A method for preparing modified 13X molecular sieve and its application

By introducing zirconium, titanium, and potassium sources into 13X molecular sieves, the adsorption performance of molecular sieves for acetylene was improved, solving the problem of insufficient selectivity of existing 13X molecular sieves and achieving higher adsorption capacity and longer service life.

CN119038573BActive Publication Date: 2026-11-10SUZHOU JINHONG GAS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411165072.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2026-11-10
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing 13X molecular sieve has limited adsorption selectivity for acetylene, which leads to rapid penetration of the adsorption column when the acetylene impurity content in ethylene is high, affecting its service life.

Method used

By introducing zirconium, titanium, and potassium sources to modify 13X molecular sieves, Lewis basic sites are increased and the interaction between zirconium atoms and acetylene is improved, thus preparing modified 13X molecular sieves with higher selective adsorption and adsorption capacity.

Benefits of technology

Modified 13X molecular sieve significantly improves adsorption selectivity and adsorption capacity for acetylene, extends adsorption breakthrough time, and has a longer service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038573B_ABST
    Figure CN119038573B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a modified 13X molecular sieve for separating acetylene from ethylene. The method involves mixing sodium, potassium, and aluminum sources in water to obtain solution A; dissolving zirconium and titanium sources separately in water and then mixing them with solution A to obtain solution B; mixing a silicon source with solution B to obtain a gel; crystallizing the gel in a hydrothermal reactor to obtain solid crystals; washing and drying the solid crystals, and then calcining them in a muffle furnace to obtain the modified 13X molecular sieve. The molecular sieve prepared by this invention exhibits strong selective adsorption of acetylene and a high adsorption capacity, with a longer adsorption breakthrough time and a longer service life. This invention is applicable to the separation of acetylene from high-purity ethylene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of adsorbents, specifically relating to a method for preparing and applying a modified 13X molecular sieve for separating acetylene from ethylene. Background Technology

[0002] High-purity ethylene is an indispensable raw material in semiconductor manufacturing, primarily used in the etching of dielectric thin films on aluminum metal surfaces and in third-generation SiC chemical vapor deposition and vapor phase epitaxial growth processes. my country's semiconductor industry is developing rapidly, leading to a continuous increase in demand for high-purity ethylene, and consequently, increasingly stringent quality requirements.

[0003] Hydrocarbon vapor cracking is one of the main methods for producing ethylene feedstock, and it is accompanied by the generation of acetylene as a byproduct. Effective removal of acetylene from ethylene is a crucial industrial process. Due to the similar physical properties of acetylene and ethylene, traditional cryogenic distillation is insufficient for achieving deep separation of acetylene and ethylene. Therefore, adsorption is the primary method for removing acetylene impurities from ethylene. Although emerging porous adsorption materials (such as metal-organic frameworks) can be designed to achieve good separation of ethylene and acetylene, their poor stability and high production costs limit their widespread application in adsorption processes.

[0004] Molecular sieves have become the preferred adsorbent in large-scale industrial production due to their simple preparation process, high stability, and low cost. Among them, 13X molecular sieve has been commercially used to adsorb acetylene from ethylene. However, because 13X molecular sieve itself has a pore size of 10 Å, it has adsorption capacity for both ethylene (kinetic diameter 4.2 Å) and acetylene (kinetic diameter 3.3 Å), but its adsorption selectivity for acetylene is limited. In practical applications, when the acetylene impurity content in ethylene is high, the adsorption column will quickly break through, affecting its service life and rendering it useless. Summary of the Invention

[0005] To address the above problems, this invention provides a method for preparing a modified 13X molecular sieve for separating acetylene from high-purity ethylene. This molecular sieve exhibits strong selective adsorption of acetylene and high adsorption capacity, with a longer adsorption breakthrough time and a longer service life.

[0006] A method for preparing modified 13X molecular sieve includes the following steps: 1) A solution A is obtained by mixing a sodium source, a potassium source, and an aluminum source in water; wherein the sodium source is one or more of sodium hydroxide, sodium bicarbonate, or sodium carbonate; the potassium source is one or more of potassium hydroxide, potassium bicarbonate, or potassium chloride; and the aluminum source is one or more of alum, aluminum sulfate, or aluminum hydroxide. 2) Dissolve the zirconium source and titanium source separately in water, and then mix them with solution A to obtain solution B; the zirconium source is one or more of zirconium nitrate, zirconium sulfate, and basic zirconium chloride, and the titanium source is one or more of titanium sulfate and sodium titanate; 3) Dissolve the silicon source in water and mix it with solution B to obtain a gel solution; the silicon source includes one or more of sodium silicate, potassium aluminum silicate, and potassium silicate; 4) The gel solution is placed in a hydrothermal reactor and crystallized at 150~250℃ for 48~72h to obtain solid crystals; 5) The solid crystals are centrifuged, washed with ethanol, washed with water, and dried. Then they are placed in a muffle furnace and calcined at 400-600°C for 12-24 hours to obtain the modified 13X molecular sieve.

[0007] Preferably, the sodium source is 1-5g, the potassium source is 0.1-2g, and the aluminum source is 2-30g. More preferably, the sodium source is 1-3g, the potassium source is 0.3-1.5g, and the aluminum source is 4-15g.

[0008] Preferably, the zirconium source is 0.05~0.5g and the titanium source is 0.05~0.5g. More preferably, the zirconium source is 0.08~0.2g and the titanium source is 0.08~0.2g.

[0009] Preferably, the total water content of the gel solution in step 3 is 30-300g; and the silicon source is 1-5g. More preferably, the total water content of the gel solution in step 3 is 50-150g; and the silicon source is 2.5-3.5g.

[0010] The present invention also provides a modified 13X molecular sieve, which is prepared by the method of claim 1; the modified 13X molecular sieve is used to purify ethylene feedstock containing 0~10 ppm acetylene impurities, wherein the acetylene impurity is not 0.

[0011] This invention also provides an application of the 13X molecular sieve, wherein the modified 13X molecular sieve is prepared by the method provided by this invention, and the 13X molecular sieve is used to purify ethylene feedstock containing 0-10 ppm acetylene impurities, wherein the acetylene impurity is not zero. The 13X molecular sieve of this invention can remove acetylene from ethylene to below 0.01 ppm. Therefore, this invention can be specifically used for separating acetylene from ethylene.

[0012] Compared with the prior art, the present invention has the following beneficial effects: 1) In the modified 13X molecular sieve prepared by this invention, zirconium and titanium atoms replace some of the aluminum and silicon atoms in the lattice, making more oxygen atoms exhibit electronegativity and providing more Lewis basic sites. Acetylene is more Lewis acid than ethylene, and more basic sites provide higher adsorption selectivity and adsorption capacity.

[0013] 2) Potassium cations have larger electron shells and atomic radii than sodium cations, and have stronger interaction forces with π electrons in acetylene, further improving the adsorption performance of molecular sieves for acetylene.

[0014] This invention introduces zirconium and titanium sources into the 13X molecular sieve system, enhancing the selective adsorption performance of the molecular sieve for acetylene. Commercially available 13X molecular sieves generally do not contain a potassium source; the introduction and proportioning of a potassium source further improves the selective adsorption performance of the molecular sieve for acetylene.

[0015] Therefore, the adsorption performance of the 13X molecular sieve prepared by this invention far exceeds that of ordinary 13X on the market.

[0016] This invention can be considered a targeted product specifically designed for the separation of acetylene from ethylene, thus distinguishing it from other general-purpose products. The molecular sieve prepared by this invention exhibits strong selective adsorption of acetylene and a high adsorption capacity. Attached Figure Description

[0017] Figure 1 These are the acetylene adsorption experiment results for each example and comparative example. Wherein, 1-4 represent Examples 1-4 respectively, and 5-8 represent Comparative Examples 1-4 respectively. Detailed Implementation

[0018] The technical solution of the present invention will be further described below with reference to specific embodiments, but the present invention is not limited to these embodiments. Example

[0019] Solution A was prepared by mixing 4g of sodium hydroxide, 1g of potassium hydroxide, and 4.56g of aluminum sulfate in 50ml of water. Solution B was prepared by dissolving 0.13g of zirconium nitrate and 0.18g of titanium sulfate in 10ml of water and adding them to solution A. Solution B was prepared by dissolving 2.73g of sodium silicate in 30ml of water and adding it to solution B. The gel was then placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were separated by centrifugation, washed with ethanol and water, dried, and then calcined in a muffle furnace at 400℃ for 12h to obtain the modified 13X molecular sieve product. Example

[0020] Solution A was prepared by mixing 4g of sodium hydroxide, 1g of potassium hydroxide, and 4.53g of aluminum sulfate in 50ml of water. Solution B was prepared by dissolving 0.07g of zirconium nitrate and 0.09g of titanium sulfate in 10ml of water and adding them to solution A. Solution B was prepared by dissolving 2.93g of sodium silicate in 30ml of water and adding it to solution B. The gel was then placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were separated by centrifugation, washed with ethanol and water, dried, and then calcined in a muffle furnace at 400℃ for 12h to obtain the modified 13X molecular sieve product. Example

[0021] Solution A was prepared by mixing 5g of sodium hydroxide and 4.70g of aluminum sulfate in 50ml of water. Solution B was prepared by dissolving 0.14g of zirconium nitrate and 0.19g of titanium sulfate in 10ml of water and adding them to solution A. Solution C was prepared by dissolving 3.04g of sodium silicate in 30ml of water and adding it to solution B. The gel was then placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were separated by centrifugation, washed with ethanol and water, dried, and then calcined in a muffle furnace at 400℃ for 12h to obtain the modified 13X molecular sieve product. Example

[0022] Solution A was prepared by mixing 4g of sodium hydroxide, 0.8g of potassium hydroxide, and 14.62g of alum in 50ml of water. Solution B was prepared by dissolving 0.16g of zirconium nitrate and 0.21g of titanium sulfate in 10ml of water and adding them to solution A. Solution B was prepared by dissolving 2.73g of sodium silicate in 30ml of water and adding it to solution B. The gel was then placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were separated by centrifugation, washed with ethanol and water, dried, and then calcined in a muffle furnace at 400℃ for 12h to obtain the modified 13X molecular sieve product.

[0023] Comparative Example 1: Solution A was prepared by mixing 5g of sodium hydroxide and 4.98g of aluminum sulfate in 60ml of water. 2.97g of sodium silicate was dissolved in 30ml of water and added to solution A to obtain a gel. The gel was placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were then separated by centrifugation, washed with ethanol and water, dried, and subsequently calcined in a muffle furnace at 400℃ for 12h to obtain the 13X molecular sieve product.

[0024] Comparative Example 2: Solution A was prepared by mixing 5g of sodium hydroxide, 0.81g of potassium chloride, and 14.76g of alum in 60ml of water. 2.24g of potassium silicate was dissolved in 30ml of water and added to solution A to obtain a gel. The gel was placed in a hydrothermal reactor and crystallized at 200℃ for 48h. The solid crystals were then centrifuged, washed with ethanol and water, dried, and subsequently calcined in a muffle furnace at 400℃ for 12h to obtain the modified 13X molecular sieve product.

[0025] Comparative Example 3: The 13X molecular sieve available on the market is 13X APG 8x12, manufactured by Honeywell.

[0026] Comparative Example 4: The 13X molecular sieve available on the market is JZ-ZMS9 13X, manufactured by Shanghai Jiuzhou.

[0027] Testing process: The 13X molecular sieve products from the above examples and comparative examples were applied to the separation of acetylene from ethylene. 20g of molecular sieve was packed into an adsorption column with a diameter of 1 / 2 inch, and the flow rate was controlled using a mass flow meter at a rate of 100 h⁻¹. -1 Ethylene standard gas containing 5 ppm acetylene was introduced into the adsorption column at space velocity. The adsorption pressure was controlled at 0.5~1 MPa and the adsorption temperature at -40℃~-20℃. After chromatographic detection of the adsorption column, acetylene breakthrough of the adsorption column was defined as an acetylene content of 0.5 ppm.

[0028] Test results: Adsorption experiment results for each example and comparative example are shown in [link to test results]. Figure 1 See Table 1.

[0029] Table 1. Results of acetylene adsorption experiments in each example and comparative example.

[0030] As shown in Table 1 and Figure 1 As shown, compared with the comparative examples, the modified 13X molecular sieve in the examples exhibited a higher adsorption capacity and a longer adsorption breakthrough time. The adsorption capacity of Example 1 was 1.6 times and 1.5 times that of Comparative Examples 3 and 4, respectively, significantly exceeding the performance of commercially available 13X molecular sieves. Comparing Examples 1 and 2 with Comparative Examples 1 and 2, it is evident that adding zirconium and titanium sources effectively improved the adsorption capacity of the molecular sieve for acetylene, i.e., improved the adsorption selectivity and adsorption capacity of the molecular sieve for acetylene. Comparing Examples 1 and 3, it is evident that adding potassium sources also improved the adsorption performance of the molecular sieve for acetylene to some extent.

[0031] The molecular sieve prepared by this invention has strong selective adsorption of acetylene and high adsorption capacity, with longer adsorption breakthrough time and longer service life.

[0032] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, and these all fall within the protection scope of the present invention.

Claims

1. A method for preparing modified 13X molecular sieve, characterized in that, The preparation method includes the following steps: 1) A solution A is obtained by mixing a sodium source, a potassium source, and an aluminum source in water; wherein the sodium source is one or more of sodium hydroxide, sodium bicarbonate, or sodium carbonate; the potassium source is one or more of potassium hydroxide, potassium bicarbonate, or potassium chloride; and the aluminum source is one or more of alum, aluminum sulfate, or aluminum hydroxide. 2) Dissolve the zirconium source and titanium source separately in water, and then mix them with solution A to obtain solution B; the zirconium source is one or more of zirconium nitrate, zirconium sulfate, and basic zirconium chloride, and the titanium source is one or more of titanium sulfate and sodium titanate; 3) Dissolve the silicon source in water and mix it with solution B to obtain a gel solution; the silicon source includes one or more of sodium silicate, potassium aluminum silicate, and potassium silicate; 4) The gel solution is placed in a hydrothermal reactor and crystallized at 150~250℃ for 48~72h to obtain solid crystals; 5) The solid crystals are centrifuged, washed with ethanol, washed with water, and dried. Then they are placed in a muffle furnace and calcined at 400-600°C for 12-24 hours to obtain the modified 13X molecular sieve.

2. The method for preparing modified 13X molecular sieve according to claim 1, characterized in that, The sodium source is 1-5g, the potassium source is 0.1-2g, and the aluminum source is 2-30g.

3. The method for preparing modified 13X molecular sieve according to claim 2, characterized in that, The sodium source is 1-3g, the potassium source is 0.3-1.5g, and the aluminum source is 4-15g.

4. The method for preparing modified 13X molecular sieve according to claim 1, characterized in that, The zirconium source is 0.05~0.5g, and the titanium source is 0.05~0.5g.

5. The method for preparing modified 13X molecular sieve according to claim 4, characterized in that, The zirconium source is 0.08~0.2g, and the titanium source is 0.08~0.2g.

6. The method for preparing modified 13X molecular sieve according to claim 1, characterized in that, In step 3, the total water content of the gel solution is 30-300g; the silicon source is 1-5g.

7. The method for preparing modified 13X molecular sieve according to claim 6, characterized in that, In step 3, the total water content of the gel solution is 50-150g; the silicon source is 2.5-3.5g.

8. A modified 13X molecular sieve, characterized in that, The modified 13X molecular sieve is prepared by the method of claim 1; the modified 13X molecular sieve is used to purify ethylene feedstock containing 0~10ppm acetylene impurities, wherein the acetylene impurity is not 0.

9. An application of a modified 13X molecular sieve, characterized in that, The modified 13X molecular sieve is prepared by the method of claim 1. The 13X molecular sieve is used to purify ethylene feedstock containing 0-10 ppm acetylene impurities, wherein the acetylene impurity is not 0.

Citation Information

Patent Citations

  • Method for preparing molecular sieve from chlorosilane

    CN102009984A

  • Chemical pretreatment method of organic waste gas containing styrene component

    CN110559844A