Microscopic determination method for grain size of original austenite of quenched and tempered steel

Through EBSD technology and HKL Channel5 software, the austenite grain size of tempered steel is directly measured, which solves the safety hazards of the use of picric acid in the existing technology and the problem of low detection success rate, and realizes the austenite grain size The precise determination of the material provides an important basis for material analysis.

CN119043835APending Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410828260.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, picric acid is used to measure the austenite grain boundary with low success rate and safety risks, making it difficult to effectively detect the original austenite grain size of tempered steel.

Method used

Using electron backscattering diffractometer (EBSD) technology, combined with scanning electron microscope and HKL Channel5 software, the original austenite grain size of the tempered steel is directly measured through sample preparation, parameter setting and data post-processing analysis to avoid hazardous use. Taste.

Benefits of technology

The precise determination of the size of the original austenite grains in tempered structure of tempered steel is achieved, providing an important theoretical basis for the evolution of the tissue during the phase transition, improving the detection success rate and eliminating safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043835A_ABST
    Figure CN119043835A_ABST
Patent Text Reader

Abstract

The invention provides a microcosmic determination method for the original austenite grain size of quenched and tempered steel. The microcosmic determination method specifically comprises the following steps: (1) preparing a sample; (2) setting EBSD parameters; feeding the prepared sample into an electron back scattering diffractometer for EBSD (electron back scattering diffraction) analysis; (3) post-processing and analyzing the data; after scanning is finished, data processing is conducted on a scanning result through EBSD post-processing software HKL Channel5, zero analysis points in a view field are removed, a pattern quality diagram of a sample tempering structure is obtained, at the moment, an original austenite grain boundary can be clearly displayed, then the outline of original austenite grains is drawn, and the appearance of the original austenite grain boundary can be displayed. And the size of the original austenite grains of the tempered structure of the sample can be directly calculated through EBSD post-processing software HKL Channel5. According to the technical scheme, the problems that in the prior art, the success rate of measuring the original austenite grain boundary through a strong corrosive agent is low, and potential safety hazards exist are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material analysis and testing, and in particular to a microscopic determination method for original austenite grain size of quenched and tempered steel. Background Art

[0002] The original austenite grain size in steel plays a very important role in optimizing its strength and toughness and other mechanical properties. It is also important for studying the phase transformation law of the organization of steel during the heat treatment process, as well as the relationship between organizational evolution and mechanical properties. Therefore, the detection of the original austenite grain size is very important. The display of austenite grains is mainly achieved by the grain boundary corrosion method, that is, by taking picric acid + other solutions, mixing them in a certain ratio, and etching at high temperature or room temperature. However, in the actual operation process, it is often necessary to try repeatedly and change the etching parameters repeatedly, and the success rate is not high. In addition, picric acid is a strong acid, dangerous and explosive, and is a registered substance with the Public Security Bureau. Many companies and universities have banned its use. Summary of the invention

[0003] Based on the above technical problems that the existing technology uses strong corrosive agents to measure the original austenite grain boundaries with a low success rate and has potential safety hazards, a microscopic determination method for the original austenite grain size of quenched and tempered steel is provided, which does not require the use of hazardous chemicals such as picric acid. The EBSD technology is used to clearly see the lath structure and the original austenite boundary contour after martensite shearing of the quenched and tempered steel (tempered structure), and the original austenite grain size can be directly determined by software.

[0004] The technical means adopted by the present invention are as follows:

[0005] A microscopic determination method for the original austenite grain size of quenched and tempered steel specifically comprises the following steps:

[0006] (1) Sample preparation

[0007] The quenched and tempered steel sample is processed by wire cutting to make the sample. The upper and lower surfaces of the sample are parallel to each other. The sample surface is ground and polished to remove the surface stress.

[0008] (2) EBSD parameter setting

[0009] The prepared samples were sent to an electron backscatter diffractometer for EBSD analysis. In order to obtain clear Kikuchi flower patterns, the parameters of the scanning electron microscope were set as follows: the acceleration voltage was 15-20 kV, the working distance was 15-20 mm, the step size was less than or equal to 1 / 10 of the average grain size of the sample, and the acquisition time was more than 1 hour;

[0010] (3) Data post-processing analysis

[0011] After the scan is completed, the scan results are processed by the EBSD post-processing software HKL Channel5: the zero resolution point in the field of view is removed to obtain the pattern quality map of the sample tempering structure. At this time, the original austenite grain boundary can be clearly displayed, and then the outline of the original austenite grain is outlined. The size of the original austenite grain of the sample tempering structure can be directly calculated by the EBSD post-processing software HKL Channel5.

[0012] Furthermore, the sample size satisfies a length of 8 to 10 mm, a width of 5 to 8 mm, and a thickness of ≤3 mm; the surface stress is removed by mechanical polishing or electrolytic polishing of the sample surface using a 0.05 μm aluminum oxide suspension + a 0.02 μm silicon oxide suspension.

[0013] Compared with the prior art, the present invention has the following advantages:

[0014] The microscopic determination method of the original austenite grain size of the quenched and tempered steel provided by the present invention does not use hazardous chemicals such as picric acid, and directly calculates the size of the original austenite grains of the quenched and tempered steel (tempered structure) through the EBSD technology, which can provide an important theoretical basis for studying the organizational evolution during the phase transformation process.

[0015] Based on the above reasons, the present invention can be widely promoted in the field of material analysis and testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0017] Figure 1 This is the pattern quality diagram obtained in Example 1 with tempered martensite as the matrix structure.

[0018] Figure 2 This is the statistical distribution diagram of the original austenite grain size in Example 1. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] The present invention provides a microscopic determination method for the original austenite grain size of quenched and tempered steel, which specifically comprises the following steps:

[0021] (1) Sample preparation

[0022] The quenched and tempered steel sample is processed by wire cutting to make the sample. The upper and lower surfaces of the sample are parallel to each other. The sample surface is ground and polished to remove the surface stress.

[0023] (2) EBSD parameter setting

[0024] The prepared samples were sent to the electron backscatter diffractometer for EBSD analysis. In order to obtain clear Kikuchi flower patterns, the parameters of the scanning electron microscope were set as follows: the acceleration voltage was 15-20 kV, the working distance was 15-20 mm, the step length was less than or equal to 1 / 10 of the average grain size of the sample, and the acquisition time was greater than 1 hour. The time should not be too short to avoid poor surface scanning image quality, which is not conducive to subsequent data post-processing analysis.

[0025] (3) Data post-processing analysis

[0026] After the scan is completed, the scan results are processed using the EBSD post-processing software HKL Channel5: the zero resolution points in the field of view are removed. The purpose of removing the zero resolution points is to fill the zero resolution points of a single or several pixel blocks on the interface to make the interface complete and obtain the pattern quality map of the sample tempering structure. At this time, the original austenite grain boundaries can be clearly displayed, and then the outline of the original austenite grains is outlined. The size of the original austenite grains of the sample's tempered structure can be directly calculated using the EBSD post-processing software HKL Channel5.

[0027] Furthermore, the sample size satisfies a length of 8 to 10 mm, a width of 5 to 8 mm, and a thickness of ≤3 mm; the surface stress is removed by mechanical polishing or electrolytic polishing of the sample surface using a 0.05 μm aluminum oxide suspension + a 0.02 μm silicon oxide suspension.

[0028] Example 1

[0029] This embodiment takes the quenched and tempered P690 low-temperature steel as an example, whose tempered structure is tempered martensite. The microscopic determination method of the original austenite grain size of the quenched and tempered steel described in the present invention is used, which specifically includes the following steps:

[0030] (1) Sample preparation

[0031] The quenched and tempered steel sample is processed by wire cutting to make the sample. The upper and lower surfaces of the sample are parallel to each other. The sample surface is polished to remove the surface stress and obtain a flat, clean and bright polished surface.

[0032] The sample size meets the requirements of length 10mm, width 8mm, and thickness 3mm;

[0033] The surface stress is removed by grinding and polishing the sample surface and then mechanically polishing with 0.05μm aluminum oxide suspension + 0.02μm silicon oxide suspension (electrolytic polishing can also be used);

[0034] (2) EBSD parameter setting

[0035] The prepared samples were sent to the electron backscatter diffractometer for EBSD analysis. In order to obtain a clear Kikuchi flower pattern, the parameters of the scanning electron microscope were set: the acceleration voltage was 15 kV, the aperture was 120 μm, the sample was firmly attached to the sample stage with a tilt angle of 70°, the working distance was 16.5 mm, the step length was 0.4 μm, and the scanning area was 280 × 200 μm. 2 , pattern collection time 1h;

[0036] (3) Data post-processing analysis

[0037] After scanning, the scanning results were processed by EBSD post-processing software HKL Channel5: the zero resolution point in the field of view was removed to obtain a pattern quality map with tempered martensite as the matrix structure. At this time, the original austenite grain boundaries can be clearly displayed, such as Figure 1 The contrast + inverse pole figure + grain boundary map with orientation difference greater than 15 degrees in this embodiment is shown, and then the outline of the original austenite grains is outlined. Then, the size of the original austenite grains of the tempered steel structure can be directly calculated through the EBSD post-processing software HKL Channel5, as shown in FIG. Figure 2 As shown, a statistical analysis was performed on the original austenite grain size of the sample in this embodiment, and the sizes of 124 relatively clear austenite grains were measured. The average size was 6.10 μm, the maximum was 43.5 μm, and the minimum was 1.4 μm.

[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A microscopic determination method for the original austenite grain size of quenched and tempered steel, characterized in that: The specific steps include: (1) Sample preparation The quenched and tempered steel sample is processed by wire cutting to make the sample. The upper and lower surfaces of the sample are parallel to each other. The sample surface is ground and polished to remove the surface stress. (2) EBSD parameter setting The prepared samples were sent to the electron backscatter diffractometer for EBSD analysis. In order to obtain clear Kikuchi flower patterns, the parameters of the scanning electron microscope were set; (3) Data post-processing analysis After the scan is completed, the scan results are processed by the EBSD post-processing software HKL Channel5: the zero resolution point in the field of view is removed to obtain the pattern quality map of the sample tempering structure. At this time, the original austenite grain boundary can be clearly displayed, and then the outline of the original austenite grain is outlined. The size of the original austenite grain of the sample tempering structure can be directly calculated by the EBSD post-processing software HKL Channel5.

2. The microscopic determination method of the original austenite grain size of quenched and tempered steel according to claim 1, characterized in that: The sample size meets the requirements of length 8-10 mm, width 5-8 mm, and thickness ≤3 mm; the surface stress is removed by mechanical polishing or electrolytic polishing of the sample surface using 0.05 μm aluminum oxide suspension + 0.02 μm silicon oxide suspension.

3. The microscopic determination method of the original austenite grain size of quenched and tempered steel according to claim 1, characterized in that: In step (2), the parameters of the scanning electron microscope are set as follows: the acceleration voltage is 15-20 kV, the working distance is 15-20 mm, the step length is less than or equal to 1 / 10 of the average grain size of the sample, and the acquisition time is greater than 1 hour.