Manufacturing method and mold of curved surface polyimide film
By coating and treating polyimide acid solutions on curved molds at high temperatures, the problem that the plane film cannot meet the accuracy requirements of curved antennas is solved, and a curved polyimide film with high accuracy and uniformity is prepared, suitable for ultra-large diameters Reflective surface material of thin film antenna.
Patent Information
- Application Number
- CN202411157294.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The polyimide film prepared in the prior art is plane and cannot meet the accuracy requirements of curved antenna reflection surfaces.
The curved polyimide film is prepared by uniformly coating the polyamic acid precursor solution on the surface of the mold and dehydrating imidizing at high temperature. The mold uses lightweight, low thermal expansion coefficient metal material, such as 7075 aviation aluminum, with the surface polished and the radius of curvature of the mold is 2 to 8 meters, which is suitable for forming high-precision curved surface shapes.
It has achieved high-precision and uniformity of curved polyimide film preparation, suitable for reflective surface materials of ultra-large diameter thin film antennas, improving profile accuracy and curved shape maintenance.
Smart Images

Figure CN119036723A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a method for manufacturing a curved polyimide film and a mold. Background Art
[0002] As a core component of the satellite system, large satellite antennas occupy an important position, and their performance indicators directly determine the realization of satellite system functions. With the improvement of technical requirements, the requirements for satellite antenna indicators are also getting higher and higher. The development of satellite antennas mainly presents the following trends: 1) The size of the antenna is increasing. In order to obtain stronger signals as much as possible, a larger antenna size is required in the orbit state to better meet the relevant needs; 2) The requirements for antenna surface accuracy are improved. Generally speaking, the root mean square error of the antenna surface error is required to be guaranteed to be 1 / 50-1 / 20 of the antenna wavelength. The promotion and application of satellite antennas in high frequency bands puts forward higher requirements for antenna surface accuracy; 3) Lower mass and smaller stowed volume. Existing launch vehicles and space shuttles have strict requirements on reserved space and weight, so satellite antennas are required to have the characteristics of light mass and small stowed volume.
[0003] The main feature of the thin film reflector antenna is that the solid reflector is replaced by a thin film structure reflector. It has the characteristics of large caliber, light weight, and small folded volume. It is an important technical direction to solve the large-scale satellite antenna. Polyimide film has become a commonly used thin film material for satellite-borne thin film antennas due to its excellent mechanical strength and tolerance to space environment. However, since the film prepared by the commonly used polyimide film preparation process is flat, the accuracy is not high when used as a curved antenna reflector. Therefore, using curved polyimide film as the reflector material of ultra-large caliber thin film antennas can effectively improve the surface accuracy of the reflector.
[0004] At present, polyimide film is usually prepared by casting polyamic acid (PAA), a soluble precursor solution of polyimide (PI), on an endless stainless steel belt, and then undergoing high-temperature imidization and stretching treatment. First, dianhydride monomer and diamine monomer are polymerized in dimethylacetamide solvent to obtain a PAA solution with suitable process viscosity and solid content, and then various additives such as release agents are added. After degassing treatment, the PAA solution is cast on a continuously running endless steel belt through a die head. After the solvent evaporates, it becomes a solid PAA film. Then, the self-supporting PAA film (cast film) is peeled off from the steel belt and introduced into an imidization furnace through a guide roller. Under high-temperature treatment, the PAA film is dehydrated, imidized, and continuously stretched longitudinally and transversely, and finally rolled up to obtain a finished PI film. The polyimide film prepared by this preparation method is flat and cannot meet the application requirements of the curved reflective surface of the antenna. Based on this requirement, a method for manufacturing a curved polyimide film is proposed. Summary of the invention
[0005] In view of the defect that the flat polyimide film in the prior art cannot meet the application requirements of the curved reflective surface of the antenna, the purpose of the present invention is to provide a method for manufacturing a curved polyimide film and a mold, which can directly prepare a curved polyimide film with high precision and good uniformity.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a method for manufacturing a curved polyimide film, comprising the following steps:
[0008] Step (1) manufacturing a mold according to the desired shape of the film reflective surface;
[0009] Step (2) preparing a polyamic acid precursor solution;
[0010] Step (3) uniformly coating the polyamic acid precursor solution on the surface of the mold to form a polyamic acid film;
[0011] Step (4) fixing the edge of the polyamic acid film at the edge of the mold using a fixed stretching fixture;
[0012] Step (5) placing the mold in an oven and baking at high temperature to perform dehydration imidization;
[0013] Step (6) demoulding to obtain a curved polyimide film.
[0014] Furthermore, in step (1), the mold is made of metal material, preferably a lightweight metal material with a low thermal expansion coefficient, and more preferably 7075 aviation aluminum.
[0015] Furthermore, in the step (1), the mold is manufactured by mechanical processing, and the surface of the mold is polished.
[0016] Furthermore, in the step (3), the polyamic acid precursor solution is applied to the surface of the mold by spraying, brushing or dipping, and the polyamic acid precursor solution is applied to the convex surface or the concave surface of the mold.
[0017] Furthermore, in step (5), the high temperature baking conditions are: firstly, heating to 300°C to 350°C, keeping the temperature for 2 to 6 hours, then heating to 400°C to 450°C, keeping the temperature for 16 to 24 hours.
[0018] In a second aspect, the present invention provides a mold for manufacturing a curved polyimide film, which is used to implement the method for manufacturing the curved polyimide film, and includes: a mold body, a mold convex surface, a mold concave surface, and a fixed stretching fixture.
[0019] Furthermore, the convex surface of the mold is used to coat a polyamic acid precursor solution to form a polyamide film.
[0020] Furthermore, the concave surface of the mold is used to coat a polyamic acid precursor solution to form a polyamide film.
[0021] Furthermore, the fixed stretching fixture is arranged at the edge of the mold to fix the edge of the polyamic acid film before the dehydration imidization treatment.
[0022] Furthermore, the mold is made of metal material, preferably a lightweight metal material with a low thermal expansion coefficient, and more preferably 7075 aviation aluminum.
[0023] Furthermore, the surface of the mold is a curved surface, preferably a spherical surface or a paraboloid.
[0024] Furthermore, the diameter of the mold is 0.8 to 2 m.
[0025] Furthermore, the radius of curvature of any point on the surface of the mold is 2 to 8 m.
[0026] The technical solution of the present invention has the following advantages:
[0027] The method provided by the present invention can directly prepare a curved polyimide film, effectively improving the profile accuracy of the reflective surface; the prepared curved polyimide film has the advantages of high profile accuracy, good uniformity, and good curved shape maintenance, and is suitable as a reflective surface material for ultra-large-aperture thin-film antennas, and can be applied to the preparation of space thin-film reflective surface antennas. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 A process flow chart of a method for manufacturing a curved polyimide film provided by an embodiment of the present invention;
[0030] Figure 2 A schematic diagram of a mold for manufacturing a curved polyimide film provided in an embodiment of the present invention;
[0031] Figure 3 Schematic diagram of preparing a curved polyimide film by concave coating in Example 1 of the present invention;
[0032] Figure 4Schematic diagram of preparing a curved polyimide film by convex coating in Example 2 of the present invention. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0034] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0035] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.
[0036] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.
[0037] In addition, the term "plurality" shall mean two or more.
[0038] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0039] The technical problem to be solved by the present invention is to overcome the problem that the polyimide film prepared by the prior art is flat and has low precision when used as a reflective surface of a curved antenna. To this end, the embodiment of the present invention provides a method for manufacturing a curved polyimide film and a mold, which can directly prepare a curved polyimide film and effectively improve the surface precision of the reflective surface. The curved polyimide film has the advantages of high precision and good uniformity, and is suitable for use as a reflective surface material for ultra-large-caliber film antennas.
[0040] See also Figure 1 The process flow of the method for manufacturing a curved polyimide film provided by an embodiment of the present invention is as follows: Figure 1 As shown, the following steps are included:
[0041] Step (1) manufacturing a mold according to the desired shape of the film reflective surface;
[0042] Step (2) preparing a polyamic acid precursor solution;
[0043] Step (3) uniformly coating the polyamic acid precursor solution on the surface of the mold to form a polyamic acid film;
[0044] Step (4) fixing the edge of the polyamic acid film at the edge of the mold using a fixed stretching fixture;
[0045] Step (5) placing the mold in an oven and baking at high temperature to perform dehydration imidization;
[0046] Step (6) demoulding to obtain a curved polyimide film.
[0047] Furthermore, in step (1), the material of the mold is metal material, preferably a lightweight metal material with a low thermal expansion coefficient, and more preferably 7075 aviation aluminum; the mold is manufactured by mechanical processing, and the surface of the mold is polished.
[0048] Furthermore, in step (3), the polyamic acid precursor solution is applied to the surface of the mold by spraying, brushing or dipping. The polyamic acid precursor solution can be applied to the convex surface or the concave surface of the mold.
[0049] Furthermore, in step (5), the high temperature baking conditions are: firstly, heating to 300°C to 350°C, keeping warm for 2 to 6 hours, then heating to 400°C to 450°C, keeping warm for 16 to 24 hours.
[0050] See also Figure 2 The manufacturing mold of the curved polyimide film provided in the embodiment of the present invention is used to implement the manufacturing method of the curved polyimide film, and includes: a mold body, a mold convex surface, a mold concave surface and a fixed stretching fixture.
[0051] Furthermore, the convex surface of the mold is used to coat a polyamic acid precursor solution to form a polyamide film.
[0052] Furthermore, the concave surface of the mold is used to coat a polyamic acid precursor solution to form a polyamide film.
[0053] Furthermore, a fixed stretching fixture is arranged at the edge of the mold to fix the edge of the polyamic acid film before the dehydration imidization treatment.
[0054] Furthermore, the mold is made of metal material, preferably a lightweight metal material with a low thermal expansion coefficient, and more preferably 7075 aviation aluminum.
[0055] Furthermore, the surface of the mold is a curved surface, preferably a spherical surface or a paraboloid.
[0056] Furthermore, the diameter of the mold is 0.8 to 2 m.
[0057] Furthermore, the radius of curvature of any point on the surface of the mold is 2 to 8 m.
[0058] The manufacturing method and mold of the curved polyimide film provided in the embodiment of the present invention can directly prepare the curved polyimide film, and effectively improve the profile accuracy of the reflective surface. The prepared curved polyimide film has high profile accuracy, good uniformity, and good curved shape maintenance, and is suitable as a reflective surface material for ultra-large-caliber film antennas, and can be applied to the preparation of space film reflective surface antennas.
[0059] Example 1
[0060] This embodiment provides a method for manufacturing a curved polyimide film, comprising the following steps:
[0061] Step (1) According to the required shape of the thin film reflective surface, 7075 aviation aluminum is used to manufacture a spherical mold by mechanical processing, and the mold has a diameter of 1.3m and a curvature radius of 6m;
[0062] Step (2) preparing a polyamic acid precursor solution;
[0063] Step (3) uses a brush coating method to evenly coat the polyamic acid precursor solution on the concave surface of the mold to form a polyamic acid film. Figure 3 As shown;
[0064] Step (4) fixing the edge of the polyamic acid film at the edge of the mold using a fixed stretching fixture;
[0065] Step (5) placing the mold in an oven, heating it to 350° C., keeping it warm for 4 hours, then heating it to 450° C., keeping it warm for 4 hours, to perform dehydration imidization;
[0066] Step (6) demoulding to obtain a curved polyimide film.
[0067] Example 2
[0068] This embodiment provides a method for manufacturing a curved polyimide film. The manufacturing steps are similar to those of Embodiment 1, except that: Step (3) uses a brush coating method to evenly coat the polyamic acid precursor solution on the convex surface of the mold. Figure 4 shown.
[0069] The present invention overcomes the problem that the polyimide film prepared by the prior art is flat and has low precision when used as a curved antenna reflector. The manufacturing method and mold of the curved polyimide film provided by the present invention can directly prepare the curved polyimide film and effectively improve the profile precision of the reflector. The prepared curved polyimide film has high profile precision, good uniformity, and good curved shape maintenance, and is suitable as a reflector material for ultra-large-caliber thin-film antennas, and can be applied to the preparation of space thin-film reflector antennas.
[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for manufacturing a curved polyimide film, characterized in that: The following steps are involved: Step (1) manufacturing a mold according to the desired shape of the film reflective surface; Step (2) preparing a polyamic acid precursor solution; Step (3) uniformly coating the polyamic acid precursor solution on the surface of the mold to form a polyamic acid film; Step (4) fixing the edge of the polyamic acid film at the edge of the mold using a fixed stretching fixture; Step (5) placing the mold in an oven and baking at high temperature to perform dehydration imidization; Step (6) demoulding to obtain a curved polyimide film.
2. The method for manufacturing a curved polyimide film according to claim 1, characterized in that: In the step (1), the material of the mold is metal material, the mold is manufactured by mechanical processing, and the surface of the mold is polished.
3. The method for manufacturing a curved polyimide film according to claim 1, wherein: In the step (3), the polyamic acid precursor solution is applied to the surface of the mold by spraying, brushing or dipping. The polyamic acid precursor solution is applied to the convex surface or the concave surface of the mold.
4. The method for manufacturing a curved polyimide film according to claim 1, characterized in that: In the step (5), the high temperature baking conditions are: firstly, heating to 300°C to 350°C, keeping the temperature for 2 to 6 hours, then heating to 400°C to 450°C, keeping the temperature for 16 to 24 hours.
5. A mold for manufacturing a curved polyimide film, used for implementing the method for manufacturing a curved polyimide film according to any one of claims 1 to 4, characterized in that: include: A mold body, a mold convex surface, a mold concave surface and a fixed stretching clamp, wherein the mold convex surface is used to coat a polyamic acid precursor solution to form a polyamide film, the mold concave surface is used to coat a polyamic acid precursor solution to form a polyamide film, and the fixed stretching clamp is arranged at the edge of the mold to fix the edge of the polyamic acid film before dehydration imidization treatment.
6. The mold for manufacturing a curved polyimide film according to claim 5, characterized in that: The material of the mold is metal material.
7. The mold for manufacturing a curved polyimide film according to claim 5, characterized in that: The mold surface is a curved surface, the diameter of the mold is 0.8 to 2 m, and the radius of curvature of any point on the surface of the mold is 2 to 8 m.
Citation Information
Cited By
Manufacturing method of flexible microwave antenna / filter with high bending resistance
CN116435794A
Method for manufacturing highly bending-resistant flexible microwave antenna / filter
CN116435794B
3D curved surface high-toughness polyimide film and preparation method thereof
CN120098298A