Photoelectrochemical ultraviolet detector with back-in prism structure and preparation method and application of photoelectrochemical ultraviolet detector

By introducing quartz and TiO2 solutions into the photoelectrochemical ultraviolet detector, the back-entry prism structure is formed, which solves the problem of ultraviolet light filtration, broadens the response range of the detector and improves sensitivity and stability.

CN119050177APending Publication Date: 2024-11-29SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185185.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing photoelectrochemical ultraviolet detectors have problems with ultraviolet light filtration, and they cannot detect ultraviolet signals below 300nm, resulting in a narrow response range.

Method used

The photoelectrochemical UV detector adopts a back-entry prism structure. By introducing quartz into the prism structure, ultraviolet light is incident from the back of the quartz, passing through the electrolyte to the photoanode, and combining TiO2 solution as the photoanode material, optimizing the photoelectric conversion efficiency and electrode performance .

Benefits of technology

The response spectrum of the detector is widened to 220-400nm, the sensitivity and response speed are improved, the ultraviolet filtration problem is solved, and the overall performance and stability of the detector are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050177A_ABST
    Figure CN119050177A_ABST
Patent Text Reader

Abstract

The invention discloses a photoelectrochemical ultraviolet detector with a back-in triangular prism structure and a preparation method and principle thereof, and belongs to the technical field of semiconductor photoelectric ultraviolet detectors, half of a first substrate is covered to serve as an electrode connected with an outer ring, the other half of the first substrate serves as a photoanode substrate, a precursor solution is coated on the first substrate, and the photoelectrochemical ultraviolet detector is prepared. Performing first annealing treatment; coating chloroplatinic acid on a second substrate, and carrying out second annealing treatment; forming a triangular prism structure by using quartz, the first substrate after annealing treatment and the second substrate after annealing treatment, and carrying out packaging treatment; after electrolyte is injected into the triangular prism structure from the top of the triangular prism structure, the top is sealed, and the photoelectrochemical ultraviolet detector of the back-in type triangular prism structure is obtained. Ultraviolet light can efficiently enter from the back of the quartz and penetrate through the electrolyte to reach the photoanode, so that the sensitivity and the response speed of the detector are improved, the serious ultraviolet light filtering problem in the photoelectrochemical ultraviolet detector is solved, and the response spectrum range is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor photoelectric ultraviolet detection devices, and in particular relates to a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure and a preparation method and application thereof. Background Art

[0002] Ultraviolet (UV) detectors have very important applications in military, biosensing, optical communication, remote control and other fields. According to the different structures and working principles, UV detectors are mainly divided into thermal detectors, photosensitive detectors and photoelectric UV detectors. Thermal detectors have poor sensitivity, photosensitive detectors also have poor thermal sensitivity and low working efficiency, and photoelectric detectors require external power during detection. Combining the above advantages and disadvantages, researchers have discovered a new self-powered photoelectrochemical UV detector.

[0003] Photoelectrochemical UV detectors have the advantages of low cost, environmental friendliness, and simple manufacturing process, and can well realize UV ​​detection. It is mainly composed of a sandwich structure device consisting of three parts: a photoanode, a counter electrode, and an electrolyte. The photoanode is composed of a conductive electrode and a semiconductor active layer. In existing research, the photoanode is mainly made based on FTO / ITO. This conductive film formed by wide-bandgap semiconductor oxides has serious UV filtering problems, that is, the devices prepared with them cannot detect UV signals below 300nm, which makes the response range of the device narrow.

[0004] In view of the narrow response range of existing photoelectrochemical ultraviolet detectors, it is urgent to develop a new type of photoelectrochemical ultraviolet detector to broaden its detection capability for ultraviolet signals below 300nm. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure to solve the serious ultraviolet light filtering problem in traditional photoelectrochemical ultraviolet detectors.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for preparing a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, comprising the following steps:

[0008] Covering half of the first substrate as an electrode connected to the outer ring and the other half as a photoanode substrate, applying a precursor solution on the first substrate, and performing a first annealing treatment;

[0009] coating chloroplatinic acid on the second substrate and performing a second annealing treatment;

[0010] Quartz, the first substrate after annealing and the second substrate after annealing are combined into a prism structure, and then packaged;

[0011] After injecting electrolyte into the interior of the prism structure from the top of the prism structure, the top is sealed to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure.

[0012] Preferably, the precursor solution is applied onto the first substrate by spin coating; the annealing temperature of the first annealing treatment is 300-550° C., and the annealing time is 60-120 min.

[0013] Preferably, the precursor solution is a TiO2 solution; the TiO2 solution is formed by mixing a mixed solution A, a mixed solution B and a mixed solution C; the mixed solution A includes: hydrochloric acid, acetic acid and the first part of ethanol; the mixed solution B includes: titanium isopropanol and the second part of ethanol; the mixed solution C includes: OP emulsifier, the third part of ethanol, ethyl cellulose and PVP.

[0014] Further preferably, the dosage ratio of hydrochloric acid: acetic acid: the first part of ethanol: titanium isopropanol: the second part of ethanol: OP emulsifier: the third part of ethanol: ethyl cellulose: PVP is (1-3) mL: (5-10) mL: (5-10) mL: (5-10) mL: (10-20) mL: (1-5) mL: (8-15) mL: (0.2-0.7) g: (0.3-0.8) g; when preparing the TiO2 solution, first stir the mixed solution A for 5-20 min; stir the mixed solution B for 5-20 min; stir the mixed solution C for 15-60 min; then mix and stir the mixed solution A, mixed solution B and mixed solution C for 15-60 min.

[0015] Preferably, chloroplatinic acid is coated on the second substrate by spin coating; the annealing temperature of the second annealing treatment is 200-400° C., and the annealing time is 60-90 min.

[0016] Preferably, the angle between the first substrate and the quartz is 20-90°, and the size of the second substrate is determined by the angle between the first substrate and the quartz; the first substrate is FTO or ITO; and the second substrate is FTO or ITO.

[0017] Preferably, the light transmittance of quartz in the visible region is 80%-95%.

[0018] Preferably, the electrolyte is deionized water or NaOH solution; the thickness of the electrolyte is 50 μm-1 cm.

[0019] The present invention also discloses a back-entry photoelectrochemical ultraviolet detector with a triangular prism structure, which is manufactured by the above-mentioned manufacturing method and comprises: a first substrate, a second substrate and a triangular prism structure composed of quartz, wherein the first substrate is coated with a first film; the second substrate is coated with a second film; and the interior of the triangular prism structure is filled with an electrolyte.

[0020] The present invention also discloses the principle of the photoelectrochemical ultraviolet detector with the back-entry triangular prism structure, including: ultraviolet light is incident perpendicular to quartz, passes through the electrolyte and reaches the first film; the electrons on the first film first reach the conductive layer of the first substrate, and then reach the second substrate through the external circuit connecting the first substrate and the second substrate; the holes on the first film first pass through the electrolyte, undergo oxidation and reduction, and then reach the second substrate, and then undergo oxidation and reduction with the electrons on the second substrate.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention discloses a method for preparing a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, wherein half of a first substrate is covered as an electrode connected to an outer ring, and the other half is used as a photoanode substrate; the electrode and the photoanode substrate are integrated on the same substrate, which simplifies the device structure, improves the space utilization rate, and may reduce the preparation cost. A precursor solution is applied to the first substrate, and a first annealing treatment is performed: the annealing treatment helps the solidification and crystallization of the precursor solution to form a stable photoanode material, thereby improving the photoelectric conversion efficiency of the detector. Chloroplatinic acid is applied to the second substrate, and a second annealing treatment is performed; after annealing with chloroplatinic acid, a platinum electrode is formed, which has good conductivity and stability, and helps to improve the electrode performance and long-term stability of the detector. Quartz, the first substrate after annealing, and the second substrate after annealing are formed into a triangular prism structure, and a packaging treatment is performed; quartz has a high light transmittance in the ultraviolet-visible light region, and it is used as a part of the triangular prism, which effectively solves the ultraviolet filtering problem of the traditional FTO / ITO substrate, so that ultraviolet signals below 300nm can be detected. The prism structure also helps to refract and focus light, thereby improving light utilization. After injecting electrolyte from the top of the prism structure into the interior of the prism structure, the top is sealed to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure; the injection of electrolyte provides the necessary ion conduction environment for the photoelectrochemical reaction, while the sealed top ensures the stability and long-term service life of the detector. The back-entry prism structure allows ultraviolet light to be efficiently incident from the back of the quartz, pass through the electrolyte and reach the photoanode, further improving the sensitivity and response speed of the detector. Compared with existing photoelectrochemical ultraviolet detectors, the present invention provides a photoelectrochemical ultraviolet detector with a back-entry prism structure by changing the structure of traditional photoelectrochemical ultraviolet detectors and adding a piece of quartz, which solves the serious ultraviolet light filtering problem in photoelectrochemical ultraviolet detectors and broadens the response spectrum range.

[0023] Furthermore, the precursor solution is a TiO2 solution. As a wide bandgap semiconductor material, TiO2 has a wide range of applications in the field of photoelectrochemistry. Using it as a precursor solution can form a photoanode with excellent photoelectric properties, thereby improving the sensitivity and response speed of the ultraviolet detector. By mixing different solutions, the composition and properties of the TiO2 solution can be adjusted to optimize the performance of the photoanode. This multi-component design provides more flexibility and controllability for the preparation of the TiO2 solution. Hydrochloric acid and acetic acid, as acidic components, can adjust the pH value of the solution and affect the crystallization process and morphology of TiO2. Ethanol, as a solvent, helps to dissolve other components and form a uniform solution. The combined action of these components helps to form a high-quality TiO2 film. Titanium isopropoxide is one of the precursors of TiO2, and TiO2 can be formed by hydrolysis and condensation reactions. Ethanol, as a solvent, helps to disperse and dissolve titanium isopropoxide, thereby forming a uniform TiO2 solution. The OP emulsifier helps to improve the wettability and dispersibility of the solution, making it easier for the TiO2 solution to be coated on the substrate and form a uniform film. Absolute ethanol as a solvent helps dissolve and disperse other ingredients. Ethyl cellulose and PVP as additives can improve the morphology and performance of TiO2 film and increase its photoelectric conversion efficiency.

[0024] Furthermore, the angle between the first substrate and the quartz is 20-90°; by adjusting the angle between the first substrate and the quartz, the light path can be optimized so that the ultraviolet light can be more effectively incident from the back of the quartz and pass through the electrolyte to reach the photoanode. This design helps to improve the light utilization and sensitivity of the detector. The size of the second substrate is determined by the angle between the first substrate and the quartz: the size of the second substrate is determined according to the angle between the first substrate and the quartz, which can ensure the stability and optical performance of the prism structure. This design makes the detector more compact and efficient in structure. The first substrate is FTO or ITO; FTO and ITO are both materials with good conductivity and light transmittance, and are suitable as substrates for photoelectrochemical ultraviolet detectors. The use of these materials can ensure that the detector has excellent electrode performance and optical performance. The second substrate is FTO or ITO; like the first substrate, the second substrate also uses FTO or ITO materials to maintain the consistency and stability of the detector. At the same time, this design also helps to improve the overall conductivity and light transmittance of the detector.

[0025] The present invention also discloses a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure obtained by the above-mentioned preparation method. The conventional photoelectrochemical ultraviolet detector uses FTO or ITO as a photoanode substrate. However, FTO / ITO has a serious ultraviolet filtering problem, and ultraviolet signals below 300nm cannot be detected. Quartz has a high transmittance in the ultraviolet-visible light region. The present application introduces quartz into the conventional photoelectrochemical ultraviolet detector, thereby preparing a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure to replace the conventional sandwich structure photoelectrochemical ultraviolet detector. Ultraviolet light is incident from the back of quartz, passes through the electrolyte and reaches the photoanode. The design of the triangular prism structure helps to refract and focus the light, thereby improving the utilization rate of light. At the same time, quartz has a high transmittance in the ultraviolet-visible light region, and as a part of the triangular prism, it further enhances the ultraviolet light absorption ability of the detector. The first thin film TiO2 is used as a photoanode material, responsible for absorbing ultraviolet light and generating photocurrent. Coated on the first substrate, a uniform and dense film can be formed to improve the photoelectric conversion efficiency of the detector. The second thin film platinum is used as the counter electrode material, which is responsible for collecting photocurrent and completing the circuit loop. Coating on the second substrate can ensure good contact with the electrolyte and improve the electrode performance and stability of the detector. The electrolyte is the medium of the photoelectrochemical reaction, which is responsible for transferring ions and completing the photoelectric conversion process. Filling inside the prism structure can ensure full contact with the photoanode and the counter electrode, and improve the sensitivity and response speed of the detector. A back-entry prism structure photoelectrochemical ultraviolet detector prepared by introducing quartz solves the ultraviolet filtering problem well.

[0026] The present invention also discloses the principle of the photoelectrochemical ultraviolet detector with the back-entry triangular prism structure. The ultraviolet light is incident perpendicular to the quartz, passes through the electrolyte and reaches the first film. The quartz has a high transmittance in the ultraviolet-visible light region, so that the ultraviolet light can efficiently pass through the quartz and reach the first film, ensuring the high sensitivity of the detector to ultraviolet light. The electrons on the first film first reach the conductive layer of the first substrate, and then reach the second substrate through the external circuit connecting the first substrate and the second substrate. The first film acts as a photoanode, absorbs ultraviolet light and generates photogenerated electrons. These electrons are transmitted through the conductive layer of the first substrate and reach the second substrate through the external circuit, ensuring the effective collection and transmission of photogenerated electrons and improving the photoelectric conversion efficiency of the detector. The holes on the film first pass through the electrolyte, undergo oxidation and reduction, and then reach the second substrate, and then undergo oxidation and reduction with the electrons on the second substrate. The holes generated on the first film are transmitted through the electrolyte and undergo oxidation and reduction reactions with the electrons on the second substrate, realizing the effective separation and transmission of photogenerated electrons and holes, further improving the photoelectric conversion efficiency and stability of the detector. The principle design of the back-entry triangular prism structure photoelectrochemical UV detector ensures efficient absorption of UV light, effective separation and transmission of photogenerated electrons and holes, and high efficiency of photoelectric conversion. It has excellent sensitivity and stability and is suitable for various occasions requiring UV detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A schematic diagram of the structure of a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention;

[0028] Figure 2 A schematic diagram of the principle of a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention;

[0029] Figure 3 A schematic diagram of the spectral range measured by a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention.

[0030] Among them: 1-first substrate; 2-second substrate; 3-quartz; 4-electrolyte; 5-first film; 6-second film. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0033] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0034] The present invention prepares a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure by adding a piece of quartz, and during the operation of the device, the ultraviolet light is always incident perpendicular to the quartz surface to solve the ultraviolet light filtering problem mentioned above and broaden the response spectrum.

[0035] See also Figure 1 A schematic diagram of the structure of a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention; as can be seen from the figure, a first substrate 1, a second substrate 2 and a quartz 3 are interconnected to form a triangular prism structure, the first substrate 1 has a first film 5 obtained by coating a solution and then annealing, the second substrate 2 has a second film 6 obtained by coating a solution and then annealing, the body of the triangular prism structure is filled with an electrolyte 4, which is in direct contact with the quartz 3, the first film 5 and the second film 6.

[0036] Figure 2 A schematic diagram of the principle of a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention; as can be seen from the figure, when ultraviolet light is irradiated on quartz 3, the ultraviolet light passes through quartz 3 and electrolyte 4 to reach the first film 5, and the electrons and holes on the first film 5 are divided into two paths. The electrons pass through the conductive layer on the first substrate 1 and move from the external circuit connecting the first substrate 1 and the second substrate 2 to the second substrate 2, and the holes undergo redox reaction with the ions in the electrolyte 4, and then undergo redox reaction again with the electrons that reach the second substrate 2 from the external circuit under the catalysis of the second film 6, and thus one cycle is completed.

[0037] Figure 3A schematic diagram of the spectral range measured by a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure provided in Example 1 of the present invention; as can be seen from the figure, in the test, the ultraviolet light is incident perpendicular to the quartz surface. In the traditional photoelectrochemical ultraviolet detector composed of FTO, the ultraviolet light first passes through the FTO and then reaches the photoactive layer. The response range of the device is 300-400nm. The photoelectrochemical ultraviolet detector with a back-entry triangular prism structure prepared by us directly passes through the high-transmittance quartz glass to reach the photoactive layer when detecting ultraviolet light, and the response range is about 220-400nm, thereby broadening the response range of the device.

[0038] The invention discloses a method for preparing a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, comprising: covering a half of a first substrate 1 as an electrode connected to an outer ring and the other half as a photoanode substrate, applying a precursor solution on the first substrate 1, and performing a first annealing treatment; coating chloroplatinic acid on a second substrate 2, and performing a second annealing treatment; forming a triangular prism structure with quartz 3, the first substrate 1 after annealing, and the second substrate 2 after annealing, and performing a packaging treatment; injecting an electrolyte 4 from the top of the triangular prism structure into the inside of the triangular prism structure, and sealing the top to obtain a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure.

[0039] The first substrate 1, the second substrate 2, the quartz 3, the electrolyte 4, the first film 5 arranged on the surface of the first substrate 1, and the second film 6 arranged on the surface of the second substrate 2. The first substrate 1, the second substrate 2 and the quartz 3 are connected by experimental glue or other chemicals that do not affect the performance of the device, and a prism structure is formed between the three. The first film 5 is a film formed by coating the prepared solution on the first substrate 1 and annealing, and the second film 6 is also a film formed by coating the solution on the second substrate 2 and annealing. The electrolyte 4 is filled in the body of the prism structure. When the device is working, the first substrate 1 and the second substrate 2 are connected through an external circuit.

[0040] The present invention has no special restrictions on the material of the first substrate 1, and the commonly used materials for preparing photoelectrochemical ultraviolet detectors in the art, namely FTO or ITO, are used.

[0041] Preferably, the first substrate 1 is FTO.

[0042] The present invention has no special limitation on the size of the first substrate 1 , and adopts the size of the photoelectrochemical ultraviolet detector substrate well known to ordinary researchers in the field.

[0043] Preferably, the first substrate 1 has a size of 1 cm×0.3 cm.

[0044] The present invention has no special limitation on the second substrate 2, and the second substrate 2 may be made of FTO or ITO, which are commonly used materials for preparing photoelectrochemical ultraviolet detectors in the art.

[0045] Preferably, the second substrate 2 is FTO.

[0046] In the present invention, the size of the second substrate 2 is determined by the angle between the first substrate 1 and the quartz 3. The second substrate 2 is a rectangle with the same length and thickness as the first substrate 1, and the plan view is a rectangle or a square (a rectangle is used as an example below). The length of the rectangle is the same as the length of the first substrate 1, and the width will change with the angle. Figure 2 It can be seen that the cross section is a triangle, one side of the triangle is the width at this point, and when the angle is constant and the other two sides (i.e. the size of the first substrate 1 and the quartz 3) are constant, the length of the other side (i.e. the required width) can be calculated from the relationship between the sides and angles of the triangle.

[0047] In the present invention, the size of the quartz 3 is preferably 14 mm×7 mm.

[0048] In the present invention, the quartz 3 and the first substrate 1 are sealed with a sealant, and the angle between the quartz 3 and the first substrate 1 can be between 20° and 90°, including 20° and 90°.

[0049] Preferably, the angle between the quartz 3 and the first substrate 1 is 60°.

[0050] Quartz 3 has high light transmittance in the ultraviolet-visible region, with a transmittance of 80%-95%.

[0051] In the present invention, the electrolyte 4 is deionized water or a NaOH solution.

[0052] Preferably, the electrolyte 4 is a NaOH solution.

[0053] In the present invention, the depth (thickness) of the electrolyte 4 is 50 micrometers to 1 centimeter.

[0054] Preferably, the volume of the electrolyte 4 is 0.078 cubic centimeters.

[0055] In the present invention, the first film 5 disposed on the surface of the first substrate 1 is preferably coated with a TiO2 solution by spin coating, with an annealing temperature of 300-550° C. and an annealing time of 60-120 min.

[0056] Preferably, the annealing temperature is 550° C. and the annealing time is 60 min.

[0057] In the present invention, the second film 6 disposed on the surface of the second substrate 2 is preferably coated with chloroplatinic acid on the second substrate 2 by spin coating, with an annealing temperature of 200-400° C. and an annealing time of 60-90 min.

[0058] Preferably, the annealing temperature of the second film 6 is 400° C., and the annealing time is 60 min.

[0059] The precursor solution is a TiO2 solution, which is mixed by a mixture A, a mixture B and a mixture C; the mixture A includes hydrochloric acid, acetic acid and the first ethanol; the mixture B includes titanium isopropanol and the second ethanol; the mixture C includes an OP emulsifier, a third ethanol, ethyl cellulose and PVP. The dosage ratio of hydrochloric acid: acetic acid: the first ethanol: titanium isopropanol: the second ethanol: OP emulsifier: the third ethanol: ethyl cellulose: PVP is (1-3) mL: (5-10) mL: (5-10) mL: (5-10) mL: (10-20) mL: (1-5) mL: (8-15) mL: (0.2-0.7) g: (0.3-0.8) g.

[0060] The present invention discloses a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, which is composed of three parts: a first substrate 1, a second substrate 2 and a quartz 3. Other structures include a first film 5 on the surface of the first substrate 1, a second film 6 on the surface of the second substrate 2, and an electrolyte 4 in the space between the first substrate 1, the second substrate 2 and the quartz 3.

[0061] The present invention proposes a back-entry type photoelectrochemical ultraviolet detector with a triangular prism structure, and its back-entry type and device principle are specifically as follows:

[0062] The ultraviolet light is incident perpendicular to the quartz surface; the ultraviolet light passes through the electrolyte 4 and reaches the first film 5; the electrons on the first film 5 first reach the conductive layer of the first substrate 1, and then reach the second substrate 2 through the external circuit connecting the first substrate 1 and the second substrate 2; the holes on the first film 5 first pass through the electrolyte, undergo oxidation and reduction, and then reach the second substrate 2, and then undergo oxidation and reduction with the electrons on the second substrate 2.

[0063] Example 1

[0064] A photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, the specific preparation steps of which are:

[0065] A first substrate 1 and a first film 5 on the surface thereof are prepared.

[0066] FTO was selected as the first substrate 1, and half of the cleaned and dried FTO conductive surface was covered with tape as an electrode connected to the outer ring, and the other half was used as a photoanode substrate.

[0067] Prepare TiO2 solution.

[0068] The TiO2 solution consists of three parts of mixed liquids with magnetic stirring. The first part of mixed liquid A includes: 1 mL of hydrochloric acid, 5 mL of acetic acid and 5 mL of ethanol; the second part of mixed liquid B includes: 5 mL of titanium isopropanol and 10 mL of ethanol; the third part of mixed liquid C includes: 1 mL of OP emulsifier and 8 mL of absolute ethanol, 0.2 g of ethyl cellulose and 0.3 g of PVP.

[0069] Mixed solution A was magnetically stirred for 5 minutes, mixed solution B was magnetically stirred for 5 minutes, and mixed solution C was magnetically stirred for 15 minutes. Then, mixed solution A, mixed solution B and mixed solution C were mixed and magnetically stirred for 15 minutes.

[0070] The prepared precursor solution TiO2 solution was spin-coated on the FTO surface and annealed at 550°C in a muffle furnace for 60 min.

[0071] A second substrate 2 and a second film 6 on the surface thereof are prepared.

[0072] FTO is selected as the second substrate 2, and the second substrate 2 is cleaned and dried.

[0073] Chloroplatinic acid is coated on the second substrate 2 by spin coating, and annealed in a muffle furnace at 400° C. for 60 minutes.

[0074] The quartz 3 is cleaned and dried.

[0075] Packaged devices.

[0076] The first substrate 1 and the quartz 3 are sealed at an angle of 60° using a sealant.

[0077] The second substrate 2 is sealed with a sealant. The first substrate 1, the second substrate 2 and the quartz 3 form a triangular prism structure.

[0078] Seal the bottom of the prism structure with sealant.

[0079] After the bottom sealant was completely air-dried, the electrolyte NaOH solution was injected from the top of the prism structure with a syringe to a thickness of 50 μm.

[0080] The top of the prism structure is sealed with a sealant to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure.

[0081] Example 2

[0082] A photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, the specific preparation steps of which are:

[0083] A first substrate 1 and a first film 5 on the surface thereof are prepared.

[0084] FTO was selected as the first substrate 1, and half of the cleaned and dried FTO conductive surface was covered with tape as an electrode connected to the outer ring, and the other half was used as a photoanode substrate.

[0085] Prepare TiO2 solution.

[0086] The TiO2 solution consists of three parts of mixed liquids with magnetic stirring. The first part of mixed liquid A includes: 1.5mL of hydrochloric acid, 7mL of acetic acid and 7mL of ethanol; the second part of mixed liquid B includes: 7mL of titanium isopropanol and 12mL of ethanol; the third part of mixed liquid C includes: 3mL of OP emulsifier and 10mL of absolute ethanol, 0.4g of ethyl cellulose and 0.5g of PVP.

[0087] Mixed solution A was magnetically stirred for 10 min, mixed solution B was magnetically stirred for 10 min, and mixed solution C was magnetically stirred for 30 min. Mixed solutions A, B, and C were then mixed and magnetically stirred for 30 min.

[0088] The prepared precursor solution TiO2 solution was spin-coated on the FTO surface and annealed at 500°C in a muffle furnace for 80 min.

[0089] A second substrate 2 and a second film 6 on the surface thereof are prepared.

[0090] FTO is selected as the second substrate 2, and the second substrate 2 is cleaned and dried.

[0091] Chloroplatinic acid is coated on the second substrate 2 by spin coating, and annealed in a muffle furnace at 350° C. for 70 minutes.

[0092] The quartz 3 is cleaned and dried.

[0093] Packaged devices.

[0094] The first substrate 1 and the quartz 3 are sealed at an angle of 20° using a sealant.

[0095] The second substrate 2 is sealed with a sealant. The first substrate 1, the second substrate 2 and the quartz 3 form a triangular prism structure.

[0096] Seal the bottom of the prism structure with sealant.

[0097] After the bottom sealant is completely air-dried, the electrolyte NaOH solution is injected from the top of the prism structure with a syringe to a thickness of 1 mm.

[0098] The top of the prism structure is sealed with a sealant to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure.

[0099] Example 3

[0100] A photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, the specific preparation steps of which are:

[0101] A first substrate 1 and a first film 5 on the surface thereof are prepared.

[0102] ITO was selected as the first substrate 1, and half of the cleaned and dried ITO conductive surface was covered with tape as an electrode connected to the outer ring, and the other half was used as a photoanode substrate.

[0103] Prepare TiO2 solution.

[0104] The TiO2 solution consists of three parts of mixed liquids with magnetic stirring. The first part of mixed liquid A includes: 2mL of hydrochloric acid, 9mL of acetic acid and 9mL of ethanol; the second part of mixed liquid B includes: 9mL of titanium isopropanol and 15mL of ethanol; the third part of mixed liquid C includes: 4mL of OP emulsifier and 12mL of absolute ethanol, 0.6g of ethyl cellulose and 0.7g of PVP.

[0105] Mixed solution A was magnetically stirred for 15 min, mixed solution B was magnetically stirred for 15 min, and mixed solution C was magnetically stirred for 45 min. Mixed solutions A, B, and C were then mixed and magnetically stirred for 45 min.

[0106] The prepared precursor solution TiO2 solution was spin-coated on the FTO surface and annealed at 400°C in a muffle furnace for 100 min.

[0107] A second substrate 2 and a second film 6 on the surface thereof are prepared.

[0108] ITO was selected as the second substrate 2, and the second substrate 2 was cleaned and dried.

[0109] Chloroplatinic acid is coated on the second substrate 2 by spin coating, and annealed in a muffle furnace at 300° C. for 80 minutes.

[0110] The quartz 3 is cleaned and dried.

[0111] Packaged devices.

[0112] The first substrate 1 and the quartz 3 are sealed at an angle of 70° using a sealant.

[0113] The second substrate 2 is sealed with a sealant. The first substrate 1, the second substrate 2 and the quartz 3 form a triangular prism structure.

[0114] Seal the bottom of the prism structure with sealant.

[0115] After the bottom sealant is completely air-dried, electrolyte deionized water is injected from the top of the prism structure with a syringe to a thickness of 5 mm.

[0116] The top of the prism structure is sealed with a sealant to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure.

[0117] Example 4

[0118] A photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, the specific preparation steps of which are:

[0119] A first substrate 1 and a first film 5 on the surface thereof are prepared.

[0120] ITO was selected as the first substrate 1, and half of the cleaned and dried ITO conductive surface was covered with tape as an electrode connected to the outer ring, and the other half was used as a photoanode substrate.

[0121] Prepare TiO2 solution.

[0122] The TiO2 solution consists of three parts of mixed liquids with magnetic stirring. The first part of mixed liquid A includes: 3mL of hydrochloric acid, 10mL of acetic acid and 10mL of ethanol; the second part of mixed liquid B includes: 10mL of titanium isopropanol and 20mL of ethanol; the third part of mixed liquid C includes: 5mL of OP emulsifier and 15mL of absolute ethanol, 0.7g of ethyl cellulose and 0.8g of PVP.

[0123] Mixed solution A was magnetically stirred for 20 min, mixed solution B was magnetically stirred for 20 min, and mixed solution C was magnetically stirred for 60 min. Mixed solutions A, B, and C were then mixed and magnetically stirred for 60 min.

[0124] The prepared precursor solution TiO2 solution was spin-coated on the FTO surface and annealed at 300°C in a muffle furnace for 120 min.

[0125] A second substrate 2 and a second film 6 on the surface thereof are prepared.

[0126] ITO was selected as the second substrate 2, and the second substrate 2 was cleaned and dried.

[0127] Chloroplatinic acid is coated on the second substrate 2 by spin coating, and annealed at 200° C. for 90 minutes in a muffle furnace.

[0128] The quartz 3 is cleaned and dried.

[0129] Packaged devices.

[0130] The first substrate 1 and the quartz 3 are sealed at an angle of 60° using a sealant.

[0131] The second substrate 2 is sealed with a sealant. The first substrate 1, the second substrate 2 and the quartz 3 form a triangular prism structure.

[0132] Seal the bottom of the prism structure with sealant.

[0133] After the bottom sealant was completely air-dried, electrolyte deionized water was injected from the top of the prism structure with a syringe to a thickness of 1 cm.

[0134] The top of the prism structure is sealed with a sealant to obtain a photoelectrochemical ultraviolet detector with a back-entry prism structure.

[0135] Traditional photoelectrochemical UV detectors use FTO or ITO as photoanode substrates. However, FTO / ITO has serious UV filtering problems, and UV signals below 300nm cannot be detected. Quartz has high transmittance in the UV-visible light region. The present application introduces quartz into traditional photoelectrochemical UV detectors, thereby preparing a back-entry triangular prism structure photoelectrochemical UV detector to replace the traditional sandwich structure photoelectrochemical UV detector. Ultraviolet light is incident from the back of quartz, passes through the electrolyte and reaches the photoanode. The photoelectrochemical UV detector with a back-entry triangular prism structure prepared by introducing quartz in the present application solves the UV filtering problem well.

[0136] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, characterized in that: The following steps are involved: Covering half of the first substrate (1) as an electrode connected to the outer ring and the other half as a photoanode substrate, applying a precursor solution on the first substrate (1), and performing a first annealing treatment; coating chloroplatinic acid on the second substrate (2) and performing a second annealing treatment; Quartz (3), a first substrate (1) after annealing, and a second substrate (2) after annealing are formed into a triangular prism structure, and packaging is performed; After injecting electrolyte (4) into the interior of the triangular prism structure from the top of the triangular prism structure, the top is sealed to obtain a photoelectrochemical ultraviolet detector with a back-entry triangular prism structure.

2. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: The precursor solution is coated on the first substrate (1) by spin coating; the annealing temperature of the first annealing treatment is 300-550° C., and the annealing time is 60-120 minutes.

3. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: The precursor solution is a TiO2 solution; The TiO2 solution is formed by mixing a mixed solution A, a mixed solution B and a mixed solution C; The mixed solution A includes hydrochloric acid, acetic acid and the first portion of ethanol; the mixed solution B includes titanium isopropanol and the second portion of ethanol; and the mixed solution C includes OP emulsifier, the third portion of ethanol, ethyl cellulose and PVP.

4. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 3, characterized in that: The amount ratio of hydrochloric acid: acetic acid: first part ethanol: titanium isopropanol: second part ethanol: OP emulsifier: third part ethanol: ethyl cellulose: PVP is (1-3) mL: (5-10) mL: (5-10) mL: (5-10) mL: (10-20) mL: (1-5) mL: (8-15) mL: (0.2-0.7) g: (0.3-0.8) g; when preparing the TiO2 solution, first stir the mixed solution A for 5-20 min; stir the mixed solution B for 5-20 min; Mixture C is stirred for 15-60 minutes; Then, the mixed solution A, the mixed solution B and the mixed solution C are mixed and stirred for 15-60 minutes.

5. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: Chloroplatinic acid is coated on the second substrate (2) by spin coating; the annealing temperature of the second annealing treatment is 200-400° C., and the annealing time is 60-90 minutes.

6. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: The angle between the first substrate (1) and the quartz (3) is 20-90°, and the size of the second substrate (2) is determined by the angle between the first substrate (1) and the quartz (3); the first substrate (1) is FTO or ITO; and the second substrate (2) is FTO or ITO.

7. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: The light transmittance of the quartz (3) in the visible region is 80%-95%.

8. The method for preparing the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure according to claim 1, characterized in that: The electrolyte (4) is deionized water or a NaOH solution; the thickness of the electrolyte (4) is 50 μm-1 cm.

9. A photoelectrochemical ultraviolet detector with a back-entry triangular prism structure, characterized in that: The method according to any one of claims 1 to 8 is used to prepare the prism structure, comprising: a first substrate (1), a second substrate (2) and a quartz (3) structure, wherein the first substrate (1) is coated with a first film (5); the second substrate (2) is coated with a second film (6); and the interior of the prism structure is filled with an electrolyte (4).

10. The principle of the photoelectrochemical ultraviolet detector with a back-entry triangular prism structure as claimed in claim 9 is characterized in that: include: Ultraviolet light is incident perpendicularly to the quartz (3), passes through the electrolyte (4) and reaches the first film (5); the electrons on the first film (5) first reach the conductive layer of the first substrate (1), and then reach the second substrate (2) through an external circuit connecting the first substrate (1) and the second substrate (2); the holes on the first film (5) first pass through the electrolyte (4), undergo oxidation and reduction, and then reach the second substrate (2), and then undergo oxidation and reduction with the electrons on the second substrate (2).