Box wall flange welding method
By releasing reinforcement ribs inside the box wall flange and cutting them off after welding, providing rigid welding support, the problem of welding deformation of the transformer box wall flange is solved, and good connection and leakage between the box wall flange and the box wall is achieved. prevent.
Patent Information
- Application Number
- CN202411457709.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-29
AI Technical Summary
The transformer box wall flange is prone to deformation due to welding stress during welding, resulting in excessive gaps on the butt surface and leakage problems.
Reinforcement ribs are reserved inside the box wall flange and cut them off after welding to provide rigid support during welding and reduce welding deformation. The specific steps include cutting reinforcement ribs with CNC air cutting machine, machining and welding, and using spot welding, interrupted welding and anti-welding processes.
It effectively reduces the deformation problem during welding of box wall flanges, ensures good connection between box wall flanges and box walls, and avoids leakage.
Smart Images

Figure CN119035997A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of transformers, and more particularly to a box wall flange welding method. Background Art
[0002] As the capacity of high-voltage, ultra-high-voltage and extra-high-voltage transformers continues to increase, the performance parameter requirements continue to increase, and the size of the transformers also increases accordingly. The box wall of some transformer products will use an extra-long flange. Due to the size limit of the box wall and the processing cost, the box wall flange is usually not machined after being cut by a gas cutting machine, and then it will be welded to the box wall of the transformer.
[0003] Since the square box wall flange is long, the weld is long. The long weld is prone to welding stress, which leads to welding deformation, thus causing the box wall flange to bulge, shrink, wave bend, etc. If the box wall flange is deformed, it is easy to make the gap between the box wall flange and the box wall too large, resulting in leakage problems.
[0004] Therefore, how to reduce the welding deformation caused by welding stress during welding of the box wall flange is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a box wall flange welding method to reduce welding deformation caused by welding stress during box wall flange welding.
[0006] To achieve the above object, the present invention provides the following technical solutions: A box wall flange welding method, comprising: A box wall flange preparation step, preparing a box wall flange to be welded, wherein the box wall flange is pre-equipped with reinforcing ribs, and the reinforcing ribs connect two mutually parallel flange edges of the box wall flange; The box wall flange welding step is to weld the box wall flange to the corresponding position of the transformer box wall; The reinforcement rib removal step is to cut off the reinforcement ribs reserved on the box wall flange.
[0007] Optionally, in the above-mentioned box wall flange welding method, the box wall flange preparation step specifically includes: Use a CNC gas cutting machine to cut the material, take the inner middle part of the box wall flange to be prepared as the initial cutting point, and start from the initial cutting point, first cut the interval between two adjacent reinforcing ribs, and then cut the interval between the reinforcing ribs at both ends and the flange edge, so as to form each of the reinforcing ribs; After the internal cutting of the box wall flange is completed, the external contour of the box wall flange to be prepared is cut. When cutting the external contour of the box wall flange, the length direction of the box wall flange is cut first, and the position with lower temperature is used as the starting point for cutting.
[0008] Optionally, in the above-mentioned box wall flange welding method, the box wall flange preparation step further includes a slag cleaning step, and the slag cleaning step is performed after the inside and the outside of the box wall flange are cut; The steps for cleaning the oxide slag are as follows: cleaning the oxide slag produced by cutting the box wall flange.
[0009] Optionally, in the above-mentioned box wall flange welding method, a machining step is further included between the box wall flange preparation step and the box wall flange welding step; The machining step is: planing off the corresponding thickness of the front side of the flange edge to process the flange edge to the target thickness, and at the same time planing off the processing grooves of preset width at both ends of the reinforcement rib, the processing grooves are the cutting positions in the reinforcement rib removal step, and the front side of the flange edge is the side of the flange edge with a threaded hole.
[0010] Optionally, in the above-mentioned box wall flange welding method, the preset width is 2-4 mm.
[0011] Optionally, in the above-mentioned box wall flange welding method, the box wall flange welding step includes: Spot welding step, spot welding the inside and outside of the box wall flange to the transformer box wall respectively, and the spot welding positions are arranged at intervals; The intermittent welding step is to first perform intermittent welding from the spot welding position at the inner center of the box wall flange to both sides step by step, and then perform intermittent welding from the spot welding position at the outer center of the box wall flange to both sides step by step; Impurity cleaning step, clean up the impurities in the intermittent welding seam; The de-welding procedure starts from the inner width direction of the box wall flange and avoids the corners, and is gradually de-welded in sections of 200 to 250 mm. After the inner welding of the box wall flange is completed, the outer part of the box wall flange is welded in the same de-welding method, and the outer weld is consistent with the inner weld in welding direction.
[0012] Optionally, in the above-mentioned box wall flange welding method, the spot welding step is specifically: first spot welding the inner four corners of the box wall flange, then spot welding the outer four corners of the box wall flange, then spot welding the inner center of the box wall flange, and finally spot welding the outer center of the box wall flange; and / or, In the intermittent welding step, the welding current of the intermittent welding is 180A, the voltage is 22V, the length of the intermittent weld is 25mm~35mm, and the spacing of the intermittent weld is 150mm~250mm; and / or, In the desoldering step, the desoldering current ranges from 250A to 300A, and the welding voltage ranges from 26 to 33 V; and / or, In both the intermittent welding step and the de-welding step, gas shielded welding is used as the welding process, the welding wire is alloy steel welding wire, the welding wire diameter is 1-1.4 mm, and the welding shielding gas is a mixture of argon and carbon dioxide.
[0013] Optionally, in the above-mentioned box wall flange welding method, the reinforcing rib removal step specifically includes: The reinforcement rib cutting steps are as follows: first cut the reinforcement rib in the middle of the box wall flange, and then symmetrically cut the reinforcement ribs on both sides of the box wall flange; The step of grinding the cutting position is to grind the cutting position of the reinforcing rib so that the cutting position is coplanar with the inner surface of the box wall flange.
[0014] Optionally, in the above-mentioned box wall flange welding method, in the reinforcement rib cutting step, a manual cutting torch is used to cut the reinforcement rib, and the manual cutting torch uses an oxygen pressure of 0.35~0.5MPa and a cutting speed of 230~350mm / min.
[0015] Optionally, in the above-mentioned box wall flange welding method, the width of the reinforcing rib is 0.5 to 0.8 times the width of the flange edge; and / or, The distance between two adjacent reinforcing ribs is 300-500 mm.
[0016] The box wall flange welding method provided by the present invention, when preparing the box wall flange, some reinforcing ribs that can connect two parallel flange edges are reserved inside the box wall flange. The box wall flange with the reserved reinforcing ribs is welded to the transformer box wall, and after the box wall flange welding is completed, the reinforcing ribs are cut off. By reserving the reinforcing ribs, the box wall flange has rigid support of the reinforcing ribs inside during welding. Even if stress is generated during the welding process, the problem of flange shrinkage and distortion can be reduced due to the rigid support of the reinforcing ribs. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 It is a front view of the box wall flange disclosed in the embodiment of the present invention; Figure 2It is a cross-sectional view of the box wall flange after being welded to the box wall according to the embodiment of the present invention; Figure 3 It is a flow chart of the box wall flange welding method disclosed in an embodiment of the present invention; Figure 4 A flow chart of the box wall method preparation steps disclosed in an embodiment of the present invention; Figure 5 Flow chart of a box wall flange welding method disclosed in another embodiment of the present invention Figure 6 A flow chart of the box wall welding steps disclosed in an embodiment of the present invention; Figure 7 The present invention is a flowchart of the rib removal step disclosed in an embodiment of the present invention.
[0019] The meanings of the reference numerals in the figures are as follows: 101-flange edge; 102-internal hole of flange; 103-reinforcement rib; 1031-processing groove; 201- Transformer box wall. DETAILED DESCRIPTION
[0020] The core of the present invention is to provide a box wall flange welding method to reduce welding deformation caused by welding stress during box wall flange welding.
[0021] The following embodiments are described with reference to the accompanying drawings. In addition, the embodiments shown below do not limit the invention contents described in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary as solutions to the inventions described in the claims. It should be noted that, for ease of description, only the parts related to the inventions are shown in the accompanying drawings. The embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0022] like Figure 1-Figure 3 As shown, the box wall flange welding method disclosed in the embodiment of the present invention includes: Step S100: preparing the box wall flange; Prepare the box wall flange to be welded, and the box wall flange is reserved with reinforcing ribs 103, and the reinforcing ribs 103 connect the two parallel flange edges 101 of the box wall flange. Specifically, according to the required size, prepare the box wall flange, reserve reinforcing ribs inside the box wall flange, and the reinforcing ribs 103 connect the two parallel flange edges 101 of the box wall flange. Taking the box wall flange as a rectangle as an example, the reinforcing ribs 103 can connect the two long sides of the box wall flange, and the reinforcing ribs 103 are parallel to the wide side of the box wall flange. Between the reinforcing ribs 103 and between the reinforcing ribs 103 and the wide side of the box wall flange are flange internal holes 102.
[0023] Step S200: welding the box wall flange; The box wall flange is welded to the corresponding position of the transformer box wall 201. Specifically, the inside of the box wall flange can be welded first, and then the outside of the box wall flange can be welded. Usually, the size of the inner hole 102 of the box wall flange is smaller than the size of the hole at the corresponding position on the transformer box wall 201, so that when welding the inside of the box wall flange, the weld is located between the back of the box wall flange and the inner wall of the hole on the transformer box wall 201.
[0024] Step S300: removing the reinforcing ribs; After the box wall flange is welded, because it will no longer be affected by welding stress, the reinforcement ribs 103 reserved on the box wall flange need to be cut off so that the box wall flange can be used normally. It should be noted that the cutting method of the reinforcement ribs is not limited, as long as the removal of the reinforcement ribs 103 can be completed. This embodiment does not require the cutting method of the reinforcement ribs.
[0025] The box wall flange welding method provided by the present invention reserves some reinforcing ribs 103 that can connect two parallel flange edges inside the box wall flange when preparing the box wall flange. The box wall flange with the reserved reinforcing ribs 103 is welded to the transformer box wall 201, and after the box wall flange welding is completed, the reinforcing ribs 103 are cut off. By reserving the reinforcing ribs 103, during welding, since the inside of the box wall flange has the rigid support of the reinforcing ribs 103, even if stress is generated during the welding process, the rigid support of the reinforcing ribs 103 can reduce the problems of flange shrinkage and distortion. Please combine Figure 4 As shown, in a specific embodiment of the present invention, the box wall flange preparation step specifically includes: S101: Internal cutting of the box wall flange; Use a CNC gas cutting machine to cut the material, and use the middle part of the interior of the box wall flange to be prepared as the initial cutting point. When cutting, start cutting from the initial cutting point as the starting point, first cut the space between two adjacent reinforcing ribs 103, and then cut the space between the reinforcing ribs 103 at both ends and the flange edge 101 to form each reinforcing rib 103, that is, by removing material, the remaining internal part of the box wall flange forms the reinforcing rib 103.
[0026] In this embodiment, the inner middle position of the box wall flange is cut first, and then the edge portion is cut, so as to prevent deformation when cutting the inner hole of the box wall flange.
[0027] When cutting, the corresponding cutting nozzle should be selected according to the thickness of the box wall flange. For example, when the thickness of the box wall flange is 36mm, the No. 3 cutting nozzle can be selected, and the middle part of the internal hole 102 of the flange can be selected as the initial cutting point, and the cutting can be started from this point. The cutting can be carried out from the length direction of the box wall flange first. The high-energy cutting gas pressure of the CNC gas cutting machine can be controlled at 0.2MPa, and the cutting speed can be controlled at 270mm / min. It should be noted that the specific cutting nozzle model, cutting gas pressure and cutting speed should be selected according to the actual scenario. The above specific data are only for the convenience of understanding this solution, and the examples made do not constitute a limitation on this solution.
[0028] The width of the reinforcing rib can be 0.5~0.8 times the width of the flange edge 101. It should be noted that the width of the flange edge 101 does not refer to the wide side size of the box wall flange, but the width of the flange edge 101 itself, that is, the size between the outer contour and the inner contour of the box wall flange.
[0029] The spacing and number of reinforcing ribs are set in proportion to the length and width of the box wall flange to be welded. In this embodiment, on the transformer box wall 201 with a thickness of 12 mm, a box wall flange with a welding length of 1450 mm and a width of 500 mm is welded, and the flange edge 101 of the box wall flange is 50 mm wide. Therefore, the width of the reinforcing rib 103 can be selected as 25-40 mm, for example, 30 mm, and the width of the spacing can be selected as 315 mm, and the number is 3.
[0030] S102: External cutting of box wall flange; After the internal cutting of the box wall flange is completed, the external contour of the box wall flange to be prepared is cut. When cutting the external contour of the box wall flange, the length direction of the box wall flange is cut first, and the position with lower temperature is used as the starting point for cutting. For example, when cutting the long side of the box wall flange, the position where the internal hole cutting of the box wall flange ends can be selected. For example, when the internal hole cutting ends at the first end of the long side, then when cutting the outside, the cutting can be started from the second end. This is because the position where the internal hole cutting just ends has a higher temperature, and the position with higher temperature should be avoided to avoid deformation due to continued temperature increase during cutting. After cutting the long side of the box wall flange, cut the wide side of the box wall flange until the cutting process of the external contour of the box wall flange is completed.
[0031] Furthermore, the box wall flange preparation step also includes: S103: cleaning slag; The step of cleaning the slag should be performed after the inside and outside of the box wall flange are cut. The step of cleaning the slag is to clean the slag generated by cutting the box wall flange to prevent the slag from affecting subsequent machining.
[0032] In the step of removing the reinforcing ribs, a manual cutting torch is usually used to cut and remove the reinforcing ribs 103. During the cutting process, the flame ejected by the manual cutting torch is likely to damage the inner edge of the box wall flange. In order to prevent the flame from being too close to the flange edge 101 and damaging the inner edge of the box wall flange when the reinforcing ribs 103 are cut off later, a machining step is added between the box wall flange preparation step and the box wall flange welding step in this embodiment, such as Figure 5 shown.
[0033] Step S110: machining; The corresponding thickness of the front side of the flange edge 101 is planed off (the front side of the flange edge 101 is the side of the flange edge 101 with the threaded hole, and the threaded hole can be drilled after the thinning of the box wall flange is completed) to process the flange edge 101 to the target thickness. After the box wall flange is cut, the thickness direction of the box wall flange needs to be processed to process the flange edge 101 to the target thickness of the box wall flange design. The reinforcing ribs 103 need to be cut off later, so in the process of machining and thinning the flange edge 101, the reinforcing ribs 103 theoretically do not need to be thinned.
[0034] In this embodiment, while the flange edge 101 is being thinned, the machining grooves 1031 (for example, Figure 2 The portion circled by the dotted line frame), that is, in this embodiment, a distance at both ends of the reinforcing rib 103 is also thinned, and the thinned portion forms a processing groove 1031. The surface at the processing groove 1031 can be coplanar with the surface of the flange edge 101, that is, when processing the flange edge 101, the processing groove 1031 can be processed in one pass. Since the reinforcing rib 103 is not completely thinned, a step is formed at the processing groove 1031. The processing groove 1031 is used as the cutting position in the reinforcing rib removal step, that is, when cutting, the position of the step can be cut so that there is a distance from the flange edge 101, so as to prevent the flame from being too close to the flange edge 101 when the reinforcing rib 103 is cut off later, thereby damaging the inner edge of the ring box wall flange.
[0035] Furthermore, the preset width of the processing groove 1031 can be designed to be 2-4 mm, for example, 3 mm. It should be noted that the preset width of the processing groove 1031 can also be designed to be other sizes, which can be specifically designed according to needs.
[0036] like Figure 6 As shown, in a specific embodiment of the present invention, the box wall flange welding step includes: S201: box wall flange spot welding; The inside and outside of the box wall flange are spot welded to the transformer box wall 201, and the spot welding positions are arranged at intervals. Specifically, the inner four corners of the box wall flange can be spot welded first, and then the outer four corners of the box wall flange can be spot welded, and then the inner center of the box wall flange can be spot welded, and finally the outer center of the box wall flange can be spot welded. That is, in this embodiment, the inner four corners, the outer four corners, the inner center and the outer center of the box wall flange need to be arranged with spot welding positions.
[0037] In this embodiment, the box wall flange can be fixed to the transformer box wall 201 by uniformly spot welding the edge and the middle of the box wall flange; at the same time, the order of spot welding the four corners first, then the middle, first the inside, and then the outside is adopted, which can enhance the advancedness of the position prone to shrinkage and reduce the possibility of deformation.
[0038] S202: intermittent welding of box wall flange; First, intermittent welding is performed gradually from the spot welding position at the inner center of the box wall flange to both sides, and then intermittent welding is performed gradually from the spot welding position at the outer center of the box wall flange to both sides. Specifically, the welding current of intermittent welding can be 180A, the voltage can be 22V, the length of the intermittent weld is 25mm~35mm (for example, 30mm), and the spacing of the intermittent weld is 150mm~250mm (for example, 200mm).
[0039] S203: impurity cleaning; Clean up the impurities in the intermittent welding seam to avoid the impurities generated by intermittent welding affecting the subsequent desoldering steps.
[0040] S204: box wall flange back welding; Starting from the inner width direction of the box wall flange and avoiding the corner position, gradually back-weld in sections of 200~250mm. The two welds at the corners of the box wall flange are at a 90° angle. After being heated, the angle is prone to stress concentration and deformation. Therefore, when welding the box wall flange, try to avoid starting and ending at the corners. It is best to avoid a distance of 100mm. After the inner and outer welds of the long and wide sides are welded and rigidly fixed and strengthened, it is not easy to deform if you weld the corners at the end.
[0041] After the internal welding of the box wall flange is completed, the same back-welding method is used to weld the outside of the box wall flange, and the welding direction of the external weld is consistent with that of the internal weld.
[0042] In the desoldering step, the welding current range of the desoldering can be 250A~300A, and the welding voltage range can be 26~33 V. It should be noted that other ranges of welding current and welding voltage can be selected, and the specific range should be selected according to the actual scenario.
[0043] Gas shielded welding is used as the welding process in both the intermittent welding step and the de-welding step. The welding wire is alloy steel welding wire with a diameter of 1-1.4 mm (e.g., 1.2 mm). The welding shielding gas is a mixture of argon and carbon dioxide (e.g., argon: carbon dioxide = 4:1).
[0044] In this embodiment, by intermittently welding the box wall flange and then gradually retreating the welding, the heat distribution of the weld between the box wall flange and the transformer box wall 201 is uniform and deformation is not easy to occur.
[0045] like Figure 7 As shown, in a specific embodiment of the present invention, the rib removal step specifically includes: S301: rib cutting; First, the reinforcing rib 103 in the middle of the box wall flange is cut, and then the reinforcing ribs 103 on both sides of the box wall flange are cut symmetrically. It should be noted that symmetrically cutting the reinforcing ribs 103 on both sides of the box wall flange does not mean that the two reinforcing ribs 103 are cut at the same time, but after cutting one of the reinforcing ribs 103, the other reinforcing rib 103 symmetrical to the reinforcing rib 103 is cut.
[0046] Taking three reinforcing ribs 103 as an example, the three reinforcing ribs 103 are respectively the first reinforcing rib, the second reinforcing rib and the third reinforcing rib from left to right. The second reinforcing rib in the middle is cut first, then the first reinforcing rib is cut, and finally the third reinforcing rib is cut.
[0047] Take five reinforcing ribs 103 as an example, the five reinforcing ribs 103 are respectively the first reinforcing rib, the second reinforcing rib, the third reinforcing rib, the fourth reinforcing rib and the fifth reinforcing rib from left to right. The third reinforcing rib in the middle is cut first, then the second reinforcing rib, then the fourth reinforcing rib, then the first reinforcing rib and finally the fifth reinforcing rib.
[0048] S302: grinding of cutting position; The cutting position of the reinforcing rib is polished so that the cutting position is coplanar with the inner surface of the box wall flange. It should be noted that since the cutting position is the position of the processing groove 1031, the processing groove 1031 has a certain width, so after the reinforcing rib is cut, a part will remain on the inner wall of the box wall flange, and the remaining part can be removed by polishing to make the inner wall of the box wall flange smooth.
[0049] Furthermore, in the reinforcement cutting step, a manual cutting torch can be used to cut the reinforcement, and the corresponding cutting nozzle is selected according to the thickness of the box wall flange. The manual cutting torch uses an oxygen pressure of 0.35~0.5MPa to make the cutting oxygen flow form a straight wind line that exceeds the thickness of the flange, and cut evenly along the machining groove 1031 reserved for machining at a cutting speed of 230~350mm / min.
[0050] In summary, the box wall flange welding method disclosed in the embodiment of the present invention reserves a plurality of equidistantly arranged reinforcing ribs 103 in the box wall flange, so that the box wall flange is rigidly supported by multiple groups of reinforcing ribs 103 from the inside. During welding, the reinforcing ribs 103 are retained to reduce the welding stress generated by high temperature during welding, which may cause problems such as flange shrinkage and distortion.
[0051] In addition, spot welding, intermittent welding, step-back welding and other welding methods are symmetrically used during welding, so that the welding deformation of the box wall flange on the transformer box wall 201 can be better controlled.
[0052] As shown in this application and claims, unless the context clearly indicates an exception, the words "a", "an", "a kind" and / or "the" do not refer to the singular, but also include the plural. Generally speaking, the terms "include" and "comprise" only indicate the inclusion of clearly identified steps and elements, and these steps and elements do not constitute an exclusive list. The method or device may also include other steps or elements. The elements defined by the sentence "includes a..." do not exclude the existence of other identical elements in the process, method, commodity or device that includes the elements.
[0053] In the description of this application, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in this application based on the specific content of the technical solution.
[0054] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0055] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core ideas of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A box wall flange welding method, characterized in that: include: A box wall flange preparation step, preparing a box wall flange to be welded, wherein the box wall flange is provided with a reinforcing rib (103) in advance, wherein the reinforcing rib (103) connects two mutually parallel flange edges (101) of the box wall flange; A box wall flange welding step, welding the box wall flange to a corresponding position of the transformer box wall (201); The reinforcement rib removal step is to cut off the reinforcement rib (103) reserved on the box wall flange.
2. The box wall flange welding method according to claim 1, characterized in that: The box wall flange preparation steps specifically include: Cutting the material using a CNC gas cutting machine, taking the inner middle part of the box wall flange to be prepared as the initial cutting point, and starting from the initial cutting point, first cutting the space between two adjacent reinforcing ribs (103), and then cutting the space between the reinforcing ribs (103) at both ends and the flange edge (101), so as to form each of the reinforcing ribs (103); After the internal cutting of the box wall flange is completed, the external contour of the box wall flange to be prepared is cut. When cutting the external contour of the box wall flange, the length direction of the box wall flange is cut first, and the position with lower temperature is used as the starting point for cutting.
3. The box wall flange welding method according to claim 2, characterized in that: The box wall flange preparation step also includes a slag cleaning step, which is performed after the inside and outside of the box wall flange are cut; The steps for cleaning the oxide slag are as follows: cleaning the oxide slag produced by cutting the box wall flange.
4. The box wall flange welding method according to claim 1, characterized in that: A machining step is also included between the box wall flange preparation step and the box wall flange welding step; The machining step comprises: planing off the corresponding thickness of the front side of the flange edge (101) to machine the flange edge (101) to a target thickness, and planing off machining grooves of a preset width at both ends of the reinforcing rib (103), wherein the machining grooves are cutting positions in the reinforcing rib removal step, and the front side of the flange edge (101) is a side of the flange edge (101) having a threaded hole.
5. The box wall flange welding method according to claim 4, characterized in that: The preset width is 2-4 mm.
6. The box wall flange welding method according to any one of claims 1 to 5, characterized in that: The box wall flange welding steps include: a spot welding step, spot welding the inside and the outside of the box wall flange to the transformer box wall (201) respectively, and the spot welding positions are arranged at intervals; The intermittent welding step is to first perform intermittent welding from the spot welding position at the inner center of the box wall flange to both sides step by step, and then perform intermittent welding from the spot welding position at the outer center of the box wall flange to both sides step by step; Impurity cleaning step, clean up the impurities in the intermittent welding seam; The de-welding procedure starts from the inner width direction of the box wall flange and avoids the corners, and is gradually de-welded in sections of 200 to 250 mm. After the inner welding of the box wall flange is completed, the outer part of the box wall flange is welded in the same de-welding method, and the outer weld is consistent with the inner weld in welding direction.
7. The box wall flange welding method according to claim 6, characterized in that: The spot welding step is specifically as follows: first spot welding the inner four corners of the box wall flange, then spot welding the outer four corners of the box wall flange, then spot welding the inner center of the box wall flange, and finally spot welding the outer center of the box wall flange; and / or, In the intermittent welding step, the welding current of the intermittent welding is 180A, the voltage is 22V, the length of the intermittent weld is 25mm~35mm, and the spacing of the intermittent weld is 150mm~250mm; and / or, In the desoldering step, the desoldering current ranges from 250A to 300A, and the welding voltage ranges from 26 to 33 V; and / or, In both the intermittent welding step and the de-welding step, gas shielded welding is used as the welding process, the welding wire is alloy steel welding wire, the welding wire diameter is 1-1.4 mm, and the welding shielding gas is a mixture of argon and carbon dioxide.
8. The box wall flange welding method according to any one of claims 1 to 5, characterized in that: The rib removal step specifically includes: The reinforcement rib cutting steps are as follows: first cut the reinforcement rib in the middle of the box wall flange, and then symmetrically cut the reinforcement ribs on both sides of the box wall flange; The step of grinding the cutting position is to grind the cutting position of the reinforcing rib so that the cutting position is coplanar with the inner surface of the box wall flange.
9. The box wall flange welding method according to claim 8, characterized in that: In the reinforcing rib cutting step, a manual cutting torch is used to cut the reinforcing rib, and the manual cutting torch uses an oxygen pressure of 0.35-0.5 MPa, and a cutting speed of 230-350 mm / min.
10. The box wall flange welding method according to any one of claims 1 to 5, characterized in that: The width of the reinforcing rib is 0.5 to 0.8 times the width of the flange edge (101); and / or, The distance between two adjacent reinforcing ribs is 300-500 mm.
Citation Information
Patent Citations
Welding method for reducing body deformation of armored car
CN105252152A
Control method for workpiece machining deformation
CN110293366A
Leak-proof structure of opening of flange of pressure vessel
CN203162137U
Rigid reinforcing rib structure capable of preventing welding deformation
CN211966446U
Lateral rod of vehicle suspension
KR1019990002242A