Method for efficiently removing oil on surface of spandex waste silk and quickly homogenizing and dissolving spandex waste silk

Through the combination of Soxhlet extraction method and specific oil removal agent, the problem of oil removal on the surface of spandex waste silk is solved, efficient oil removal and homogeneous dissolution is achieved, production costs and environmental impact are reduced, and the spinning of waste silk is ensured. and performance.

CN119041059APending Publication Date: 2024-11-29ZHEJIANG SCI-TECH UNIV +3

Patent Information

Application Number
CN202411095862.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The oil agent on the surface of spandex waste wire is difficult to remove, resulting in the fan blockage and performance deterioration during the spinning process. The existing cleaning methods require a large amount of cleaning liquid and organic solvents, which increases production costs and environmental pressure.

Method used

The surface oil agent of waste silk is extracted by Soxhlet extraction method, and its components are determined, and the emulsified oil cleaning agent, oil degreasing agent QTQ-104 or nylonext oil degreasing agent Goon108 is treated, combining mild temperature and stirring conditions to achieve high efficiency Degreasing and homogeneous dissolving.

Benefits of technology

The oil removal process is simplified, the cost is reduced, the fan is blocked and performance losses are avoided, the spinning and rebound performance of the waste wire is ensured, and the additional cleaning agent is required.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004987914370000011
    Figure HDA0004987914370000011
  • Figure HDA0004987914370000012
    Figure HDA0004987914370000012
  • Figure HDA0004987914370000021
    Figure HDA0004987914370000021
Patent Text Reader

Abstract

The invention discloses a method for efficiently removing oil on the surface of spandex waste silk and rapidly homogenizing and dissolving the surface of the spandex waste silk, and relates to the technical field of oil removal, the method comprises the following steps: extracting an oil agent on the surface of the spandex waste silk to obtain an extracted oil agent, and determining components of the extracted oil agent; according to the components of the extracted oil agent, an oil removing agent is selected, the spandex waste silk is put into the oil removing agent to be treated, the treatment temperature is 50-70 DEG C, and the treatment time is 20-40 min; the use amount of the degreasing agent is 1-6 mg / ml. The method for treating the waste silk is simple and easy to understand, convenient to operate and beneficial to large-scale application of the technology. The degreasing agent is easy to obtain, conditions such as treatment time and treatment temperature are not harsh and are in a conventional process condition range, and the method is convenient to popularize and apply. The oil removal conditions are simple and easy to obtain, the oil removal effect of the waste silk can be kept, the influence of an oil agent contained in the waste silk on follow-up operation is eliminated, and the economic and time cost can be saved while the oil removal effect is guaranteed for enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil removal, and in particular to a method for efficiently removing oil from the surface of waste spandex yarn and rapidly and homogeneously dissolving the oil. Background Art

[0002] In the spandex production process, a large amount of waste silk is often generated due to spinning, broken yarn failures, and abnormal winding. According to relevant data statistics, the scrap rate per ton of silk is generally around 15kg. According to my country's current spandex production capacity of 800,000 t / a, the annual waste silk volume is as high as 12,000t. Waste silk accounts for the largest proportion of waste in spandex production, so the research on the recycling and treatment of spandex waste silk is also the most comprehensive. At present, the methods for recycling and reusing spandex waste silk include three main methods: waste silk dissolution and respinning technology, waste silk depolymerization to prepare polyurethane derivatives, and waste silk filling with other polymers.

[0003] Waste silk respinning technology is a waste silk disposal method currently adopted by most spandex manufacturers. Its advantages are that no additional equipment investment is required, the cost is low, and the recycling efficiency is high. Wang Baohua and others cut the spandex waste silk into 5 cm short silks and put them into a dissolving kettle for stirring and dissolving. At the same time, in order to prevent the thermal oxidation degradation of polyurethane in the high-temperature channel, antioxidants were added, and finally the waste silk respinning products were prepared. Wu Zhonghu directly put the dried waste silk into the conventional spandex stock solution, and then added dimethylacetamide, mixed evenly and spun it. These two methods seem simple and easy, but they ignore the influence of the oil agent carried by the waste silk itself on the subsequent spinning process and the changes in the performance indicators of the waste silk products. The most important problem that needs to be solved in the respinning of waste silk is how to remove the oil agent on the surface of the waste silk.

[0004] Before being spun into yarn cakes, spandex is oiled to avoid adhesion between yarns. The oil used usually contains more than 50% of organic siloxanes, which will dissolve in the spinning solution during the waste yarn recovery process. When the siloxane-containing yarn is dried in a hot air tunnel, the siloxane undergoes oxidation and degradation to produce substances such as silicon dioxide, which adsorbs and blocks the tunnel filter, eventually causing the fan to fail. There are currently two solutions to this problem: one is to regularly stop production and disassemble and clean the tunnel fan. This method not only seriously affects the production progress, but also increases the labor intensity of employees. The other is to remove oil and clean the spandex waste yarn. Hu Weiwei et al. disclosed a method for cleaning the surface of spandex to remove oil. The method soaks the spandex waste yarn in a special cleaning solution, assists with ultrasonic oscillation treatment, and then soaks and rinses it in an organic solvent for a second time, and finally hot air dries it to obtain spandex waste yarn with no oil on the surface. After cleaning, the silicon content on the surface of the waste yarn tends to zero. However, this method requires the use of a large amount of cleaning fluid and organic solvent, which increases the cost of production; and the recycling and reuse of cleaning fluid and organic solvent is also a key problem that must be solved. Yu Zongbao and others sprayed an aqueous solution of 1% by mass of end-capped polyether-modified polysiloxane on the surface of the spandex waste silk, and then heated and dried it to remove the auxiliaries and foreign matter attached to the surface of the spandex waste silk. This invention does not require the use of additional cleaning agents, avoids the adverse effects of cleaning agents on the performance of spandex waste silk, and greatly saves process costs. After the waste silk is dissolved and respun, its mechanical properties are significantly deteriorated compared with conventional spandex, which is manifested as shorter elongation and weaker elasticity. In order to make up for the loss of product rebound performance during the reproduction of waste silk, Liu Yahui and others added a cross-linking agent with trifunctional groups during the dissolution and maturation of the waste silk, and increased the method of chemical cross-linking to make the finished spandex have better rebound performance.

[0005] The waste silk has a large specific surface area and is easy to agglomerate, making it difficult to remove the surface oil. When the waste silk is subsequently spun and dried, it will undergo oxidative degradation and block the fan, causing the fan to fail. Secondly, maintaining efficient and homogeneous dissolution of the waste silk and inhibiting degradation is a prerequisite for achieving its spinnability. Summary of the invention

[0006] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a method for efficiently removing oil from the surface of waste spandex yarn and rapidly and homogeneously dissolving the same.

[0007] The technical solution of the present invention is as follows:

[0008] A method for efficiently removing oil from the surface of waste spandex yarn and rapidly dissolving it in a homogeneous manner comprises the following steps:

[0009] S1: extracting the surface oil of the spandex waste yarn to obtain an extracted oil, and determining the composition of the extracted oil;

[0010] S2: Select a degreasing agent according to the composition of the extracted oil agent, and place the spandex waste into the degreasing agent for treatment.

[0011] As a preferred embodiment of the present invention, in step S1, the components of the extraction oil agent include dimethyl silicone oil, long-chain aliphatic hydrocarbons and carbonyl substances.

[0012] As a preferred embodiment of the present invention, in step S2, the deoiling agent is at least one of emulsified soap oil cleaning agent, deoiling agent QTQ-104, and nylon spandex deoiling agent Goon108.

[0013] As a preferred embodiment of the present invention, in step S2, the treatment temperature is 50-70°C and the treatment time is 20-40 minutes.

[0014] As a preferred embodiment of the present invention, in step S2, the amount of degreasing agent used is 1-6 mg / ml.

[0015] As a preferred embodiment of the present invention, in step S2, the amount of degreasing agent used is 4 mg / ml.

[0016] As a preferred embodiment of the present invention, in step S2, stirring is performed while the treatment is performed.

[0017] As a preferred embodiment of the present invention, in step S1, the extraction is specifically as follows: weigh the heavy spandex waste, control the reflux rate to 8-12 minutes / time, and perform Soxhlet extraction for 3-5 hours.

[0018] The beneficial effects of the present invention are:

[0019] 1. The method for treating waste silk of the present invention is simple and easy to understand, has a low operating threshold, and is conducive to large-scale application in technology.

[0020] 2. The degreasing agent used in the present invention is easily available, and the processing time, processing temperature and other conditions are not harsh and are within the range of conventional process conditions, which is convenient for the promotion and application of the present invention.

[0021] 3. The degreasing conditions of the present invention are simple and easy to obtain, and the degreasing effect of the waste silk can be maintained, eliminating the influence of the oil contained in the waste silk on subsequent operations, thereby ensuring the degreasing effect for the enterprise and saving economic and time costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a graph showing the relationship between waste silk extraction time and extraction rate.

[0023] Figure 2 This is the infrared spectrum of the extracted oil.

[0024] Figure 3 This is a graph showing the relationship between the oil removal rate and the different concentrations of three degreasing agents at 70°C.

[0025] Figure 4 This is a graph showing the relationship between the oil removal rate and the different concentrations of three degreasing agents at 60°C.

[0026] Figure 5 This is a graph showing the relationship between the oil removal rate and the different concentrations of three degreasing agents at 50°C.

[0027] Figure 6 This is a graph showing the relationship between the oil removal rate and the different treatment times of the three oil removers at 70°C and the oil remover concentration of 4 mg / ml. DETAILED DESCRIPTION

[0028] The purpose of the present invention is achieved through the following solutions:

[0029] First, use the Soxhlet extraction method to extract the surface oil of the waste silk:

[0030] 4 g of waste silk was taken, and the waste silk oil was first extracted by Soxhlet extraction method, and the optimal extraction time was 4 h;

[0031] According to the above experimental method, about 4 grams of spandex waste silk was weighed, the reflux rate was controlled to be about 10 minutes / time, Soxhlet extraction was performed for 4 hours, and the measurement was repeated three times. The average extraction rate of spandex waste silk extract was 4.35%. The results are as follows Figure 1 ;

[0032] Further, infrared spectroscopy was used to analyze the oil, referring to Figure 2 , determine the ingredients contained in the oil agent, it can be known that the textile extract contains dimethyl silicone oil, long-chain aliphatic hydrocarbons and carbonyl substances.

[0033] According to the degreasing process and the degreasing agent dosage gradient range designed in the single factor experiment, the effects of degreasing agent dosage and degreasing agent type on the degreasing efficiency of spandex waste yarn were determined:

[0034] Each time, select an appropriate amount of waste spandex yarn for use, then choose one of the three degreasers, weigh an appropriate amount of the degreaser in a beaker, add 100 ml of deionized water to the beaker, put it into a constant temperature magnetic stirrer and stir to make the solution uniform, then add the waste spandex yarn into a water bath heating container, select the temperature, and stir at a constant temperature for a certain period of time, then wash the waste yarn with water, then put it into an oven to dry it to a dry state, and finally weigh it again.

[0035] The spandex waste yarn is weighed 2 g each time.

[0036] The three degreasing agents are emulsified soap oil cleaning agent, degreasing agent QTQ-104, and nylon spandex degreasing agent Goon108.

[0037] The experimental conditions are a treatment temperature of 70° C. and a treatment time of 30 min.

[0038] The degreasing agent dosage gradient range is 1-6 mg / ml.

[0039] The treatment temperature was adjusted to 60°C and 50°C respectively, and the above experiment was repeated.

[0040] According to the above experiments, the optimal degreasing temperature of 60°C and the optimal degreasing agent concentration of 4 mg / ml were selected, and the effects of degreasing treatment time and degreasing agent type on the degreasing efficiency of spandex waste yarn were determined according to the degreasing process and the degreasing treatment time gradient range designed in the single factor experiment:

[0041] Each time, select an appropriate amount of waste spandex yarn for use, then choose one of the three degreasing agents, weigh a certain amount of degreasing agent in a beaker, add 100 ml of deionized water to the beaker, put it into a constant temperature magnetic stirrer and stir to make the solution uniform, select the temperature, then add the waste spandex yarn into a water bath heating container, perform timing treatment according to the selected treatment time gradient range, wash the waste yarn with water, then put it into an oven to dry it to a dry state, and finally weigh it again.

[0042] 2 g of the spandex waste yarn was weighed each time, and 0.4 g of degreasing agent was added each time.

[0043] The experimental condition is a processing temperature of 60°C.

[0044] The three degreasing agents are emulsified soap oil cleaning agent, degreasing agent QTQ-104, and nylon spandex degreasing agent Goon108.

[0045] The oil removal treatment time gradient range is 5-40 min.

[0046] The present invention sets a degreasing temperature range, a degreasing agent concentration range, a processing time range and a range of easily available degreasing agent types that are conducive to reducing losses, and determines the optimal process conditions that can achieve sufficient degreasing effects through single-factor testing. While making the degreasing method simple and easy to implement, it ensures the control of degreasing costs and the easy availability of degreasing conditions, and fully considers the actual benefits of the application of the invention.

[0047] The mechanism of the present invention is:

[0048] The present invention first extracts spandex waste silk by Soxhlet extraction method to determine the oil content (4.35%) in the waste silk, and determines the type of oil contained in the waste silk (dimethyl silicone oil, long-chain aliphatic hydrocarbons and carbonyl substances) by infrared spectroscopy test, thereby selecting a suitable degreasing agent category for subsequent process exploration; under three set commonly used temperature conditions, a single factor test is carried out to screen out the optimal degreasing concentration and degreasing temperature within the set process parameter range, thereby determining the treatment time and concentration, and then determining the optimal treatment time within the treatment time range; finally, the optimal process conditions that meet the degreasing effect are screened out.

[0049] Therefore, the present invention selects a mild cleaning agent and optimizes the physical ripening parameters to quickly and efficiently remove the oil on the surface of the waste silk to prevent its subsequent decomposition and clogging of the fan. At the same time, the low-temperature crushing-normal-temperature dissolution-ribbon plus screw circulation stirring technology is comprehensively used to accelerate the homogeneous dissolution of the waste silk and inhibit the degradation of its molecular weight.

[0050] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0051] The materials involved in the following examples can all be obtained from commercial channels.

[0052] Example 1

[0053] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of emulsified soap oil cleaning agent into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 70℃ water bath for 30min, after heating, take out the degreased waste silk, wash it with water twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0054] Under the treatment conditions of 70℃ and 30min, the relationship between the concentration of emulsified soap oil cleaning agent and the oil removal rate is as follows: Figure 3 shown.

[0055] Example 2

[0056] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of degreaser QTQ-104 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 70℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0057] Under the treatment conditions of 70℃ and 30min, the relationship between the concentration of degreasing agent QTQ-104 and the degreasing rate is as follows: Figure 3 shown.

[0058] Example 3

[0059] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of nylon spandex degreaser Goon108 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 70℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0060] Under the conditions of 70℃ and 30min treatment, the relationship between the concentration of nylon spandex degreasing agent Goon108 and the degreasing rate is as follows: Figure 3 shown.

[0061] Example 4

[0062] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of emulsified soap oil cleaning agent into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 60℃ water bath for 30min, after heating, take out the deoiled waste silk, wash it with water twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0063] Under the treatment conditions of 60℃ and 30min, the relationship between the concentration of emulsified soap oil cleaning agent and the oil removal rate is as follows: Figure 4 shown.

[0064] Example 5

[0065] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of degreaser QTQ-104 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 60℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0066] Under the treatment conditions of 60℃ and 30min, the relationship between the concentration of degreasing agent QTQ-104 and the degreasing rate is as follows Figure 4 shown.

[0067] Example 6

[0068] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of nylon spandex degreaser Goon108 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 60℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0069] Under the conditions of 60℃ and 30min treatment, the relationship between the concentration of nylon spandex degreasing agent Goon108 and the degreasing rate is as follows: Figure 4 shown.

[0070] Example 7

[0071] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of emulsified soap oil cleaning agent into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 70℃ water bath for 30min, after heating, take out the degreased waste silk, wash it with water twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0072] Under the treatment conditions of 50℃ and 30min, the relationship between the concentration of emulsified soap oil cleaning agent and the oil removal rate is as follows: Figure 5 shown.

[0073] Example 8

[0074] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of degreaser QTQ-104 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 50℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0075] Under the treatment conditions of 50℃ and 30min, the relationship between the concentration of degreasing agent QTQ-104 and the degreasing rate is as follows: Figure 5 shown.

[0076] Example 9

[0077] Add 0.1g, 0.2g, 0.3g, 0.4g, 0.5g and 0.6g of nylon spandex degreaser Goon108 into a 250ml beaker filled with 100ml deionized water, put them into a magnetic stirrer and stir for one minute, then take them out and add 2g of spandex waste silk to each cup, seal the cup mouth with plastic film, put them into a 50℃ water bath for 30min, after heating, take out the degreased waste silk, wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0078] Under the conditions of 50℃ and 30min treatment, the relationship between the concentration of nylon spandex degreasing agent Goon108 and the degreasing rate is as follows: Figure 5 shown.

[0079] Example 10

[0080] Add 0.4g of emulsified soap detergent to 250ml beakers containing 100ml of deionized water, stir in a magnetic stirrer for one minute, take out and add 2g of spandex waste to each cup, seal the cup mouth with plastic film, repeat the above steps to obtain six samples. Put the six samples into a 60℃ water bath for 5, 10, 20, 30, and 40min respectively. After heating, take out the degreased waste silk and wash it twice, then put it into an oven to dry it, and finally weigh the dried waste silk.

[0081] Under the treatment conditions of 60℃ and degreasing agent concentration of 4mg / ml, the relationship between degreasing time and degreasing rate of emulsified soap oil cleaning agent is as follows: Figure 6 shown.

[0082] Embodiment 11

[0083] 0.4g of degreasing agent QTQ-104 was added to 250ml beakers containing 100ml of deionized water, and then placed in a magnetic stirrer for one minute. After taking out, 2g of spandex waste was added to each cup, and then the cup mouth was sealed with plastic film. Repeat the above steps to obtain six samples. The six samples were placed in a 60℃ water bath for 5, 10, 20, 30, and 40 minutes respectively. After heating, the degreased waste was taken out and washed twice, then placed in an oven to dry, and finally the dried waste was weighed.

[0084] Under the treatment conditions of 60℃ and degreasing agent concentration of 4mg / ml, the relationship between degreasing time and degreasing rate of degreasing agent QTQ-104 is as follows: Figure 6 shown.

[0085] Example 12

[0086] 0.4g of nylon spandex degreasing agent Goon108 was added to a 250ml beaker containing 100ml deionized water, and then placed in a magnetic stirrer for one minute. After taking it out, 2g of spandex waste was added to each cup, and then the cup mouth was sealed with a plastic film. Repeat the above steps to obtain six samples. The six samples were placed in a 60℃ water bath for 5, 10, 20, 30, and 40 minutes respectively. After heating, the degreased waste was taken out and washed twice, then placed in an oven to dry it, and finally the dried waste was weighed.

[0087] Under the treatment conditions of 60℃ and degreasing agent concentration of 4mg / ml, the relationship between degreasing time and degreasing rate of nylon spandex degreasing agent Goon108 is as follows: Figure 6 shown.

[0088] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof, characterized in that: The following steps are involved: S1: extracting the surface oil of the spandex waste yarn to obtain an extracted oil, and determining the composition of the extracted oil; S2: Select a degreasing agent according to the composition of the extracted oil agent, and place the spandex waste into the degreasing agent for treatment.

2. The method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S1, the components of the extraction oil include dimethyl silicone oil, long-chain aliphatic hydrocarbons and carbonyl substances.

3. The method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S2, the degreasing agent is at least one of emulsified soap oil cleaning agent, degreasing agent QTQ-104, and nylon spandex degreasing agent Goon108.

4. The method for efficient surface degreasing of spandex waste yarn and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S2, the treatment temperature is 50-70°C and the treatment time is 20-40 minutes.

5. The method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S2, the amount of degreasing agent used is 1-6 mg / ml.

6. The method for efficient surface oil removal and rapid homogeneous dissolution of spandex waste according to claim 1, characterized in that: In step S2, the amount of degreasing agent used is 4 mg / ml.

7. The method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S2, stirring is performed while the treatment is performed.

8. The method for efficient surface degreasing of spandex waste and rapid homogeneous dissolution thereof according to claim 1, characterized in that: In step S1, the extraction is specifically as follows: weigh the heavy spandex waste, control the reflux rate to 8-12 minutes / time, and perform Soxhlet extraction for 3-5 hours.

Citation Information

Patent Citations

  • Regeneration method of dry spinning spandex waste silk

    CN101760799A

  • Surface deoiling and cleaning method of polyurethane fiber waste silk

    CN103343404A

  • Production process of nylon Simiantan fabric

    CN107700252A

  • Method for extracting spandex surface oil agent via supercritical carbon dioxide

    CN109023786A

Cited By

  • Dyeing and finishing pretreatment process of nylon spandex fabric

    CN121087813A