650MPa-grade thick gauge steel with good corrosion resistance and production method of 650MPa-grade thick gauge steel
By adopting specific chemical composition and smelting processes in mining truck wheel materials, the problem of insufficient impact and corrosion resistance of existing materials is solved, and the improvement of high strength, toughness and corrosion resistance is achieved, and the service of wheel parts is extended life.
Patent Information
- Application Number
- CN202411139150.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
AI Technical Summary
During service, the existing mining truck wheel materials have not received any attention due to impact resistance and corrosion resistance, resulting in a decrease in the life of the parts.
Chemical components are C: 0.05-0.10%, Si≤0.50%, Mn: 1.4-1.8%, P≤0.030%, S≤0.010%, Nb: 0.025-0.060%, Ti: 0.040-0.070%, Sb: 0.05 ~0.26%, Al: 0.45~1.0% of 650MPa grade thick specification steel, and through specific smelting process steps, including conventional smelting, heating, rough rolling, finishing rolling, rapid cooling and coiling, control process parameters to improve the material Corrosion resistance.
While ensuring the yield strength ≥500MPa, the tensile strength 650~780MPa, and the elongation ≥24%, the impact resistance and corrosion resistance of the material are significantly improved, so that its impact force ≥200J in 20℃ is ≥200J in comparison with the corrosion of Q355B Rate ≤5%.
Smart Images

Figure BDA0005000261320000061 
Figure BDA0005000261320000071 
Figure BDA0005000261320000072
Abstract
Description
Technical Field
[0001] The invention relates to automobile steel and a production method, in particular to 650MPa grade thick specification steel with good corrosion resistance and a production method, and is particularly suitable for product steel plates with a thickness of 16 to 24 mm. Background Art
[0002] With the development of the infrastructure industry and the demand for large-scale engineering construction, the application of mining trucks is increasing. Mining trucks and other vehicles are used in harsh conditions, and the service reliability of various vehicle components is required to be high. The wheel is the moving component of the vehicle and carries a large load, especially for mining trucks, which are used in harsh conditions. In order to ensure the service reliability of mining truck spokes, the material is required to have good strength and toughness, and at the same time have the performance of acid soil corrosion resistance.
[0003] The current mining truck wheel materials are basically developed with strength and forming performance, but the impact resistance and corrosion resistance of steel in service are not paid attention to, which leads to many problems of reduced service life of mining truck wheel parts due to impact failure or corrosion failure in actual service. Therefore, the present invention mainly solves the problem of improving the impact resistance and corrosion resistance of the material while meeting the corresponding strength and elongation of the wheel material, thereby increasing the service life of mining truck wheel parts.
[0004] After searching:
[0005] The document with Chinese patent application number CN201410116557.1 discloses a steel for heavy truck ultra-thick steel spokes and its manufacturing method, with the mass percentage of trace elements as follows: carbon: 0.07-0.12%; silicon: 0.05-0.15%; manganese: 0.7-1.1%; niobium: 0.01-0.03%; titanium: 0.01-0.03%; phosphorus ≤0.015%; sulfur ≤0.005%; aluminum: 0.02-0.05%; nitrogen: ≤0.006%. The manufacturing method is to obtain a casting billet through KR desulfurization and LF treatment, perform rough rolling and finish rolling, laminar cooling, and coil to obtain the required steel, which meets the requirements of heavy truck spoke steel for easy spinning, surface quality and performance stability, and greatly reduces the breakage rate of heavy truck wheels. The document does not involve toughness and corrosion resistance.
[0006] The document with Chinese patent application number: CN202011378962.2 discloses "A 540MPa grade thick gauge automobile spoke steel", which includes: 0.05-0.10wt% C, 1.00-2.00wt% Mn, 0.05-0.30wt% Si, 0.02-0.05wt% Nb, 0.01-0.05wt% Ti, 0.01-0.05wt% Als, P≤0.020wt%, S≤0.010wt%, and the balance is Fe. The metallographic structure is ferrite + pearlite, with a yield strength of ≥450MPa, a tensile strength of ≥540MPa, an elongation of ≥20%, a 180° cold bending test d=a qualified, and a grain size of ≥10. This document does not involve toughness and corrosion resistance.
[0007] The document with Chinese patent application number CN201610392108.9 discloses "A thick-gauge heavy-duty truck wheel spoke steel and its preparation method", which is composed of the following weight percentage components: C: 0.07-0.10%, Si: 0.01-0.20%, Mn: 0.85-1.00%, P: 0.01%-0.025%, S: 0.01%-0.015%, Als: 0.010-0.050%, and the rest is Fe and unavoidable impurities. The document does not involve corrosion resistance.
[0008] The document with Chinese patent application number CN201410786247.0 discloses "A 600MPa grade thick gauge hot-rolled spoke steel and its manufacturing method", which specifically relates to a 600MPa grade thick gauge hot-rolled spoke steel and its manufacturing method. The chemical composition mass percentage of the spoke steel is 0.06-0.12% C, 0.20-0.60% Si, 0.80-1.20% Mn, 0.02-0.06% Alt, 0.50-1.00% Cr, 0.03-0.08% P, S≤0.005%, N≤0.006%, and the balance is Fe and unavoidable impurities. The billet heating temperature is 1150-1250℃, the finishing rolling temperature is 760-840℃, and after rolling, a conventional cooling process is adopted, and the steel is cooled to below 350℃ at a cooling rate of 20-100℃ / s for coiling. The steel plate has excellent processing performance and fatigue performance, and does not add elements such as Nb, V, Mo, and Ni, thereby saving production costs. The document does not involve corrosion resistance.
[0009] The document with Chinese patent application number: CN201810404146.0 discloses "A method for producing 590MPa-grade spoke steel", and its process is: finishing rolling of strip steel; using ultra-fast cooling and high-pressure rapid cooling process to cool the strip steel to 640°C; cooling the strip steel to the target coiling temperature according to conventional laminar cooling; air cooling the strip steel to room temperature. Although it solves the technical problems that the test production of 590MPa-grade spoke steel in the prior art cannot meet the standard requirements, and the addition of alloying elements such as Mn, Nb, and V is increased in order to improve the tensile strength, resulting in increased costs, worsening banded structure and center segregation, it achieves the technical effect of improving tensile strength, meeting standard requirements, and low cost, but does not involve corrosion resistance. Summary of the invention
[0010] The present invention aims to overcome the shortcomings of the corrosion resistance of the prior art and provide a 650MPa grade thick gauge steel and a production method thereof with good corrosion resistance, while ensuring a yield strength of ≥500MPa, a tensile strength of 650-780MPa, an elongation of ≥24%, an impact energy of ≥200J at -20°C, and a corrosion rate of ≤5% relative to that of Q355B.
[0011] Measures to achieve the above objectives:
[0012] A 650MPa grade thick gauge steel with good corrosion resistance, the components and weight percentage contents of which are: C: 0.05-0.10%, Si≤0.50%, Mn: 1.4-1.8%, P≤0.030%, S≤0.010%, Nb: 0.025-0.060%, Ti: 0.040-0.070%, Sb: 0.05-0.26%, Al: 0.45-1.0%, and the balance is balanced iron and unavoidable impurities.
[0013] Preferably, the weight percentage of Sb is 0.08-0.21%.
[0014] Preferably, the weight percentage of Al is 0.50-0.66%.
[0015] A method for producing 650MPa grade thick gauge steel with good corrosion resistance, comprising the following steps:
[0016] 1) Conventional smelting and continuous casting into billets;
[0017] 2) Heating the ingot: Control the ingot temperature to be no less than 920°C and the ingot heating temperature to be between 1220°C and 1270°C;
[0019] 3) performing rough rolling and controlling the rough rolling end temperature to be between 1000°C and 1080°C;
[0020] 4) Perform finish rolling and control the final rolling temperature at 800-840°C;
[0021] 5) Rapid cooling, cooling to 580-660° C. at a cooling rate of 70-130° C. / s;
[0022] 6) Coil the steel sheet: control the coiling temperature at 500-570°C;
[0023] 7) Reserved.
[0024] Preferably, the heating temperature of the casting is controlled at 1220-1245°C.
[0025] Preferably, the rapid cooling is performed at a rate of 90 to 130° C. / s to a temperature of 585 to 635° C.
[0026] Functions and mechanisms of the components and main processes in the present invention
[0027] Carbon: Carbon is a cheap solid solution strengthening element. According to the application range of this steel, it is mainly used for forming parts such as wheel spokes, which are generally processed by stamping or spinning. If its content is less than 0.05%, it cannot meet the strength requirements. If its content is greater than 0.10%, it cannot meet the good forming performance of the material. Therefore, its content is limited to 0.05-0.10%.
[0028] Antimony: Sb can form Sb2O5 corrosion-resistant oxide film on the steel surface, form SbOCl precipitation and adhesion in the anode micro-area, fill corrosion cracks or voids, and improve the barrier effect of corrosion Cl - The ability of Sb to penetrate the steel can improve the corrosion resistance of the steel in environments such as pickling soil; however, Sb is easily enriched in the grain boundaries, affecting the formability and toughness of the steel; therefore, the Sb content of the present invention is controlled to be 0.05% to 0.26%, preferably 0.08% to 0.21%.
[0029] Aluminum: The addition of Al can reduce the corrosion current density of steel. The corrosion product forms FeAl2O4 with cation selectivity, which inhibits the formation of Cl - The rust layer penetrates into the metal matrix, making the rust layer and the matrix more closely bonded, thereby improving the protectiveness of the rust layer. The Al content is controlled to be 0.45% to 1.0%, preferably 0.5% to 0.66%.
[0030] Manganese: Manganese is the most effective element for improving strength and toughness. If its content is less than 1.40%, it cannot meet the material strength requirements; however, adding a large amount of manganese will increase the hardenability of steel, increase crack sensitivity due to the appearance of weld hardening layer, and increase the alloy cost of steel. In view of this,
[0031] The upper limit is 1.80%, so the content is limited to the range of 1.40 to 1.80%.
[0032] Titanium: Titanium is one of the most economical elements to improve the strength of steel. With the appropriate process to exert the precipitation of TiC, the steel can reach the designed strength level. If the titanium content is less than 0.04%, insufficient precipitation will cause the strength to fail to reach the designed lower limit, and titanium content higher than 0.07% will cause the tensile strength to exceed the upper limit requirement. Therefore, its content is limited to the range of 0.04-0.07%.
[0033] The reason why the heating temperature of the casting blank is controlled within the range of 1220-1270° C. is that the Ti element and Nb element precipitated in the blank need to be fully heated and dissolved.
[0034] The reason why the rough rolling end temperature is controlled at 1000-1080° C. in the present invention is to ensure that the grain size after the rough rolling is not too large.
[0035] The reason why the finishing rolling temperature is controlled at 800-840° C. in the present invention is to control the grain size of the steel material after finishing rolling and promote the ferrite phase transformation in the subsequent cooling process.
[0036] The reason why the present invention controls the cooling rate to 70-130°C / S and cools to 580-660°C is that the high cooling rate can inhibit the grain growth of the steel plate during the cooling process, thereby ensuring good strength and elongation.
[0037] The reason why the coiling temperature is controlled at 500-570° C. in the present invention is to ensure that the steel plate obtains the final required ferrite ratio and grain size, thereby enabling the steel plate to obtain good impact toughness.
[0038] Compared with the prior art, the present invention has a -20°C impact energy of ≥200J and a corrosion rate of ≤5% relative to Q355B while ensuring a yield strength of ≥500MPa, a tensile strength of 650-780MPa, and an elongation of ≥24%. DETAILED DESCRIPTION
[0039] The present invention is described in detail below:
[0040] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0041] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0042] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.
[0043] Each embodiment of the present invention is produced according to the following steps:
[0044] 1) Conventional smelting and continuous casting into billets;
[0045] 2) Heating the ingot: Control the ingot temperature to be no less than 920°C and the ingot heating temperature to be between 1220°C and 1270°C;
[0047] 3) performing rough rolling and controlling the rough rolling end temperature at 1000-1080°C;
[0048] 4) Perform finish rolling and control the final rolling temperature at 800-840°C;
[0049] 5) Rapid cooling, cooling to 580-660° C. at a cooling rate of 70-130° C. / s;
[0050] 6) Coil the steel sheet: control the coiling temperature at 500-570°C;
[0051] 7) Reserved.
[0052] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0053]
[0054]
[0055] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0056]
[0057] Table 3 Performance test list of various embodiments of the present invention and comparative examples
[0058]
[0059]
[0060] Note: The embodiments in Table 2 and Table 3 correspond to the embodiment in Table 1;
[0061] The experimental conditions of the full immersion corrosion rate are as follows: the full immersion corrosion test is conducted according to "JB / T7901-1999 Metal Materials Laboratory Uniform Corrosion Full Immersion Test Method", the temperature is 23±2°C, 10% H2SO4+3.5% NaCl solution, full immersion for 24 hours, simulating the corrosion of steel by the acidic high-salinity soil leaching solution in the mine. The test results show that the corrosion rate of the steel of the present invention relative to Q355B is within 5%.
[0062] It can be seen from the results in Table 3 above that the steel of the present invention has a yield strength of ≥500MPa, a tensile strength of 650-780MPa, an elongation of ≥24%, an impact energy of ≥200J at -20°C, and a corrosion rate of ≤5% relative to that of Q355B, and has good corrosion resistance.
[0063] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A 650MPa grade thick gauge steel with good corrosion resistance, the components and weight percentages of which are: C: 0.05-0.10%, Si≤0.50%, Mn: 1.4-1.8%, P≤0.030%, S≤0.010%, Nb: 0.025-0.060%, Ti: 0.040~0.070%, Sb: 0.05~0.26%, Al: 0.45~1.0%, and the balance is iron and inevitable impurities.
2. A 650MPa grade thick gauge steel with good corrosion resistance as claimed in claim 1, Features: The weight percentage of Sb is 0.08-0.21%.
3. A 650MPa grade thick gauge steel with good corrosion resistance as claimed in claim 1, Features: The weight percentage of Al is between 0.50 and 0.66%.
4. A method for producing a 650MPa grade thick gauge steel with good corrosion resistance as claimed in claim 1, comprising the steps of: 1) Conventional smelting and continuous casting into billets; 2) Heating the ingot: Control the ingot temperature to be no less than 920°C and the ingot heating temperature to be between 1220°C and 1270°C; 3) performing rough rolling and controlling the rough rolling end temperature to be between 1000°C and 1080°C; 4) Perform finish rolling and control the final rolling temperature at 800-840°C; 5) Rapid cooling, cooling to 580-660° C. at a cooling rate of 70-130° C. / s; 6) Coil the steel sheet: control the coiling temperature at 500-570°C; 7) Reserved.
5. A method for producing a 650MPa grade thick gauge steel with good corrosion resistance as claimed in claim 4, Features: The heating temperature of the casting is controlled at 1220-1245°C.
6. A method for producing a 650MPa grade thick gauge steel with good corrosion resistance as claimed in claim 4, Features: The rapid cooling speed is 90-130°C / S while cooling to 585-635°C.
Citation Information
Patent Citations
High-performance and hot-rolled wear-resistant steel sheet and production method thereof
CN111254351A
Ultrahigh-strength steel for sanitation trucks and production method thereof
CN111575589A
Hot-rolled strip steel for low-cost thick-specification high-strength pipe pile and preparation method of hot-rolled strip steel
CN115627415A