Preparation method of MOF-based Cu (I) monatomic catalytic material

By anchoring and reducing Cu(I) sites in situ on the Ce-MOF-88 framework, the problems of stability of single-atom catalysts at high temperatures and high cost of precious metals are solved, and low-cost and efficient catalytic performance is achieved. The catalytic energy barrier is significantly reduced, especially in the hydrogenation reaction.

CN119034813AActive Publication Date: 2024-11-29UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410937253.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The prior art is difficult to stabilize the active site of a single-atom catalyst at high temperatures, and the precious metal catalyst is costly, which affects its performance and economicality in the hydrogenation reaction.

Method used

The Ce-MOF-808 carrier was synthesized by solvothermal method, and the divalent metal ions were reduced to monovalent metal ions anchored by ethanol soaking and vacuum high-temperature activation treatment, and a single-atom Cu(I with adjustable electrons and geometric structures were prepared. ) catalyst, anchored on the Ce-MOF-88 framework, realizes in situ reduction of Cu(I) sites and microenvironmental control of active sites.

Benefits of technology

The preparation of a low-cost and adjustable single-atom Cu(I) catalyst is achieved, which significantly improves the catalytic performance. Especially in hydrogenation reaction, the Cu(I) site is a dual active site for H2 activation, effectively reducing the The catalytic energy barrier improves the selectivity and efficiency of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034813A_ABST
    Figure CN119034813A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an MOF-based Cu (I) monatomic catalytic material, and belongs to the field of preparation of high-quality aviation fuel through MOF-based monatomic catalytic hydrogenation. The preparation method comprises the following steps: adding a monocarboxylic acid regulator into a mixed solution of soluble cerium salt and an organic ligand, synthesizing a Ce-based MOFs carrier with high crystallinity and adjustable size through a solvothermal method, uniformly dispersing the Ce-based MOFs carrier into the solution, adding a solution containing metal salt under a stirring condition, and uniformly stirring to obtain the Ce-based MOFs catalyst. Then divalent metal ions are reduced into monovalent metal ions through ethanol soaking and vacuum high-temperature activation treatment, the monovalent metal ions are anchored to metal nodes, and the Ce-based MOFs anchored metal monatomic catalyst is prepared. The MOFs-based monatomic catalytic material prepared by the invention has Cu (I) capable of being reduced in situ and is in monatomic dispersion, the used raw materials are low in cost and easy to obtain, monatomic metal electrons and geometric structures anchored on metal Ce6 nodes are adjustable, and the active site microenvironment is controllable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of preparing high-quality aviation fuel by MOF-based single-atom catalytic hydrogenation, and specifically relates to a preparation method of atomically dispersed non-precious metal single-atom Cu(I) catalytic material anchored on Ce-MOF-88. Background Art

[0002] Emerging single-atom catalysts (SACs), also known as atomically dispersed catalysts, have attracted extensive attention due to their well-defined active sites, maximum atomic utilization, and tunable electronic and geometric structures, which not only make it possible to design and construct catalysts with high activity, selectivity, and stability, but also deepen the understanding of structure-activity relationships and catalytic reaction mechanisms. In order to prevent single-atom catalysts from easily migrating and sintering at high temperatures due to high surface energy, loading SACs onto high-surface-area supports with strong channel transport capabilities is an effective strategy to stabilize single-atom active sites and maintain catalytic performance under harsh reaction conditions. Therefore, the rational design of a porous structure that can be precisely coordinated with the support and precisely control its electronic and microenvironment is of great significance to improve the catalytic performance.

[0003] Metal-organic frameworks (MOFs) are well-known for their ultra-high specific surface area, finely tuned structure, designable functionality and pore size. Therefore, the research on MOFs-supported SACs (SACs-MOFs) has received extensive attention. Atomically dispersed noble metals, such as Pt, Rh, Pa, Ir, Ru and Au, have become key catalysts for a large number of important chemical reactions in the energy and environmental fields due to their high activity, selectivity and stability. However, the high cost of these noble metals poses a challenge that needs to be addressed. Through post-processing synthesis, noble metal-free single atoms (Co2+) on MOFs clusters have been synthesized. 2+ 、Ni 2+ 、Zn 2+ 、Al 3+ 、Ti 4+ 、Mo 6+ ) show excellent catalytic performance in cycloaddition reactions, alkane oxidation, CO oxidation and other catalytic fields. Rare earth MOFs (RE-MOFs) are a subclass of MOFs that demonstrate the unique characteristics of MOFs chemistry and the complex intrinsic properties of rare earth elements. The combination of single atoms anchored in RE-MOFs provides an ideal platform for the manufacture of single atom catalysts. Transition metal Cu is low-cost and can promote H in hydrogenation reactions. 2 Therefore, using multifunctional RE-MOFs to effectively anchor Cu single atoms and precisely control their microenvironment to improve catalytic hydrogenation performance is a long-pursued and challenging synthetic technology. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a preparation method of single-atom Cu(I) anchored in Ce-MOF-88 catalytic material with adjustable electronic and geometric structures, controllable active site microenvironment, low cost and high atomic utilization.

[0005] The present invention provides a method for preparing a MOF-based Cu(I) single-atom catalytic material, comprising the following steps:

[0006] 1) A certain amount of monocarboxylic acid regulator is added to the mixed solution of soluble cerium salt and organic ligand, and a Ce-based MOFs carrier with high crystallinity and adjustable size is synthesized by solvothermal method;

[0007] 2) At a certain temperature, the Ce-based MOFs carrier is evenly dispersed in the solution, and a solution containing a metal salt is added under stirring conditions. The divalent metal ions are then reduced to monovalent metal ions and anchored to the metal nodes through ethanol immersion and vacuum high-temperature activation treatment to obtain a Ce-based MOFs anchored metal single atom catalyst.

[0008] The specific preparation steps are:

[0009] 1) Synthesis of Ce-MOF-808

[0010] Add N,N-dimethylformamide (DMF), formic acid, and trimesic acid (H 3 BTC) and cerium (IV) ammonium nitrate aqueous solution (NH 4 ) 2 Ce(NO 3 ) 6 The molar ratio of each component is (NH 4 ) 2 Ce(NO 3 ) 6 :H 3 BTC:Formic acid:DMF:H 2 O = 1~3: 1: 100~0: 155: 1~10, the round-bottom flask was sealed, heated in an oil bath at 100 °C with vigorous stirring for 10~30 min, and after cooling to room temperature, the white precipitate was centrifuged in the mother liquor, washed, and dried to obtain Ce-MOF-808.

[0011] 2) Synthesis of Ce-MOF-808-xCu-y

[0012] The soluble anchor metal salt copper acetate monohydrate was dissolved in DMF, and then Ce-MOF-808 was added to form a suspension, and then the suspension was placed in a reactor of a polytetrafluoroethylene-lined stainless steel reactor for post-modification reaction, and reacted in an oven at 100 ~ 120 ° C for 24 ~ 36 h. After cooling to room temperature, the mother liquor was poured out and washed with DMF until DMF was colorless. The obtained solid material was soaked in DMF, then soaked in acetone, exchanged with acetone, and then ethanol or vacuum activation or ethanol and vacuum activation treatment was performed to obtain Ce-MOF-808-xCu-y, where x = 20, 25, 30 wt%.

[0013] Furthermore, the concentration of formic acid in step 1) is 99%.

[0014] Furthermore, the white precipitate in step 1) is centrifuged in the mother liquor, washed, and dried by centrifuging the white precipitate twice in DMF to remove DMF, then washing the solid with acetone and centrifuging it four times, and the obtained white solid is dried in a vacuum at 60°C.

[0015] Furthermore, the copper acetate monohydrate added in step 2) is preferably added in an amount of 25 wt %.

[0016] Furthermore, the DMF washing times in step 2) is 3 times.

[0017] Furthermore, the immersion in DMF in step 2) is 36 hours, during which the DMF is replaced every 10 to 12 hours; the immersion in acetone is 30 to 40 hours, during which the acetone is replaced every 10 to 12 hours.

[0018] Furthermore, the ethanol or vacuum activation or ethanol and vacuum activation treatment in step 2) is specifically:

[0019] (1) Ethanol treatment is to place the solid in an ethanol solution at 60 ~ 80 °C for 4 ~ 7 h and then dry it to obtain Ce-MOF-808-xCu-E (y = E represents ethanol treatment);

[0020] (2) Vacuum activation treatment is to exchange the solvent with acetone and then dry it, and then vacuum activate it at 80 ~ 150 °C for 1 ~ 5 h to obtain Ce-MOF-808-xCu-A (y = A indicates vacuum activation treatment);

[0021] (3) Ethanol and vacuum activation treatment is to exchange the solvent with acetone, then perform ethanol treatment, place the solid in an ethanol solution at 60 ~ 80 °C for 4 ~ 7 h, dry it, and then perform vacuum activation treatment at 80 ~ 150 °C for 1 ~ 5 h to obtain Ce-MOF-808-xCu-EA (y = EA represents ethanol and activation treatment).

[0022] Furthermore, the synthesis reaction described in step 2) obtains Ce-MOF-808-xCu-y, preferably y=EA, and the ethanol treatment time is preferably 6 h, and the activation treatment is at a temperature of 100 °C for 5 h;.

[0023] Furthermore, the vacuum activation or ethanol and vacuum activation drying treatment is vacuum drying at 80° C. for 24 h.

[0024] Features of the present invention:

[0025] The present invention selects Ce-MOF-808 with 6 coordination frameworks to anchor Cu, which can not only significantly promote the rich coordination of unsaturated centers as the accessibility of active sites, but also make the MOF structure mesoporous through the regulation of regulators. A series of atomically dispersed single-atom Cu(II) anchored in Ce-MOF-8088 framework with strong metal loading interaction (SMSI) effect were designed and synthesized. 6 A series of Ce-MOF-808-xCu-y were synthesized on the node. The in-situ reduction of Cu(II) active sites to Cu(I) sites was achieved through ethanol treatment and subsequent thermal activation. The present invention is a technical solution proposed on the basis of systematically studying the hydrogenation reaction pathways of DCPD on different metal active centers and revealing the low-energy route on single-atom Cu anchored MOF-808 through density functional theory (DFT) calculations. In addition, the Cu(I) site is used as H 2 The activated dual active sites generate a pair of protons and hydride (*H δ+ -H δ- ), effectively reducing the catalytic hydrogenation energy barrier. The present invention provides a valuable synthesis method for further utilizing (improving) the catalytic effect in non-precious metal Cu(I) site MOFs, proves the excellent hydrogenation performance of the catalyst, and provides a rational design of multi-active site synergistic catalysts. It provides a new way to develop new efficient and highly selective DCPD hydrogenation catalytic materials.

[0026] In summary, the advantages of the present invention are: (1) a new type of MOFs-based single-atom catalytic material is developed; (2) the prepared MOFs-based single-atom catalytic material has Cu(I) that can be reduced in situ and is single-atom dispersed; (3) the raw materials provided by the method of the present invention are cheap and easy to obtain, and the anchoring of the metal Ce 6The single-atom metal electronics and geometric structures at the nodes are adjustable, and the microenvironment of the active sites is controllable. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the XRD pattern of Ce-MOF-808 prepared with different amounts of formic acid added obtained in Example 1 of the present invention.

[0028] Figure 2 The N of Ce-MOF-808 prepared by adding different amounts of formic acid obtained in Example 1 of the present invention 2 Adsorption-desorption curve diagram.

[0029] Figure 3 This is a comparative analysis chart of X-ray diffraction of Ce-MOF-88 and Ce-MOF-808-25Cu-EA obtained in Example 1 of the present invention and standard MOF-808.

[0030] Figure 4 TEM and EDS images of Ce-MOF-88 and Ce-MOF-808-25Cu-EA obtained in Example 1 of the present invention.

[0031] Figure 5 XPS graphs of Cu in Ce-MOF-88 and Ce-MOF-808-25Cu obtained in Example 3 of the present invention under different treatment conditions.

[0032] Figure 6 This is a comparative analysis chart of the performance of Ce-MOF-88 and Ce-MOF-808-25Cu under different treatment conditions obtained in Example 3 of the present invention.

[0033] Figure 7 This is a comparative analysis diagram of the hydrogenation performance of Ce-MOF-808-xCu-EA obtained after adding different amounts of Cu metal salt in Example 4 of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below in conjunction with specific implementation methods.

[0035] Example 1

[0036] After DMF (12 mL) and formic acid (0, 1.6, 2.4, 3.2, 4.0 mL, 99%) were added to a round-bottom flask, H 3 BTC (224 mg, 1.06 mmol). Add (NH 4 ) 2 Ce(NO 3 ) 6(6 mL, 0.533 M) in water. The round-bottom flask was sealed and heated in an oil bath at 100 °C with vigorous stirring for 15 min. After cooling to room temperature, the white precipitate was centrifuged in the mother liquor, washed, and centrifuged twice in DMF (20 mL). To remove DMF from the product, the solid was subsequently washed and centrifuged four times with acetone (20 mL). The obtained white solid was dried in vacuo at 60 °C. 1 mmol Cu(OAc) 2 ·H 2 O (25 wt%, 200 mg) was dissolved in 60 mL DMF, and then 200 mg Ce-MOF-808 was added. The suspension was placed in a 100 mL polytetrafluoroethylene-lined stainless steel reactor and reacted in an oven at 100 °C for 24 h. After cooling to room temperature, the mother liquor was poured out and washed with DMF three times (3×50 mL) until the DMF was colorless. The obtained solid material was soaked in DMF (50 mL) for 36 h, during which the DMF was replaced every 12 h. The DMF-soaked material was soaked in acetone (50 mL) for 36 h, during which the acetone was replaced every 12 h. After exchanging the solvent with acetone, the solid was placed in an ethanol solution at 70 °C for 6 h, vacuum dried at 80 °C for 24 h, and vacuum activated at 100 °C for 5 h before the reaction. By anchoring atomically dispersed Cu(II) sites on the Ce of the Ce-MOF-808 framework 6 At the node, Ce-MOF-808-25Cu-EA was synthesized, and the added Cu(II) was reduced to Cu(I) in situ via ethanol treatment and subsequent thermal activation process.

[0037] The DCPD hydrogenation was carried out in a 50 ml stainless steel sealed autoclave, into which 200 uL DCPD, 5 ml cyclohexane (solvent) and 20 mg active catalyst were loaded. 2 Enter the sealed autoclave and then release it, repeating 2 to 3 times to remove the air in the reactor. Then pass H 2 , the pressure was adjusted to 2 MPa, stirred and heated to 100 °C, and the speed was set to 600 r / min. After the reaction, the product was analyzed by gas chromatography-mass spectrometry. Cyclic stability test: After the cyclic reaction, the reactants and catalysts were added to the ethanol solution and centrifuged, and vacuum dried at 60 °C overnight before the next round of reaction.

[0038] After the reaction is completed, remove the product and centrifuge. Take out 50 uL of the supernatant with a pipette and put it into a gas chromatography vial (ANW2ml injection bottle with blue cap and pad, ANW2ml transparent injection bottle), add cyclohexane to 1.5 mL, and mix well. The gas chromatograph (Agilent6820) uses an FID detector and a DB-5 capillary column (30 m×0.32 mm×0.25 μm).

[0039] The prepared single-atom Cu(I) catalyst has excellent catalytic performance for the hydrogenation reaction of DCPD under the conditions of 100 ℃, 2 MPa, and 15 h. The conversion rate of DCPD is 100% and the selectivity of dihydrodicyclopentadiene (DHDCPD) is 100%.

[0040] like Figure 1 The XRD patterns of Ce-MOF-808 prepared with different amounts of formic acid added. It can be seen that the addition of formic acid increases the crystallinity of MOFs.

[0041] like Figure 2 N of Ce-MOF-808 prepared with different formic acid addition amounts 2 Adsorption-desorption curves. It can be seen that 80eq of formic acid has a larger pore structure.

[0042] like Figure 3 X-ray diffraction patterns of Ce-MOF-88 and Ce-MOF-808-25Cu-EA. It can be seen that the MOFs crystal form remains intact

[0043] like Figure 4 TEM and EDS images of Ce-MOF-88 and Ce-MOF-808-25Cu-EA. It can be seen that Cu is evenly distributed and exists in the form of single atoms.

[0044] Example 2

[0045] After DMF (12 mL) and formic acid (4.0 mL, 99%) were added to a round-bottom flask, H 3 BTC (224 mg, 1.06 mmol). Add (NH 4 ) 2 Ce(NO 3 ) 6 (6 mL, 0.533 M) in water. The round-bottom flask was sealed and heated in an oil bath at 100 °C with vigorous stirring for 15 min. After cooling to room temperature, the white precipitate was centrifuged in the mother liquor, washed, and centrifuged twice in DMF (20 mL). To remove DMF from the product, the solid was subsequently washed and centrifuged four times with acetone (20 mL). The obtained white solid was dried in vacuo at 60 °C. 1 mmol Cu(OAc)2 ·H 2 O was dissolved in 60 mL DMF, and then 200 mg Ce-MOF-808 was added. The suspension was placed in a 100 mL polytetrafluoroethylene-lined stainless steel reactor and reacted in an oven at 100 °C for 24 h. After cooling to room temperature, the mother liquor was poured out and washed with DMF 3 times (3×50 mL) until the DMF was colorless. The obtained solid material was soaked in DMF (50 mL) for 36 h, during which the DMF was replaced every 12 h. The DMF-soaked material was soaked in acetone (50 mL) for 36 h, during which the acetone was replaced every 12 h. After vacuum drying at 80 °C for 24 h, it was vacuum activated at 100 °C for 5 h. Ce-MOF-808-25Cu-A was obtained.

[0046] Example 3

[0047] After DMF (12 mL) and formic acid (4.0 mL, 99%) were added to a round-bottom flask, H 3 BTC (224 mg, 1.06 mmol). Add (NH 4 ) 2 Ce(NO 3 ) 6 (6 mL, 0.533 M) in water. The round-bottom flask was sealed and heated in an oil bath at 100 °C with vigorous stirring for 15 min. After cooling to room temperature, the white precipitate was centrifuged in the mother liquor, washed, and centrifuged twice in DMF (20 mL). To remove DMF from the product, the solid was subsequently washed and centrifuged four times with acetone (20 mL). The obtained white solid was dried in vacuo at 60 °C. 1 mmol Cu(OAc) 2 ·H 2 O was dissolved in 60 mL DMF, and then 200 mg Ce-MOF-808 was added. The suspension was placed in a 100 mL polytetrafluoroethylene-lined stainless steel reactor and reacted in an oven at 100 °C for 24 h. After cooling to room temperature, the mother liquor was poured out and washed with DMF 3 times (3×50 mL) until the DMF was colorless. The obtained solid material was soaked in DMF (50 mL) for 36 h, during which the DMF was replaced every 12 h. The DMF-soaked material was soaked in acetone (50 mL) for 36 h, during which the acetone was replaced every 12 h. After exchanging the solvent with acetone, the solid was placed in an ethanol solution at 70 °C for 6 h and vacuum dried at 80 °C for 24 h. The active site Cu in the obtained Ce-MOF-808-25Cu-E single atom catalyst is more in Cu(II).

[0048] like Figure 5The XPS graphs of Cu in Ce-MOF-88 and Ce-MOF-808-25Cu under different treatment conditions are used to analyze the valence changes. It can be seen that more Cu appears after ethanol and activation treatment. + .

[0049] like Figure 6 The performance comparison analysis of Ce-MOF-88 and Ce-MOF-808-25Cu is shown in the figure. The test reaction time is 10 h. It can be seen that the single-atom and uniformly distributed Cu(I) in Ce-MOF-808 after ethanol and activation treatment is beneficial to improving the catalytic performance.

[0050] Example 4

[0051] After DMF (12 mL) and formic acid (4.0 mL, 99%) were added to a round-bottom flask, H 3 BTC (224 mg, 1.06 mmol). Add (NH 4 ) 2 Ce(NO 3 ) 6 (6 mL, 0.533 M) in water. The round-bottom flask was sealed and heated in an oil bath at 100 °C with vigorous stirring for 15 min. After cooling to room temperature, the white precipitate was centrifuged in the mother liquor, washed, and centrifuged twice in DMF (20 mL). To remove DMF from the product, the solid was subsequently washed and centrifuged four times with acetone (20 mL). The obtained white solid was dried in vacuo at 60 °C. Cu(OAc) 2 ·H 2 O (20 wt%: 157 mg; 25 wt%: 200 mg, 1 mmol; 30wt%: 269 mg) was dissolved in 60 mL DMF, and then 200 mg Ce-MOF-808 was added. The suspension was placed in a 100 mL polytetrafluoroethylene-lined stainless steel reactor and reacted in an oven at 100 °C for 24 h. After cooling to room temperature, the mother liquor was poured out and washed with DMF 3 times (3×50 mL) until the DMF was colorless. The obtained solid material was soaked in DMF (50 mL) for 36 h, during which the DMF was replaced every 12 h. The DMF-soaked material was soaked in acetone (50 mL) for 36 h, during which the acetone was replaced every 12 h. After exchanging the solvent with acetone, the solid was placed in an ethanol solution at 70 °C for 6 h, vacuum dried at 80 °C for 24 h, and vacuum activated at 100 °C for 5 h before reacting. Ce-MOF-808 catalysts with different Cu doping amounts were obtained, from Figure 7It can be seen that when the test reaction time is 15 h, Ce-MOF-808-20Cu-EA, Ce-MOF-808-25Cu-EA, and Ce-MOF-808-30Cu-EA all have good catalytic hydrogenation DCPD performance.

[0052] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.

Claims

1. A method for preparing a MOF-based Cu(I) single-atom catalytic material, characterized in that: The specific preparation steps are as follows: 1) Synthesis of Ce-MOF-808 Add N,N-dimethylformamide (DMF), formic acid, trimesic acid (H3BTC) and cerium (IV) ammonium nitrate aqueous solution (NH4)2Ce(NO3)6 into a round-bottom flask. The molar ratio of each component is (NH4)2Ce(NO3)6: H3BTC: formic acid: DMF: H2O = 1~3: 1: 100~0: 155: 1~10. Seal the round-bottom flask, stir vigorously and heat in an oil bath at 100 °C for 10 to 30 minutes. After cooling to room temperature, the white precipitate is centrifuged in the mother liquor, washed and dried to obtain Ce-MOF-808. 2) Synthesis of Ce-MOF-808-xCu-y The soluble anchor metal salt cupric acetate monohydrate is dissolved in DMF, and then Ce-MOF-808 is added to form a suspension, and then the suspension is placed in a reactor of a polytetrafluoroethylene-lined stainless steel reactor for post-modification reaction. The reaction is carried out in an oven at 100 to 120 °C for 24 to 36 hours. After cooling to room temperature, the mother liquor is poured out and washed with DMF until DMF is colorless. The obtained solid material is soaked in DMF and then in acetone, and the solvent is exchanged with acetone, followed by ethanol or vacuum activation or ethanol and vacuum activation treatment to obtain Ce-MOF-808-xCu-y, wherein x = 20, 25, 30 wt%.

2. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: The formic acid concentration in step 1) is 99%.

3. The method for preparing the MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: In step 1), the white precipitate is centrifuged in the mother liquor, washed and dried by centrifuging the white precipitate twice in DMF to remove DMF, then washing the solid with acetone and centrifuging it four times, and the obtained white solid is dried in a vacuum at 60°C.

4. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: The copper acetate monohydrate added in step 2) is preferably added in an amount of 25 wt %.

5. The method for preparing the MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: The DMF washing times in step 2) is 3 times.

6. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: The immersion in DMF of step 2) is 36 hours, during which the DMF is replaced every 10 to 12 hours; the immersion in acetone is 30 to 40 hours, during which the acetone is replaced every 10 to 12 hours.

7. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 1, characterized in that: The ethanol or vacuum activation or ethanol and vacuum activation treatment described in step 2) is specifically: (1) Ethanol treatment is to place the solid in an ethanol solution at 60 ~ 80 °C for 4 ~ 7 h and then dry it to obtain Ce-MOF-808-xCu-E, where y = E represents ethanol treatment; (2) Vacuum activation treatment is to exchange the solvent with acetone and then dry it, and then vacuum activate it at 80 ~ 150 °C for 1 ~ 5 h to obtain Ce-MOF-808-xCu-A, y = A represents vacuum activation treatment; (3) Ethanol and vacuum activation treatment is to exchange the solvent with acetone, then perform ethanol treatment, place the solid in an ethanol solution at 60 ~ 80 °C for 4 ~ 7 h, dry it, and then perform vacuum activation treatment at 80 ~ 150 °C for 1 ~ 5 h to obtain Ce-MOF-808-xCu-EA, where y = EA represents ethanol and activation treatment.

8. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 1 or 7, characterized in that: The synthesis reaction described in step 2) obtains Ce-MOF-808-xCu-y, preferably y=EA, and the ethanol treatment time is preferably 6 h, and the activation treatment is at a temperature of 100°C for 5 h.

9. The method for preparing a MOF-based Cu(I) single-atom catalytic material according to claim 7, characterized in that: The vacuum activation or ethanol and vacuum activation drying treatment is vacuum drying at 80° C. for 24 h.

Citation Information

Patent Citations

  • Method for preparing superfine cerium dioxide supported metal monatomic catalyst from cluster-based framework material

    CN114293223A

  • Catalyst for synthesizing dimethyl carbonate from carbon dioxide and methanol and preparation method thereof

    CN116809050A

  • Preparation method of rare earth MOFs catalytic material for hydrogenation of dicyclopentadiene

    CN116903868A

  • Metal particle Cu-loaded CeO2 catalyst for catalytic synthesis of methanol through hydrogenation of carbon dioxide as well as preparation method and application of metal particle Cu-loaded CeO2 catalyst

    CN118059873A

Cited By

  • Method for preparing sustainable aviation fuel crude oil from polyhydric alcohols and crude oil prepared by method

    CN120536155A

  • Method for preparing unrefined SAF intermediate using polyols and the SAF intermediate prepared thereby

    US12668751B1