Method for rapidly separating out salt to increase lithium content in lithium precipitation mother liquor
By using a combination of composite alcohol and regulator in the lithium deposited mother liquor, multiple concentration steps and reduced pressure separation are carried out, the problem of loss and separation of lithium during the concentration process of lithium deposited mother liquor is solved, and efficient recovery and high lithium are achieved Concentration enrichment simplifies process flow and reduces energy consumption.
Patent Information
- Application Number
- CN202411157522.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing MVR concentration purification and lithium sedimentation process, lithium is prone to form a slurry composite sodium-potassium lithium salt during the concentration of lithium mother liquor, resulting in the loss of lithium and increased energy consumption, and the chemical or physical properties of lithium, sodium and potassium. Similarly, it increases the difficulty of separation of lithium, resulting in low recovery efficiency of lithium.
Using composite alcohol additives and hydrolyzed weak alkaline regulators, the initial concentration and multiple concentration steps are used, cooling and stirring and decompression separation, selectively reduce the Glauber's salt content in the concentrate, improve the concentration enrichment of lithium, and achieve efficient recovery of lithium. .
It realizes high concentration enrichment of lithium, reduces lithium loss and energy consumption, simplifies the process flow, improves the recovery efficiency of lithium, avoids the lithium inclusion problem, and solves the proportion of Glauber's salt lithium produced during the concentration process. Problems of excessive height and difficulty in separation.
Smart Images

Figure CN119040655A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for rapidly precipitating salt to increase the lithium content in lithium precipitation mother liquor. Background Art
[0002] The brine purification liquid is added with sodium carbonate to obtain lithium carbonate, thereby achieving lithium precipitation. However, due to the high solubility of lithium carbonate in the lithium precipitation mother liquor, about 1 / 4 of the lithium is in the lithium precipitation mother liquor, and this part of lithium has great recovery value. At present, the MVR concentration and purification lithium precipitation process is usually used to recover this part of lithium, but the open-circuit sodium potassium salt in this method will cause the loss of some lithium. In the lithium precipitation mother liquor concentration section, the sodium potassium salt separated by the horizontal screw centrifuge in the vacuum cooling flash evaporation process of the concentrated liquid carries part of the lithium precipitation, accounting for about 0.15%-0.3% of the salt content. Therefore, it has to be returned to the system with the ingredients again, not only without the effective open-circuit production system of sodium potassium salt, but also resulting in the consumption of energy and raw and auxiliary materials for the secondary treatment of lithium.
[0003] In the existing MVR concentration and purification process for lithium precipitation, the higher the lithium content in the concentrate, the more conducive it is to the extraction of lithium carbonate, because the lithium precipitation mother liquor is preferentially enriched and concentrated on the main sodium potassium sulfate during the concentration process. The difficulty of separating lithium is increased due to the similar chemical or physical properties of lithium, sodium and potassium. For example, when the lithium content in the concentrate is higher than 7-9g / L, a large amount of mirabilite and glauberite are saturated and precipitated, carrying the loss of lithium salts, accounting for about 0.15%-0.3% of the salt content. Further concentration of the lithium precipitation mother liquor, in severe cases, forms a molten composite sodium potassium lithium salt that is enriched in the flash evaporation equipment and is forced to stop and clean up. The effective enrichment of lithium content in the lithium precipitation mother liquor concentrate is an important bottleneck problem in the development of the sulfate lithium extraction industry. Summary of the invention
[0004] The invention provides a method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother liquor. The composite alcohol additive and the regulator used in the invention can accelerate the precipitation of sodium sulfate and potassium sulfate salts in a lithium precipitation mother liquor concentrate, and selectively reduce the sodium sulfate content in the concentrate, thereby achieving high-concentration enrichment of lithium in the lithium precipitation mother liquor, and facilitating the extraction of lithium from the lithium precipitation mother liquor. The method is rapid, efficient, low-cost, and simple in process. The composite alcohol solvent and the regulator can be recovered or concentrated and precipitated for salting by means of reduced pressure separation.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0007] After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively;
[0008] The primary concentration step comprises: cooling the concentrated lithium precipitation mother liquor obtained in the previous step to below 25-40° C., adding the concentrated lithium precipitation mother liquor to a desalting kettle, then adding a composite alcohol additive and a hydrolysis weak alkaline regulator to the desalting kettle, stirring for 5-10 minutes at a stirring rate of 100-200 r / min, then standing for 20-90 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing concentrated lithium precipitation mother liquor;
[0009] The secondary concentration step comprises: removing the composite alcohol additive and the regulator from the alcohol-containing concentrated lithium precipitation mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain the concentrated lithium precipitation mother liquor.
[0010] Specifically, the pressure of the reduced pressure separation in the secondary concentration step is -0.9 to -0.6 MPa, and the temperature is 55-90°C.
[0011] Specifically, the temperature is preheated to 55-90° C. before the secondary concentration step.
[0012] Specifically, the initial concentration step of the lithium precipitation mother liquor specifically includes the following steps: concentrating the lithium precipitation mother liquor to a lithium content of 7 to 9 g / L at a temperature of 60 to 100° C., a pressure of −0.6 to 1 MPa and a stirring rate of 100 to 200 r / min.
[0013] Specifically, the volume ratio of the composite alcohol additive to the regulator is 4 to 10:1, and the amount of the composite alcohol additive added is 5 to 50% of the volume of the concentrated lithium precipitation mother solution. V / V %.
[0014] Specifically, the composite alcohol additive is a mixture of two or more alcohols with different polarities in any proportion.
[0015] Specifically, the composite alcohol additive is a mixture of two or more of methanol, ethanol, n-propanol and isopropanol in any proportion.
[0016] Specifically, the hydrolysis weak alkaline regulator is a mixture of ammonia water and urea in a mass ratio of 5 to 10:1; the mass concentration of the ammonia water is 10-25%.
[0017] Specifically, the filter residue solid obtained after each concentration step is washed 2-3 times with the composite alcohol additive, and then the washing liquid is recovered, and the recovered washing liquid and the alcohol-containing concentrated lithium precipitation mother liquor obtained through the first concentration step are mixed and subjected to a secondary concentration step together.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother liquor; the composite alcohol regulating solvent of the present invention can accelerate the precipitation of sodium sulfate and potassium sulfate salts in a concentrated solution of a lithium precipitation mother liquor, and selectively reduce the content of mirabilite in the concentrated solution, thereby achieving high-concentration enrichment of lithium in the lithium precipitation mother liquor, thereby facilitating the extraction of lithium from the lithium precipitation mother liquor; the method is rapid, efficient, low-cost, and simple in process; the composite alcohol solvent and the regulating agent can be recovered or concentrated and precipitated for salting by means of reduced pressure separation.
[0019] The present invention utilizes the polarity of the alcohol solvent to change the precipitation rate of potassium glauberite in the concentrated solution to avoid the lithium peritectic problem, solve the problem that the proportion of lithium in flash distillation output of glauberite is too high, separation is difficult, and the sulfate method glauberite cannot be opened. At the same time, the concentration of the concentrated solution is greatly increased to improve the precipitation recovery capacity of the lithium precipitation mother liquor. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a scanning electron microscope image of flash concentrated Glauber's salt complex salt;
[0021] Figure 2 is a scanning electron microscope image of the glauberite precipitated by single-stage adjustment in Example 5;
[0022] Figure 3 This is the multi-stage salt precipitation XRD spectrum of Example 4;
[0023] Figure 4 This is the multi-stage salt precipitation XRD spectrum of Example 5;
[0024] Figure 5 This is the multi-stage salt precipitation XRD spectrum of Example 6;
[0025] Figure 6 is the XRD spectrum of the multi-stage salt precipitation of the salt in Example 7;
[0026] Figure 7 is a graph showing the effect of 5% compound alcohol addition on lithium concentration in Example 4;
[0027] Figure 8 is a graph showing the effect of 10% compound alcohol addition on lithium concentration in Example 5;
[0028] Fig. 9 is a graph showing the effect of 20% compound alcohol addition on lithium concentration in Example 6;
[0029] Fig.10 This is a graph showing the effect of the addition amount of 30% of the complex alcohol on lithium concentration in Example 7. DETAILED DESCRIPTION
[0030] The following specific examples are intended to further illustrate the present invention rather than to limit the scope of protection of the claims.
[0031] Example 1
[0032] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0033] After the initial concentration step of the lithium precipitation mother liquor, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively; the primary concentration step includes: taking 500 mL of the lithium precipitation mother liquor, cooling it to a concentrated solution below 40° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring for 10 minutes at a stirring rate of 200 r / min, then standing for 90 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation mother liquor;
[0034] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0035] The above two concentration steps are repeated until a large amount of lithium precipitation is detected in the lithium concentrate and then the process is stopped.
[0036] The pressure of the reduced pressure separation in the secondary concentration step was -0.65 MPa and the temperature was 90°C.
[0037] The temperature was preheated to 90°C before the secondary concentration step.
[0038] Concentrating the lithium precipitation mother liquor comprises the following steps: concentrating the lithium precipitation mother liquor to a lithium content of 7 g / L at a temperature of 100° C., a pressure of −0.6 MPa and a stirring rate of 100 r / min.
[0039] The volume ratio of the compound alcohol additive to the regulator is 10:1, and the compound alcohol additive accounts for 50% of the volume of the concentrate. V / V %.
[0040] The composite alcohol additive is a mixture of any proportion of two or three of methanol, ethanol, n-propanol, and isopropanol. (The composite alcohol additive of this embodiment is a mixture of methanol and isopropanol in a volume ratio of 10:1)
[0041] The regulator is a mixture of ammonia water and urea in a mass ratio of 10:1; the mass concentration of the ammonia water is 25%.
[0042] Example 2
[0043] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0044] After the initial concentration step of the lithium precipitation mother liquor, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step performed successively; the primary concentration step includes: taking 500 mL of the lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring for 5 minutes at a stirring rate of 100 r / min, then standing for 20 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0045] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0046] The above two concentration steps are repeated until a large amount of lithium precipitation is detected in the lithium concentrate and then the process is stopped.
[0047] The pressure of the reduced pressure separation in the secondary concentration step was -0.9 MPa and the temperature was 55°C.
[0048] The temperature was preheated to 55°C before the secondary concentration step.
[0049] Concentrating the lithium precipitation mother liquor comprises the following steps: concentrating the lithium precipitation mother liquor to a lithium content of 8 g / L at a temperature of 60° C., a pressure of −0.6 to 1 MPa and a stirring rate of 150 r / min.
[0050] The volume ratio of the compound alcohol additive to the regulator is 4:1, and the compound alcohol additive accounts for 5% of the volume of the concentrate. V / V %.
[0051] The composite alcohol additive is a mixture of any proportion of two or three of methanol, ethanol, n-propanol and isopropanol. (In this embodiment, the volume ratio of methanol: ethanol: n-propanol = 10:2:1)
[0052] The regulator is a mixture of ammonia water and urea in a mass ratio of 20:1; the mass concentration of the ammonia water is 17%.
[0053] Example 3
[0054] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0055] After the initial concentration step of the lithium precipitation mother liquor, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively; the primary concentration step includes: taking 500 mL of the lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring for 8 minutes at a stirring rate of 150 r / min, then standing for 30 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0056] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0057] The above two concentration steps are repeated until a large amount of lithium precipitation is detected in the lithium concentrate and then the process is stopped.
[0058] The pressure of the vacuum separation in the secondary concentration step was -0.8 MPa and the temperature was 75°C.
[0059] The temperature was preheated to 75°C before the secondary concentration step.
[0060] Concentrating the lithium precipitation mother liquor comprises the following steps: concentrating the lithium precipitation mother liquor to a lithium content of 9 g / L at a temperature of 80° C., a pressure of −0.6 MPa and a stirring rate of 100 r / min.
[0061] The volume ratio of the compound alcohol additive to the regulator is 8:1, and the compound alcohol additive accounts for 20% of the volume of the concentrate. V / V %.
[0062] The composite alcohol additive is a mixture of any proportion of two or three of methanol, ethanol, n-propanol, and isopropanol. (In this embodiment, the volume ratio of methanol: ethanol: isopropanol = 10:1:1)
[0063] The regulator is a mixture of ammonia water and urea in a mass ratio of 5:1; the mass concentration of the ammonia water is 20%.
[0064] Example 4
[0065] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0066] After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively;
[0067] The primary concentration step comprises: taking 500 mL of lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring it fully at 200 r / min for 5 minutes, standing it for 30 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0068] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0069] The composite alcohol additive uses ethanol and methanol in a volume ratio of 1:3, ammonia water (mass concentration of 17%) dissolved in an equal amount of urea as a regulator.
[0070] The amount of the compound alcohol additive added is 5% of the volume of the concentrated lithium precipitation mother solution, and the regulator is 10% of the amount of the compound alcohol additive;
[0071] The pressure of the vacuum separation in the secondary concentration step was -0.8 MPa and the temperature was 75°C.
[0072] The above two processes will be repeated until a large amount of lithium precipitation is detected in the lithium concentrate and the experiment is stopped.
[0073] Example 5
[0074] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0075] After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively;
[0076] The primary concentration step comprises: taking 500 mL of lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring it fully at 200 r / min for 5 minutes, standing it for 30 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0077] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0078] The composite alcohol additive uses ethanol and methanol in a volume ratio of 1:3, ammonia water (mass concentration of 17%) dissolved in an equal amount of urea as a regulator.
[0079] The added amount of the composite alcohol additive is 10% of the volume of the concentrated lithium precipitation mother solution, and the regulator is 10% of the amount of the composite alcohol additive;
[0080] The pressure of the vacuum separation in the secondary concentration step was -0.8 MPa and the temperature was 75°C.
[0081] The above two processes will be repeated until a large amount of lithium precipitation is detected in the lithium concentrate and the experiment is stopped.
[0082] Example 6
[0083] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0084] After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively;
[0085] The primary concentration step comprises: taking 500 mL of lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring it fully at 200 r / min for 5 minutes, standing it for 30 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0086] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0087] The composite alcohol additive uses ethanol and methanol in a volume ratio of 1:3, ammonia water (mass concentration of 17%) dissolved in an equal amount of urea as a regulator.
[0088] The amount of the compound alcohol additive added is 20% of the volume of the concentrated lithium precipitation mother solution, and the regulator is 10% of the amount of the compound alcohol additive;
[0089] The pressure of the vacuum separation in the secondary concentration step was -0.8 MPa and the temperature was 75°C.
[0090] The above two processes will be repeated until a large amount of lithium precipitation is detected in the lithium concentrate and the experiment is stopped.
[0091] Example 7
[0092] A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution comprises the steps of initially concentrating the lithium precipitation mother solution,
[0093] After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively;
[0094] The primary concentration step comprises: taking 500 mL of lithium precipitation mother liquor, cooling it to a concentrated solution below 25° C., adding it to a desalting kettle, then adding a composite alcohol additive and a regulator to the desalting kettle, stirring it fully at 200 r / min for 5 minutes, standing it for 30 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing lithium precipitation concentrated mother liquor;
[0095] The secondary concentration step comprises: removing the alcohol additive and the regulator from the alcohol-precipitated lithium concentrated mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain a concentrated solution.
[0096] The composite alcohol additive uses ethanol and methanol in a volume ratio of 1:3, ammonia water (mass concentration of 17%) dissolved in an equal amount of urea as a regulator.
[0097] The added amount of the composite alcohol additive is 30% of the volume of the concentrated lithium precipitation mother solution, and the regulator is 10% of the amount of the composite alcohol additive;
[0098] The pressure of the vacuum separation in the secondary concentration step was -0.8 MPa and the temperature was 75°C.
[0099] The above two processes will be repeated until a large amount of lithium precipitation is detected in the lithium concentrate and the experiment is stopped.
[0100] Example 8
[0101] The difference from Example 1 is that the solid after the first concentration is washed twice with the composite alcohol additive, and then the washing liquid is recovered and sent to the second concentration step together with the alcohol-precipitated lithium-containing concentrated mother liquor obtained after the first concentration.
[0102] Multi-stage salt precipitation crystal structure analysis
[0103] The comparative example is the original one of the enterprise. After acidification and neutralization, the lithium precipitation mother liquor is concentrated to 7g / L in MVR once, and then directly enters the secondary concentration step to be concentrated to 9g / L, and then the salt is flashed out and passed through a horizontal screw centrifuge to obtain flash salt with a water content of 8-10%.
[0104] Flash evaporation is the process of entering the flash evaporator at about 90-100°C after MVR. The flash vacuum is -0.8-0.9MPa. The solution is further vaporized and concentrated. The flash outlet temperature is about 60°C.
[0105] Compare the potassium glauberite (such as Figure 1 ) and the scanning electron microscopy image of the sodium sulfate precipitated by adding the composite alcohol additive and the regulator (Example 5) ( Figure 2 ),like Figure 1 As shown in Figure 2, the salt precipitated by flash evaporation is a large block crystal, such as Figure 2As shown, the precipitated mirabilite particles are adjusted to be rod-shaped. Large crystals are easy to cover the concentrated lithium salt to form a complex salt, causing lithium loss, while the regular rod-shaped crystals are about 3-8μm and have a small grain size, which helps to reduce the lithium loss caused by peritectic during the growth of mirabilite crystals.
[0106] XRD characterization of salt precipitation crystals Figure 3-6 As shown, 5%, 10%, 20%, and 30% of the volume ratio of the lithium precipitation mother solution were selected as the alcohol additive (Examples 4-7), and 1% of the volume of the lithium precipitation mother solution (compound alcohol: regulator = 10:1) was used as the regulator to adjust the solution. The XRD spectrum of the salt precipitation sample showed that the first concentrated salt precipitation salt sample had a good crystal form, and the characteristic peak position of potassium glauberite was around 30° and 22°. The results showed that it contained potassium glauberite crystals, and 20% of the compound alcohol ( Figure 5 ) added, the peak position of potassium glauberite is most similar. 30% complex alcohol ( Figure 6 ) added, the first salt precipitation impurity peak is too much, but its characteristic peak position is still around 30°. In the subsequent concentrated salt precipitation of potassium glauberite, there are irregular peaks at around 20° and 60°, and the characteristic peak appears at a low angle, indicating the precipitation of lithium. 5% complex alcohol ( Figure 3 ) added, the characteristic peak of the third concentrated salt precipitation XRD spectrum appears at 22°. This shows that most of the initial salt precipitation is glauberite, and other metal complex salts will precipitate with the increase of concentrated salt precipitation; the amount of lithium brought out by glauberite in the salt precipitation with low concentration of 5% complex alcohol added is relatively low.
[0107] Effect of the amount of compound alcohol added on lithium concentrate
[0108] The concentration of lithium ions in the solution was detected by flame atomic absorption spectrometry. Figure 7-10 The effect of adding different percentages of compound alcohol on lithium concentration. When the lithium ion concentration reaches saturation or close to saturation, lithium will decrease with the precipitation of potassium and sodium salts, resulting in a decrease in lithium ion concentration. This shows that in the lithium precipitation mother liquor recovery process of the company, evaporation and concentration are first performed and then crystallization and precipitation are performed. The crystallized potassium and sodium salts will contain a part of lithium salts that are not recycled, resulting in a decrease in the lithium salt recovery rate. Adding compound alcohol before evaporation and concentration can effectively improve the concentration efficiency of lithium salts.
[0109] like Figure 7 The results show that the lithium concentration of the solution with 5% compound alcohol and regulator increases with the increase of the number of times of concentration and salt precipitation. The concentration of lithium is concentrated from 9.5g / L to 16.4g / L after concentration and salt precipitation. During the fourth concentration and salt precipitation, a large amount of lithium is precipitated, resulting in a decrease in the lithium concentration to 10.7g / L. Figure 8) added solution was concentrated and precipitated once, and the lithium concentration was concentrated from 9.7g / L to 15.7g / L. Compared with the addition of 5% compound alcohol and regulator, the concentration efficiency was faster, but the concentration was not stable enough. During the second and third concentrations, the lithium concentration gradually decreased, indicating that a large amount of lithium had been precipitated in the second concentration. 20% compound alcohol and regulator ( Fig. 9 ) was added, the solution was concentrated to 13.9g / L after one concentration and salt precipitation, and the concentration efficiency was faster than that of 5% compound alcohol and regulator. Except that the lithium concentration did not increase in the second concentration and salt precipitation, the lithium concentration gradually increased with the increase of the number of concentration and salt precipitation. After 4 concentrations and salt precipitation, the lithium concentration reached 18.4g / L. 30% compound alcohol and regulator ( Fig.10 ) was added, and the solution was concentrated from 11.3g / L to 17.7g / L after two times of salt precipitation. During the third concentration and salt precipitation, lithium precipitated in large quantities and the concentration dropped to 12.8g / L.
[0110] Multi-stage salt precipitation capability analysis
[0111] The mass of the salt precipitated by the compound alcohol and the corresponding regulator after drying is shown in Table 1. The effect of the dosage of the compound alcohol and the corresponding regulator on the salt precipitation of the concentrated solution is different. Among them, the mass of the precipitated salt is the smallest when 5% of the compound alcohol and the corresponding regulator are added, and the mass of the potassium and sodium salt precipitated by 30% of the compound alcohol and the corresponding regulator is the largest. In the second salt precipitation, the mass of the precipitated salt increased when 5% of the compound alcohol and the corresponding regulator were added, indicating that the salt precipitation was incomplete when the compound alcohol and the corresponding regulator were added for the first time. After the first concentration, the ion concentration increased, the compound alcohol and the corresponding regulator changed the solubility of each salt, and the mass of the precipitated salt increased accordingly. For the addition of 10%, 20% and 30% of the compound alcohol and the corresponding regulator, the mass of the second precipitated salt decreased significantly, indicating that more salt was precipitated when the compound alcohol and the corresponding regulator were added for the first time. When 30% of the compound alcohol and the corresponding regulator were added, the difference between the first and second salt precipitation masses was greater than the difference between the addition of 10% and 20% of the compound alcohol and the corresponding regulator, indicating that the first salt precipitation of 30% of the compound alcohol and the corresponding regulator was more thorough. The changes in the quality of the salt precipitation in the subsequent two times are the same as the previous two changes. The increase in the quality of the salt precipitation is due to the increase in the ion concentration in the solution and the precipitation of a part of the lithium salt.
[0112] Table 1 Salt precipitation quality of Examples 4-7
[0113]
[0114] Analysis of salt ion content
[0115] Table 2 Ion ratio in the precipitated salt of Examples 4-7
[0116]
[0117] Table 2 shows the proportion of ions in the precipitated salts of Examples 4-7, reflecting the ion content in the precipitated salts with different concentrations of composite alcohols and corresponding amounts of regulators. Among them, Example 4 has a large amount of lithium precipitation in the third salt precipitation; 10%, 20% and 30% composite alcohols and corresponding regulators are added to the experiment and a large amount of lithium ions are precipitated in the second salt precipitation. The addition of Examples 6 and 7 precipitates potassium ions more completely after one salt precipitation, and Example 4 is more thorough after three salt precipitations, indicating that 5% composite alcohol and the corresponding regulator precipitate mainly potassium glauberite in the first three salt precipitations. The greater the mass percentage of potassium and sodium ions, the more potassium and sodium ions are contained in the precipitated salt, thereby reducing the precipitation of lithium ions and impurity ions, allowing the lithium ions in the solution to be retained, and the concentration process is more stable.
[0118] After adding compound alcohol and corresponding regulator, glauberite can be separated and precipitated. After concentration, some lithium salt and complex salt will precipitate due to the increase in concentration. This case comparison found that 5% compound alcohol and corresponding regulator added to lithium precipitation mother liquor can precipitate glauberite to a large extent, and lithium salt can be concentrated to about 16g / L, and the lithium ion content brought out by the precipitated salt is low.
[0119] Example 8: Using a composite alcohol to wash the solid after the first concentration can further reduce the problem of lithium loss caused by the concentrated salt. The washing time can be extended by soaking or other methods, so that the lithium can be stripped more thoroughly from the potassium salt.
[0120] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for rapidly precipitating salt to increase the lithium content in a lithium precipitation mother solution, comprising the steps of initially concentrating the lithium precipitation mother solution, Features: After the initial lithium precipitation mother liquor concentration step, more than one concentration and salt precipitation step is included, and each concentration and salt precipitation step includes a primary concentration step and a secondary concentration step which are performed successively; The primary concentration step comprises: cooling the concentrated lithium precipitation mother liquor obtained in the previous step to below 25-40° C., adding the concentrated lithium precipitation mother liquor to a desalting kettle, then adding a composite alcohol additive and a hydrolysis weak alkaline regulator to the desalting kettle, stirring for 5-10 minutes at a stirring rate of 100-200 r / min, then standing for 20-90 minutes, and then performing solid-liquid separation to remove the filter residue to obtain an alcohol-containing concentrated lithium precipitation mother liquor; The secondary concentration step comprises: removing the composite alcohol additive and the regulator from the alcohol-containing concentrated lithium precipitation mother liquor obtained in the primary concentration step by decompressing and separating the mother liquor to obtain the concentrated lithium precipitation mother liquor.
2. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1, Features: The pressure of the reduced pressure separation in the secondary concentration step is -0.9 to -0.6 MPa, and the temperature is 55-90°C.
3. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1, Features: Preheat the temperature to 55-90°C before the secondary concentration step.
4. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1, Features: The initial concentration step of the lithium precipitation mother liquor specifically includes the following steps: concentrating the lithium precipitation mother liquor to a lithium content of 7 to 9 g / L at a temperature of 60 to 100° C., a pressure of −0.6 to 1 MPa and a stirring rate of 100 to 200 r / min.
5. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1, Features: The volume ratio of the composite alcohol additive to the regulator is 4 to 10:1, and the amount of the composite alcohol additive added is 5 to 50% of the volume of the concentrated lithium precipitation mother liquor. V / V %.
6. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1 or 5, Features: The composite alcohol additive is a mixture of two or more alcohols with different polarities in any proportion.
7. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 6, Features: The composite alcohol additive is a mixture of two or more of methanol, ethanol, n-propanol and isopropanol in any proportion.
8. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1 or 5, Features: The hydrolysis weak alkaline regulator is a mixture of ammonia water and urea in a mass ratio of 5 to 10:1; the mass concentration of the ammonia water is 10-25%.
9. A method for increasing the lithium content in lithium precipitation mother solution by rapid salt precipitation according to claim 1, Features: The filter residue solid obtained after each concentration step is washed 2-3 times with the composite alcohol additive, and then the washing liquid is recovered, and the recovered washing liquid is mixed with the alcohol-containing concentrated lithium precipitation mother liquor obtained through the first concentration step, and a secondary concentration step is performed together.