TiO2 / MnO2 heterostructure nano-catalysis and nickel microalloying double-strategy regulation magnesium-based composite material and preparation method thereof

Through dual-strategic regulation of TiO2/MnO2 heterostructure catalyst and Mg-Ni alloy, the problem of insufficient hydrogen absorption and discharge performance of magnesium-based hydrogen storage materials is solved, and high-capacity rapid hydrogen absorption and gentle hydrogen release are achieved, which simplifies the process cycle. Promote the commercial application of magnesium-based hydrogen storage materials.

CN119040715APending Publication Date: 2024-11-29SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411168110.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to the slow hydrogen absorption and release kinetics, stable thermodynamic performance and difficulty in activation, the existing regulation strategy has failed to simultaneously touch the internal structural changes and phase composition of hydrogen storage materials. .

Method used

Using the dual strategies of TiO2/MnO2 heterostructure nanocatalysis and nickel microalloyization to regulate magnesium-based composite materials. By constructing nanoTiO2/MnO2 heterostructure catalyst and Mg-Ni alloy, the catalyst is uniformly distributed on the surface of the matrix material and promotes hydrogen atoms. Diffusion and by mechanical alloying and high-pressure hydrogenation treatment, the Mg2NiH4 phase is formed to reduce the hydrogen release temperature.

Benefits of technology

It significantly improves the hydrogen absorption rate and difficulty of hydrogen release of magnesium-based hydrogen storage materials, achieves high-capacity rapid hydrogen absorption and efficient hydrogen release, and has mild hydrogen release conditions, simplifies the process cycle and is easy to commercially promote.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040715A_ABST
    Figure CN119040715A_ABST
Patent Text Reader

Abstract

The invention discloses a TiO2 / MnO2 heterostructure nano-catalysis and nickel microalloying double-strategy regulation magnesium-based composite material and a preparation method thereof, a nano TiO2 / MnO2 heterostructure is selected as a catalyst, and the content of the nano TiO2 / MnO2 heterostructure accounts for 2-15 wt.%; mg-xNi alloy is selected as a hydrogen storage material matrix, and the content of the Mg-xNi alloy accounts for gt; %, 85 wt.%; wherein in the Mg-xNi alloy, the content of magnesium is 75-97 wt%, and the content of nickel is 3-25 wt%; tiO2 / MnO2 has the size of a nano material and the characteristics of a heterostructure; the particle size d of the nano TiO2 / MnO2 heterostructure is equal to 10 to 40 nm; the Mg < 2 > Ni intermediate phase exists in the Mg < x > Ni alloy. According to the surface catalysis double-strategy regulation and control based on microalloying, the magnesium-rich Mg-Ni alloy is prepared by constructing the TiO2 / MnO2 heterostructure nano-catalyst and adopting mechanical alloying, so that the purposes of improving the hydrogen absorption rate and the hydrogen desorption difficulty at the same time are achieved, and high-capacity rapid hydrogen absorption and efficient hydrogen desorption are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogen storage alloy materials, and specifically relates to a magnesium-based composite material regulated by dual strategies of TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying and a preparation method thereof. Background Art

[0002] At present, solid-state hydrogen storage technology is considered to be the most promising hydrogen storage technology due to its advantages of high safety and high hydrogen storage density. Among them, magnesium-based solid-state hydrogen storage materials are regarded as the mainstream of future hydrogen storage technology due to their advantages such as large hydrogen storage capacity, abundant resources and low cost. However, the commercial application of magnesium-based hydrogen storage materials is restricted by problems such as slow hydrogen absorption and desorption kinetics, stable thermodynamic properties and difficulty in activation.

[0003] In the prior art, DOI:10.1016 / j.jallcom.2023.171610;

[0004] DOI:10.1016 / j.ijhydene.2023.11.213, the regulation strategy is single, only targeting the surface for catalytic modification, and failing to touch the internal structure changes and phase composition of the hydrogen storage material.

[0005] To this end, researchers have optimized and modified magnesium-based hydrogen storage materials by means of matrix alloying, surface catalysis, and nano-sizing. Although improvements have been made to varying degrees on this basis, it is still difficult to simultaneously achieve high capacity, rapid hydrogen absorption, and mild hydrogen release conditions. Analysis of the reasons found that the current regulation strategy is single, and while maintaining high capacity, it fails to simultaneously touch upon the key links that affect thermodynamics and kinetics. Summary of the invention

[0006] In order to overcome the above problems in the prior art, the purpose of the present invention is to provide a magnesium-based composite material and a preparation method thereof by dual-strategy regulation of TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying, and dual-strategy regulation of surface catalysis based on microalloying, by constructing TiO2 / MnO2 heterogeneous structure nanocatalyst and using mechanical alloying to prepare magnesium-rich Mg-Ni alloy, so as to achieve the problems of simultaneously improving the hydrogen absorption rate and the difficulty of hydrogen desorption, and realize high-capacity rapid hydrogen absorption and efficient hydrogen desorption.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A dual-strategy regulation of magnesium-based composite materials using TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying, wherein nano-TiO2 / MnO2 heterogeneous structure is selected as catalyst, and its content accounts for 2-15wt.%; Mg-xNi alloy is selected as hydrogen storage material matrix, and its content accounts for >85wt.%;

[0009] Among them, the Mg-xNi alloy has a magnesium content of 75-97wt.%, and a nickel content of 3-25wt.%; TiO2 / MnO2 has the characteristics of nanomaterial size and heterogeneous structure;

[0010] The particle size of nano-TiO2 / MnO2 heterostructure is d = 10 ~ 40nm;

[0011] There is a Mg2Ni intermediate phase in the Mg-xNi alloy.

[0012] The nano-TiO2 / MnO2 of the composite material is evenly distributed on the surface of the matrix material, promoting the dissociation of H2 molecules and providing channels for the diffusion of hydrogen atoms. The matrix material is composed of Mg and Mg2Ni phases, and the two phases exist at the same time to provide diffusion channels for hydrogen atoms. At the same time, Mg2Ni has a lower decomposition temperature, which can improve the hydrogen absorption and desorption performance of magnesium-based hydrogen storage materials.

[0013] A TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual-strategy regulated magnesium-based composite material and a preparation method thereof, specifically comprising the following steps:

[0014] Step 1: Catalyst Nano-sizing

[0015] The tetrabutyl titanate solution is added into the polytetrafluoroethylene liner and stirred. While stirring, hydrofluoric acid is dripped into the tetrabutyl titanate solution drop by drop and stirred continuously. Then, the solution is placed in a hydrothermal kettle for hydrothermal reaction. After the reaction, the solution is centrifugally washed with deionized water and anhydrous ethanol, and then dried. The dried sample is placed in a muffle furnace for calcination. The final product is nano-TiO2.

[0016] Step 2: Catalyst surface carbonization

[0017] The nano-TiO2 synthesized in step 1 is added to the glucose solution, stirred, centrifuged and washed with deionized water and anhydrous ethanol, and then dried. The dried sample is placed in a tube furnace and calcined under the protection of Ar atmosphere. The calcined product is nano-TiO2@C. C is used as a reducing agent to coat TiO2, thereby protecting TiO2 and reducing KMnO4 to MnO2.

[0018] Step 3: In situ synthesis of nano-TiO2 / MnO2 heterostructures

[0019] The nano-TiO2@C synthesized in step 2 is added to a potassium permanganate solution, stirred, and then placed in a hydrothermal reactor for hydrothermal reaction. After the reaction is completed, it is centrifugally washed with deionized water and dried. The final product is an in-situ synthesized nano-TiO2 / MnO2 heterostructure; C and KMnO4 undergo redox reaction to generate MnO2 in-situ on the TiO2 surface;

[0020] Step 4: Simultaneous alloying and pre-hydrogenation treatment

[0021] After mixing Mg powder and Ni powder, alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill, and the ball milling atmosphere is H2, and Mg-Ni binary alloy powder with Mg2Ni phase is obtained after ball milling;

[0022] Step 5: Ball milling catalytic modification

[0023] The nano-TiO2 / MnO2 heterostructure prepared in step 3 is mixed with the Mg-Ni binary alloy powder prepared in step 4, and they are ball-milled for a short time using a ball mill to uniformly mix the two; a catalytically modified magnesium-based composite material is obtained; the catalyst is uniformly distributed on the surface of the Mg-Ni binary alloy, and the reaction between the matrix and the catalyst is promoted, and a NiTi phase is generated in situ.

[0024] Step 6: High-pressure catalytic hydrogenation modification

[0025] The material prepared in step 5 is placed in a high-pressure hydrogenation reactor for high-pressure hydrogenation to obtain a magnesium-based composite material hydride, and Mg is converted into MgH2, and Mg2Ni is converted into Mg2NiH4;

[0026] Step 7: Grain refinement

[0027] The magnesium-based composite material hydride prepared in step 6 is subjected to ball milling to refine its particles to obtain a magnesium-based composite material with fine and uniform particle size, thereby effectively reducing the agglomeration and coating inhibition phenomena occurring in step 5.

[0028] In the step 1, 20 to 40 mL of tetrabutyl titanate solution is added to a polytetrafluoroethylene liner and stirred. While stirring, 3 to 6 mL of hydrofluoric acid is dripped into the tetrabutyl titanate solution dropwise and stirred for 15 to 60 minutes. Subsequently, the tetrabutyl titanate solution is placed in a hydrothermal kettle and subjected to a hydrothermal reaction at 150 to 200° C. After the reaction is completed, the tetrabutyl titanate solution is centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 to 100° C. for 6 to 12 hours. The dried sample is placed in a muffle furnace for calcination at a calcination temperature of 400 to 600° C.

[0029] In the step 2, the mass of TiO2 is 1 to 3 g, the solubility of the glucose solution is 0.02 to 0.06 mol / L, and the volume is 50 to 300 mL. After stirring for 8 to 12 hours, the solution is centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 to 100° C. for 6 to 10 hours. The dried sample is placed in a tubular furnace and calcined under the protection of an Ar atmosphere at a calcination temperature of 400 to 600° C.

[0030] In the step 3, the mass of TiO2@C is 1-3 g, the solubility of potassium permanganate solution is 0.003-0.01 mol / L, the volume is 20-80 mL, and after stirring for 15-60 min, it is placed in a hydrothermal kettle and subjected to a hydrothermal reaction at 80-150° C. After the reaction is completed, it is centrifugally washed with deionized water and dried at 60-100° C. for 6-12 h.

[0031] In the step 4, Mg powder and Ni powder are mixed in a mass ratio of (75-97): (25-3), and alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill, so that Mg and Ni undergo a mechanochemical reaction to generate a Mg2Ni intermediate phase. The ball milling atmosphere is H2, the hydrogen pressure is 2-10 bar, the ball-to-material ratio is (10-40): 1, the rotation speed is 800-1000 r / min, and the ball milling is performed for 8-12 hours.

[0032] In step 5, the nano-TiO2 / MnO2 heterostructure and the Mg-Ni binary alloy powder are mixed in a mass ratio of (2-15):(85-98), the ball milling atmosphere is Ar, the ball-to-material ratio is (10-40):1, the rotation speed is 500-800 r / min, and the ball milling time is 10-60 min.

[0033] In step 6, the hydrogen pressure is 3-8 MPa, the temperature is 300-350° C., and the hydrogenation time is 8-12 h.

[0034] In step 7, the ball milling atmosphere is H2, the ball-to-material ratio is (10-30):1, the rotation speed is 400-800 r / min, and the ball milling time is 1-2 h.

[0035] The TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulates the magnesium-based composite material for hydrogen storage. TiO2 / MnO2 undergoes a mechanochemical reaction with Mg2Ni to generate a NiTi phase in situ, and multiple phases of Mg, MgH2, Mg2Ni, Mg2NiH4, and TiO2 exist simultaneously, and the multiphase boundaries provide diffusion channels for hydrogen atoms.

[0036] Beneficial effects of the present invention:

[0037] The present invention uses magnesium-nickel alloy as a matrix research object, which can significantly reduce the dehydrogenation temperature of magnesium-based hydrogen storage materials. Magnesium and nickel can form a Mg2Ni intermediate phase after compounding, which is converted into Mg2NiH4 after hydrogenation. Mg2NiH4 has a lower decomposition temperature than MgH2. Nano-TiO2 / MnO2 heterostructure is selected as a catalyst to optimize the kinetics of magnesium-based hydrogen storage materials. Due to its high catalytic activity, TiO2 can promote the dissociation of H2 molecules and provide a fast channel for the diffusion of hydrogen atoms. The nano-TiO2 / MnO2 heterostructure prepared by the present invention has an increased specific surface area and can provide more active sites and diffusion channels.

[0038] The present invention uses a combination of mechanochemical reaction and high-pressure hydrogenation. The mechanochemical reaction can simultaneously realize alloying and pre-hydrogenation treatment, and then the composite hydrogen storage material can be synthesized by short-time high-pressure hydrogenation. The method has a simple preparation process and a short process cycle. During the reaction process, due to the catalytic effect and multi-phase synergistic effect, the hydrogen storage material has the characteristics of high capacity, rapid hydrogen absorption and desorption, mild hydrogen desorption conditions and easy activation. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The present invention is a flow chart for preparing the composite material.

[0040] Figure 2 The figure shows the phase composition and microscopic morphology of the nano-TiO2 / MnO2 heterostructure of the present invention.

[0041] Figure 3 The figure shows the phase composition and microscopic morphology of the composite material of the present invention.

[0042] Figure 4 It is the hydrogen storage performance of the composite material of the present invention. DETAILED DESCRIPTION

[0043] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0044] Example 1

[0045] The TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulated magnesium-based composite material of the present invention is composed of Mg-Ni magnesium-rich alloy and nano-TiO2 / MnO2 heterogeneous structure, wherein the nano-TiO2 / MnO2 heterogeneous structure accounts for 5wt.%, and the rest is Mg-Ni alloy.

[0046] Step 1, catalyst nano-sizing: 25 mL of tetrabutyl titanate solution was added to a polytetrafluoroethylene liner and stirred. While stirring, 4.5 mL of hydrofluoric acid was dripped into the tetrabutyl titanate solution drop by drop, and stirring was continued for 30 min. Subsequently, it was placed in a hydrothermal kettle and hydrothermally reacted at 180 ° C for 24 h. After the reaction, it was centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 ° C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 500 ° C for 2 h. The final product was nano-TiO2.

[0047] Step 2, carbonization of catalyst surface: Add the nano-TiO2 (1 g) synthesized in step 1 to 100 mL of glucose solution (0.04 mol / L), stir for 12 hours, centrifuge and wash with deionized water and anhydrous ethanol, and then dry at 60°C for 10 hours. Place the dried sample in a tube furnace and calcine it under the protection of Ar atmosphere at a temperature of 500°C for 2 hours. The calcined product is nano-TiO2@C.

[0048] Step 3, in-situ synthesis of nano-TiO2 / MnO2 heterostructure: Add the nano-TiO2@C (1 g) synthesized in step 2 to 40 mL of potassium permanganate solution (0.005 mol / L), stir for 30 min, place it in a hydrothermal kettle, and hydrothermally react at 120° C. for 5 h. After the reaction, centrifuge and wash it with deionized water, and dry it at 60° C. for 10 h. The final product is the in-situ synthesized nano-TiO2 / MnO2 heterostructure.

[0049] Step 4, simultaneous alloying and pre-hydrogenation treatment: Mg powder and Ni powder are mixed in a certain mass ratio, wherein Mg accounts for 95wt.%, and Ni accounts for 5wt.%, and then alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill. The ball milling atmosphere is H2, the hydrogen pressure is 5 bar, the ball-to-material ratio is 20:1, the rotation speed is 1000r / min, and the Mg-Ni binary alloy powder is obtained after ball milling for 10 hours.

[0050] Step 5, ball milling catalytic modification: the nano-TiO2 / MnO2 heterostructure prepared in step 3 is mixed with the Mg-Ni binary alloy powder prepared in step 4 in a certain mass ratio, wherein TiO2 / MnO2 accounts for 5wt.%, and the Mg-Ni binary alloy accounts for 95wt.%. The nano-TiO2 / MnO2 heterostructure is mixed with the Mg-Ni binary alloy powder ... a ball mill for a short time to make the nano-TiO2 / MnO2 homogeneously mixed. The ball milling atmosphere is Ar, the ball-to-material ratio is 20:1, the rotation speed is 600r / min, and the ball milling time is 45min.

[0051] Step 6, high pressure catalytic hydrogenation modification: the material prepared in step 5 is placed in a high pressure hydrogenation reactor for high pressure hydrogenation. The hydrogen pressure is 6 MPa, the temperature is 350° C., and the hydrogenation time is 10 h.

[0052] Step 7, particle refinement: The material prepared in step 6 is subjected to ball milling for particle refinement. The ball milling atmosphere is H2, the ball-to-material ratio is 20:1, the rotation speed is 600 r / min, and the ball milling time is 1.5 h. A magnesium-based composite material modified by TiO2 / MnO2 catalysis is obtained.

[0053] The composite material obtained through this embodiment is characterized by uniform particle size, easy activation during hydrogen absorption and desorption, and mild hydrogen absorption conditions.

[0054] Example 2

[0055] The TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulated magnesium-based composite material of the present invention is composed of Mg-Ni magnesium-rich alloy and nano-TiO2 / MnO2 heterogeneous structure, wherein the nano-TiO2 / MnO2 heterogeneous structure accounts for 10wt.%, and the rest is Mg-Ni alloy.

[0056] Step 1, catalyst nano-sizing: 25 mL of tetrabutyl titanate solution was added to a polytetrafluoroethylene liner and stirred. While stirring, 4.5 mL of hydrofluoric acid was dripped into the tetrabutyl titanate solution drop by drop, and stirring was continued for 30 min. Subsequently, it was placed in a hydrothermal kettle and hydrothermally reacted at 200 ° C for 18 h. After the reaction, it was centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 500 ° C for 2 h. The final product was nano-TiO2.

[0057] Step 2, carbonization of catalyst surface: Add the nano-TiO2 (1 g) synthesized in step 1 to 100 mL of glucose solution (0.04 mol / L), stir for 12 h, centrifuge and wash with deionized water and anhydrous ethanol, and then dry at 60°C for 10 h. Place the dried sample in a tube furnace and calcine it under the protection of Ar atmosphere at a temperature of 500°C for 2 h. The calcined product is nano-TiO2@C.

[0058] Step 3, in-situ synthesis of nano-TiO2 / MnO2 heterostructure: Add the nano-TiO2@C (1 g) synthesized in step 2 to 40 mL of potassium permanganate solution (0.005 mol / L), stir for 30 min, place it in a hydrothermal kettle, and hydrothermally react at 120° C. for 5 h. After the reaction, centrifuge and wash it with deionized water, and dry it at 60° C. for 10 h. The final product is the in-situ synthesized nano-TiO2 / MnO2 heterostructure.

[0059] Step 4, simultaneous alloying and pre-hydrogenation treatment: Mg powder and Ni powder are mixed in a certain mass ratio, wherein Mg accounts for 92wt.%, and Ni accounts for 8wt.%, and then alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill. The ball milling atmosphere is H2, the hydrogen pressure is 8 bar, the ball-to-material ratio is 10:1, the rotation speed is 1000r / min, and the Mg-Ni binary alloy powder is obtained after ball milling for 8h.

[0060] Step 5, ball milling catalytic modification: the nano-TiO2 / MnO2 heterostructure prepared in step 3 is mixed with the Mg-Ni binary alloy powder prepared in step 4 in a certain mass ratio, wherein TiO2 / MnO2 accounts for 10wt.%, and the Mg-Ni binary alloy accounts for 90wt.%. The nano-TiO2 / MnO2 heterostructure is mixed with the Mg-Ni binary alloy powder ... a ball mill for a short time to make the nano-TiO2 / MnO2 homogeneous mixture uniformly mixed. The ball milling atmosphere is Ar, the ball-to-material ratio is 10:1, the rotation speed is 800r / min, and the ball milling time is 30min.

[0061] Step 6, high pressure catalytic hydrogenation modification: the material prepared in step 5 is placed in a high pressure hydrogenation reactor for high pressure hydrogenation. The hydrogen pressure is 8 MPa, the temperature is 300° C., and the hydrogenation time is 8 h.

[0062] Step 7, particle refinement: The material prepared in step 6 is subjected to ball milling for particle refinement. The ball milling atmosphere is H2, the ball-to-material ratio is 10:1, the rotation speed is 800 r / min, and the ball milling time is 1 h. A magnesium-based composite material modified by TiO2 / MnO2 catalysis is obtained.

[0063] The composite material obtained through this embodiment is characterized by uniform particle size, easy activation during hydrogen absorption and desorption, and mild hydrogen absorption conditions.

[0064] Example 3

[0065] The TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulated magnesium-based composite material of the present invention is composed of Mg-Ni magnesium-rich alloy and nano-TiO2 / MnO2 heterogeneous structure, wherein the nano-TiO2 / MnO2 heterogeneous structure accounts for 8wt.%, and the rest is Mg-Ni alloy.

[0066] Step 1, catalyst nano-sizing: 25 mL of tetrabutyl titanate solution was added to a polytetrafluoroethylene liner and stirred. While stirring, 4.5 mL of hydrofluoric acid was dripped into the tetrabutyl titanate solution drop by drop, and stirring was continued for 30 min. Subsequently, it was placed in a hydrothermal kettle and hydrothermally reacted at 180 ° C for 24 h. After the reaction, it was centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 500 ° C for 2 h. The final product was nano-TiO2.

[0067] Step 2, carbonization of catalyst surface: Add the nano-TiO2 (1 g) synthesized in step 1 to 100 mL of glucose solution (0.04 mol / L), stir for 12 h, centrifuge and wash with deionized water and anhydrous ethanol, and then dry at 60°C for 10 h. Place the dried sample in a tube furnace and calcine it under the protection of Ar atmosphere at a temperature of 500°C for 2 h. The calcined product is nano-TiO2@C.

[0068] Step 3, in-situ synthesis of nano-TiO2 / MnO2 heterostructure: Add the nano-TiO2@C (1 g) synthesized in step 2 to 40 mL of potassium permanganate solution (0.005 mol / L), stir for 30 min, place it in a hydrothermal kettle, and hydrothermally react at 120° C. for 5 h. After the reaction, centrifuge and wash it with deionized water, and dry it at 60° C. for 10 h. The final product is the in-situ synthesized nano-TiO2 / MnO2 heterostructure.

[0069] Step 4, simultaneous alloying and pre-hydrogenation treatment: Mg powder and Ni powder are mixed in a certain mass ratio, wherein Mg accounts for 90wt.%, and Ni accounts for 10wt.%, and then alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill. The ball milling atmosphere is H2, the hydrogen pressure is 3 bar, the ball-to-material ratio is 30:1, the rotation speed is 800r / min, and the Mg-Ni binary alloy powder is obtained after ball milling for 12h.

[0070] Step 5, ball milling catalytic modification: the nano-TiO2 / MnO2 heterostructure prepared in step 3 is mixed with the Mg-Ni binary alloy powder prepared in step 4 in a certain mass ratio, wherein TiO2 / MnO2 accounts for 15wt.%, and the Mg-Ni binary alloy accounts for 85wt.%. The nano-TiO2 / MnO2 heterostructure is briefly ball milled in a ball mill to uniformly mix the two. The ball milling atmosphere is Ar, the ball-to-material ratio is 30:1, the rotation speed is 500r / min, and the ball milling time is 20min.

[0071] Step 6, high pressure catalytic hydrogenation modification: the material prepared in step 5 is placed in a high pressure hydrogenation reactor for high pressure hydrogenation. The hydrogen pressure is 4 MPa, the temperature is 320°C, and the hydrogenation time is 12 hours.

[0072] Step 7, particle refinement: The material prepared in step 6 is subjected to particle refinement by ball milling. The ball milling atmosphere is H2, the ball-to-material ratio is 30:1, the rotation speed is 400 r / min, and the ball milling time is 2 h. A magnesium-based composite material modified by TiO2 / MnO2 catalysis is obtained.

[0073] The composite material obtained through this embodiment is characterized by uniform particle size, easy activation during hydrogen absorption and desorption, and mild hydrogen absorption conditions.

[0074] Figure 1 The process flow chart of the dual-strategy regulation of magnesium-based composite materials by TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying in the present invention. As can be seen from the flow chart, the catalyst is finely regulated in structure through strategies such as nano-sizing, surface carbonization, and in-situ synthesis; a magnesium-nickel powder alloy is prepared by mechanical alloying, and pre-hydrogenation is performed on it at the same time; and a magnesium-based composite material regulated by TiO2 / MnO2 heterogeneous structure nanocatalysis and nickel microalloying dual strategies is prepared by introducing catalyst ball milling modification and high-pressure hydrogenation treatment. The hydrogen storage material prepared by this method can achieve simultaneous regulation of its kinetics, thermodynamics, and activation properties, and has a short process cycle, which is easy to promote commercial hydrogen storage materials.

[0075] Figure 2 The XRD spectrum and SEM images of nano-TiO2 / MnO2 heterogeneous structure. From the XRD spectrum, it can be seen that the peak corresponding to MnO2 appears in the spectrum of TiO2, proving that MnO2 has been successfully introduced through the in-situ synthesis method. From the SEM image, it can be observed that the TiO2 / MnO2 heterogeneous structure exists in the form of square particles, and the particle size is between 10 and 40nm, successfully realizing the nano-processing of the catalyst structure.

[0076] Figure 3 The XRD spectrum and SEM image of the Mg8Ni-10wt.%TiO2 / MnO2 composite hydrogen storage material. It can be seen from the XRD spectrum that the composite hydrogen storage material contains multiple phases, mainly MgH2, Mg2NiH4, TiO2, NiTi, MgO, etc. The generation of Mg2NiH4 and the coexistence of multiple phases can reduce the hydrogen absorption and desorption temperature of the hydrogen storage material and improve its thermodynamic properties. From the SEM image, it can be observed that the nano-square particles are evenly distributed on the surface of the MgH2 particles, which can promote the dissociation of H2. At the same time, the interface between the catalyst and the MgH2 particles can provide a channel for the diffusion of hydrogen atoms, accelerating the diffusion of hydrogen atoms.

[0077] Figure 4 The activation hydrogen absorption curve and hydrogen absorption kinetic curve of the nano Mg8Ni-5wt.%TiO2 / MnO2 composite hydrogen storage material. As can be seen from the left figure, the first hydrogen absorption performance and the third hydrogen absorption performance curve of the invented material basically coincide, both reaching more than 90% of the theoretical hydrogen storage capacity, that is, the first hydrogen absorption achieves the activation effect, proving that the invented material is a hydrogen storage material that does not require activation. As can be seen from the figure, the invented material has excellent hydrogen storage performance under low temperature conditions. The dual-strategy regulation of nano-catalysis and nickel micro-alloying promotes the dissociation and diffusion mass transfer process of H2 molecules through coordinated regulation and optimization from the surface and the inside, and accelerates the hydrogen absorption kinetics of the material.

[0078] The present invention further optimizes magnesium-based hydrogen storage materials by means of dual-strategy coordinated regulation. First, by introducing Ni elements to reduce the thermodynamic stability of MgH2, Mg and Ni can form a Mg2Ni intermediate phase, and after hydrogenation, a Mg2NiH4 phase is formed. The existence of multiple phases can provide channels for hydrogen diffusion. At the same time, the theoretical hydrogen storage capacity of Mg2NiH4 can reach 3.6wt.%, and the introduction of Ni elements in an appropriate amount to prepare a Mg-Ni binary magnesium-rich alloy can also meet the requirements of high-capacity hydrogen storage. Therefore, the present invention prepares a magnesium-rich Mg-Ni binary alloy as a matrix research object. TiO2 is widely used in the field of catalysis due to its high catalytic activity. The preparation of nano-TiO2 / MnO2 heterostructures can maintain the high activity state of TiO2, and can also increase the specific surface area. It is applied to the surface catalysis of magnesium-based hydrogen storage materials, which is expected to meet the needs of rapid absorption and release of hydrogen. In terms of process, mechanical alloying and mechanical hydrogenation are carried out simultaneously, and the matrix material is pre-hydrogenated during alloying. The catalyst is introduced before high-pressure hydrogenation to carry out a catalytic hydrogenation reaction. The whole process can shorten the activation time of the hydrogen storage material to solve the problem of difficulty in activating the magnesium-based hydrogen storage material. Therefore, the present invention selects nano-TiO2 / MnO2 heterostructure to catalyze the Mg-Ni binary alloy to develop a magnesium-based hydrogen storage material with high capacity, fast hydrogen absorption, mild hydrogen release conditions and easy activation.

Claims

1. A TiO 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composites, It is characterized in that Select nano-TiO 2 / MnO 2 The heterogeneous structure is used as a catalyst, and its content accounts for 2-15wt.%; Mg-xNi alloy is selected as the hydrogen storage material matrix, and its content accounts for >85wt.%; The Mg-xNi alloy has a magnesium content of 75-97wt.%, and a nickel content of 3-25wt.%; TiO 2 / MnO 2 Possessing nanomaterial size and heterogeneous structure characteristics; Nano-TiO 2 / MnO 2 The particle size of the heterostructure is d = 10 to 40 nm; The Mg-xNi alloy contains Mg 2 Ni intermediate phase.

2. TiO according to claim 1 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composites, It is characterized in that Nano-TiO Composite Materials 2 / MnO 2 Evenly distributed on the surface of the base material, promoting H 2 The dissociation of molecules provides a channel for the diffusion of hydrogen atoms. The matrix material is composed of Mg and Mg 2 The Ni phase is composed of two phases, and the coexistence of the two phases provides diffusion channels for hydrogen atoms.

3. A TiO according to claim 1 or 2 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that The specific steps include: Step 1: Catalyst Nano-sizing The tetrabutyl titanate solution was added to the polytetrafluoroethylene liner and stirred. While stirring, hydrofluoric acid was dripped into the tetrabutyl titanate solution drop by drop and stirred continuously. Then, the solution was placed in a hydrothermal kettle for hydrothermal reaction. After the reaction, the solution was centrifuged and washed with deionized water and anhydrous ethanol, and then dried. The dried sample was placed in a muffle furnace for calcination. The final product was nano-TiO 2 ; Step 2: Catalyst surface carbonization The nano-TiO synthesized in step 1 2 The sample was added to the glucose solution, stirred, centrifuged and washed with deionized water and anhydrous ethanol, and then dried. The dried sample was placed in a tube furnace and calcined under the protection of Ar atmosphere. The calcined product was nano-TiO 2 @C; Step 3: In situ synthesis of nano-TiO 2 / MnO 2 Heterogeneous structures The nano-TiO synthesized in step 2 2 @C was added to potassium permanganate solution, stirred, and placed in a hydrothermal kettle for hydrothermal reaction. After the reaction was completed, it was centrifuged and washed with deionized water and dried. The final product was in-situ synthesized nano-TiO 2 / MnO 2 Heterogeneous structures; Step 4: Simultaneous alloying and pre-hydrogenation treatment After mixing Mg powder and Ni powder, alloying treatment and pre-hydrogenation treatment were carried out in a high-energy ball mill. The ball milling atmosphere was H 2 , after ball milling, Mg 2 Mg-Ni binary alloy powder of Ni phase; Step 5: Ball milling catalytic modification The nano-TiO prepared in step 3 2 / MnO 2 The heterogeneous structure is mixed with the Mg-Ni binary alloy powder prepared in step 4, and a ball mill is used to briefly mill the powder so that the two are evenly mixed; A catalytically modified magnesium-based composite material is obtained; Step 6: High-pressure catalytic hydrogenation modification placing the material prepared in step 5 in a high-pressure hydrogenation reactor for high-pressure hydrogenation to obtain a magnesium-based composite material hydride; Step 7: Grain refinement The magnesium-based composite material hydride prepared in step 6 is refined by ball milling to obtain a magnesium-based composite material with fine and uniform particle size.

4. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In the step 1, 20 to 40 mL of tetrabutyl titanate solution is added to a polytetrafluoroethylene liner and stirred. While stirring, 3 to 6 mL of hydrofluoric acid is dripped into the tetrabutyl titanate solution dropwise and stirred for 15 to 60 minutes. Subsequently, the tetrabutyl titanate solution is placed in a hydrothermal kettle and subjected to a hydrothermal reaction at 150 to 200° C. After the reaction is completed, the tetrabutyl titanate solution is centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60 to 100° C. for 6 to 12 hours. The dried sample is placed in a muffle furnace for calcination at a calcination temperature of 400 to 600° C.

5. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In step 2, TiO 2 The mass is 1-3 g, the solubility of the glucose solution is 0.02-0.06 mol / L, and the volume is 50-300 mL. After stirring for 8-12 hours, it is centrifugally washed with deionized water and anhydrous ethanol, and then dried at 60-100°C for 6-10 hours. The dried sample is placed in a tubular furnace and calcined under the protection of Ar atmosphere at a calcination temperature of 400-600°C.

6. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In the step 3, the mass of TiO2@C is 1-3 g, the solubility of potassium permanganate solution is 0.003-0.01 mol / L, the volume is 20-80 mL, and after stirring for 15-60 min, it is placed in a hydrothermal kettle and subjected to a hydrothermal reaction at 80-150° C. After the reaction is completed, it is centrifugally washed with deionized water and dried at 60-100° C. for 6-12 h.

7. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In step 4, Mg powder and Ni powder are mixed in a mass ratio of (75-97): (25-3), and alloying treatment and pre-hydrogenation treatment are performed using a high-energy ball mill, so that Mg and Ni undergo a mechanochemical reaction to generate Mg 2 Ni intermediate phase, ball milling atmosphere is H 2 , hydrogen pressure is 2-10 bar, ball-to-material ratio is (10-40):1, rotation speed is 800-1000 r / min, and ball milling is 8-12 hours.

8. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In step 5, nano-TiO 2 / MnO 2 The heterogeneous structure and Mg-Ni binary alloy powder are mixed in a mass ratio of (2-15):(85-98), the ball milling atmosphere is Ar, the ball-to-material ratio is (10-40):1, the rotation speed is 500-800 r / min, and the ball milling time is 10-60 min.

9. A TiO according to claim 3 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composite materials and preparation methods thereof, It is characterized in that In step 6, the hydrogen pressure is 3-8 MPa, the temperature is 300-350° C., and the hydrogenation time is 8-12 h; In step 7, the ball milling atmosphere is H 2 , the ball-to-material ratio is (10-30):1, the rotation speed is 400-800r / min, and the ball milling time is 1-2h.

10. A TiO according to any one of claims 1 to 9 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy to regulate the application of magnesium-based composites, It is characterized in that The TiO 2 / MnO 2 Heterogeneous structure nanocatalysis and nickel microalloying dual strategy regulation of magnesium-based composites for hydrogen storage, TiO 2 / MnO 2 With Mg 2 Ni undergoes a mechanochemical reaction to generate NiTi phase in situ, and Mg, MgH 2 Mg 2 Ni、Mg 2 NeA 4 、TiO 2 Multiple phases exist simultaneously, and multiphase boundaries provide diffusion channels for hydrogen atoms.

Citation Information

Cited By

  • Carbon nanofiber loaded MnTi bimetallic microsphere as well as preparation method and application thereof

    CN120024867A