Gradient doped hollow cobalt oxide material and preparation method and application thereof
By introducing gradient-doped hollow cobalt oxide material into the positive electrode material of lithium-ion battery, the hollow core is used to relieve stress and improve the lithium-ion storage capacity through the surface gradient doping metal elements, the lithium-ion battery material is solved due to volume during charging and discharging. The stability problems caused by changes have significantly improved the battery's circulation performance and capacity.
Patent Information
- Application Number
- CN202411148928.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The existing lithium-ion battery positive electrode materials generate uneven residual stress due to volume changes during charging and discharging, resulting in rapid attenuation of the material. The existing doping methods cannot effectively improve the cyclic stability of the material.
The gradient-doped hollow cobalt oxide material is used to alleviate stress and improve the storage capacity of lithium ions and improve the structural stability of the material by setting a pore-shaped hollow core inside the material and distributing the surface gradient inside the material.
Effectively reduce internal stress of the material, improve battery circulation performance and capacity, and extend battery life.
Smart Images

Figure CN119050341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a gradient-doped hollow cobalt oxide material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have now become the most important electrochemical energy storage system. With the explosive growth of electronic products and the wider use of lithium-ion batteries, the demand for cathode materials with higher energy density, longer life and higher safety is also increasing. As the earliest commercialized and most successfully applied cathode material for lithium-ion batteries, the cathode material LiCoO2 (lithium cobalt oxide) has attracted widespread attention due to its extremely high volume energy density, good conductivity, and abundant resources. However, batteries for electronic products often require higher voltages. Increasing the upper limit of the charging voltage (excessive delithiation) will bring a series of problems, such as material phase change, interface side reactions, cobalt metal dissolution and oxygen evolution, which will lead to rapid attenuation of material performance, especially cycle performance.
[0003] In the prior art, it is usually preferred to introduce heterogeneous metal atoms into the lithium cobalt oxide lattice through element doping, such as Al, Ti, Zr, Mo, Ni, etc., so as to enhance the stability of the material during the electrochemical cycle. At the same time, elements such as Ni can also increase the lithium storage capacity of the battery. However, in the prior art, doping is usually achieved by calcining mixed materials, and the distribution of doped elements is random, which has limited effect on the improvement of the electrochemical and mechanical properties of the material. A more effective doping method is urgently needed.
[0004] Therefore, during the battery charging and discharging process, as the positive electrode material particles continuously undergo lithium insertion and extraction, the material will continuously shrink and expand. This reciprocating volume change will generate a large amount of uneven residual stress inside the material, causing cracks inside the particles. Therefore, it is necessary to provide a gradient-doped hollow cobalt oxide material that can alleviate the internal stress of the positive electrode material and improve the battery cycle stability. Summary of the invention
[0005] The purpose of the present invention is to provide a gradient-doped hollow cobalt oxide material and a preparation method and application thereof. The core of the gradient-doped hollow cobalt oxide material is a hollow structure, which can serve as a buffer for material deformation and reduce the generation of internal stress. The outer layer on the surface of the hollow core is gradiently doped with metal elements, which can not only provide lithium ion storage, but also improve the material structure stability and ensure cycle stability.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a gradient-doped hollow cobalt oxide material, wherein the gradient-doped hollow cobalt oxide material comprises a hollow core and an outer layer on the surface of the hollow core, wherein the outer layer comprises a cobalt oxide material;
[0008] The outer layer is gradiently distributed with doped metal elements, and the content of the doped metal elements decreases gradually from a side close to the hollow core to a side far from the hollow core.
[0009] The gradient-doped hollow cobalt oxide material of the present invention has a porous hollow core, which can relieve the stress generated by the material and avoid the problem of cracks inside the particles caused by a large amount of uneven residual stress generated inside the positive electrode material due to volume changes during the charging and discharging process. In addition, the outer layer of the surface of the hollow core of the present invention is gradiently distributed with doped metal elements, and the content of the doped metal elements gradually decreases from the inside to the outside (i.e., from the core to the outer layer away from the core). Therefore, the content of doped metal elements inside the outer layer of the present invention is relatively high, which can provide more lithium ion storage, and the content of doped metal elements gradually decreases outwards, realizing low-concentration doping, which can improve the structural stability of the material, thereby further improving the cycle performance of the material.
[0010] Preferably, the volume of the hollow core accounts for 1-10% of the total volume of the gradient-doped hollow cobalt oxide material, for example, it can be 1%, 3%, 5%, 7%, 9% or 10%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0011] The proportion of the hollow core described in the present invention will affect the stress relief effect. If the proportion of the hollow core is too small, the stress relief effect will decrease. If the proportion of the hollow core is too large, the material tap density will be low, resulting in a low battery capacity.
[0012] Preferably, the doping metal element includes any one of nickel, aluminum, magnesium, niobium or titanium, or a combination of at least two of them.
[0013] When the doped metal element described in the present invention is nickel, the capacity of the material can be increased while improving the structural stability of the material. If aluminum is doped, the voltage and lithium ion transmission efficiency of the material can be increased. Therefore, the present invention can select different doped metal elements according to different needs.
[0014] Preferably, in the gradient-doped hollow cobalt oxide material, the content of the doped metal element is 0.5-10wt%, for example, 0.5wt%, 5wt% or 10wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] In a second aspect, the present invention provides a method for preparing the gradient-doped hollow cobalt oxide material as described in the first aspect, the preparation method comprising the following steps:
[0016] (1) subjecting a doping metal source, a first precipitant solution and a complexing agent solution to a first coprecipitation reaction to obtain a doping seed crystal;
[0017] (2) subjecting the doped seed crystals, the cobalt source solution and the second precipitant solution of step (1) to a second coprecipitation reaction to obtain a precursor coated with the doped seed crystals;
[0018] (3) Calcining the precursor of the coated doped seed crystal in step (2) to obtain the gradient-doped hollow cobalt oxide material.
[0019] The present invention first prepares particles containing only doped metal elements through a first coprecipitation reaction. For example, when the doped metal element is nickel, nickel hydroxide particles are first prepared, and a second coprecipitation reaction is performed on the nickel hydroxide particles as the core to grow a coated cobalt precursor, such as preparing nickel core cobalt carbonate particles. Finally, after calcination, the doped seed crystals are decomposed to form a hollow core, and the doped metal elements diffuse into the outer layer to form a gradient structure, which not only forms a gradient-doped hollow cobalt oxide material, but also makes the material more compact and has a higher tap density.
[0020] Preferably, the calcination in step (3) comprises first calcining at 300-400°C, for example, 300°C, 350°C or 400°C, and then heating to 600-800°C for secondary calcination, for example, 600°C, 700°C or 800°C, but is not limited to the listed values, and other values within the numerical range not listed are also applicable.
[0021] The calcination of the present invention goes through two stages, wherein in the first stage of calcination, the inner core shrinks and decomposes to stabilize the material structure, and the elements begin to migrate outward; in the second stage of calcination, the outer layer of cobalt precursor such as cobalt carbonate coated on the surface of the inner core decomposes into cobalt oxide, and at the same time, the doped metal elements completely migrate into the cobalt oxide to obtain a gradient-doped hollow cobalt oxide material.
[0022] If the present invention only performs one calcination at a low temperature, the diffusion of the doped metal elements and the formation of the cobalt oxide material will be affected; if the present invention does not perform the first stage of low-temperature calcination and directly performs the second stage of high-temperature calcination, the material will shrink rapidly at high temperature, causing the core and the shell to peel off, hindering the diffusion of the doped elements and destroying the material structure.
[0023] Preferably, the time of the primary calcination is 1-3 hours, for example, 1 hour, 2 hours or 3 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] Preferably, the secondary calcination time is 5-10 h, for example, 5 h, 7 h, 9 h or 10 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the second precipitant solution in step (2) comprises an ammonium carbonate precipitant.
[0026] Preferably, the ammonium carbonate precipitant includes ammonium bicarbonate and / or ammonium carbonate.
[0027] Preferably, the pH of the second coprecipitation reaction in step (2) is 7.0-8.5, for example, 7.0, 7.5, 8.0 or 8.5, and the stirring rate is 100-200 r / min, for example, 100 r / min, 150 r / min or 200 r / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, in step (2), the second coprecipitation reaction is stopped after the product particle size D50 is 5-20 μm, for example, it can be 5 μm, 10 μm, 15 μm or 20 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the particle size D50 of the doped seed in step (1) is 0.5-5 μm, for example, 0.5 μm, 1 μm, 2 μm or 5 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] The particle size of the kernel doped seed of the present invention will affect the volume proportion of the formed hollow core. If the particle size D50 of the doped seed is too small, the volume proportion of the formed hollow core will be too small. If the particle size D50 of the doped seed is too large, the volume proportion of the formed hollow core will be too large.
[0031] Preferably, the temperature of the first coprecipitation reaction in step (1) is 50-60°C, for example, 50°C, 55°C or 60°C, and the time is 1-5h, for example, 1h, 2h, 3h, 4h or 5h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the step (1) of subjecting the doping metal source, the first precipitant solution and the complexing agent solution to a first coprecipitation reaction comprises the following steps:
[0033] The first precipitant solution and the complexing agent solution are mixed to obtain a base solution, and the doping metal source solution is introduced into the base solution to perform a first coprecipitation reaction.
[0034] Preferably, the first precipitant solution in step (1) comprises a metal hydroxide.
[0035] Preferably, the metal hydroxide comprises sodium hydroxide and / or potassium hydroxide.
[0036] Preferably, the complexing agent solution in step (1) comprises aqueous ammonia.
[0037] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:
[0038] (1) mixing a hydroxide solution and aqueous ammonia to obtain a first base solution, introducing a doping metal source into the first base solution, performing a first coprecipitation reaction at 50-60° C. for 1-5 h, and then washing, filtering and drying to obtain a doping seed crystal with a D50 of 0.5-5 μm, wherein the doping seed crystal includes a hydroxide containing a doping metal element;
[0039] (2) using an ammonium carbonate precipitant solution as a second base liquid, adding the doped seed crystals described in step (1) into the second base liquid, then passing a cobalt source solution and an ammonium carbonate precipitant solution into the second base liquid, performing a second coprecipitation reaction at a pH of 7.0-8.5 and a stirring rate of 100-200 r / min, and stopping the reaction when the product particle size D50 is 5-20 μm, then separating the slurry obtained by the second coprecipitation reaction into solid and liquid, washing, and drying at 60-80° C. to obtain a precursor coated with the doped seed crystals;
[0040] (3) The precursor of the coated doped seed crystal in step (2) is calcined at 300-400° C. for 1-3 h, and then heated to 600-800° C. for a second calcination for 5-10 h to obtain the gradient-doped hollow cobalt oxide material.
[0041] In a third aspect, the present invention provides a lithium cobalt oxide positive electrode material, which is obtained by mixing and sintering a lithium source and the gradient-doped hollow cobalt oxide material as described in the first aspect.
[0042] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium cobalt oxide positive electrode material as described in the third aspect.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] The present invention provides an internal buffer space for the expansion and contraction of the material by arranging a porous hollow core inside the material, thereby reducing the breakage and pulverization and peeling of the positive electrode material caused by the volume change outside the material. In addition, the present invention uses element gradient doping, internal high-concentration doping can significantly increase the material capacity, and external low-concentration doping can introduce heterogeneous metal atoms into the lattice, which can enhance the structural stability of the material during the electrochemical cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a cross-sectional view of the gradient-doped hollow cobalt oxide material described in Example 1 of the present invention;
[0046] Figure 2a This is a cross-sectional view of a nickel content line scan of the gradient-doped hollow cobalt oxide material described in Example 1 of the present invention, Figure 2b This is a line scan result of the cross-sectional nickel content of the gradient-doped hollow cobalt oxide material described in Example 1 of the present invention. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Example 1
[0049] This embodiment provides a gradient-doped hollow cobalt oxide material, the gradient-doped hollow cobalt oxide material comprising a hollow core and an outer layer on the surface of the hollow core, the outer layer comprising a cobalt oxide material; nickel elements are gradiently distributed in the outer layer, and the content of the nickel decreases gradually from a side close to the hollow core to a side away from the hollow core;
[0050] The volume of the hollow core accounts for about 5% of the total volume of the gradient-doped hollow cobalt oxide material;
[0051] The content of nickel in the gradient-doped hollow cobalt oxide material is 5wt%;
[0052] The preparation method of the gradient-doped hollow cobalt oxide material comprises the following steps:
[0053] (1) adding sodium hydroxide solution and ammonia water as a first bottom liquid into a reaction kettle, passing 1 mol / L nickel sulfate solution into the first bottom liquid, performing a first coprecipitation reaction at 55° C. for 3 h, and then washing, filtering and drying to obtain nickel hydroxide particles with a D50 of 3 μm;
[0054] (2) using 20 g / L ammonium bicarbonate solution as a second base liquid, adding the nickel hydroxide particles described in step (1) into the second base liquid, then passing 80 g / L cobalt salt solution and 20 g / L ammonium bicarbonate solution into the second base liquid, performing a second coprecipitation reaction at a pH of 8 and a stirring rate of 150 r / min, and stopping the reaction when the particle size D50 of the product particle is 15 μm, and then performing solid-liquid separation, washing and drying the slurry obtained by the second coprecipitation reaction at 70° C. to obtain cobalt carbonate coated with nickel cores;
[0055] (3) The cobalt carbonate coated with the nickel core in step (2) is heated to 350° C. at a heating rate of 10° C. / min, and calcined for 2 h. Then, the temperature is increased to 700° C. at a heating rate of 5° C. / min and calcined for 8 h. To obtain the gradient-doped hollow cobalt oxide material, the cross-sectional view of the gradient-doped hollow cobalt oxide material is as shown in FIG. Figure 1 As shown by Figure 1 It can be seen that the material obtained by the present invention contains a porous hollow core; the cross-sectional nickel content line scan of the gradient-doped hollow cobalt oxide material is as follows: Figure 2a The line scan results are shown as Figure 2b As shown by Figure 2a and Figure 2b It can be seen that in the gradient-doped hollow cobalt oxide material of the present invention, the nickel content gradually decreases from the inside to the outside.
[0056] Example 2
[0057] This embodiment provides a gradient-doped hollow cobalt oxide material, the gradient-doped hollow cobalt oxide material comprising a hollow core and an outer layer on the surface of the hollow core, the outer layer comprising a cobalt oxide material; nickel elements are gradiently distributed in the outer layer, and the content of the nickel decreases gradually from a side close to the hollow core to a side away from the hollow core;
[0058] The volume of the hollow core accounts for about 1% of the total volume of the gradient-doped hollow cobalt oxide material;
[0059] The content of nickel in the gradient-doped hollow cobalt oxide material is 0.5wt%;
[0060] The preparation method of the gradient-doped hollow cobalt oxide material comprises the following steps:
[0061] (1) adding sodium hydroxide solution and ammonia water as a first bottom liquid into a reaction kettle, passing a 1 mol / L nickel sulfate solution into the first bottom liquid, performing a first coprecipitation reaction at 50° C. for 1 h, and then washing, filtering and drying to obtain nickel hydroxide particles with a D50 of 0.5 μm;
[0062] (2) using 20 g / L ammonium bicarbonate solution as a second base liquid, adding the nickel hydroxide particles described in step (1) into the second base liquid, then passing 80 g / L cobalt salt solution and 20 g / L ammonium bicarbonate solution into the second base liquid, performing a second coprecipitation reaction at a pH of 7.0 and a stirring rate of 100 r / min, and stopping the reaction when the particle size D50 of the product particles reaches 5 μm, and then separating the slurry obtained by the second coprecipitation reaction into solid and liquid, washing and drying at 80° C. to obtain cobalt carbonate coating the nickel core;
[0063] (3) The cobalt carbonate coated with the nickel core in step (2) is heated to 300° C. at a heating rate of 10° C. / min, calcined for 1 hour, and then heated to 600° C. at a heating rate of 5° C. / min for a second calcination for 5 hours to obtain the gradient-doped hollow cobalt oxide material.
[0064] Example 3
[0065] This embodiment provides a gradient-doped hollow cobalt oxide material, the gradient-doped hollow cobalt oxide material comprising a hollow core and an outer layer on the surface of the hollow core, the outer layer comprising a cobalt oxide material; nickel elements are gradiently distributed in the outer layer, and the content of the nickel decreases gradually from a side close to the hollow core to a side away from the hollow core;
[0066] The volume of the hollow core accounts for about 10% of the total volume of the gradient-doped hollow cobalt oxide material;
[0067] The content of nickel in the gradient-doped hollow cobalt oxide material is 10wt%;
[0068] The preparation method of the gradient-doped hollow cobalt oxide material comprises the following steps:
[0069] (1) adding sodium hydroxide solution and ammonia water as a first bottom liquid into a reaction kettle, passing 1 mol / L nickel sulfate solution into the first bottom liquid, performing a first coprecipitation reaction at 60° C. for 5 h, and then washing, filtering and drying to obtain nickel hydroxide particles with a D50 of 5 μm;
[0070] (2) using 20 g / L ammonium bicarbonate solution as a second base liquid, adding the nickel hydroxide particles described in step (1) into the second base liquid, then passing 80 g / L cobalt salt solution and 20 g / L ammonium bicarbonate solution into the second base liquid, performing a second coprecipitation reaction at a pH of 8.5 and a stirring rate of 200 r / min, and stopping the reaction when the particle size D50 of the product particle is 20 μm, and then separating the slurry obtained by the second coprecipitation reaction into solid and liquid, washing and drying at 80° C. to obtain cobalt carbonate coated with nickel cores;
[0071] (3) The cobalt carbonate coated with the nickel core in step (2) is heated to 400° C. at a heating rate of 10° C. / min, calcined for 3 h, and then heated to 800° C. at a heating rate of 5° C. / min for a second calcination for 10 h to obtain the gradient-doped hollow cobalt oxide material.
[0072] Example 4
[0073] The present embodiment provides a gradient-doped hollow cobalt oxide material. The gradient-doped hollow cobalt oxide material is the same as that in Embodiment 1 except that in the preparation method thereof, the particle size D50 of the nickel hydroxide particles in step (1) is 0.2 μm, so that the obtained gradient-doped hollow cobalt oxide material is adaptively changed.
[0074] Example 5
[0075] The present embodiment provides a gradient-doped hollow cobalt oxide material. The gradient-doped hollow cobalt oxide material is the same as that in Embodiment 1 except that in the preparation method thereof, the particle size D50 of the nickel hydroxide particles in step (1) is 6 μm, so that the obtained gradient-doped hollow cobalt oxide material can be adaptively changed.
[0076] Example 6
[0077] The present embodiment provides a gradient-doped hollow cobalt oxide material. The gradient-doped hollow cobalt oxide material is the same as that in Example 1, except that in the preparation method, the cobalt carbonate coating the nickel core in step (2) is heated to 700° C. at a heating rate of 5° C. / min and calcined for 10 h to make the obtained gradient-doped hollow cobalt oxide material adaptable.
[0078] Example 7
[0079] The present embodiment provides a gradient-doped hollow cobalt oxide material. The gradient-doped hollow cobalt oxide material is the same as that in Example 1, except that in the preparation method, the cobalt carbonate coating the nickel core in step (2) is heated to 400° C. at a heating rate of 10° C. / min and calcined for 10 h to make the obtained gradient-doped hollow cobalt oxide material adaptable.
[0080] Example 8
[0081] The present embodiment provides a gradient-doped hollow cobalt oxide material. The gradient-doped hollow cobalt oxide material is the same as that of Embodiment 1 except that in the preparation method, the nickel sulfate solution in step (1) is replaced with an aluminum chloride solution in equal concentration to make the obtained gradient-doped hollow cobalt oxide material adaptable.
[0082] Comparative Example 1
[0083] This comparative example provides a cobalt oxide material, which is the same as Example 1 except that in its preparation method, step (1) is not performed and nickel hydroxide particles are not added in step (2), so that the adaptability of the obtained material changes.
[0084] Comparative Example 2
[0085] This comparative example provides a cobalt oxide material doped with nickel. The cobalt oxide material is the same as Example 1 except that in its preparation method, step (1) is not performed, and nickel hydroxide particles are not added in step (2). At the same time, 1 mol / L nickel sulfate solution, 80 g / L cobalt salt solution, and 20 g / L ammonium bicarbonate solution are introduced into the second base liquid for coprecipitation reaction, so that the adaptability of the obtained material changes.
[0086] The cobalt oxide material obtained in the above embodiments and comparative examples is mixed with lithium hydroxide and sintered to prepare a lithium cobalt oxide positive electrode material, 80wt% of the positive electrode active material, 10wt% of Super-P and 10wt% of polyvinylidene fluoride are dispersed in an N-methylpyrrolidone solution to prepare an electrode slurry, which is coated on an aluminum foil and dried to obtain a positive electrode plate; a lithium ion battery is prepared using the obtained positive electrode plate, and the preparation method of the lithium ion battery is as follows: 1mol / L LiPF6 is used as an electrolyte, a metal lithium sheet is used as a negative electrode, a polyethylene diaphragm, and the above positive electrode plate is used as a positive electrode, and a CR2032 button battery is assembled. The button battery is tested for charge and discharge at 25°C, a voltage range of 2.75-4.6V, a charge and discharge current density of 1C, and 100 cycles.
[0087] The test results are shown in Table 1:
[0088] Table 1
[0089]
[0090]
[0091] From Table 1 we can see that:
[0092] It can be seen from Example 1 and Comparative Examples 1-2 that the present invention provides an internal buffer space for the expansion and contraction of the material by arranging a porous hollow core inside the material, and can improve the capacity and cycle performance of the battery through gradient doping; It can be seen from Example 1 and Examples 4-5 that the present invention can control the proportion of the hollow core inside the cobalt oxide material by controlling the particle size of the doped seed crystal, thereby further ensuring the cycle performance of the battery; It can be seen from Example 1 and Examples 6-7 that the present invention can ensure the formation of the hollow core through two-stage calcination, and can achieve a gradient distribution of doped metal elements; It can be seen from Example 1 and Example 8 that the present invention can selectively dope different types of metal elements.
[0093] In summary, the present invention provides a gradient-doped hollow cobalt oxide material and a preparation method and application thereof. The core of the gradient-doped hollow cobalt oxide material is a hollow structure, which can serve as a buffer for material deformation and reduce internal stress generation. The outer layer on the core surface is gradiently doped with metal elements, which can not only provide lithium ion storage, but also improve the material structure stability and ensure cycle stability.
[0094] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A gradient-doped hollow cobalt oxide material, characterized in that: The gradient-doped hollow cobalt oxide material comprises a hollow core and an outer layer on the surface of the hollow core, wherein the outer layer comprises a cobalt oxide material; The outer layer is gradiently distributed with doped metal elements, and the content of the doped metal elements decreases gradually from a side close to the hollow core to a side far from the hollow core.
2. The gradient-doped hollow cobalt oxide material according to claim 1, characterized in that: The volume of the hollow core accounts for 1-10% of the total volume of the gradient-doped hollow cobalt oxide material; Preferably, the doped metal element comprises any one or a combination of at least two of nickel, aluminum, magnesium, niobium or titanium; Preferably, in the gradient-doped hollow cobalt oxide material, the content of the doped metal element is 0.5-10 wt %.
3. A method for preparing the gradient-doped hollow cobalt oxide material as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) subjecting a doping metal source, a first precipitant solution and a complexing agent solution to a first coprecipitation reaction to obtain a doping seed crystal; (2) subjecting the doped seed crystals, the cobalt source solution and the second precipitant solution of step (1) to a second coprecipitation reaction to obtain a precursor coated with the doped seed crystals; (3) Calcining the precursor of the coated doped seed crystal in step (2) to obtain the gradient-doped hollow cobalt oxide material.
4. The preparation method according to claim 3, characterized in that: The calcination in step (3) includes first calcining at 300-400°C and then heating to 600-800°C for secondary calcination; Preferably, the time of the first calcination is 1-3h; Preferably, the secondary calcination time is 5-10 hours.
5. The preparation method according to claim 3 or 4, characterized in that: Step (2) the second precipitant solution comprises an ammonium carbonate precipitant; Preferably, the ammonium carbonate precipitant comprises ammonium bicarbonate and / or ammonium carbonate; Preferably, the pH of the second coprecipitation reaction in step (2) is 7.0-8.5, and the stirring rate is 100-200 r / min.
6. The preparation method according to any one of claims 3 to 5, characterized in that: Step (2) the second coprecipitation reaction is continued until the particle size D50 of the product is 5-20 μm and then the reaction is stopped; Preferably, the particle size D50 of the doped seed crystal in step (1) is 0.5-5 μm; Preferably, the temperature of the first coprecipitation reaction in step (1) is 50-60° C. and the time is 1-5 h.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The step (1) of subjecting the doping metal source, the first precipitant solution and the complexing agent solution to a first coprecipitation reaction comprises the following steps: The first precipitant solution and the complexing agent solution are mixed to obtain a base solution, and the doping metal source solution is introduced into the base solution to perform a first coprecipitation reaction; Preferably, the first precipitant solution in step (1) comprises a metal hydroxide; Preferably, the complexing agent solution in step (1) comprises aqueous ammonia.
8. The preparation method according to any one of claims 3 to 7, characterized in that: The preparation method comprises the following steps: (1) mixing a metal hydroxide solution and ammonia water to obtain a first base solution, introducing a doping metal source into the first base solution, performing a first coprecipitation reaction at 50-60° C. for 1-5 hours, and then washing, filtering and drying to obtain a doping seed crystal with a D50 of 0.5-5 μm, wherein the doping seed crystal includes a hydroxide containing a doping metal element; (2) using an ammonium carbonate precipitant solution as a second base liquid, adding the doped seed crystals described in step (1) into the second base liquid, then passing a cobalt source solution and an ammonium carbonate precipitant solution into the second base liquid, performing a second coprecipitation reaction at a pH of 7.0-8.5 and a stirring rate of 100-200 r / min, and stopping the reaction when the product particle size D50 is 5-20 μm, then separating the slurry obtained by the second coprecipitation reaction into solid and liquid, washing, and drying at 60-80° C. to obtain a precursor coated with the doped seed crystals; (3) The precursor of the coated doped seed crystal in step (2) is calcined at 300-400° C. for 1-3 h, and then heated to 600-800° C. for a second calcination for 5-10 h to obtain the gradient-doped hollow cobalt oxide material.
9. A lithium cobalt oxide positive electrode material, characterized in that: The lithium cobalt oxide positive electrode material is obtained by mixing and sintering a lithium source and the gradient-doped hollow cobalt oxide material as claimed in claim 1 or 2.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium cobalt oxide positive electrode material as claimed in claim 9.