Method for extracting lithium from spodumene
By promoting the selective leaching of lithium from spodumene through calcination and bicarbonate reaction, the problems of high impurity content and low recovery rate in the lithium extraction process of spodumene in the existing technology are solved, and a high-efficiency and low-impurity lithium extraction effect is achieved.
Patent Information
- Application Number
- CN202411366016.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies for lithium extraction from spodumene suffer from problems such as high impurity content, difficulty in solution purification, high requirements for equipment corrosion resistance, and low lithium recovery rate. In particular, in acid and alkaline processes, it is difficult to achieve selective leaching of minerals such as aluminum and silicon, and the filtration performance is poor.
The process involves calcining spodumene to convert it into β-spodumene, which is then mixed with a lithium extraction agent and solvent containing bicarbonate. The lithium extraction reaction is carried out at a set temperature to form a buffer solution, which promotes selective leaching of lithium, reduces the concentration of aluminum and silicon in the solution, avoids the formation of gel-like impurities, and achieves efficient separation.
It achieves highly selective separation of lithium, high lithium extraction rate, good filtration performance, low impurity content in lithium-rich solution, simplifies production process and reduces subsequent impurity removal costs.
Smart Images

Figure CN119040658A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium salt preparation, and in particular to a method for extracting lithium from spodumene. Background Art
[0002] At present, my country's lithium carbonate output accounts for more than 30% with spodumene as the main raw material. It is the resource type with the highest degree of commercial lithium extraction, and the technical process is relatively mature. The lithium extraction processes are mainly divided into two categories: acid method and alkaline method. The acid method includes sulfuric acid method, sulfate roasting method and chloride roasting method. The alkaline method includes limestone method, Na2CO3 roasting alkaline method and soda ash pressure cooking method.
[0003] However, the acid process has the advantages of strong adaptability to raw materials, high lithium extraction rate, and simple operation, but the process has poor selectivity, high impurity content in the leachate, great difficulty in solution purification, high requirements for equipment corrosion resistance, and the acidic wastewater produced has a great impact on the environment. The alkaline process has the advantages of short process, small material flow, and no acidic wastewater, but this method has poor selectivity for leaching minerals such as aluminum and silicon in the ore, and the concentration of silicon and aluminum in the leachate is high, resulting in poor slurry filtration performance and difficulty in impurity removal. Compared with the acid method, the lithium recovery rate is lower. Therefore, there is an urgent need for a method for efficient and low-impurity lithium extraction from spodumene to achieve controllable impurities, thereby simplifying the production process and reducing subsequent impurity removal costs. Summary of the invention
[0004] The present application provides a method for extracting lithium from spodumene to solve the following technical problem: how to reduce impurities in a lithium-rich solution obtained by extracting lithium from spodumene.
[0005] In a first aspect, the present application provides a method for extracting lithium from spodumene, the method comprising:
[0006] The spodumene is roasted to obtain β-spodumene;
[0007] The β-spodumene, the lithium extracting agent containing bicarbonate and the solvent are mixed to obtain a mixed solution;
[0008] Under the condition of set temperature, the mixed solution is subjected to lithium extraction reaction to obtain a lithium extraction solution.
[0009] Optionally, the bicarbonate includes at least one of the following: sodium bicarbonate, ammonium bicarbonate, and potassium bicarbonate.
[0010] Optionally, the weight ratio of the β-spodumene to the bicarbonate-containing lithium extraction agent is 1:(0.4-0.6).
[0011] Optionally, the liquid-to-solid ratio of the mixed solution is 4-15.
[0012] Optionally, the solvent comprises water.
[0013] Optionally, the set temperature is 265°C to 300°C.
[0014] Optionally, the lithium extraction reaction time is 30 min to 90 min.
[0015] Optionally, the median particle size of the β-spodumene is 40 μm to 100 μm.
[0016] Optionally, the calcination process parameters include: a calcination temperature of 800° C. to 1100° C., and a calcination time of 0.5 h to 5 h.
[0017] Optionally, the method further includes:
[0018] The lithium extraction solution is subjected to solid-liquid separation to obtain a lithium-rich solution; wherein the composition of the lithium-rich solution meets the following indicators: Al 3+ The concentration is less than 0.01g / L, Si 2+ The concentration is <0.1g / L.
[0019] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0020] The method for extracting lithium from spodumene provided in an embodiment of the present application comprises: roasting spodumene to obtain β-spodumene; mixing the β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; and subjecting the mixed solution to a lithium extraction reaction under a set temperature to obtain a lithium extraction solution. The morphology of spodumene is a strip-like structure with a smooth surface. Spodumene is roasted to convert it into β-spodumene. The morphology of the β-spodumene is a loose structure with cracks, which can promote the subsequent lithium extraction reaction. The lithium extraction agent containing bicarbonate can form a mild buffer solution with the solvent. The cations contained in the bicarbonate in the mild buffer solution undergo a replacement reaction with the lithium in the β-spodumene under the condition of a set temperature, and the lithium is precipitated in the form of lithium carbonate, thereby achieving a high lithium extraction rate. At the same time, the mixed solution is subjected to a lithium extraction reaction, so that impurities such as aluminum, silicon, and sodium in the β-spodumene are mainly present in the form of NaAlSi2O6, thereby achieving selective leaching of lithium in the β-spodumene. At the same time, under the buffer solution system, the equilibrium concentration of aluminum and silicon in the solution can be reduced, and the lithium in the solution is preferentially present in the form of carbonate, thereby avoiding the formation of Li2Al2O4·xH2O and Li2SiO3·xH2O gel-like lithium aluminum and lithium silicon hydrates in the lithium extraction solution. In summary, this method can achieve selective separation of lithium, with a high lithium extraction rate and good filtration performance of the lithium extraction solution. The lithium-rich solution obtained by subsequent filtration of the lithium extraction solution has low content of impurities such as aluminum and silicon. Therefore, the impurities in the lithium-rich solution obtained by extracting lithium from spodumene are reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0023] Figure 1 A schematic flow chart of a method for extracting lithium from spodumene provided in an embodiment of the present application. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0025] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0026] In this application, the terms "including", "comprising", etc. mean "including but not limited to".
[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0028] The acid method in the lithium extraction process of spodumene has the problems of high impurity content in the solution, great difficulty in solution purification, high requirements for corrosion resistance of equipment, and great impact of acidic wastewater on the environment. The alkaline method has strong leaching properties for aluminum, silicon and other minerals in the ore, poor slurry filtration performance, difficulty in removing impurities from lithium-rich leachate, and low lithium recovery rate. The existing technology is difficult to achieve selective leaching of aluminum, silicon and other minerals during the leaching process, resulting in poor filtration performance of the leached slurry, and high aluminum and silicon content in the lithium-rich leachate affects impurity removal. Therefore, it is necessary to develop a method for extracting lithium from spodumene with high efficiency and low impurity, so as to achieve controllable impurities, simplify the production process, and reduce the cost of filtration and subsequent impurity removal. Therefore, the present application provides a method for extracting lithium from spodumene, Figure 1 A schematic diagram of a method for extracting lithium from spodumene provided in an embodiment of the present application; see Figure 1 , the method comprising:
[0029] S1, calcining spodumene to obtain β-spodumene;
[0030] In some embodiments, the calcination process parameters include: a calcination temperature of 800° C. to 1100° C., and a calcination time of 0.5 h to 5 h.
[0031] In the embodiment of the present application, spodumene can be crushed and ground before roasting. The morphology of spodumene is a smooth and flat strip-like structure. Spodumene is roasted to convert spodumene into β-spodumene. The morphology of the β-spodumene is loose and has a crack-like structure, which can promote the subsequent lithium extraction reaction. The roasting temperature can be 800℃~1100℃, and the roasting time can be 0.5h~5h. The spodumene with α-spodumene is more efficient in phase conversion to β-spodumene, and the phase conversion is more thorough, which is conducive to the subsequent leaching and lithium extraction reaction. Exemplarily, the above-mentioned roasting temperature can be 800℃, 850℃, 900℃, 950℃, 1000℃, 1050℃, 1100℃, etc.; the above-mentioned roasting time can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, etc.
[0032] In some embodiments, the median particle size of the β-spodumene is 40 μm to 100 μm.
[0033] In the embodiment of the present application, the median particle size of β-spodumene can be 40 μm to 100 μm, and the median particle size of suitable β-spodumene is
[0034] The particle size can improve the subsequent lithium extraction rate of β-spodumene. At the same time, if the median particle size of β-spodumene is less than 40 μm, it may cause difficulty in solid-liquid separation of the subsequent lithium extraction solution. Exemplarily, the median particle size of the β-spodumene can be 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, etc.
[0035] S2, mixing the β-spodumene, the lithium extraction agent containing bicarbonate and the solvent to obtain a mixed solution;
[0036] In some embodiments, the weight ratio of the β-spodumene to the bicarbonate-containing lithium extraction agent is 1:(0.4-0.6).
[0037] In the embodiment of the present application, the weight ratio of β-spodumene to the lithium extraction agent containing bicarbonate can be 1:(0.4-0.6), so as to increase the lithium extraction rate as much as possible. At the same time, if the weight ratio of β-spodumene to the lithium extraction agent containing bicarbonate is lower than 1:0.6, it means that the lithium extraction agent containing bicarbonate is too high, which may cause the impurities such as aluminum and silicon in β-spodumene to leach into the solution during the lithium extraction reaction, affecting the filtration and subsequent impurity removal. Exemplarily, the weight ratio of the above-mentioned β-spodumene to the lithium extraction agent containing bicarbonate can be 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, etc.
[0038] In some embodiments, the liquid-to-solid ratio of the mixed solution is 4-15.
[0039] In the embodiment of the present application, the liquid-to-solid ratio of the mixed solution can be 4 to 15. The appropriate liquid-to-solid ratio of the mixed solution can ensure the lithium concentration in the subsequent lithium extraction solution; and ensure the viscosity of the mixed solution, promote the lithium extraction reaction of the lithium extraction agent and spodumene, and improve the lithium extraction rate. Exemplarily, the liquid-to-solid ratio of the mixed solution can be 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, etc.
[0040] In some embodiments, the solvent comprises water.
[0041] In the embodiment of the present application, the solvent can be water, which is economical and environmentally friendly, and water can dissolve and disperse the lithium extraction agent and spodumene well, thereby facilitating the lithium extraction reaction between the lithium extraction agent and spodumene and improving the lithium extraction rate.
[0042] S3. Under a set temperature condition, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution.
[0043] In the embodiment of the present application, the mixed solution is subjected to a lithium extraction reaction, so that the impurities such as aluminum, silicon, and sodium in β-spodumene are mainly present in the form of NaAlSi2O6, thereby achieving selective leaching of lithium in β-spodumene. At the same time, under the buffer solution system, the equilibrium concentrations of aluminum and silicon in the solution can be reduced, and the lithium in the solution is preferentially present in the form of carbonate, thereby avoiding the formation of Li2Al2O4·xH2O and Li2SiO3·xH2O gel-like lithium aluminum and lithium silicon hydrates in the lithium extraction solution, thereby achieving selective separation of lithium, a high lithium extraction rate, and good filtration performance of the lithium extraction solution.
[0044] In some embodiments, the bicarbonate salt comprises at least one of the following: sodium bicarbonate, ammonium bicarbonate, potassium bicarbonate.
[0045] In an embodiment of the present application, the bicarbonate may be a combination of one or more of sodium bicarbonate, ammonium bicarbonate, and potassium bicarbonate. The lithium extraction agent containing bicarbonate can form a mild buffer solution with the solvent. The cations (sodium ions, ammonium ions, potassium ions) contained in the bicarbonate in the mild buffer solution undergo a replacement reaction with the lithium in β-spodumene under the condition of a set temperature, and the lithium is precipitated in the form of lithium carbonate to achieve a high lithium extraction rate. If carbonate is used for lithium extraction reaction, it may lead to a low leaching rate of spodumene. Although the leaching rate can increase with the increase of carbonate addition, there is still a gap in leaching rate compared with the acid method, and the silicon and aluminum content in the leachate gradually increases with the increase of carbonate addition. After leaching, aluminum and silicon in the mineral exist in the solution in a colloidal suspension state in the form of zeolite and lithium silicate, which affects the lithium extraction rate; if a strong base is used for lithium extraction reaction, the spodumene mineral is mainly composed of quartz (SiO2) and spodumene (LiAlSi2O6) phases. Under the alkaline system, the leaching rates of Al2O3, SiO2, CaO, and MgO in spodumene minerals are compared with those of carbonates, and the Al, Si, and Ca content in the leachate is too high, which makes it difficult to purify the solution and is not conducive to the subsequent preparation of high-purity lithium salt products; if acid is used, the spodumene lithium extraction rate is high, the operation is simple, and no high-temperature crystal conversion roasting is required. However, the use of the acid method will also lead to a high impurity content in the leachate, making it difficult to purify the solution. In addition, the acid method has high requirements on the corrosion resistance of the equipment, and the recovery of acidic wastewater generated by the leaching process needs to be considered.
[0046] In some embodiments, the set temperature is 265°C to 300°C.
[0047] In the embodiment of the present application, the set temperature can be 265°C to 300°C, that is, the temperature of the lithium extraction reaction can be 265°C to 300°C, which can ensure the lithium extraction effect of the lithium extraction reaction and improve the lithium extraction rate; if the temperature of the lithium extraction reaction is higher than 300°C, it may cause impurities such as aluminum, silicon, and calcium in β-spodumene to enter the lithium extraction solution, making it difficult to achieve selective leaching, affecting subsequent impurity removal. Exemplarily, the set temperature can be 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, etc.
[0048] In some embodiments, the lithium extraction reaction time is 30 min to 90 min.
[0049] In the embodiment of the present application, the time of the lithium extraction reaction can be 30min to 90min, which can be combined with the above-mentioned set temperature to ensure the lithium extraction effect of the lithium extraction reaction and improve the lithium extraction rate; if the time of the lithium extraction reaction is longer than 90min, the lithium extraction rate will not be improved, and gelled compounds such as lithium aluminum and lithium silicon are easily formed in the lithium extraction solution, affecting the filtration performance of the lithium extraction solution. Exemplarily, the time of the above-mentioned lithium extraction reaction can be 30min, 40min, 50min, 60min, 70min, 80min, 90min, etc. In addition, stirring can be used to assist in the conduct of the above-mentioned lithium extraction reaction.
[0050] In some embodiments, the method further comprises:
[0051] The lithium extraction solution is subjected to solid-liquid separation to obtain a lithium-rich solution; wherein the composition of the lithium-rich solution meets the following indicators: Al 3+ The concentration is less than 0.01g / L, Si 2+ The concentration is <0.1g / L.
[0052] In the embodiments of the present application, after the lithium extraction reaction, impurities such as aluminum and silicon remain in the solid phase of the lithium extraction solution in the form of NaAlSi2O6 and can be separated by filtration to obtain a lithium-rich solution. The lithium-rich solution has good filtration performance, and the content of impurities such as aluminum and silicon in the lithium-rich leaching solution is low. The potassium and sodium ions in the solution can be removed by washing during the product preparation stage, which is helpful for the subsequent preparation of high-quality lithium salt products.
[0053] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0054] Example 1
[0055] A method for extracting lithium from spodumene, comprising:
[0056] S11, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 40 μm;
[0057] S21, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.4, and the liquid-to-solid ratio of the mixed solution is 4;
[0058] S31. Under a set temperature condition, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 265° C., and the lithium extraction reaction time is 30 min.
[0059] S41, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0060] The lithium extraction rate in Example 1 is 96%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.001g / L, Si 2+ The concentration is 0.02g / L.
[0061] Example 2
[0062] A method for extracting lithium from spodumene, comprising:
[0063] S12, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 60 μm;
[0064] S22, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.45, and the liquid-to-solid ratio of the mixed solution is 8;
[0065] S32. Under a set temperature condition, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 270° C., and the lithium extraction reaction time is 40 minutes.
[0066] S42, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0067] The lithium extraction rate in Example 2 is 97%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.002g / L, Si 2+ The concentration is 0.04g / L.
[0068] Example 3
[0069] A method for extracting lithium from spodumene, comprising:
[0070] S13, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 80 μm;
[0071] S23, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.5, and the liquid-to-solid ratio of the mixed solution is 12;
[0072] S33. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 280° C., and the lithium extraction reaction time is 60 min.
[0073] S43, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0074] The lithium extraction rate in Example 3 is 98%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.005g / L, Si 2+ The concentration is 0.06g / L.
[0075] Example 4
[0076] A method for extracting lithium from spodumene, comprising:
[0077] S14, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 80 μm;
[0078] S24, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.55, and the liquid-to-solid ratio of the mixed solution is 15;
[0079] S34. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 290° C., and the lithium extraction reaction time is 80 min.
[0080] S44, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0081] The lithium extraction rate in Example 4 is 98.5%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.005g / L, Si 2+ The concentration is 0.08g / L.
[0082] Example 5
[0083] A method for extracting lithium from spodumene, comprising:
[0084] S15, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 100 μm;
[0085] S25, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is ammonium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.6, and the liquid-to-solid ratio of the mixed solution is 4;
[0086] S35. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 300° C. and the lithium extraction reaction time is 90 minutes.
[0087] S45, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0088] The lithium extraction rate in Example 5 is 99%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.008g / L, Si 2+ The concentration is 0.08g / L.
[0089] Example 6
[0090] A method for extracting lithium from spodumene, comprising:
[0091] S16, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 70 μm;
[0092] S26, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is ammonium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.58, and the liquid-to-solid ratio of the mixed solution is 10;
[0093] S36. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 280° C., and the lithium extraction reaction time is 60 minutes.
[0094] S46, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0095] The lithium extraction rate in Example 6 is 96.5%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.004g / L, Si 2+ The concentration is 0.04g / L.
[0096] Example 7
[0097] A method for extracting lithium from spodumene, comprising:
[0098] S17, roasting spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 90 μm;
[0099] S27, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is ammonium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.55, and the liquid-to-solid ratio of the mixed solution is 12;
[0100] S37. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 280° C., and the lithium extraction reaction time is 60 min.
[0101] S47, separating the lithium extraction solution into solid and liquid to obtain a lithium-rich solution.
[0102] The lithium extraction rate in Example 7 is 97.5%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.003g / L, Si 2+ The concentration is 0.05g / L.
[0103] Example 8
[0104] A method for extracting lithium from spodumene, comprising:
[0105] S18, roasting spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 90 μm;
[0106] S28, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is ammonium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.55, and the liquid-to-solid ratio of the mixed solution is 15;
[0107] S38. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 265° C., and the lithium extraction reaction time is 80 min.
[0108] S48, separating the lithium extraction solution into solid and liquid to obtain a lithium-rich solution.
[0109] The lithium extraction rate in Example 8 is 96%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.002g / L, Si 2+ The concentration is 0.05g / L.
[0110] Comparative Example 1
[0111] A method for extracting lithium from spodumene, comprising:
[0112] S19, roasting spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 40 μm;
[0113] S29, mixing β-spodumene, a lithium extraction agent and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium hydroxide, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.4, and the liquid-to-solid ratio of the mixed solution is 4;
[0114] S39. Under the condition of a set temperature, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 265° C., and the lithium extraction reaction time is 30 minutes.
[0115] S49, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0116] The lithium extraction rate in Comparative Example 1 is 96%, and the Al content in the lithium-rich solution is 3+ The concentration is 0.1g / L, Si 2+ The concentration is 3.0g / L.
[0117] Comparative Example 2
[0118] A method for extracting lithium from spodumene, comprising:
[0119] S110, calcining spodumene to obtain β-spodumene; wherein the median particle size of the β-spodumene is 40 μm;
[0120] S210, mixing β-spodumene, a lithium extraction agent containing bicarbonate, and a solvent to obtain a mixed solution; wherein the lithium extraction agent is sodium bicarbonate, the solvent is water, the weight ratio of β-spodumene to the lithium extraction agent is 1:0.2, and the liquid-to-solid ratio of the mixed solution is 4;
[0121] S310. Under a set temperature condition, subjecting the mixed solution to a lithium extraction reaction to obtain a lithium extraction solution; wherein the set temperature is 265° C., and the lithium extraction reaction time is 30 minutes.
[0122] S410, performing solid-liquid separation on the lithium extraction solution to obtain a lithium-rich solution.
[0123] The lithium extraction rate in Comparative Example 2 was 82%, and the Al content in the lithium-rich solution was 3+ The concentration is 0.001g / L, Si 2+ The concentration is 0.02g / L.
[0124] It can be seen from Examples 1 to 8 and Comparative Examples 1 to 2 that the method for extracting lithium from spodumene provided in the embodiments of the present application realizes the selective separation of lithium from spodumene, and the lithium extraction rate is high, which can reach more than 96%, the filtration performance of the lithium extraction solution is good, and the content of impurities such as aluminum and silicon in the lithium-rich solution is low, Al < 0.01g / L, Si < 0.1g / L. However, from the analysis of Comparative Example 1 and Example 1, it can be seen that the lithium extraction agent in Comparative Example 1 is sodium hydroxide. Although the lithium extraction rate is high, the aluminum and silicon impurities in the lithium extraction solution are high; and from the analysis of Comparative Example 2 and Example 1, it can be seen that the amount of lithium extraction agent in Comparative Example 2 is low, and the lithium extraction rate is significantly reduced.
[0125] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0126] (1) The method for extracting lithium from spodumene provided in the embodiment of the present application solves the problems of high content of impurities such as aluminum and silicon in the spodumene leachate, which leads to difficulty in slurry filtration and long impurity removal process, while ensuring a high leaching rate;
[0127] (2) In the process of efficient hydrothermal leaching of lithium in the loose blocky β-spodumene with cracks after roasting, bicarbonate is used to form a buffer solution. After leaching, the impurities such as aluminum, silicon, and sodium in the spodumene and quartz minerals in the ore are mainly present in the form of NaAlSi2O6, thereby realizing the selective leaching of lithium in the spodumene ore. At the same time, under the buffer solution system, the equilibrium concentration of aluminum and silicon in the solution can be reduced, and the lithium in the solution is preferentially present in the form of carbonate, thereby avoiding the formation of Li2Al2O4·xH2O and Li2SiO3·xH2O gel-like lithium aluminum and lithium silicon hydrates, which make it difficult to separate the solid and liquid of the lithium extraction solution;
[0128] (3) The method for extracting lithium from spodumene provided in the embodiment of the present application realizes the selective separation of lithium from spodumene, has a high lithium extraction rate, and has good filtration performance of the lithium extraction solution. The content of impurities such as aluminum and silicon in the lithium-rich solution is low, with Al < 0.01 g / L and Si < 0.1 g / L.
[0129] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for extracting lithium from spodumene, characterized in that: The method comprises: The spodumene is roasted to obtain β-spodumene; The β-spodumene, the lithium extracting agent containing bicarbonate and the solvent are mixed to obtain a mixed solution; Under the condition of set temperature, the mixed solution is subjected to lithium extraction reaction to obtain a lithium extraction solution.
2. The method according to claim 1, characterized in that The bicarbonate includes at least one of the following: sodium bicarbonate, ammonium bicarbonate, and potassium bicarbonate.
3. The method according to claim 1, characterized in that The weight ratio of the β-spodumene to the bicarbonate-containing lithium extraction agent is 1:(0.4-0.6).
4. The method according to claim 1, characterized in that The liquid-to-solid ratio of the mixed solution is 4-15.
5. The method according to claim 1 or 4, characterized in that: The solvent includes water.
6. The method according to claim 1, characterized in that The set temperature is 265°C to 300°C.
7. The method according to claim 1 or 6, characterized in that: The lithium extraction reaction time is 30 min to 90 min.
8. The method according to claim 1, characterized in that The median particle size of the β-spodumene is 40 μm to 100 μm.
9. The method according to claim 1, characterized in that: The calcination process parameters include: a calcination temperature of 800° C. to 1100° C. and a calcination time of 0.5 h to 5 h.
10. The method according to claim 1, characterized in that The method further comprises: The lithium extraction solution is subjected to solid-liquid separation to obtain a lithium-rich solution; wherein the composition of the lithium-rich solution meets the following indicators: Al 3+ The concentration is less than 0.01g / L, Si 2+ The concentration is <0.1g / L.
Citation Information
Cited By
Method for extracting lithium
CN120888788A