[0019] Furthermore, the thermal curing temperature is 70-80° C., and the thermal curing time is 20-30 hours.
[0020] Furthermore, the activation method includes immersing the separation layer in a polar solvent to activate the separation layer.
[0021] Furthermore, the polar solvent includes at least one of DMF, DMAC and DMSO.
[0022] Furthermore, the polar solvent soaks the separation layer for 5 to 8 minutes.
[0023] In a second aspect, a polar solvent resistant nanofiltration membrane is prepared by the preparation method as described in any one of the above items.
[0024] In a third aspect, a use of the polar solvent resistant nanofiltration membrane described above in material separation, drug concentration and product refining.
[0025] Compared with the prior art, the present invention has at least the following beneficial effects:
[0026] The method for preparing a polar solvent resistant nanofiltration membrane provided by the present invention uses a polyethylene membrane as a substrate. Compared with polysulfone as a substrate for a reverse osmosis / nanofiltration membrane, the polyethylene has a larger porosity and pore size, so the generated membrane product has a higher flux and is also more solvent resistant. Compared with directly using a polyethylene membrane or modifying it hydrophilically by impregnation, or modifying the surface by coating a PES-type polymer, the present invention oxidizes the polyethylene membrane by using a strong oxidant, potassium permanganate, which can not only form carboxyl (-COOH), carbonyl (-C=O) and hydroxyl (-OH) groups on the membrane material to increase the hydrophilicity of the polyethylene membrane, but also the oxidation of potassium permanganate has an etching effect, which can remove the weak bonding layer on the surface of the polyethylene membrane, increase the surface roughness, and thus enhance the adhesion of subsequent interfacial polymerization and fiber layers. force; at the same time, the oxidation of potassium permanganate can deposit nano manganese dioxide particles on the polyethylene fibers, and the nano manganese dioxide particles can form hydrogen bonds with subsequent interfacial polymerization products, thereby enhancing the solvent resistance of the membrane; compared with the common polyamide layer, the present invention performs interfacial polymerization reaction on a polyethylene substrate with hexachlorocyclotriphosphazene and a polyphenol compound and thermally cures the reaction to generate a polyether polymer separation layer, and the polymer separation layer is more solvent-resistant; compared with direct film formation after interfacial polymerization, the present invention adds an activation treatment, for example, a polar solvent can be used for activation treatment, and the slight swelling effect of the polar solvent can be used to further improve the membrane flux without reducing the membrane desalination rate. At the same time, the polar solvent dissolves some small molecular fragments on the membrane and can repair some loose sites on the membrane surface.
[0027] The polar solvent resistant nanofiltration membrane provided by the present invention can not only effectively filter and separate different components in a solution, but also has high solvent resistance and long-term stability. The nanofiltration membrane can work stably in a solvent for a long time, maintain high separation performance and flux, and can avoid the phenomenon that the common polyamide and polyimide separation layers swell after long-term use in a solvent environment, resulting in a decrease in membrane separation performance.
[0028] The application of the polar solvent resistant nanofiltration membrane provided by the present invention can avoid the problem that the nanofiltration membrane is easily corroded and swells and plasticizes when it contacts with organic solvents, and the application effect is outstanding. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1A process flow chart of a method for preparing a polar solvent-resistant nanofiltration membrane provided in one embodiment of the present invention;
[0031] Figure 2 A schematic diagram of an interfacial polymerization reaction provided in one embodiment of the present invention. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] According to a first aspect of the present invention, there is provided a method for preparing a polar solvent resistant nanofiltration membrane, comprising the following steps:
[0034] (a) a polyethylene film is oxidized and modified by potassium permanganate to obtain a modified polyethylene film;
[0035] (b) Hexachlorocyclotriphosphazene and polyphenol compounds are interfacially polymerized and thermally cured on the surface of the modified polyethylene membrane to form a polymer separation layer, and then the polymer separation layer is activated to obtain a polar solvent resistant nanofiltration membrane.
[0036] In the present invention, the polyethylene film is first oxidized by potassium permanganate, a strong oxidant, to improve its hydrophilicity, and then hexachlorocyclotriphosphazene and polyphenol compounds are subjected to interfacial polymerization reaction on the polyethylene film (substrate) to generate polyether compounds containing cyclotriphosphazene (cyclotriphosphazene derivatives) as a polymer separation layer. The molecular structure of the cyclotriphosphazene derivative contains phosphorus and nitrogen structures with single and double bonds arranged alternately, so it has excellent heat resistance, flame retardancy, solvent resistance and radiation resistance, which can greatly enhance the solvent resistance of the membrane product; then, the coating crosslinking density is increased by thermal curing, the coating stability and bonding strength are enhanced, and activation treatment is performed to improve the membrane performance, thereby obtaining a polar solvent resistant nanofiltration membrane.
[0037] The method for preparing a polar solvent resistant nanofiltration membrane provided by the present invention uses a polyethylene membrane as a substrate. Compared with polysulfone as a substrate for a reverse osmosis / nanofiltration membrane, the polyethylene has a larger porosity and pore size, so the generated membrane product has a higher flux and is also more solvent resistant. Compared with directly using a polyethylene membrane or modifying it hydrophilically by impregnation, or modifying the surface by coating a PES-type polymer, the present invention oxidizes the polyethylene membrane by using a strong oxidant, potassium permanganate, which can not only form carboxyl (-COOH), carbonyl (-C=O) and hydroxyl (-OH) groups on the membrane material to increase the hydrophilicity of the polyethylene membrane, but also the oxidation of potassium permanganate has an etching effect, which can remove the weak bonding layer on the surface of the polyethylene membrane, increase the surface roughness, and thus enhance the adhesion of subsequent interfacial polymerization and fiber layers. force; at the same time, the oxidation of potassium permanganate can deposit nano manganese dioxide particles on the polyethylene fibers, and the nano manganese dioxide particles can form hydrogen bonds with subsequent interfacial polymerization products, thereby enhancing the solvent resistance of the membrane; compared with the common polyamide layer, the present invention performs interfacial polymerization reaction on a polyethylene substrate with hexachlorocyclotriphosphazene and a polyphenol compound and thermally cures the reaction to generate a polyether polymer separation layer, and the polymer separation layer is more solvent-resistant; compared with direct film formation after interfacial polymerization, the present invention adds an activation treatment, for example, a polar solvent can be used for activation treatment, and the slight swelling effect of the polar solvent can be used to further improve the membrane flux without reducing the membrane desalination rate. At the same time, the polar solvent dissolves some small molecular fragments on the membrane and can repair some loose sites on the membrane surface.
[0038] In a preferred embodiment, the method for oxidative modification of the present invention comprises the following steps:
[0039] The polyethylene film is immersed in a potassium permanganate solution to obtain a modified polyethylene film.
[0040] The polyethylene film is immersed in a potassium permanganate solution, the concentration of the potassium permanganate solution can be 0.1-0.2 mol / L, and its typical but non-limiting concentration is, for example, 0.1 mol / L, 0.12 mol / L, 0.14 mol / L, 0.16 mol / L, 0.18 mol / L, and 0.2 mol / L. The temperature of the potassium permanganate solution can be 50-60°C, and its typical but non-limiting temperature is, for example, 50°C, 52°C, 54°C, 56°C, 58°C, and 60°C; the polyethylene film can be immersed for 36-60 hours, and its typical but non-limiting time is, for example, 36 hours, 38 hours, 40 hours, 45 hours, 50 hours, 55 hours, and 60 hours; after immersion, the polyethylene film is taken out and rinsed with deionized water, and then dried at 70°C to obtain the modified polyethylene film. Under the action of potassium permanganate, the surface of the polyethylene fiber is oxidized to produce highly active oxygen-containing groups such as carboxyl (-COOH), carbonyl (-C=O) and hydroxyl (-OH), thereby increasing the hydrophilicity of the polyethylene film; in addition, potassium permanganate also has a certain etching effect due to its oxidizing property, which can remove the weak binding layer on the polyethylene surface, thereby increasing the surface roughness of the polyethylene fiber, thereby enhancing the adhesion between the subsequent interfacial polymerization and the fiber layer; at the same time, oxidation can also cause nano-manganese dioxide particles to be deposited on the polyethylene fiber, and the existing nano-manganese dioxide particles can form hydrogen bonds with the subsequent interfacial polymerization products, thereby enhancing the solvent resistance of the film.
[0041] In a preferred embodiment, the polyphenol compounds include but are not limited to at least one of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, bisphenol S, 4,4'-dihydroxydiphenyl disulfide, 4,4'-dihydroxydiphenyl propane, 3,5,4'-trihydroxystilbene and their derivatives. Hexachlorocyclotriphosphazene reacts with the above polyphenol compounds to generate polyether compounds containing cyclotriphosphazene. The polyether polymer separation layer is more stable than conventional polyamide and more resistant to solvents.
[0042] In a preferred embodiment, the temperature of thermal curing can be 70-80°C, and typical but non-limiting temperatures are, for example, 70°C, 72°C, 74°C, 76°C, 78°C, and 80°C; the duration of thermal curing can be 20-30h, and typical but non-limiting durations are, for example, 20h, 22h, 24h, 26h, 28h, and 30h. The above-mentioned thermal curing temperature and duration are more conducive to further improving the crosslinking density of the coating, and are more conducive to further enhancing the stability and bonding strength of the coating.
[0043] In a preferred embodiment, the activation method includes but is not limited to immersing the separation layer in a polar solvent to activate the separation layer; wherein the polar solvent includes but is not limited to at least one of DMF, DMAC and DMSO.
[0044] In the present invention, the polar solvent may soak the separation layer for 5 to 8 minutes, and a typical but non-limiting time is, for example, 5 minutes, 6 minutes, 7 minutes, or 8 minutes, which is more conducive to further improving the activation effect.
[0045] The present invention uses a polar (mixed) solvent to activate the membrane layer after interfacial polymerization and thermal curing, and utilizes the slight swelling effect of the polar solvent to further increase the membrane flux without reducing the membrane desalination rate. At the same time, the polar (mixed) solvent dissolves some small molecular fragments on the membrane, and can repair some loose sites on the membrane surface.
[0046] A typical preparation method of a polar solvent resistant nanofiltration membrane, see Figure 1 , including the following steps:
[0047] (1) Modification of the base film: The polyethylene base film was immersed in a potassium permanganate (KMnO4) solution with a concentration of 0.1 to 0.2 mol / L and a solution temperature of 55°C. After immersion for 2 days, the base film was rinsed with deionized water and dried at 70°C to obtain a modified polyethylene base film.
[0048] Under the action of potassium permanganate, the surface of polyethylene fiber is oxidized to produce highly active oxygen-containing groups such as carboxyl (-COOH), carbonyl (-C=O) and hydroxyl (-OH), which can increase the hydrophilicity of polyethylene; in addition, potassium permanganate also has a certain etching effect due to its oxidizing property, which can remove the weak binding layer on the surface of polyethylene, increase the roughness of the fiber surface, and thus enhance the adhesion between the subsequent interfacial polymerization product and the fiber layer; in addition, oxidation can cause nano manganese dioxide particles to be deposited on polyethylene fibers, which can form hydrogen bonds with the subsequent interfacial polymerization product, thereby enhancing the solvent resistance of the film;
[0049] (2) Aqueous phase preparation: preparing an aqueous phase solution by mixing aromatic phenol, aqueous phase additive and pure water;
[0050] The aromatic phenol (polyphenol compound) may be at least one of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, bisphenol S, 4,4'-dihydroxydiphenyl disulfide, 4,4'-dihydroxydiphenyl propane, 3,5,4'-trihydroxystilbene, etc. or their derivatives;
[0051] The aqueous phase additive may be at least one of NaOH, KOH and sodium carbonate (base), and at least one of sodium dodecyl sulfonate, sodium dodecyl sulfate and sodium dodecylbenzene sulfonate (surfactant);
[0052] The concentration of aromatic phenol is 0.5-1 mol / L. NaOH, KOH or sodium carbonate can deprotonate aromatic phenol to convert it into more reactive aryl sodium oxide (concentration 1.5-3 mol / L). The mass fraction of surfactant is 0.03-5 wt%;
[0053] (3) Oil phase preparation: Hexachlorocyclotriphosphazene (HCCP), an oil phase additive and a solvent are prepared into an oil phase solution, wherein the HCCP concentration is 0.1 to 0.2 mol / L;
[0054] The oil phase additive may be at least one of methyl trioctyl ammonium chloride and hexadecyl trimethyl ammonium bromide, with a concentration of 0.1 to 0.2 wt %; the solvent may be at least one of n-heptane, benzene, petroleum ether and dichloromethane;
[0055] (4) Preparation of functional layer (interfacial polymerization IP, see Figure 2 ): the modified polyethylene-based film of step (1) is immersed in the aqueous solution of step (2), wherein the aqueous phase immersion time can be 5 to 10 minutes, and after being taken out, the excess phenol solution is removed with nitrogen or a rubber roller, and then immersed in the oil phase solution of step (3), wherein the oil phase immersion time can be 5 to 10 minutes, and then taken out;
[0056] It should be noted that the modified polyethylene-based membrane can also be immersed in the oil phase solution first, and then immersed in the water phase solution;
[0057] (5) Thermal curing treatment: The product after the interfacial polymerization in step (4) is sent to an oven for thermal curing treatment, wherein the thermal curing temperature can be 70° C. and the thermal curing time can be 24 hours to increase the crosslinking density of the coating and enhance the stability and bonding strength of the coating;
[0058] (6) Solvent activation treatment: After the product after heat curing in step (5) is cooled to room temperature, the separation layer is immersed in a polar (mixed) solvent for activation treatment, and then the excess solvent is washed away with deionized water to obtain a polar solvent resistant nanofiltration membrane;
[0059] The polar solvent may be at least one of DMF, DMAC and DMSO.
[0060] The preparation method provided by the present invention comprises the following steps: a polyethylene film is modified by a potassium permanganate oxidation method, and nano manganese dioxide particles are introduced while generating polar functional groups, so that the hydrophilicity can be enhanced and the solvent resistance can be improved; on the surface of the modified polyethylene film, an interfacial polymerization reaction is carried out by HCCP and a polyphenol compound, so that the problem of coating an ultrafiltration layer and affecting the membrane flux can be avoided, and cyclotriphosphazene is introduced into the separation layer, so that the solvent resistance of the prepared membrane layer is enhanced; and through a heat curing treatment, the crosslinking density is increased and the stability and the bonding force are enhanced; and a polar solvent is used for activation treatment, so that the membrane performance is effectively improved.
[0061] According to a second aspect of the present invention, there is provided a polar solvent resistant nanofiltration membrane prepared by any of the preparation methods described above.
[0062] The polar solvent resistant nanofiltration membrane provided by the present invention can not only effectively filter and separate different components in a solution, but also has high solvent resistance and long-term stability. The nanofiltration membrane can work stably in a solvent for a long time, maintain high separation performance and flux, and can avoid the phenomenon that the common polyamide and polyimide separation layers swell after long-term use in a solvent environment, resulting in a decrease in membrane separation performance.
[0063] According to a third aspect of the present invention, there is provided a use of the polar solvent resistant nanofiltration membrane described above in material separation, drug concentration and product purification.
[0064] The application of the polar solvent resistant nanofiltration membrane provided by the present invention can avoid the problem that the nanofiltration membrane is easily corroded and swells and plasticizes when it contacts with organic solvents, and the application effect is outstanding.
[0065] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0066] Example 1
[0067] A method for preparing a polar solvent resistant nanofiltration membrane comprises the following steps:
[0068] S1: Purchase polyethylene battery separator on the market, with a thickness of 20 μm, a pore size of 0.1-0.2 μm, and a contact angle of 110°;
[0069] S2: Modification of base film: The polyethylene membrane was immersed in a potassium permanganate solution with a concentration of 0.2 mol / L for 2 days at a temperature of 55°C, then taken out, rinsed, and dried at 70°C. The pore size of the membrane surface was about 0.15 μm, and the contact angle was 70°C, thereby obtaining a modified polyethylene base film;
[0070] S3: aqueous phase preparation: 4,4'-dihydroxydiphenyl disulfide, NaOH, sodium dodecyl sulfate and pure water are prepared into an aqueous phase solution;
[0071] Among them, the concentration of 4,4'-dihydroxydiphenyl disulfide is 0.5 mol / L, the concentration of NaOH is 2 mol / L, and the mass fraction of sodium dodecyl sulfate is 0.2 wt%;
[0072] S4: oil phase preparation: hexachlorocyclotriphosphazene (HCCP), hexadecyltrimethylammonium bromide and toluene are prepared into an oil phase solution, wherein the concentration of HCCP is 0.1 mol / L and the concentration of hexadecyltrimethylammonium bromide is 0.1 wt %;
[0073] S5: Preparation of functional layer (interfacial polymerization): The modified polyethylene-based membrane of step S2 is immersed in the aqueous solution of step S3 for 6 minutes and then taken out, and then the excess phenol solution is removed by nitrogen or a rubber roller, and then immersed in the oil phase solution of step S4 for 5 minutes and then taken out;
[0074] S6: thermal curing treatment: sending the product after the interfacial polymerization in step S5 into an oven for thermal curing treatment, wherein the thermal curing temperature is 70° C. and the thermal curing time is 24 hours, so as to increase the crosslinking density of the coating and enhance the stability and bonding strength of the coating;
[0075] S7: solvent activation treatment: After the product after heat curing in step S6 is cooled to room temperature, it is immersed in a mixed solution of DMAC and DMF, wherein the volume ratio of DMAC and DMF is 4:6, and the immersion time is 8 minutes. Then, the excess solvent is washed away with deionized water to obtain a polar solvent resistant nanofiltration membrane.
[0076] Example 2
[0077] A method for preparing a polar solvent resistant nanofiltration membrane comprises the following steps:
[0078] S1: Purchase polyethylene battery separator on the market, with a thickness of 20 μm, a pore size of 0.1-0.2 μm, and a contact angle of 110°;
[0079] S2: Modification of base film: The polyethylene membrane was immersed in a potassium permanganate solution with a concentration of 0.2 mol / L for 2 days at a temperature of 55°C, then taken out, rinsed, and dried at 70°C. The pore size of the membrane surface was about 0.15 μm, and the contact angle was 70°C, thereby obtaining a modified polyethylene base film;
[0080] S3: aqueous phase preparation: 4,4'-dihydroxybenzophenone, KOH, sodium dodecylbenzene sulfonate and pure water are prepared into an aqueous phase solution;
[0081] Among them, the concentration of 4,4'-dihydroxybenzophenone is 0.6 mol / L, the concentration of KOH is 2 mol / L, and the mass fraction of sodium dodecylbenzene sulfonate is 0.2 wt%;
[0082] S4: oil phase preparation: hexachlorocyclotriphosphazene (HCCP), hexadecyltrimethylammonium bromide and toluene are prepared into an oil phase solution, wherein the concentration of HCCP is 0.1 mol / L and the concentration of hexadecyltrimethylammonium bromide is 0.1 wt%;
[0083] S5: Preparation of functional layer (interfacial polymerization): The modified polyethylene-based membrane of step S2 is placed in the aqueous solution of step S3 for 8 minutes and then taken out, and then the excess phenol solution is removed by nitrogen or a rubber roller, and then placed in the oil phase solution of step S4 for 6 minutes and then taken out;
[0084] S6: thermal curing treatment: sending the product after the interfacial polymerization in step S5 into an oven for thermal curing treatment, wherein the thermal curing temperature is 70° C. and the thermal curing time is 24 hours, so as to increase the crosslinking density of the coating and enhance the stability and bonding strength of the coating;
[0085] S7: solvent activation treatment: after the product of the interfacial polymerization in step S5 is cooled to room temperature, it is immersed in a mixed solution of DMAC and DMF, wherein the volume ratio of DMAC and DMF is 1:1, and the immersion time is 5 minutes. Then, the excess solvent is washed away with deionized water to obtain a polar solvent resistant nanofiltration membrane.
[0086] Example 3
[0087] The difference between this embodiment and embodiment 1 is that in step S3, 4,4'-dihydroxybiphenyl is used in an equal amount to replace 4,4'-dihydroxydiphenyl disulfide, thereby configuring an aqueous phase solution;
[0088] The remaining steps are the same as those in Example 1 to obtain a polar solvent-resistant nanofiltration membrane.
[0089] Example 4
[0090] The difference between this embodiment and embodiment 1 is that in step S3, bisphenol S is used in an equal amount to replace 4,4'-dihydroxydiphenyl disulfide, thereby configuring an aqueous phase solution;
[0091] The remaining steps are the same as those in Example 1 to obtain a polar solvent-resistant nanofiltration membrane.
[0092] Example 5
[0093] The difference between this embodiment and embodiment 1 is that in step S3, 3,5,4'-trihydroxyphenylethylene is used to replace 4,4'-dihydroxydiphenyl disulfide in an equal amount, thereby configuring an aqueous phase solution;
[0094] The remaining steps are the same as those in Example 1 to obtain a polar solvent-resistant nanofiltration membrane.
[0095] Comparative Example 1
[0096] The difference between this comparative example and Example 1 is that step S2 is to modify the base film by soaking in a hydroxyl-containing hydrophilic modifying agent, and the method is as follows:
[0097] S2: base film modification: soak the polyethylene membrane in a PVA (polyvinyl alcohol) modification solution, wherein the modification solution comprises: PVA concentration 1wt%, DMAC concentration 5wt%, and the rest water; soak for 15 minutes and then dry to obtain a modified polyethylene base film;
[0098] The remaining steps are the same as those in Example 1 to obtain a nanofiltration membrane.
[0099] Comparative Example 2
[0100] The difference between this comparative example and Example 1 is that the solvent activation treatment in step S7 is not performed;
[0101] The remaining steps are the same as those in Example 1 to obtain a nanofiltration membrane.
[0102] Comparative Example 3
[0103] The difference between this comparative example and Example 1 is that a polysulfone ultrafiltration membrane is used, an aqueous solution of piperazine is used as an aqueous phase solution, trimesoyl chloride is used as an oil phase, and Isopar-G is used as a solvent, and a nanofiltration membrane is prepared by interfacial polymerization, and the method is as follows:
[0104] S1: Polysulfone flat ultrafiltration membrane as the porous support layer;
[0105] S2: Aqueous phase solution: The aqueous phase solution contains piperazine at a concentration of 0.5% and also contains triethylamine and sodium dodecyl sulfate, with a mass fraction of 0.1% sodium dodecyl sulfate;
[0106] S3: oil phase solution: the mass concentration of trimesoyl chloride in the oil phase solution is 3%;
[0107] S4: immerse the polysulfone flat ultrafiltration membrane in the aqueous solution, let it stand for 10 minutes, then take it out, remove the excess solution with a rubber roller, and then introduce the oil phase solution to allow the two monomers to undergo interfacial polymerization reaction for 3 minutes;
[0108] S5: Drying the membrane after interfacial polymerization to obtain a nanofiltration membrane.
[0109] Test example
[0110] The nanofiltration membranes prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to retention and flux tests, respectively; the test method was as follows: the operating pressure was 0.6 MPa, the test solution was 1 g / L magnesium sulfate solution, the solution temperature was 25°C, the pH was 6.5-7.5, and the water flux and desalination rate of the test membrane were measured after 30 minutes of operation; the test results are shown in Table 1.
[0111] The nanofiltration membranes prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to solvent resistance tests, respectively, and the solvent was DMAC; the test method was: the membranes were immersed in the solvents, respectively, at room temperature for 20 days, and the flux of the membranes after immersion and the retention of 1 g / L magnesium sulfate were tested; the test results are shown in Table 2.
[0112] In Comparative Example 1, the hydrophilic additive was not firmly bonded to the polyethylene layer, so the desalination rate of the membrane was attenuated to a certain extent; in Comparative Example 3, the nanofiltration membrane had limited resistance to polar solvents. After being soaked in polar solvents, the desalination layer was damaged, the desalination rate decreased, and the flux increased.
[0113] Table 1
[0114]
[0115] Table 2
[0116]
[0117] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a polar solvent resistant nanofiltration membrane, characterized in that: The following steps are involved: (a) a polyethylene film is oxidized and modified by potassium permanganate to obtain a modified polyethylene film; (b) interfacial polymerization and thermal curing of hexachlorocyclotriphosphazene and polyphenol compounds on the surface of the modified polyethylene membrane to form a polymer separation layer, and then activating the polymer separation layer to obtain the polar solvent resistant nanofiltration membrane.
2. The preparation method according to claim 1, characterized in that: The oxidation modification method comprises the following steps: The polyethylene film is immersed in a potassium permanganate solution to obtain a modified polyethylene film.
3. The preparation method according to claim 2, characterized in that: The concentration of the potassium permanganate solution is 0.1-0.2 mol / L; The soaking temperature is 50-60° C., and the soaking time is 36-60 hours.
4. The preparation method according to claim 1, characterized in that: The polyphenol compound includes at least one of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, bisphenol S, 4,4'-dihydroxydiphenyl disulfide, 4,4'-dihydroxydiphenyl propane, 3,5,4'-trihydroxystilbene and derivatives thereof.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The temperature of the thermal curing is 70-80° C., and the duration of the thermal curing is 20-30 hours.
6. The preparation method according to any one of claims 1 to 4, characterized in that: The activation method includes immersing the separation layer in a polar solvent to activate the separation layer.
7. The preparation method according to claim 6, characterized in that: The polar solvent includes at least one of DMF, DMAC and DMSO.
8. The preparation method according to claim 6, characterized in that: The polar solvent soaks the separation layer for 5 to 8 minutes.
9. A polar solvent resistant nanofiltration membrane prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the polar solvent resistant nanofiltration membrane according to claim 9 in material separation, drug concentration and product purification.
Citation Information
Cited By
Preparation method and application of polar-solvent-resistant nanofiltration membrane
CN119565406A