Processing technology for improving wettability of cylindrical battery cell
By adopting the processing technology of horizontal placement and reverse rotation of the roller in the manufacturing of cylindrical battery cells, the problem of insufficient electrolyte wetting caused by the compaction of the core is solved, and the battery performance and production efficiency are significantly improved.
Patent Information
- Application Number
- CN202411254054.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-09
AI Technical Summary
During the manufacturing process, the core of the cylindrical cell is too tight, resulting in a decrease in internal porosity, hindering the penetration and infiltration of the electrolyte and affecting the battery performance and safety.
A processing technology that improves the wetting properties of the cylindrical battery cell is adopted. By placing the core horizontally and controlling its rotation, and combining the reverse-rotating kneading roller for surface kneading, the compactness of the core is reduced, the internal space is increased, and the electrolysis is improved. The wetting properties of the liquid. The process includes placing a core in the positioning groove, setting a kneading roller and applying a predetermined pressure, performing continuous kneading and processing, and combining vacuum drying, ultrasonic vibration and plasma processing to optimize the effect.
Without affecting the stability of the cell structure, the wetting properties of the electrolyte are significantly improved, the overall performance of the battery is improved, the production efficiency is optimized and the manufacturing cost is reduced.
Smart Images

Figure BDA0005033413080000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary battery preparation, and in particular relates to a processing technology for improving the wettability of a cylindrical battery core. Background Art
[0002] Cylindrical cells are widely used in portable electronic devices, power tools, electric vehicles and other fields due to their compact structure, high energy density and mature manufacturing process. However, cylindrical cells face a key challenge in the manufacturing process: how to ensure that the electrolyte can fully infiltrate the electrode material while ensuring the stability of the cell structure.
[0003] The traditional cylindrical battery manufacturing process usually adopts a high-tension winding method to ensure the compactness and mechanical strength of the core structure. Although this method can improve the energy density and structural stability of the battery, it also leads to a serious problem: the core is too compact, the internal porosity is reduced, and the penetration and infiltration of the electrolyte are hindered.
[0004] Sufficient electrolyte infiltration is crucial to the performance of the battery. It not only affects the capacity and rate performance of the battery, but is also directly related to the cycle life and safety of the battery. Insufficient infiltration will reduce the utilization of electrode materials, increase the internal resistance of the battery, and may even cause safety hazards.
[0005] At present, the industry has tried a variety of methods to improve the wettability of the electrolyte, such as extending the injection time, increasing the injection pressure, using low-viscosity electrolyte, etc. However, these methods either have limited effects or bring other adverse effects. For example, extending the injection time will reduce production efficiency, and using low-viscosity electrolyte may affect the long-term stability of the battery.
[0006] Therefore, a new processing technology is urgently needed that can effectively reduce the compactness of the core and increase the internal gap without affecting the stability of the battery cell structure, thereby significantly improving the wettability of the electrolyte. This can not only improve the overall performance of the battery, but also optimize production efficiency and reduce manufacturing costs. Summary of the invention
[0007] The purpose of the present invention is to provide a processing technology for improving the wettability of cylindrical battery cells in response to the deficiencies of the prior art, which can effectively reduce the compactness of the core and increase the internal gap without affecting the stability of the battery cell structure, thereby improving the wettability of the electrolyte.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A processing technology for improving the wettability of a cylindrical battery cell comprises the following steps:
[0010] S1. Place the wound core horizontally in a positioning fixture with a positioning groove;
[0011] S2, controlling the winding core to rotate around its axis at a first preset speed;
[0012] S3, arranging one or more kneading rollers above the winding core, wherein the axis of the kneading rollers is parallel to the axis of the winding core, and controlling the kneading rollers to rotate at a second preset speed in a direction opposite to the rotation direction of the winding core;
[0013] S4, making the kneading roller contact with the surface of the winding core and applying a predetermined pressure;
[0014] S5, continuously kneading the surface of the winding core for a preset time.
[0015] Preferably, the first preset speed is 40-80 rpm, and the second preset speed is 50-90 rpm.
[0016] Preferably, the predetermined pressure is 10-15 N / cm 2 , the preset time is 1 to 10 seconds.
[0017] Preferably, the wound winding core is inserted into a winding needle that coincides with its axis, and the winding core is rotated by driving a motor to control the winding needle to rotate.
[0018] Preferably, the depth of the positioning groove is 1 / 4 to 1 / 2 of the diameter of the winding core.
[0019] Preferably, there are at least two kneading rollers, and the at least two kneading rollers are spaced apart along the axis, and the axis of each kneading roller coincides.
[0020] Preferably, the kneading roller is made of metal or plastic with a smooth surface, the diameter of the kneading roller is 30-40 mm, and the total length of the kneading roller is equal to the length of the winding core.
[0021] Preferably, the method further comprises pre-treating the core in a vacuum drying oven before the kneading treatment; the pre-treatment temperature is 55 to 65° C. and the time is 1 to 3 hours.
[0022] Preferably, the method further comprises a cooling and shaping step after kneading, wherein the roll core is placed in an environment with a temperature of 25° C. and a relative humidity of ≤30% to cool for 10 to 30 minutes.
[0023] Preferably, the method further comprises applying ultrasonic vibration to the winding core during the kneading process, wherein the frequency of the ultrasonic vibration is 20 to 40 kHz and the power is 50 to 100 W.
[0024] Preferably, in step S5, the surface of the core is subjected to a multi-stage kneading treatment, and the multi-stage kneading treatment includes three stages:
[0025] The first stage: the pressure is 5-8N / cm 2 , speed is 80-90rpm, knead continuously for 1-3s;
[0026] The second stage: the pressure is 10-13N / cm 2 , speed is 50-60rpm, knead continuously for 2-6s;
[0027] The third stage: the pressure is 15-18N / cm 2 , speed is 30-40rpm, knead continuously for 1 to 3 seconds.
[0028] Preferably, the method further comprises the step of performing plasma treatment on the surface of the core after kneading, wherein the plasma treatment uses oxygen plasma and the treatment time is 20-60 seconds.
[0029] Compared with the prior art, the present invention has at least the following beneficial effects:
[0030] 1) The present invention achieves uniform kneading treatment on the surface of the core by placing the core horizontally and controlling its rotation, combined with counter-rotating kneading rollers; this method can effectively reduce the compactness of the core, increase the internal gap, and significantly improve the wettability of the electrolyte without affecting the stability of the battery cell structure.
[0031] 2) The contact between the kneading roller and the surface of the core and the predetermined pressure applied can accurately control the kneading intensity to avoid damage to the core; the preset continuous kneading time ensures the consistency and controllability of the treatment, which is beneficial to quality control in mass production. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The present application provides a processing technology for improving the wettability of a cylindrical battery cell, comprising the following steps:
[0034] S1. Core positioning: Place the wound core horizontally in a positioning jig with a positioning groove; the positioning jig is made of high-strength engineering plastic, and the depth of the positioning groove is 1 / 4 to 1 / 2 of the core diameter to ensure that the core is stably placed and has enough surface exposed to the rubbing roller.
[0035] S2. Rotation of the winding core: Control the winding core to rotate around its axis at a first preset speed; insert the winding core onto a winding needle that coincides with its axis, and rotate the winding core by driving the winding needle to rotate by a motor, wherein the motor may be a precision stepping motor, and the speed may be precisely adjusted to accommodate winding cores of different specifications;
[0036] S3. Kneading roller setting: one or more kneading rollers are set above the winding core; the axis of the kneading roller is parallel to the axis of the winding core, and is driven by an independent servo motor to rotate in a direction opposite to the rotation direction of the winding core at a second preset speed;
[0037] S4. Pressure application: The kneading roller is brought into contact with the surface of the core and a predetermined pressure is applied. The pressure can be adjusted by a precise air pressure control system and can be adjusted in real time according to the core specifications and kneading requirements.
[0038] S5. Continuous kneading: The surface of the core is rubbed continuously for a preset time; the kneading time can be precisely controlled by the PLC control system to ensure the consistency of the treatment.
[0039] In one embodiment of the present application, the first preset speed is 40-80 rpm, and the second preset speed is 50-90 rpm, so as to ensure the kneading effect while minimizing the impact on the core structure.
[0040] In one embodiment of the present application, the predetermined pressure is 10-15 N / cm 2 , the preset time is 1 to 10 seconds. It provides highly adaptable processing parameters for cores of different specifications, which can ensure the kneading effect and avoid over-processing.
[0041] In one embodiment of the present application, at least two kneading rollers are provided, and at least two kneading rollers are arranged at intervals along the axis, and the axis of each kneading roller coincides. The arrangement of multiple kneading rollers can process different parts of the core at the same time, thereby improving processing efficiency and uniformity.
[0042] In one embodiment of the present application, the kneading roller is made of metal or plastic with a smooth surface, the diameter of the kneading roller is 30-40 mm, and the total length of the kneading roller is equal to the length of the winding core. The optimization of the material and size of the kneading roller ensures the stability of the kneading process and the integrity of the winding core surface.
[0043] In one embodiment of the present application, the step of pre-treating the core in a vacuum drying oven before the kneading treatment is also included; the pre-treatment temperature is 55-65°C and the time is 1-3 hours. The vacuum drying pre-treatment step can remove residual moisture in the core and create ideal conditions for the subsequent kneading treatment.
[0044] In one embodiment of the present application, a cooling and shaping step is further included after kneading is completed, wherein the core is placed in an environment with a temperature of 25° C. and a relative humidity of ≤30% to cool for 10 to 30 minutes. The cooling and shaping step helps stabilize the core structure and prevent the rebound effect after kneading.
[0045] In one embodiment of the present application, ultrasonic vibration is applied to the core during the kneading process, wherein the frequency of the ultrasonic vibration is 20 to 40 kHz and the power is 50 to 100 W. The introduction of ultrasonic vibration can further promote the relaxation of the internal structure of the core and enhance the kneading effect.
[0046] In one embodiment of the present application, in step S5, the surface of the core is subjected to a multi-stage kneading treatment, and the multi-stage kneading treatment includes three stages:
[0047] The first stage: the pressure is 5-8N / cm 2 , speed is 80-90rpm, knead continuously for 1-3s;
[0048] The second stage: the pressure is 10-13N / cm 2 , speed is 50-60rpm, knead continuously for 2-6s;
[0049] The third stage: the pressure is 15-18N / cm 2 , speed is 30-40rpm, knead continuously for 1 to 3 seconds.
[0050] Among them, the multi-stage kneading treatment achieves progressive relaxation from the surface to the deep layer by gradually increasing pressure and reducing speed, which is more conducive to maintaining the overall structure of the core.
[0051] In one embodiment of the present application, the step of plasma treating the surface of the core after kneading is further included, wherein the plasma treatment uses oxygen plasma and the treatment time is 20-60 seconds. The plasma treatment can improve the affinity of the core surface and further improve the infiltration effect of the electrolyte.
[0052] In summary, the present invention achieves the goal of effectively reducing the compactness of the core and increasing the internal gap without affecting the stability of the core structure through a carefully designed kneading process combined with multiple optimization measures. This method not only improves the wettability of the electrolyte, but also has the advantages of simple operation, strong adaptability, and high controllability.
[0053] The implementation and advantages of this application will be further explained below in conjunction with specific embodiments.
[0054] Example 1
[0055] The present embodiment provides a processing technology for improving the wettability of a cylindrical battery cell, comprising the following steps:
[0056] S1. Place the wound core horizontally in a positioning jig with a positioning groove; the positioning jig is made of polytetrafluoroethylene, and the depth of the positioning groove is 1 / 4 of the core diameter to ensure that the core is stably placed and has enough surface exposed to the kneading roller;
[0057] S2. Control the winding core to rotate around its axis at a speed of 60 rpm; insert the winding core into the winding needle that coincides with its axis, and drive the winding needle to rotate by a stepper motor to rotate the winding core;
[0058] S3. Three kneading rollers are arranged above the core, spaced apart along the axis, and the axis of each kneading roller coincides, the axis of the kneading roller is parallel to the axis of the core, and is driven by an independent servo motor to rotate at a speed of 70 rpm in the opposite direction of the rotation direction of the core; wherein the kneading roller is made of stainless steel with a smooth surface, a diameter of 30 mm, and a total length equal to the length of the core;
[0059] S4. Make the kneading roller contact the surface of the core and apply a pressure of 12N / cm 2 ; The pressure is adjusted by a precise air pressure control system, which ensures the kneading effect while avoiding excessive extrusion and deformation;
[0060] S5. Continuously rub the surface of the core for a preset time of 5 seconds; the rubbing time is precisely controlled by the PLC control system to ensure the consistency of the treatment.
[0061] Among them, the core is formed by stacking and winding the positive electrode sheet, the separator and the negative electrode sheet in sequence. After the winding is completed, the core is fixed with tape; wherein the positive electrode sheet includes aluminum foil and a positive electrode active material layer arranged on the aluminum foil, the positive electrode active material layer includes 95wt% of positive electrode active material (NCM523), 2wt% of conductive agent (Ketjen black) and 3wt% of binder (PVDF); the negative electrode sheet includes copper foil and a negative electrode active material layer arranged on the copper foil, the negative electrode active material layer includes 95wt% of negative electrode active material (graphite), 2wt% of conductive agent (conductive carbon black) and 3wt% of binder (SBR); the separator adopts a polyolefin separator with a thickness of 16μm.
[0062] The processed roll core is placed in an aluminum-plastic film, packaged using a heat sealer, and injected with a predetermined amount of electrolyte (1MLiPF6 EC / DMC / EMC=1:1:1) to obtain a soft-pack cylindrical battery.
[0063] Example 2
[0064] Different from Example 1, this example is based on Example 1, and before the kneading treatment, the core is placed in a vacuum drying oven for pretreatment, the pretreatment temperature is 60°C, and the time is 2 hours. After the pretreatment is completed, the core is taken out and the kneading treatment is performed according to the steps of Example 1.
[0065] Example 3
[0066] Different from Example 2, this example further includes a cooling and shaping step after kneading, in which the core is placed in an environment with a temperature of 25° C. and a relative humidity of ≤30% for cooling for 20 minutes. The cooling and shaping step helps to stabilize the core structure and prevent the rebound effect after kneading.
[0067] The rest is the same as in Example 2 and will not be described again here.
[0068] Example 4
[0069] Different from Example 3, this embodiment, based on Example 3, further includes applying ultrasonic vibration to the core during the kneading process, specifically, ultrasonic vibrators are provided on both sides of the kneading roller, and the ultrasonic vibrators are electrically connected to the ultrasonic generator; in step S5, the ultrasonic generator is controlled to output ultrasonic waves with a frequency of 28kHz and a power of 70W, and the ultrasonic vibrator applies ultrasonic vibration to the core, and the duration is consistent with the kneading time. Applying ultrasonic vibration to the core while kneading can further promote the formation of pores inside the core and improve the wettability of the electrolyte. At the same time, the high-frequency stress generated by the ultrasonic vibration is conducive to relieving the winding stress.
[0070] The rest is the same as in Example 3 and will not be described again here.
[0071] Example 5
[0072] Different from the fourth embodiment, in the present embodiment, on the basis of the fourth embodiment, in step S5, the surface of the core is subjected to a multi-stage kneading treatment, and the multi-stage kneading treatment includes three stages:
[0073] The first stage: the pressure is 6N / cm 2 , speed is 85rpm, knead continuously for 2s;
[0074] The second stage: the pressure is 12N / cm 2 , speed is 55rpm, knead continuously for 4s;
[0075] The third stage: the pressure is 16N / cm 2 , speed is 35rpm, knead continuously for 2s.
[0076] Among them, through multi-stage kneading treatment, using a higher speed and a lower pressure in the early stage of kneading can quickly remove the protrusions on the surface of the core; using a moderate speed and pressure in the middle stage of kneading can effectively reduce the overall compactness of the core; using a lower speed and a higher pressure in the later stage of kneading can finally flatten and shape the surface of the core, thereby obtaining the best kneading effect.
[0077] The rest is the same as in Example 4 and will not be described again here.
[0078] Example 6
[0079] Different from Example 5, this embodiment further includes a step of plasma treatment of the surface of the core after kneading, wherein the plasma treatment uses oxygen plasma and the treatment time is 40 seconds. Plasma treatment can improve the affinity of the core surface and further improve the wetting effect of the electrolyte.
[0080] The rest is the same as in Example 5 and will not be described again here.
[0081] Comparative Example 1
[0082] The core is prepared by a conventional winding process, and the wound core is not subjected to a rubbing treatment.
[0083] The following electrochemical performance tests were performed on the cylindrical batteries prepared in the examples and comparative examples, respectively. The test results are shown in Table 1.
[0084] 1. Electrolyte wettability test:
[0085] 1) injecting a predetermined amount of electrolyte into the treated core under vacuum;
[0086] 2) After standing for 24 hours, take out the core and measure the actual absorbed electrolyte mass with a precision balance;
[0087] 3) Electrolyte wetting rate = (actually absorbed electrolyte mass / theoretically calculated maximum absorption amount) × 100%.
[0088] 2. First charge and discharge efficiency test:
[0089] 1) Assembling the processed core into a battery;
[0090] 2) Use the battery test system to perform the first charge and discharge at a rate of 0.1C;
[0091] 3) Initial charge and discharge efficiency = (initial discharge capacity / initial charge capacity) × 100%.
[0092] 3. Capacity retention test after 100 cycles:
[0093] 1) Use the battery test system to perform 100 charge and discharge cycles at 1C rate;
[0094] 2) Record the 1st and 100th discharge capacities;
[0095] 3) Capacity retention after 100 cycles = (100th discharge capacity / 1st discharge capacity) × 100%.
[0096] 4. Rate performance (3C / 0.5C capacity ratio) test:
[0097] 1) Perform a complete charge and discharge at a rate of 0.5C and record the discharge capacity;
[0098] 2) Then perform a complete charge and discharge at a 3C rate and record the discharge capacity;
[0099] 3) 3C / 0.5C capacity ratio = (discharge capacity at 3C rate / discharge capacity at 0.5C rate) x 100%.
[0100] The above test results are specifically shown in Table 1 below.
[0101] Table 1
[0102]
[0103] The test results in Table 1 are analyzed as follows:
[0104] 1. Comparative analysis of embodiments and comparative examples:
[0105] 1) Electrolyte Wetting Rate: The electrolyte wetting rates of Examples 1-6 range from 88% to 97%, while that of Comparative Example 1 is 76%; the wetting rates of all Examples are significantly higher than those of the Comparative Example.
[0106] 2) Initial charge and discharge efficiency: The initial charge and discharge efficiency of Examples 1-6 ranged from 89% to 94%, while that of Comparative Example 1 was 82%; the initial charge and discharge efficiency of all Examples was higher than that of the Comparative Example.
[0107] 3) Capacity retention after 100 cycles: The capacity retention of Examples 1-6 ranges from 86% to 93%, while that of Comparative Example 1 is 79%; the capacity retention of all Examples is higher than that of the Comparative Example.
[0108] 4) Rate performance: The 3C / 0.5C capacity ratios of Examples 1-6 are 80% to 89%, respectively, while that of Comparative Example 1 is 71%; the rate performances of all Examples are significantly better than those of the Comparative Example.
[0109] In summary, the battery prepared by the processing technology of the present invention is significantly superior to the conventional battery without kneading treatment in various performance indicators, especially in terms of electrolyte infiltration rate and rate performance.
[0110] 2. Comparative analysis between various embodiments
[0111] 1) Electrolyte wetting rate: From Example 1 to Example 6, the wetting rate gradually increased to 88%, 91%, 93%, 95%, 96% and 97%, respectively. With each additional optimization step, the wetting rate increased by about 2 percentage points on average.
[0112] 2) Initial charge and discharge efficiency: From Example 1 to Example 6, the initial charge and discharge efficiency gradually increased to 89%, 90%, 91%, 92%, 93% and 94%, respectively. With each additional optimization step, the efficiency increased by about 1 percentage point on average.
[0113] 3) Capacity retention after 100 cycles: From Example 1 to Example 6, the capacity retention rate gradually increased to 86%, 88%, 90%, 91%, 92% and 93%, respectively. The increase in optimization steps increased the capacity retention rate by about 1.5 percentage points each time on average.
[0114] 4) Rate performance: From Example 1 to Example 6, the 3C / 0.5C capacity ratio gradually increased to 80%, 82%, 84%, 86%, 87% and 89%, respectively. With each additional optimization step, the rate performance increased by about 2 percentage points on average.
[0115] In summary, there is an obvious synergistic effect between the optimization steps. With the increase of optimization steps, various performance indicators show a steady improvement trend. Among them, the improvement of electrolyte infiltration rate and rate performance is the most significant, indicating that the processing technology of the present invention is particularly effective in improving electrolyte distribution and increasing electrode material utilization.
[0116] It should be noted that the contents not described in detail in this specification belong to the prior art known to professional and technical personnel in the field and will not be repeated here.
[0117] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A processing technology for improving the wettability of cylindrical battery cells. It is characterized in that The following steps are involved: S1. Place the wound core horizontally in a positioning fixture with a positioning groove; S2, controlling the winding core to rotate around its axis at a first preset speed; S3, arranging one or more kneading rollers above the winding core, wherein the axis of the kneading rollers is parallel to the axis of the winding core, and controlling the kneading rollers to rotate at a second preset speed in a direction opposite to the rotation direction of the winding core; S4, making the kneading roller contact with the surface of the winding core and applying a predetermined pressure; S5, continuously kneading the surface of the winding core for a preset time.
2. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The first preset speed is 40-80 rpm, and the second preset speed is 50-90 rpm.
3. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The predetermined pressure is 10-15 N / cm 2 , the preset time is 1 to 10 seconds.
4. The process for improving wettability of cylindrical battery cells according to claim 1, Features: At least two kneading rollers are provided, and the at least two kneading rollers are arranged at intervals along the axis, and the axis of each kneading roller coincides.
5. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The kneading roller is made of metal or plastic with a smooth surface, the diameter of the kneading roller is 30-40 mm, and the total length of the kneading roller is equal to the length of the winding core.
6. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The method further comprises the step of pre-treating the core in a vacuum drying oven before the kneading treatment; the pre-treatment temperature is 55 to 65° C. and the time is 1 to 3 hours.
7. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The method further comprises a cooling and shaping step after the kneading is completed, wherein the roll core is placed in an environment with a temperature of 25° C. and a relative humidity of ≤30% to cool for 10 to 30 minutes.
8. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The method further comprises applying ultrasonic vibration to the winding core during the kneading process, wherein the frequency of the ultrasonic vibration is 20 to 40 kHz and the power is 50 to 100 W.
9. The process for improving wettability of cylindrical battery cells according to claim 1, Features: In step S5, the surface of the core is subjected to a multi-stage kneading treatment, and the multi-stage kneading treatment includes three stages: The first stage: the pressure is 5-8N / cm 2 , speed is 80-90rpm, knead continuously for 1-3s; The second stage: the pressure is 10-13N / cm 2 , speed is 50-60rpm, knead continuously for 2-6s; The third stage: the pressure is 15-18N / cm 2 , speed is 30-40rpm, knead continuously for 1 to 3 seconds.
10. The process for improving wettability of cylindrical battery cells according to claim 1, Features: The process also includes a step of performing plasma treatment on the surface of the core after kneading, wherein the plasma treatment uses oxygen plasma and the treatment time is 20-60 seconds.
Citation Information
Patent Citations
Method and device for infiltrating battery cell with electrolyte
CN111540957A
Device and method for spin-drying and infiltrating battery core of cylindrical battery
CN111786001A
Flattening method for all-tab cylindrical battery
CN114361555A
Cylindrical battery electrolyte infiltration device
CN221102167U
Manufacturing process for secondary battery
KR1020170004217A
Cited By
Method for improving infiltration efficiency of electronic cigarette cell and electronic cigarette cell
CN120261714A