High-strength hydrogen embrittlement-resistant stainless steel

By adding Nb and V microalloy elements to stainless steel and adopting specific heat treatment processes, the problem of hydrogen-induced delayed fracture of high-strength steel during the thermoforming process is solved, which significantly improves the anti-hydrogen embrittlement performance and ductility, and enhances the safety of use .

CN119040746APending Publication Date: 2024-11-29JIANGSU XIHU SPECIAL STEEL
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411214412.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

High-strength steels are prone to hydrogen-induced delayed fracture during the thermal forming process, which affects the safety of use. The prior art is difficult to effectively reduce their hydrogen-induced fracture sensitivity.

Method used

Using stainless steel containing Nb and V microalloy elements, the hydrogen embrittlement sensitivity is reduced by refining austenite grains and forming high-efficiency hydrogen traps in the matrix, combined with tempering and quenching processes.

Benefits of technology

It significantly improves the anti-hydrogen embrittlement properties and ductility of stainless steel, delays the breaking time and reduces the sensitivity of hydrogen embrittlement, and enhances the safety of use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides high-strength hydrogen embrittlement-resistant stainless steel. The high-strength hydrogen embrittlement-resistant stainless steel comprises, by mass, 0.1%-0.4% of C, 0.2%-0.5% of Si, 4.5%-5.5% of Mn, smaller than or equal to 0.01% of P, smaller than or equal to 0.002% of S, 0.6%-1.0% of Cr, 0.1%-0.2% of V, smaller than or equal to 0.08% of Nb, 0.001%-0.005% of B and the balance Fe. Nb and V microalloy elements are added on the basis of original stainless steel, so that austenite grains are refined, and meanwhile, a high-performance hydrogen trap is formed in a matrix, so that the hydrogen-induced delayed fracture resistance of the steel is improved. The stainless steel is treated by a hot forming process, a steel plate is subjected to isothermal annealing, a tempering process is added, the temperature and time of the tempering process are controlled, and finally quenching is performed, so that the brittleness intergranular fracture of the obtained stainless steel is obviously reduced, and the hydrogen embrittlement sensitivity of the stainless steel is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of stainless steel production and manufacturing, and in particular to high-strength hydrogen embrittlement-resistant stainless steel. Background Art

[0002] With the continuous development of my country's high-end industry, advanced high-strength steel has been increasingly used. However, with the increase in strength, the delayed fracture sensitivity of steel has gradually increased, especially for hot-formed steel. The deformation during the hot forming process will cause the steel matrix to have strong residual stress. In a hydrogen-containing environment, hydrogen-induced delayed fracture is prone to occur, which seriously affects the safety of use. Therefore, it is necessary to improve the existing high-strength steel, reduce its hydrogen-induced fracture sensitivity, and enhance the safety of high-strength steel use.

[0003] At present, the main research directions for the research on hydrogen embrittlement resistance of stainless steel are to add specific trace elements or to refine the grains of stainless steel by heat treatment process. However, in the research and development of stainless steel, the ratio of each element and the improvement of manufacturing process, any change of factors will cause a chain of influences and changes. After experiments, our company has obtained a high-strength hydrogen embrittlement resistant stainless steel. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high-strength hydrogen embrittlement resistant stainless steel.

[0005] To achieve the above object, the present invention adopts the following technical solutions: A high-strength hydrogen embrittlement-resistant stainless steel comprises, by mass%, C: 0.1%-0.4%, Si: 0.2%-0.5%, Mn: 4.5%-5.5%, P≤0.01%, S≤0.002, Cr: 0.6%-1.0%, V: 0.1%-0.2%, Nb≤0.08%, B: 0.001%-0.005%, and the balance is Fe.

[0006] The preparation process of the stainless steel comprises the following steps: S1, melting and pouring into ingot according to the set composition; S2, heating the ingot at 1200°C for 1.5-2h and then rolling it, with the final rolling temperature at 900°C, and finally rolling it into a steel plate with a thickness of 6mm; S3, isothermally annealing the hot rolled steel plate in the two-phase region at 650°C for 6h; S4, after pickling the steel plate, rolling is performed for 4-5 times, and the thickness of the final rolled steel plate is 2mm; S5, cooling the steel plate to room temperature; S6. Heat the steel plate to 480-520°C for tempering, and keep the temperature for 1 hour; S7, taking out the heat-treated stainless steel plate, immediately transferring it to a hot forming mold, and quenching it to 150°C; S8. Take the stainless steel plate out of the hot forming mold and cool it to room temperature.

[0007] Preferably, in terms of mass %, (Nb+V) in the stainless steel is ≤0.2%.

[0008] Preferably, the stainless steel contains 0.14% V in terms of mass %.

[0009] Preferably, the stainless steel contains 1.0% Cr in terms of mass %.

[0010] Preferably, the grain size of the stainless steel is 5 μm on average.

[0011] Preferably, in the stainless steel, the average size of fine carbide precipitates with a size of more than 10 nm is 16 nm, and the average size of fine carbide precipitates with a size of less than 10 nm is 5.5 nm.

[0012] Further, in S4, the steel plate is pickled using 18% hydrochloric acid and rolled on a 450 type rolling mill for 4-5 passes.

[0013] Furthermore, in S7, the quenching method is water cooling quenching.

[0014] Furthermore, in S5 and S8, the cooling method is air cooling.

[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. By adding Nb and V microalloying elements to the original stainless steel, the austenite grains are refined and high-efficiency hydrogen traps are formed in the matrix, thereby improving the steel's resistance to hydrogen-induced delayed fracture and hydrogen embrittlement.

[0016] 2. Control the content of Nb and V to effectively improve the hydrogen embrittlement resistance of stainless steel while ensuring the ductility and other properties of stainless steel.

[0017] 3. In the preparation process of the high-strength hydrogen embrittlement-resistant stainless steel of the present invention, the isothermal annealing time of the steel plate is set to 6 hours, and a tempering process is added at the same time, and the temperature and time of the tempering process are controlled, and finally quenching is performed. The brittle intergranular fracture of the obtained stainless steel is significantly reduced, and the hydrogen embrittlement sensitivity of the stainless steel is effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] none DETAILED DESCRIPTION

[0019] In order to provide a further understanding of the purpose, structure, features, and functions of the present invention, the following detailed description is given in conjunction with the embodiments.

[0020] A high-strength hydrogen embrittlement-resistant stainless steel comprises, by mass%, C: 0.1%-0.4%, Si: 0.2%-0.5%, Mn: 4.5%-5.5%, P≤0.01%, S≤0.002, Cr: 0.6%-1.0%, V: 0.1%-0.2%, Nb≤0.08%, B: 0.001%-0.005%, and the balance is Fe.

[0021] The preparation process of the stainless steel comprises the following steps: S1, melting and pouring into ingot according to the set composition; S2, heating the ingot at 1200°C for 1.5-2h and then rolling it, with the final rolling temperature at 900°C, and finally rolling it into a steel plate with a thickness of 6mm; S3, isothermally annealing the hot rolled steel plate in the two-phase region at 650°C for 6h; S4, after pickling the steel plate, rolling is performed for 4-5 times, and the thickness of the final rolled steel plate is 2mm; S5, cooling the steel plate to room temperature; preferably, air cooling to room temperature; S6. Heat the steel plate to 480-520°C for tempering, and keep the temperature for 1 hour; preferably, the tempering temperature is set to 500°C.

[0022] S7, taking out the heat-treated stainless steel plate, immediately transferring it to a hot forming mold, and quenching it to 150°C; S8. Take the stainless steel plate out of the hot forming mold and cool it to room temperature; preferably, air cool it to room temperature.

[0023] The high-strength hydrogen embrittlement-resistant stainless steel of the present invention adds Nb and V microalloying elements on the basis of the original 22MnB5 stainless steel. Nb and V are elements that easily form carbonitrides, which can refine austenite grains and form high-efficiency hydrogen traps in the matrix, thereby improving the hydrogen-induced delayed fracture resistance of the steel.

[0024] V is added to 22MnB5 stainless steel: 0.1%-0.2%. V has a good effect on improving strength and grain refinement. It can also form carbonitrides with carbon (C) or nitrogen (N) and be used as a capture point for hydrogen invading the steel. It also plays a role in inhibiting the intrusion of hydrogen inside the steel material and reducing the occurrence of corrosion.

[0025] Nb≤0.08% is added to 22MnB5 stainless steel. Nb microalloying can improve the hydrogen embrittlement resistance of steel, mainly because Nb element acts as a reversible hydrogen trap, which can capture hydrogen atoms, thereby reducing the diffusion coefficient of hydrogen in steel and reducing the occurrence of hydrogen embrittlement. In addition, the addition of Nb element can also greatly improve the hydrogen embrittlement resistance of steel by regulating the microstructure. However, excessive Nb content will form coarse carbonitrides, which will lead to a decrease in the ductility of stainless steel. After testing, Nb is limited to 0.08%.

[0026] The high-strength hydrogen embrittlement-resistant stainless steel of the present invention is compared with the traditional 22MnB5 hot-formed steel. After quenching trial production, the average austenite size of the 22MnB5 stainless steel is 12 μm, while the average austenite size of the stainless steel of the present invention is 8 μm. The microalloying elements Nb and V are segregated at the austenite grain boundaries, which hinders the grain growth of the austenite of the hot-formed steel and plays a role in refining the grains.

[0027] The high-strength hydrogen embrittlement-resistant stainless steel of the present invention is compared with the traditional 22MnB5 hot-formed steel. The overall grain size of the stainless steel of the present invention is smaller than that of the traditional 22MnB5 stainless steel, and there are more small-angle grain boundaries, and the grain size is more uniform, and the hydrogen embrittlement sensitivity is lower.

[0028] The high-strength hydrogen embrittlement-resistant stainless steel of the present invention and the traditional 22MnB5 hot-formed steel were subjected to hydrogen embrittlement sensitivity experiments under the same conditions. The time corresponding to the delayed fracture of the high-strength hydrogen embrittlement-resistant stainless steel of the present invention was significantly longer than that of the traditional 22MnB5 hot-formed steel. The analysis is as follows: the stainless steel of the present invention uses Nb, V and C to create a large number of hydrogen traps inside the material, and the aggregation areas of C, Nb, V and H basically overlap, so that the concentration of hydrogen that can be enriched along the maximum stress gradient direction is greatly reduced, effectively inhibiting hydrogen diffusion, thereby delaying the time of delayed fracture; while the traditional 22MnB5 steel has no correlation between the hydrogen and C element distribution inside, and cannot inhibit hydrogen diffusion, resulting in a relatively higher hydrogen embrittlement sensitivity.

[0029] In the stainless steel preparation process of the present invention, more reverse austenite and ferrite are formed in the initial stage of the stainless steel plate annealing process, and a small amount of cementite is included; as the annealing time increases to 6 hours, the content of reverse austenite increases to about 18% and the size increases, and the carbide disappears. After the stainless steel plate is tempered, the brittle intergranular fracture of the stainless steel is significantly reduced, and the hydrogen embrittlement sensitivity of the stainless steel is effectively reduced.

[0030] In one embodiment, in the stainless steel, (Nb+V) is ≤0.2% by mass. Too much content will reduce the ductility of the stainless steel and increase the cost.

[0031] In one embodiment, the stainless steel contains 0.14% V by mass. Furthermore, the stainless steel contains 1.0% Cr by mass. The VC precipitate phase can effectively inhibit hydrogen embrittlement while improving the strength of the material. As the V content increases, the size of VC increases and the number increases. However, when the mass fraction of V exceeds 1%, large-sized undissolved VC will appear, which is easy to cause hydrogen embrittlement. 0.14% V combined with 1% Cr for multi-micro alloying can obtain the best hydrogen embrittlement resistance and work hardening ability.

[0032] In a preferred embodiment, a high-strength hydrogen embrittlement-resistant stainless steel includes, by mass%, C: 0.2%, Si: 0.3%, Mn: 5%, P≤0.01%, S≤0.002, Cr: 0.7%, V: 0.1%, Nb: 0.06%, B: 0.002%, and the balance is Fe.

[0033] The average grain size of the stainless steel in this embodiment is 5 μm. Compared with the traditional 22MnB5 hot-formed steel, the grain size is smaller and more uniform, and the hydrogen embrittlement resistance is better.

[0034] In this embodiment, the average size of fine carbide precipitates with a size of more than 10 nm in the stainless steel is 16 nm, and the average size of fine carbide precipitates with a size of less than 10 nm is 5.5 nm.

[0035] The high-strength hydrogen embrittlement-resistant stainless steel of the present invention has smaller and more uniform grain sizes, more small-angle boundaries, and a smaller average size of fine carbide precipitates, and thus has better hydrogen embrittlement resistance. The high-strength hydrogen embrittlement-resistant stainless steel of the present invention is subjected to a hydrogen embrittlement sensitivity test under bending loading conditions. When the span reaches 70 mm and the stress reaches 1622 MPa, it can still remain free from cracking for 300 hours under hydrogen environment solution conditions.

[0037] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the spirit and scope of the present invention are all within the scope of patent protection of the present invention.

Claims

1. A high-strength hydrogen embrittlement-resistant stainless steel, characterized in that: In terms of mass%, it includes C: 0.1%-0.4%, Si: 0.2%-0.5%, Mn: 4.5%-5.5%, P≤0.01%, S≤0.002, Cr: 0.6%-1.0%, V: 0.1%-0.2%, Nb≤0.08%, B: 0.001%-0.005%, and the balance is Fe; The preparation process of the stainless steel comprises the following steps: S1, melting and pouring into ingot according to the set composition; S2, heating the ingot at 1200°C for 1.5-2h and then rolling it, with the final rolling temperature at 900°C, and finally rolling it into a steel plate with a thickness of 6mm; S3, isothermally annealing the hot rolled steel plate in the two-phase region at 650°C for 6h; S4, after pickling the steel plate, rolling is performed for 4-5 times, and the thickness of the final rolled steel plate is 2mm; S5, cooling the steel plate to room temperature; S6. Heat the steel plate to 480-520°C for tempering, and keep the temperature for 1 hour; S7, taking out the heat-treated stainless steel plate, immediately transferring it to a hot forming mold, and quenching it to 150°C; S8. Take the stainless steel plate out of the hot forming mold and cool it to room temperature.

2. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: In terms of mass %, (Nb+V) in the stainless steel is ≤0.2%.

3. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 2, characterized in that: In terms of mass %, the stainless steel contains 0.14% of V.

4. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 3, characterized in that: The stainless steel contains 1.0% Cr in terms of mass%.

5. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: The grain size of the stainless steel is 5 μm on average.

6. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: In the stainless steel, the average size of fine carbide precipitates with a size of 10 nm or more is 16 nm, and the average size of fine carbide precipitates with a size of 10 nm or less is 5.5 nm.

7. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: In S4, the steel plate is pickled using 18% hydrochloric acid and rolled in 4-5 passes on a 450 type rolling mill.

8. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: In S7, the quenching method is water cooling quenching.

9. The high-strength hydrogen embrittlement-resistant stainless steel according to claim 1, characterized in that: In S5 and S8, the cooling method is air cooling.

Citation Information

Cited By

  • Industrial production method of 1500MPa stainless steel hot-formed steel hot-rolled product

    CN119956054A

  • Hydrogen embrittlement-resistant ultrahigh-strength steel with gradient structure and preparation method of hydrogen embrittlement-resistant ultrahigh-strength steel

    CN121538389A

  • High-strength hydrogen-embrittlement-resistant stainless steel

    WO2026045488A1