Membrane electrode with anti-reverse pole function and preparation method and application thereof

By using an ordered carbon nanotube layer to support anti-reverse catalyst and Pt catalyst in the fuel cell membrane electrode, the reverse corrosion problem caused by insufficient hydrogen in the anode catalytic layer is solved, and the reliability and safety of the membrane electrode are improved , and reduces costs.

CN119050389APending Publication Date: 2024-11-29DONGFENG MOTOR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064011.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the vehicle-mounted applications, existing fuel cells have insufficient hydrogen in the anode catalytic layer due to start-stop, rapid load change and other working conditions, causing corrosion of the reverse electrode carbon carrier, reducing the reliability and safety of the fuel cell. In the current anti-reverse electrode measures, IrO2 is present. The addition of the cost increases.

Method used

The first carbon nanotube layer and the second carbon nanotube layer arranged in an orderly manner are used to load anti-reverse catalysts and Pt catalysts in the anode and cathode catalytic layers respectively, and the amount of anti-reverse catalysts is reduced by atomic deposition method. Improve the anti-reverse performance of the membrane electrode.

Benefits of technology

At the lower anti-reverse catalyst dosage, the reliability and safety of the membrane electrode are significantly improved, the loading of Pt and Ir is reduced, the cost is reduced, and the anti-reverse performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050389A_ABST
    Figure CN119050389A_ABST
Patent Text Reader

Abstract

The invention relates to a membrane electrode with an anti-reverse pole function and a preparation method and application thereof, and belongs to the technical field of fuel cells. The membrane electrode comprises an anode catalyst layer, the anode catalyst layer comprises a first carbon nanotube layer and a first catalyst which are arranged in order, and the extension direction of carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer; the first catalyst is loaded on the first carbon nanotube layer, and the first catalyst comprises an anti-reverse-pole catalyst; by introducing the anti-antipole catalyst into the anode catalyst layer in an ordered form, the use amount of the anti-antipole catalyst can be reduced, a relatively good anti-antipole effect is achieved, and the reliability and safety of the membrane electrode are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of fuel cell technology, and in particular to a membrane electrode with anti-reverse polarity function, and a preparation method and application thereof. Background Art

[0002] As a clean and sustainable power generation device, fuel cells directly convert the chemical energy of fuel and oxidant into electrical energy through electrochemical reactions, and have the characteristics of high efficiency, no pollution and long life. Among them, proton exchange membrane fuel cells (PEMFC) are widely used due to their high energy conversion rate (40% to 60%), low operating temperature, high specific power and fast startup speed.

[0003] The core component of PEMFC is the membrane electrode (MEA), which consists of a proton exchange membrane (PEM) in the center, a catalyst layer (CL) coated thereon, and a gas diffusion layer (GDL) on the outside. The main components of the catalyst layer are Pt / C catalyst and perfluorosulfonic acid ion polymer (ionomer), and are divided into positive and negative electrodes, where the cathode is used to catalyze the oxygen reduction reaction (ORR) and the anode is used to catalyze the hydrogen oxidation reaction (HOR).

[0004] During the operation of the on-board fuel cell, the anode catalyst layer may be insufficient in hydrogen due to start-stop, rapid load changes and other operating conditions, resulting in reverse polarity. The corrosion of the carbon support of the anode catalyst layer caused by reverse polarity is irreversible, which will significantly reduce the reliability and safety of the fuel cell. At present, the main measure to resist reverse polarity at the membrane electrode level is to add an anti-reverse polarity catalyst iridium oxide (IrO2) to the catalyst layer, and promote the electrolysis of water by IrO2 to replace the carbon corrosion reaction. However, the price of Ir is more expensive than Pt, and the addition of IrO2 in the catalyst layer will significantly increase the cost of the membrane electrode. Summary of the invention

[0005] The present application provides a membrane electrode with anti-reverse polarity function and a preparation method and application thereof, which can achieve better anti-reverse polarity effect under the premise of lower anti-reverse polarity catalyst dosage.

[0006] In the first aspect, the present application provides a membrane electrode with anti-reverse polarity function, the membrane electrode includes an anode catalyst layer, the anode catalyst layer includes an ordered first carbon nanotube layer and a first catalyst, the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer; the first catalyst is loaded on the first carbon nanotube layer, and the first catalyst includes an anti-reverse polarity catalyst.

[0007] As an optional embodiment, the anti-reversal catalyst comprises Ir and / or Ir-based materials; and / or

[0008] The loading of the anti-reversal catalyst is 5 μg / cm2 ~15 μg / cm 2 .

[0009] As an optional embodiment, the anode catalyst layer further includes a second catalyst, the second catalyst is supported on the first carbon nanotube layer, and the second catalyst includes Pt and / or a Pt-based material; and / or

[0010] The loading of the second catalyst is 10 μg / cm 2 ~30 μg / cm 2 .

[0011] As an optional embodiment, the membrane electrode further includes a proton exchange membrane and a cathode catalyst layer, the proton exchange membrane is arranged between the anode catalyst layer and the cathode catalyst layer, the cathode catalyst layer includes a second carbon nanotube layer and a third catalyst arranged in an ordered manner, the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, the third catalyst is loaded on the second carbon nanotube layer, and the third catalyst includes Pt and / or a Pt-based material; and / or

[0012] The loading of the third catalyst is 40 μg / cm 2 ~60 μg / cm 2 .

[0013] In a second aspect, the present application provides a method for preparing a membrane electrode having an anti-reverse polarity function, the method comprising:

[0014] Obtaining a first carbon nanotube layer with orderly arrangement;

[0015] The first catalyst is loaded on the first carbon nanotube layer, and then an ion polymer is sprayed to obtain an anode catalyst layer; the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer, and the first catalyst includes an anti-reverse polarity catalyst;

[0016] The anode catalyst layer, the proton exchange membrane and the cathode catalyst layer are assembled to obtain a membrane electrode.

[0017] As an optional implementation manner, the first carbon nanotube layer with ordered arrangement comprises:

[0018] obtaining a substrate, the substrate comprising an aluminum foil and an iron film attached to the aluminum foil;

[0019] Etching the iron film on the substrate to form mutually isolated iron particles, and removing oxides on the surface of the iron film to obtain an intermediate plate;

[0020] A carbon source is used to deposit carbon on the middle plate to form orderly arranged carbon nanotubes to obtain a first carbon nanotube layer.

[0021] As an optional implementation manner, the thickness of the aluminum film is 5 μm to 30 μm; and / or

[0022] The thickness of the iron film is 0.5nm to 2nm; and / or

[0023] The carbon source includes a mixed gas of C2H2 and H2, and the mixing ratio of C2H2 and H2 is 1:(5-20).

[0024] As an optional embodiment, the loading the first catalyst on the first carbon nanotube layer comprises depositing an Ir-containing precursor on the first carbon nanotube layer by an atomic deposition method; and / or

[0025] The Ir-containing precursor includes at least one of chloroiridic acid, iridium acetylacetonate, iridium trichloride and iridium tetrachloride; and / or

[0026] The deposition rate of the Ir-containing precursor is and / or

[0027] The method further comprises loading a second catalyst on the first carbon nanotube, wherein the second catalyst comprises Pt and / or a Pt-based material; and / or

[0028] The loading of the second catalyst on the first carbon nanotube comprises depositing a Pt-containing precursor on the first carbon nanotube layer by an atomic deposition method; and / or

[0029] The Pt-containing precursor includes at least one of chloroplatinic acid, chloroplatinous acid, platinum acetylacetonate, bis(ethylenediamine)platinum acetate and trimethylmethylcyclopentadienylplatinum; and / or

[0030] The deposition rate of the Pt-containing precursor is

[0031] As an optional embodiment, the method for preparing the cathode catalyst layer includes:

[0032] Obtaining a second carbon nanotube layer with orderly arrangement;

[0033] The third catalyst is loaded on the second carbon nanotube layer, and then an ion polymer is sprayed to obtain a cathode catalyst layer; the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, and the third catalyst includes Pt and / or Pt-based materials.

[0034] In a third aspect, the present application provides a fuel cell, comprising the membrane electrode provided in the first aspect or the membrane electrode produced by the method provided in the second aspect.

[0035] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0036] The membrane electrode provided in the embodiment of the present application can reduce the usage of the anti-reverse polarity catalyst by introducing it into the anode catalyst layer in an ordered form, thereby achieving a better anti-reverse polarity effect and effectively improving the reliability and safety of the membrane electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0039] Figure 1 A schematic diagram of a process for a method provided in an embodiment of the present application;

[0040] Figure 2 A polarization curve diagram of the fuel cell provided in Example 1 of the present application;

[0041] Figure 3 A polarization curve diagram of a fuel cell after anti-reverse polarity test provided in Example 1 of the present application;

[0042] Figure 4 This is a test curve diagram of the anti-reverse polarity performance of the fuel cell provided in Example 1 of the present application. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0044] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0045] An embodiment of the present application provides a membrane electrode with anti-reverse polarity function, wherein the membrane electrode includes an anode catalyst layer, the anode catalyst layer includes a first carbon nanotube layer and a first catalyst arranged in an ordered manner, the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer; the first catalyst is loaded on the first carbon nanotube layer, and the first catalyst includes an anti-reverse polarity catalyst.

[0046] The membrane electrode can reduce the usage of the anti-reverse polarity catalyst by introducing it into the anode catalyst layer in an ordered form, achieve a better anti-reverse polarity effect, and effectively improve the reliability and safety of the membrane electrode.

[0047] In some embodiments, the anti-reversal catalyst comprises Ir and / or Ir-based materials. Further, the anti-reversal catalyst has a loading of 5 μg / cm 2 ~15 μg / cm 2 .

[0048] For example, the anti-reversal catalyst loading may be 5 μg / cm 2 , 6μg / cm 2 , 7μg / cm 2 , 8μg / cm 2 , 9μg / cm 2 , 10μg / cm 2 , 11μg / cm 2 , 12μg / cm 2 , 13μg / cm 2 , 14μg / cm 2 or 15 μg / cm 2 etc., which can also be 5 μg / cm 2 ~15 μg / cm 2 Any value in the range.

[0049] In some embodiments, the anode catalyst layer further comprises a second catalyst, the second catalyst is loaded on the first carbon nanotube layer, and the second catalyst comprises Pt and / or a Pt-based material. Further, the loading amount of the second catalyst is 10 μg / cm 2 ~30 μg / cm 2 .

[0050] For example, the loading of the second catalyst may be 10 μg / cm 2 , 12μg / cm 2 , 14μg / cm 2 , 16μg / cm 2 , 18μg / cm 2 , 20μg / cm 2 , 22μg / cm 2, 24μg / cm 2 , 26μg / cm 2 , 28μg / cm 2 or 30 μg / cm 2 etc., which can also be 10 μg / cm 2 ~30 μg / cm 2 Any value in the range.

[0051] In some embodiments, the membrane electrode also includes a proton exchange membrane and a cathode catalyst layer, the proton exchange membrane is arranged between the anode catalyst layer and the cathode catalyst layer, the cathode catalyst layer includes an ordered second carbon nanotube layer and a third catalyst, the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, the third catalyst is loaded on the second carbon nanotube layer, and the third catalyst includes Pt and / or Pt-based materials.

[0052] Furthermore, the loading of the third catalyst is 40 μg / cm 2 ~60 μg / cm 2 For example, the third catalyst loading may be 40 μg / cm 2 42μg / cm 2 44μg / cm 2 46μg / cm 2 , 48μg / cm 2 , 50μg / cm 2 , 52μg / cm 2 , 54μg / cm 2 , 56μg / cm 2 , 58μg / cm 2 or 60 μg / cm 2 etc., which can also be 40 μg / cm 2 ~60 μg / cm 2 Any value in the range.

[0053] The membrane electrode constructs a vertical array of carbon nanotubes to deposit catalysts in an orderly manner. Under the same catalytic effect, the Pt loading and Ir loading in the membrane electrode catalyst layer are significantly reduced. The mass activity of Pt is nearly an order of magnitude higher than that of the current commercial membrane electrode, which can effectively reduce costs. The low Ir loading of the anode can achieve an anti-reverse polarity function that exceeds the average level of commercial membrane electrodes, effectively improving the reliability and safety of the membrane electrode.

[0054] Figure 1 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 1 As shown, based on a general inventive concept, an embodiment of the present application also provides a method for preparing a membrane electrode with anti-reverse polarity function.

[0055] The method is used for preparing the above-mentioned membrane electrode. The specific content of the membrane electrode can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.

[0056] In some embodiments, the method comprises:

[0057] S1. Obtaining a first carbon nanotube layer in an ordered arrangement;

[0058] In some embodiments, the first carbon nanotube layer having an ordered arrangement comprises:

[0059] S1.1. Obtain a substrate, the substrate comprising an aluminum foil and an iron film attached to the aluminum foil;

[0060] In some embodiments, the thickness of the aluminum film is 5 μm to 30 μm; the thickness of the iron film is 0.5 nm to 2 nm. Exemplarily, the thickness of the aluminum film can be 5 μm, 7 μm, 9 μm, 11 μm, 13 μm, 15 μm, 17 μm, 19 μm, 21 μm, 23 μm, 25 μm, 27 μm, 29 μm or 30 μm, etc., and it can also be any value in the range of 5 μm to 30 μm. The thickness of the iron film can be 0.5 nm, 0.7 nm, 0.9 nm, 1.1 nm, 1.3 nm, 1.5 nm, 1.7 nm, 1.9 nm or 2 nm, etc., and it can also be any value in the range of 0.5 nm to 2 nm.

[0061] Specifically, in this embodiment, commercial aluminum foil is deposited with an iron film in an electron beam evaporator to obtain a substrate. The thickness of the commercial aluminum foil used is 5 to 30 μm; the iron particles used to deposit the iron film are heated in a graphite crucible, and the deposition rate is controlled by controlling the voltage and current of the PECVD system. By controlling the deposition time, the thickness of the iron film is controlled to be 0.5 to 2 nm.

[0062] S1.2. etching the iron film on the substrate to form mutually isolated iron particles and removing oxides on the surface of the iron film to obtain an intermediate plate;

[0063] Specifically, in this embodiment, an aluminum foil coated with an iron film is fixed on a stainless steel substrate and placed in an inductively coupled radio frequency plasma enhanced chemical vapor deposition (RF-PECVD) system to etch the continuous iron film into isolated iron particles while removing oxides on the iron surface to obtain an intermediate plate.

[0064] S1.3. Use a carbon source to deposit carbon on the middle plate to form ordered carbon nanotubes to obtain a first carbon nanotube layer.

[0065] In some embodiments, the carbon source includes a mixture of C2H2 and H2, wherein the mixing ratio of C2H2 and H2 is 1:(5-20). Exemplarily, the mixing ratio of C2H2 and H2 can be 1:5, 1:7, 1:9, 1:11, 1:13, 1:15, 1:17, 1:19 or 1:20, etc., and can also be any value within the range of 1:(5-20).

[0066] Specifically, in this embodiment, a vertical array of carbon nanotubes (VACNTs) is grown by introducing a mixed gas of C2H2 and H2 to obtain an aluminum foil loaded with VACNTs (i.e., the first carbon nanotube layer in an ordered arrangement), wherein the mixing ratio of C2H2 to H2 is 1:5 to 1:20.

[0067] S2. loading a first catalyst on the first carbon nanotube layer, and then spraying an ion polymer to obtain an anode catalyst layer; the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer, and the first catalyst includes an anti-reverse polarity catalyst;

[0068] In some embodiments, loading the first catalyst on the first carbon nanotube layer includes depositing an Ir-containing precursor on the first carbon nanotube layer using an atomic deposition method.

[0069] Furthermore, the Ir-containing precursor includes at least one of chloroiridic acid, iridium acetylacetonate, iridium trichloride and iridium tetrachloride.

[0070] The deposition rate of the Ir-containing precursor is

[0071] In some embodiments, the method further comprises loading a second catalyst on the first carbon nanotubes, wherein the second catalyst comprises Pt and / or a Pt-based material.

[0072] Furthermore, loading the second catalyst on the first carbon nanotube layer includes depositing a Pt-containing precursor on the first carbon nanotube layer by an atomic deposition method.

[0073] Furthermore, the Pt-containing precursor includes at least one of chloroplatinic acid, chloroplatinous acid, platinum acetylacetonate, bis(ethylenediamine)platinum acetate and trimethylmethylcyclopentadienylplatinum. The deposition rate of the Pt-containing precursor is It should be noted that the Pt-containing precursor used cannot be sodium chloroplatinate, potassium chloroplatinate and other salts, which will have a poisonous effect on the final membrane electrode.

[0074] Specifically, in this embodiment, a precursor containing Pt (including one of chloroplatinic acid, chloroplatinous acid, acetylacetonate platinum, bis(ethylenediamine)acetate platinum, and trimethylmethylcyclopentadiene platinum) and a precursor containing Ir (one of chloroiridic acid, iridium acetylacetonate, iridium trichloride, and iridium tetrachloride) are used to deposit Pt and Ir nanoparticles on VACNTs using an atomic layer deposition (ALD) method to obtain PtIr / VACNTs, and a diluted Nafion solution is sprayed on PtIr / VACNTs using electrostatic spraying, and the anode catalyst layer is obtained after drying. The deposition rates of Pt and Ir are controlled to be The deposition time is controlled according to its loading requirements.

[0075] S3. Assembling the anode catalyst layer, the proton exchange membrane and the cathode catalyst layer to obtain a membrane electrode.

[0076] Specifically, the anode catalyst layer and the cathode catalyst layer are simultaneously hot-pressed and transferred to both sides of the proton exchange membrane to obtain a catalyst-coated proton exchange membrane (CCM), and then a gas diffusion layer is prepared to obtain a membrane electrode.

[0077] In some embodiments, the method for preparing the cathode catalyst layer includes: obtaining a second carbon nanotube layer with an ordered arrangement; loading a third catalyst on the second carbon nanotube layer, and then spraying an ion polymer to obtain a cathode catalyst layer; the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, and the third catalyst includes Pt and / or Pt-based materials.

[0078] Specifically, in this embodiment, commercial aluminum foil is deposited with an iron film in an electron beam evaporator to obtain a substrate. The thickness of the commercial aluminum foil used is 5 to 30 μm; the iron particles used to deposit the iron film are heated in a graphite crucible, and the deposition rate is controlled by controlling the voltage and current of the PECVD system. By controlling the deposition time, the thickness of the iron film is controlled to be 0.5-2nm. The aluminum foil coated with the iron film is fixed on a stainless steel substrate and placed in an inductively coupled radio frequency plasma enhanced chemical vapor deposition (RF-PECVD) system to etch the continuous iron film into isolated iron particles while removing the oxide on the iron surface to obtain an intermediate plate. A vertical array of carbon nanotubes (VACNTs) is grown by introducing a mixed gas of C2H2 and H2 to obtain an aluminum foil loaded with VACNTs (i.e., an ordered second carbon nanotube layer). Among them, the mixing ratio of C2H2 to H2 is 1:5-1:20. Using a Pt-containing precursor (including one of chloroplatinic acid, chloroplatinous acid, acetylacetonato platinum, bis(ethylenediamine)acetate platinum, and trimethylmethylcyclopentadiene platinum), Pt nanoparticles are deposited on VACNTs using the ALD method to obtain Pt / VACNTs, and a diluted Nafion solution is sprayed on the Pt / VACNTs using electrostatic spraying, and the cathode catalyst layer is obtained after drying. It should be noted that the Pt-containing precursor used cannot be sodium chloroplatinate, potassium chloroplatinate and other salts, which will have a poisonous effect on the final membrane electrode.

[0079] This method improves the electronic conductivity by ordering the carbon carrier, has better super-hydrophobicity, and can effectively prevent flooding. The ordering of the carbon carrier greatly improves the utilization rate of Pt, and simultaneously realizes the loading of low-content Ir in the anode catalyst layer, with anti-reverse polarity performance that exceeds the average level of current commercial membrane electrodes. In addition, the commercial aluminum foil used in the process of constructing vertical array carbon nanotubes is low in cost, which is conducive to the mass production and expansion of this ordered membrane electrode.

[0080] Based on a general inventive concept, an embodiment of the present application further provides a fuel cell, which includes the membrane electrode provided above or the membrane electrode manufactured by the method provided above.

[0081] The fuel cell is realized based on the above-mentioned membrane electrode or the membrane electrode prepared by the above-mentioned method. The specific contents of the membrane electrode or the above-mentioned method can refer to the above-mentioned embodiments. Since the fuel cell adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0082] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0083] Example 1

[0084] A fuel cell, the preparation process of which is as follows:

[0085] 1) Two pieces of 15μm thick commercial aluminum foil were deposited with an iron film in an electron beam evaporator, and the thickness of the iron film was controlled to be 1nm. Subsequently, the aluminum foil coated with the iron film was fixed on a stainless steel substrate and placed in an inductively coupled radio frequency plasma enhanced chemical vapor deposition (RF-PECVD) system to etch the continuous iron film into isolated iron particles while removing the oxide on the iron surface. Subsequently, a mixture of C2H2 and H2 (20sccm:200sccm) was introduced to grow vertical arrays of carbon nanotubes (VACNTs). Two pieces of aluminum foil loaded with VACNTs were obtained.

[0086] 2) The precursors were trimethylmethylcyclopentadienyl platinum and chloroiridic acid, and Pt and Ir nanoparticles were co-deposited on VACNTs using atomic layer deposition (ALD) to obtain the anode catalyst layer PtIr / VACNTs, with the Pt loading controlled to 20 μg / cm 2 , Ir loading is 10 μg / cm 2 .

[0087] 3) The precursors were selected as trimethyl methylcyclopentadienyl platinum, and Pt nanoparticles were deposited on VACNTs using the ALD method to obtain the cathode catalyst layer Pt / VACNTs, and the Pt loading was controlled to be 50 μg / cm 2 .

[0088] 4) Using electrostatic spraying, 150 μL and 500 μL of 5% Nafion solution were sprayed on PtIr / VACNTs and Pt / VACNTs respectively. After drying, the anode catalyst layer and the cathode catalyst layer were simultaneously hot-pressed and transferred to both sides of the proton exchange membrane to obtain a catalyst-coated proton exchange membrane (CCM).

[0089] The performance tests of the embodiments and comparative examples were carried out under the following conditions: the single cell test was carried out using a Qunyi test bench 850e, and the prepared membrane electrode (5 cm 2 ) Place carbon paper on both sides and load into a fixture with a graphite plate flow field. The battery temperature is 80°C, the humidity of the cathode and anode is 100% RH / 100% RH, the back pressure is 150kPa / 150kPa, the excess coefficient H2 / Air=1.5 / 4.0, and after activation at 0.505V for 3h, perform polarization curve test (humidity and back pressure remain unchanged, the excess coefficients are 1.5 / 2.5 and 1.5 / 4.0 respectively. Note that no back pressure is added for the reverse pole test, the anode hydrogen is switched to nitrogen to simulate the reverse pole condition, the battery temperature is 65°C, and the current density is 200mAcm -2 ).

[0090] Figure 2 The polarization curve diagram of the fuel cell provided in Example 1 of the present application is as follows: Figure 2As shown in the figure, when the excess coefficient ratio is 1.5 / 2.5, the ordered membrane electrode sample has a high conductivity at 2000 mA cm -2 The corresponding voltage at the current density is 0.593V and the output power is 1.19Wcm -2 When the cathode air excess coefficient is increased to 4, the corresponding voltage and output power increase to 0.603V and 1.206W cm -2 . Figure 4 This is a test curve diagram of the anti-reverse polarity performance of the fuel cell provided in Example 1 of the present application, Figure 4 It can be obtained that the water electrolysis platform time for the anti-reverse polarity test is 98 minutes. Figure 3 The polarization curve diagram of the fuel cell after the anti-reverse polarity test provided in Example 1 of the present application is shown in FIG. Figure 3 It can be obtained that when the excess coefficient ratio after activation is 1.5 / 2.5, the corresponding voltage and output power under the same electric density of the polarization curve are 0.524V and 1.048W cm -2 The corresponding attenuation rate is 11.6%.

[0091] From the above, we can see that the average output voltage of the membrane electrode can reach 0.6V@2A / cm 2 , which can meet the requirements of medium-power fuel cells, and the mass activity of Pt is nearly an order of magnitude higher than that of the current commercial membrane electrode, which can effectively reduce costs. At the same time, the Ir loading is significantly reduced by the ordering of the carrier in the anode catalyst layer, and the anti-reverse polarity time can reach 98 minutes by improving water vapor transport and mass transfer, which exceeds the average level of current commercial membrane electrodes (45 to 90 minutes).

[0092] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0093] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.

[0094] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A membrane electrode with anti-reverse polarity function, It is characterized in that The membrane electrode comprises an anode catalyst layer, which comprises an ordered first carbon nanotube layer and a first catalyst, wherein the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer; the first catalyst is loaded on the first carbon nanotube layer, and the first catalyst comprises an anti-reverse polarity catalyst.

2. The membrane electrode with anti-reverse polarity function according to claim 1, It is characterized in that The anti-reversal catalyst comprises Ir and / or Ir-based materials; and / or The loading of the anti-reversal catalyst is 5 μg / cm 2 ~15 μg / cm 2 .

3. The membrane electrode with anti-reverse polarity function according to claim 1, It is characterized in that The anode catalyst layer further comprises a second catalyst, the second catalyst is supported on the first carbon nanotube layer, and the second catalyst comprises Pt and / or a Pt-based material; and / or The loading of the second catalyst is 10 μg / cm 2 ~30 μg / cm 2 .

4. The membrane electrode with anti-reverse polarity function according to claim 1, It is characterized in that The membrane electrode further comprises a proton exchange membrane and a cathode catalyst layer, wherein the proton exchange membrane is disposed between the anode catalyst layer and the cathode catalyst layer, the cathode catalyst layer comprises an ordered second carbon nanotube layer and a third catalyst, the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, the third catalyst is loaded on the second carbon nanotube layer, and the third catalyst comprises Pt and / or a Pt-based material; and / or The loading of the third catalyst is 40 μg / cm 2 ~60 μg / cm 2 .

5. A method for preparing a membrane electrode having an anti-reverse polarity function, It is characterized in that The method comprises: Obtaining a first carbon nanotube layer with orderly arrangement; The first catalyst is loaded on the first carbon nanotube layer, and then an ion polymer is sprayed to obtain an anode catalyst layer; the extension direction of the carbon nanotubes in the first carbon nanotube layer is perpendicular to the extension surface of the anode catalyst layer, and the first catalyst includes an anti-reverse polarity catalyst; The anode catalyst layer, the proton exchange membrane and the cathode catalyst layer are assembled to obtain a membrane electrode.

6. The method for preparing a membrane electrode having an anti-reverse polarity function according to claim 5, It is characterized in that The first carbon nanotube layer obtained in an ordered arrangement comprises: obtaining a substrate, the substrate comprising an aluminum foil and an iron film attached to the aluminum foil; Etching the iron film on the substrate to form mutually isolated iron particles, and removing oxides on the surface of the iron film to obtain an intermediate plate; A carbon source is used to deposit carbon on the middle plate to form orderly arranged carbon nanotubes to obtain a first carbon nanotube layer.

7. The method for preparing a membrane electrode having an anti-reverse polarity function according to claim 5, It is characterized in that The thickness of the aluminum film is 5 μm to 30 μm; and / or The thickness of the iron film is 0.5nm to 2nm; and / or The carbon source includes C 2 H 2 and H 2 The mixed gas, the C 2 H 2 and H 2 The mixing ratio is 1:(5~20).

8. The method for preparing a membrane electrode having an anti-reverse polarity function according to claim 5, It is characterized in that The loading of the first catalyst on the first carbon nanotube layer comprises depositing an Ir-containing precursor on the first carbon nanotube layer by an atomic deposition method; and / or The Ir-containing precursor includes at least one of chloroiridic acid, iridium acetylacetonate, iridium trichloride and iridium tetrachloride; and / or The deposition rate of the Ir-containing precursor is and / or The method further comprises loading a second catalyst on the first carbon nanotube, wherein the second catalyst comprises Pt and / or a Pt-based material; and / or The loading of the second catalyst on the first carbon nanotube comprises depositing a Pt-containing precursor on the first carbon nanotube layer by an atomic deposition method; and / or The Pt-containing precursor includes at least one of chloroplatinic acid, chloroplatinous acid, platinum acetylacetonate, bis(ethylenediamine)platinum acetate and trimethylmethylcyclopentadienylplatinum; and / or The deposition rate of the Pt-containing precursor is 9. The method for preparing a membrane electrode having an anti-reverse polarity function according to claim 5, It is characterized in that The preparation method of the cathode catalyst layer comprises: Obtaining a second carbon nanotube layer with orderly arrangement; The third catalyst is loaded on the second carbon nanotube layer, and then an ion polymer is sprayed to obtain a cathode catalyst layer; the extension direction of the carbon nanotubes in the second carbon nanotube layer is perpendicular to the extension surface of the cathode catalyst layer, and the third catalyst includes Pt and / or Pt-based materials.

10. A fuel cell, It is characterized in that The fuel cell comprises the membrane electrode according to any one of claims 1 to 4 or the membrane electrode produced by the method according to any one of claims 5 to 9.