Chromium-nickel co-doped Co (OH) F electrode material and preparation method and application thereof

Through the preparation of chromium-nickel co-doped Co(OH)F electrode material, the problem of poor conductivity of Co(OH)F nanoelectrode materials is solved, the electrochemical performance of supercapacitors is improved, and high specific capacitance and excellent rate performance are achieved.

CN119049887APending Publication Date: 2024-11-29JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411268891.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing Co(OH)F nanoelectrode materials have poor electrical conductivity and low electronic conductivity, which limits their large-scale application in high-performance supercapacitors.

Method used

Using chromium-nickel co-doped Co(OH)F electrode material and its preparation method, by stirring and sonicating the soluble cobalt salt, nickel salt, chromium salt, ammonium fluoride and hydrazine hydrate in a specific ratio, followed by hydrothermal heat Reaction, cooling, centrifugation, drying and grinding, and chromium-nickel co-doped Co(OH)F electrode material with a large specific surface area was prepared.

Benefits of technology

The electrochemical performance of supercapacitors is improved, and high specific capacitance and excellent rate performance are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049887A_ABST
    Figure CN119049887A_ABST
Patent Text Reader

Abstract

The invention discloses a chromium-nickel co-doped Co (OH) F electrode material and a preparation method and application thereof, and belongs to the technical field of electrode materials, and the preparation method comprises the following steps: step 1, mixing soluble cobalt salt, nickel salt, chromium salt, ammonium fluoride, hydrazine hydrate and deionized water to obtain a mixed solution; and 2, carrying out a hydrothermal reaction on the mixed solution to obtain a reactant, and sequentially cooling, centrifuging, drying and grinding the reactant to obtain the chromium-nickel co-doped Co (OH) F electrode material. The electrode material prepared by the invention has a relatively large specific surface area, and the electrochemical performance of the supercapacitor can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode materials, and in particular relates to a chromium-nickel co-doped Co(OH)F electrode material and a preparation method and application thereof. Background Art

[0002] With the massive consumption of traditional fossil fuels, global warming and environmental pollution have rapidly intensified, and there is an urgent need to find renewable and sustainable alternative energy sources. Supercapacitors, as a new type of device with the characteristics of rapid energy storage, high power density, and high reliability, have attracted widespread attention. In order to meet the growing demand for energy density in the future, it is necessary to continuously improve the performance of supercapacitors. The key to the development of supercapacitors is to find suitable electrode materials. There are three commonly used electrode materials: carbon materials, conductive polymers, and transition metal compounds. Compared with carbon materials, transition metal compounds have higher specific capacity and better cycle stability than conductive polymers, so transition metal compounds have received widespread attention. With the development of science and technology, researchers have developed Co(OH)F nanoelectrode materials. Although this material has improved a certain capacitance, the existing Co(OH)F nanoelectrode materials have poor conductivity and low electronic conductivity, which hinders their large-scale application in high-performance supercapacitors. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a chromium-nickel co-doped Co(OH)F electrode material and a preparation method and application thereof. The electrode material has a large specific surface area and is applied in the preparation of supercapacitors to improve the electrochemical performance of supercapacitors.

[0004] A method for preparing a chromium-nickel co-doped Co(OH)F electrode material comprises the following steps:

[0005] Step 1: Mix soluble cobalt salt, nickel salt, chromium salt, ammonium fluoride, hydrazine hydrate and deionized water to obtain a mixed solution;

[0006] Step 2: subjecting the mixed solution to a hydrothermal reaction, and obtaining a reactant, sequentially cooling, centrifuging, drying and grinding the reactant to obtain a chromium-nickel co-doped Co(OH)F electrode material.

[0007] In step 1, the mass ratio of the soluble cobalt salt, nickel salt, chromium salt and ammonium fluoride is 7.2-7.6:1.5-1.8:0.8-1.1:4.6-4.9.

[0008] The volume ratio of hydrazine hydrate and deionized water in step 1 is 1-2:250-350 ml.

[0009] The soluble cobalt salt is cobalt nitrate, cobalt chloride or cobalt acetate; the nickel salt includes nickel nitrate, nickel chloride and nickel acetate; the chromium salt includes chromium nitrate and chromium chloride.

[0010] The mixing process in step 1 is carried out under stirring and ultrasonic conditions in sequence, the stirring speed is 5000-8000 r / min, and the time is 1-1.5 h; the power of the ultrasound is 70-90 W, and the time is 0.5-1 h.

[0011] In step 2, the hydrothermal reaction temperature is 120-160° C., and the time is 6-12 h; the centrifugal speed is 7000-9000 r / min, and the time is 20-50 min; the drying is carried out by oven drying, and the drying temperature is 55-75° C., and the time is 12-18 h.

[0012] A chromium-nickel co-doped Co(OH)F electrode material is prepared by adopting the preparation method of the chromium-nickel co-doped Co(OH)F electrode material.

[0013] The invention discloses an application of a chromium-nickel co-doped Co(OH)F electrode material, and applies the chromium-nickel co-doped Co(OH)F electrode material to the preparation of supercapacitors.

[0014] Through the above design scheme, the present invention can bring the following beneficial effects: a chromium-nickel co-doped Co(OH)F electrode material and a preparation method and application thereof, having high specific capacitance and excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The present invention is further described below with reference to the accompanying drawings and specific embodiments:

[0016] Figure 1 This is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 of the present invention;

[0017] Figure 2 This is an X-ray diffraction pattern of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 of the present invention;

[0018] Figure 3 This is a constant current charge-discharge curve diagram of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 of the present invention;

[0019] Figure 4 The rate performance curve of the chromium-nickel co-doped Co(OH)F electrode material prepared by Example 1 of the present invention;

[0020] Figure 5 This is a nitrogen adsorption-desorption curve of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 of the present invention;

[0021] Figure 6 This is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 2 of the present invention;

[0022] Figure 7 This is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 3 of the present invention;

[0023] Figure 8 This is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified. The following experimental methods and detection methods are conventional methods unless otherwise specified; the following reagents and raw materials are commercially available unless otherwise specified.

[0025] Example 1

[0026] A method for preparing a chromium-nickel co-doped Co(OH)F electrode material comprises the following steps:

[0027] (1) 580 mg of cobalt nitrate, 120 mg of nickel nitrate, 70 mg of chromium nitrate, and 370 mg of NH 4 F, 120 μl of hydrazine hydrate (N 2 H 4 ·H 2 (2) adding into deionized water to obtain a mixed solution;

[0028] (2) adding the mixed solution of step (1) into a stainless steel autoclave with a Teflon liner having a volume of 50 mL and maintaining the autoclave at 140° C. for a solvothermal reaction for 6 h, then naturally cooling the autoclave to room temperature, collecting the sample and washing it several times, and then centrifuging, drying, and grinding it to obtain a chromium-nickel co-doped Co(OH)F electrode material;

[0029] Example 2

[0030] A method for preparing a chromium-nickel co-doped Co(OH)F electrode material comprises the following steps:

[0031] (1) 620 mg of cobalt nitrate, 130 mg of nickel nitrate, 80 mg of chromium nitrate, and 390 mg of NH4 F, 120 μl of hydrazine hydrate (N 2 H 4 ·H 2 (2) adding into deionized water to obtain a mixed solution;

[0032] (2) adding the mixed solution of step (1) into a stainless steel autoclave with a Teflon liner having a volume of 50 mL and maintaining the autoclave at 150° C. for a solvothermal reaction for 8 h, then naturally cooling the autoclave to room temperature, collecting the sample and washing it several times, and then centrifuging, drying, and grinding it to obtain a chromium-nickel co-doped Co(OH)F electrode material;

[0033] Example 3

[0034] A method for preparing a chromium-nickel co-doped Co(OH)F electrode material comprises the following steps:

[0035] (1) 600 mg of cobalt nitrate, 140 mg of nickel nitrate, 85 mg of chromium nitrate, and 390 mg of NH 4 F, 120 μl of hydrazine hydrate (N 2 H 4 ·H 2 (2) adding into deionized water to obtain a mixed solution;

[0036] (2) adding the mixed solution of step (1) into a stainless steel autoclave with a Teflon liner having a volume of 50 mL and maintaining the autoclave at 120° C. for a solvothermal reaction for 10 h, then naturally cooling the autoclave to room temperature, collecting the sample and washing it several times, and then centrifuging, drying, and grinding to obtain a chromium-nickel co-doped Co(OH)F electrode material;

[0037] Comparative Example 1

[0038] A method for preparing a chromium-nickel co-doped Co(OH)F electrode material comprises the following steps:

[0039] (1) 620 mg of cobalt nitrate, 130 mg of nickel nitrate, 80 mg of chromium nitrate, and 400 mg of NH 4 F, 120 μl of hydrazine hydrate (N 2 H 4 ·H 2 (2) adding into deionized water to obtain a mixed solution;

[0040] (2) adding the mixed solution of step (1) into a stainless steel autoclave with a Teflon liner having a volume of 50 mL and maintaining the autoclave at 180° C. for a solvothermal reaction for 8 h, then naturally cooling the autoclave to room temperature, collecting the sample and washing it several times, and then centrifuging, drying, and grinding to obtain a chromium-nickel co-doped Co(OH)F electrode material;

[0041] The preparation steps of Comparative Example 1 are the same as those of Example 2, except that the reaction temperature is changed from 150°C to 180°C.

[0042] The following conclusions can be drawn from Examples 1-3 of the present invention and Comparative Example 1:

[0043] Figure 1 is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1. Figure 1 It can be seen that the electrode material is composed of nanoparticles, which are evenly dispersed without obvious agglomeration.

[0044] Figure 2 is the X-ray diffraction pattern of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1, Figure 2 It can be seen that the diffraction peaks of the chromium-nickel co-doped Co(OH)F electrode material correspond one to one with the standard card, indicating that no other impurities are generated, proving that a homogeneous phase with high crystallinity is synthesized in this embodiment.

[0045] Figure 3 This is the constant current charge and discharge curve of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1. Calculation shows that the material has a specific capacitance of 863F / g at a current density of 1A / g, indicating that it has high capacitance performance and also proves that the material has good electrochemical properties.

[0046] Figure 4 The specific capacitance and current density of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 are plotted in a dotted line graph. The material still has a higher specific capacitance at a higher current density, indicating that the material has excellent rate performance.

[0047] Figure 5 The nitrogen adsorption-desorption curve of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 1 shows that the material has a nitrogen adsorption-desorption rate of 131 m 2 The high specific surface area of ​​​​1.1747 W / g indicates that this material has a larger specific surface area and more active sites.

[0048] Figure 6 is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 2, Figure 6 It can be seen that the electrode material sample is composed of nanoparticles, which are evenly dispersed without obvious agglomeration.

[0049] Figure 7 is a scanning electron microscope image of the chromium-nickel co-doped Co(OH)F electrode material prepared in Example 3, Figure 7It can be seen that the electrode material sample is mainly composed of nanoparticles, but it has obvious agglomeration phenomenon, which affects the performance of the electrode material.

[0050] Figure 8 This is a scanning electron microscope image of a comparative sample of the chromium-nickel co-doped Co(OH)F electrode material prepared in Comparative Example 1. Figure 8 It can be seen that the sample is mainly composed of nanoparticles, but a small amount of impurities appear in it, indicating that the synthesis method of Comparative Example 1 cannot synthesize pure phase chromium-nickel co-doped Co(OH)F material; and the results show that the reaction temperature has a great influence on the morphology of chromium-nickel co-doped Co(OH)F material. When the temperature is lower than 140°C, the nanoparticles show obvious agglomeration phenomenon; when the temperature is higher than 180°C, side reactions occur, impurities appear in the material, and the performance of the electrode material is affected.

[0051] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a chromium-nickel co-doped Co(OH)F electrode material, characterized by: The following steps are included: Step 1: Mix soluble cobalt salt, nickel salt, chromium salt, ammonium fluoride, hydrazine hydrate and deionized water to obtain a mixed solution; Step 2: subjecting the mixed solution to a hydrothermal reaction, and obtaining a reactant, sequentially cooling, centrifuging, drying and grinding the reactant to obtain a chromium-nickel co-doped Co(OH)F electrode material.

2. The method for preparing a chromium-nickel co-doped Co(OH)F electrode material according to claim 1, characterized in that: The mass ratio of the soluble cobalt salt, nickel salt, chromium salt and ammonium fluoride is 7.2-7.6:1.5-1.8:0.8-1.1:4.6-4.

9.

3. The method for preparing a chromium-nickel co-doped Co(OH)F electrode material according to claim 1, characterized in that: The volume ratio of hydrazine hydrate and deionized water in step 1 is 1-2:250-350 ml.

4. The method for preparing a chromium-nickel co-doped Co(OH)F electrode material according to claim 1 or 2, characterized in that: The soluble cobalt salt is cobalt nitrate, cobalt chloride or cobalt acetate; the nickel salt includes nickel nitrate, nickel chloride and nickel acetate; the chromium salt includes chromium nitrate and chromium chloride.

5. The method for preparing a chromium-nickel co-doped Co(OH)F electrode material according to claim 1, characterized in that: The mixing process in step 1 is carried out under stirring and ultrasonic conditions in sequence, the stirring speed is 5000-8000 r / min, and the time is 1-1.5 h; the power of the ultrasound is 70-90 W, and the time is 0.5-1 h.

6. The method for preparing a chromium-nickel co-doped Co(OH)F electrode material according to claim 1, characterized in that: In step 2, the hydrothermal reaction temperature is 120-160° C., and the time is 6-12 h; the centrifugal speed is 7000-9000 r / min, and the time is 20-50 min; the drying is carried out by oven drying, and the drying temperature is 55-75° C., and the time is 12-18 h.

7. A chromium-nickel co-doped Co(OH)F electrode material, characterized by: The electrode material is prepared by the method for preparing a chromium-nickel co-doped Co(OH)F electrode material as described in claim 1.

8. An application of chromium-nickel co-doped Co(OH)F electrode material, characterized by: The chromium-nickel co-doped Co(OH)F electrode material prepared in claim 1 is applied to the preparation of supercapacitors.