Lithium ion secondary battery
By using graphite particles and amorphous carbon particles in the negative active material layer in the lithium-ion secondary battery, and adding fluorosulfonate and methoxysulfonate to the electrolyte, the lithium-ion secondary battery was solved. The problem of difficult to take into account both the output characteristics and the high temperature storage characteristics in the low SOC area, achieving high output and good storage characteristics of the battery.
Patent Information
- Application Number
- CN202380035578.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-27
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-29
AI Technical Summary
The output characteristics and high-temperature storage characteristics of existing lithium-ion secondary batteries in low SOC areas are difficult to take into account, and the capacity reduction and resistance increase cannot be suppressed in a long-term high-temperature environment.
The negative electrode active material layer contains graphite particles and amorphous carbon particles, and fluorosulfonate and methoxysulfonate are added as additives to the electrolyte solution to form a solid electrolyte interface film to improve the output characteristics and storage stability of the battery. .
The output characteristics improvement and high temperature storage characteristics in the low SOC region are achieved, the internal resistance is reduced, and the battery capacity and output performance are maintained.
Smart Images

Figure CN119054124A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a lithium ion secondary battery. Background Art
[0002] In the automobile industry, fuel consumption restrictions and environmental restrictions are being strengthened in various countries and regions. In order to comply with these restrictions, the technical development of electric vehicles that do not emit carbon dioxide and use batteries as power sources, and fuel cell vehicles that use hydrogen as a fuel source has attracted much attention. However, electric vehicles have problems such as insufficient charging infrastructure and a long charging time compared to oil supply, and fuel cell vehicles have problems such as the infrastructure of hydrogen stations requires a lot of cost and fuel cells are expensive. Therefore, PHEV (Plug-in Hybrid Electric Vehicle) and HEV (Hybrid Electric Vehicle), which use both internal combustion engines and batteries as power sources and have low carbon dioxide emissions, have become strong candidates for responding to fuel consumption restrictions and environmental restrictions.
[0003] In PHEV and HEV, lithium ion secondary batteries are generally used. In patent document 1, as a lithium ion secondary battery, the following battery is recorded, the non-aqueous electrolyte comprises an electrolyte and a non-aqueous solvent and at least one compound selected from lithium fluorophosphate, lithium bis(fluorosulfonyl)imide and lithium difluorophosphate, and the negative electrode comprises a negative electrode active material containing Si or Si metal oxide and graphite particles. In patent document 2, as a lithium ion secondary battery, the following battery is recorded, the non-aqueous electrolyte comprises lithium hexafluorophosphate (LiPF6) as an electrolyte, and also comprises vinylene carbonate (VC), lithium dioxalate borate (LiBOB) and lithium difluorooxalate borate (LiDFOB) as additives.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-106174
[0007] Patent Document 2: Japanese Patent Application Publication No. 2020-167054 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] In PHEVs and HEVs, lithium ion secondary batteries are required that have a small resistance increase even in a low state of charge (SOC) region and provide a stable output, and that can suppress a decrease in capacity and a resistance increase even in a long-term high-temperature storage environment.
[0010] The techniques described in Patent Documents 1 and 2 cannot achieve both improvement in output characteristics in a low SOC region and improvement in high-temperature storage characteristics, and a technique for achieving both these is required.
[0011] A main object of the present invention is to provide a lithium ion secondary battery capable of achieving both improvement in output characteristics in a low SOC region and improvement in high-temperature storage characteristics.
[0012] Technical solutions for solving technical problems
[0013] The lithium-ion secondary battery of the present invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a current collector and a negative electrode active material layer disposed on at least one side of the current collector, wherein the negative electrode active material layer comprises a negative electrode active material comprising graphite particles and amorphous carbon particles, and the electrolyte comprises at least a non-aqueous solvent, an electrolyte salt and an additive, wherein the additive comprises a fluorosulfonate and a methoxysulfonate.
[0014] Effects of the Invention
[0015] According to the present invention, it is possible to provide a lithium ion secondary battery capable of achieving both improvement in output characteristics in a low SOC region and improvement in high-temperature storage characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a perspective view of the appearance of a lithium ion secondary battery according to an embodiment.
[0017] Figure 2 It is an exploded perspective view of the lithium ion secondary battery according to the embodiment.
[0018] Figure 3 It is an exploded perspective view showing a state in which a part of the winding group according to the embodiment is unfolded.
[0019] Figure 4 This is a conceptual diagram showing a mixed state of graphite particles (A) and graphite particles carrying amorphous carbon fine particles (B) in a negative electrode active material layer according to an embodiment. DETAILED DESCRIPTION
[0020] Hereinafter, the embodiments will be described with reference to the accompanying drawings as appropriate. The following description represents a specific example of the content of the present invention, and the present invention is not limited to these descriptions, and a person skilled in the art can make various changes and corrections within the scope of the technical idea disclosed in this specification. In addition, in the entire figure used to illustrate the present invention, the components with the same function are marked with the same figure mark, and their repeated descriptions are sometimes omitted. In addition, sometimes for the convenience of explanation, the dimensional ratio of the drawings is different from the actual ratio, or a part of the components is omitted from the drawings. In addition, in the present application, the numerical range represented by the symbol "~" includes each of the numerical values recorded before and after the symbol "~" as the lower limit and upper limit.
[0021] Figure 1 , 2 The lithium-ion secondary battery 100 of the embodiment shown has a battery can 1 and a battery cover 6. The battery can 1 has a rectangular bottom surface 1d, a side surface including a pair of relatively large-area opposed wide side surfaces 1b and a pair of relatively small-area opposed narrow side surfaces 1c, and an opening 1a opened upward at the upper ends of the wide side surfaces 1b and the narrow side surfaces 1c. In this case, the upper side refers to Figure 1 , 2 Z direction.
[0022] The opening 1a of the battery can 1 is sealed by a battery cover 6. The battery cover 6 is in a substantially rectangular flat plate shape, and is welded so as to close the opening 1a of the battery can 1, thereby sealing the battery can 1.
[0023] The battery cover 6 is integrally provided with a gas discharge valve 10. When the pressure in the battery can 1 increases, the gas discharge valve 10 opens to discharge gas from the inside of the battery can 1, thereby reducing the pressure in the battery can 1. Thus, the safety of the lithium ion secondary battery 100 can be ensured.
[0024] The battery cover 6 is provided with a liquid injection port 9 for injecting electrolyte into the battery can 1. The liquid injection port 9 is sealed by a liquid injection plug 11 after the electrolyte is injected into the battery can 1. The liquid injection plug 11 is joined to the battery cover 6 by laser welding, seals the liquid injection port 9, and seals the lithium ion secondary battery 100.
[0025] The battery cover 6 is further provided with a positive electrode side through hole 46 and a negative electrode side through hole 26 .
[0026] A positive electrode external terminal 14 and a negative electrode external terminal 12 are provided above the battery cover 6. A positive electrode collector plate 44 and a negative electrode collector plate 24 are provided below the battery cover 6 and inside the battery can 1.
[0027] Examples of the materials for forming the positive electrode external terminal 14 and the positive electrode current collector plate 44 include aluminum alloys, and examples of the materials for forming the negative electrode external terminal 12 and the negative electrode current collector plate 24 include copper alloys.
[0028] The positive electrode external terminal 14 and the negative electrode external terminal 12 each have a welded joint portion for welding a bus bar or the like. The welded joint portion has a rectangular block shape protruding upward from the battery cover 6. The lower surface of the welded joint portion faces the surface of the battery cover 6, and the upper surface of the welded joint portion is located at a predetermined height and is substantially parallel to the battery cover 6.
[0029] The positive electrode collector plate 44 has a rectangular plate-shaped positive electrode collector plate base 41 facing the lower surface of the battery cover 6, and a positive electrode side connection end 42 extending from the side end of the positive electrode collector plate base 41 along the wide side 1b of the battery can 1 toward the bottom surface 1d. Similarly, the negative electrode collector plate 24 has a rectangular plate-shaped negative electrode collector plate base 21 facing the lower surface of the battery cover 6, and a negative electrode side connection end 22 extending from the side end of the negative electrode collector plate base 21 along the wide side 1b of the battery can 1 toward the bottom surface 1d. The positive electrode side opening hole 43 and the negative electrode side opening hole 23 are formed in the positive electrode collector plate base 41 and the negative electrode collector plate base 21, respectively.
[0030] The positive electrode connecting portion 14a and the negative electrode connecting portion 12a are provided so as to protrude from the lower surfaces of the positive electrode external terminal 14 and the negative electrode external terminal 12. The positive electrode connecting portion 14a and the negative electrode connecting portion 12a are formed integrally with the positive electrode external terminal 14 and the negative electrode external terminal 12, respectively.
[0031] The positive electrode connection part 14a has a cylindrical shape that can be inserted into the positive electrode side through hole 46 of the battery cover 6 and the positive electrode side opening hole 43 of the positive electrode collector plate base 41. Similarly, the negative electrode connection part 12a has a cylindrical shape that can be inserted into the negative electrode side through hole 26 of the battery cover 6 and the negative electrode side opening hole 23 of the negative electrode collector plate base 21. The positive electrode connection part 14a passes through the positive electrode side through hole 46 of the battery cover 6 and the positive electrode side opening hole 43 of the positive electrode collector plate base 41 and penetrates the battery cover 6 and the positive electrode collector plate base 41. The positive electrode external terminal 14 and the positive electrode collector plate 44 are electrically connected via the positive electrode connection part 14a and are fixed to the battery cover 6. Similarly, the negative electrode connection part 12a passes through the negative electrode side through hole 26 of the battery cover 6 and the negative electrode side opening hole 23 of the negative electrode collector plate base 21 and penetrates the battery cover 6 and the negative electrode collector plate base 21. The negative electrode external terminal 12 and the negative electrode current collecting plate 24 are electrically connected via a negative electrode connecting portion 12 a and are fixed to the battery cover 6 .
[0032] The positive external terminal 14 is electrically connected to the winding group 3 described later via the positive electrode connection portion 14a and the positive electrode collector plate 44. Similarly, the negative external terminal 12 is electrically connected to the winding group 3 via the negative electrode connection portion 12a and the negative electrode collector plate 24. When the lithium ion secondary battery 100 is charged, power is supplied from an external power source to the winding group 3 via the positive electrode external terminal 14, the positive electrode connection portion 14a and the positive electrode collector plate 44, and the negative electrode external terminal 12, the negative electrode connection portion 12a and the negative electrode collector plate 24. When the lithium ion secondary battery 100 is discharged, power is supplied from the winding group 3 to an external load via the positive electrode external terminal 14, the positive electrode connection portion 14a and the positive electrode collector plate 44, and the negative electrode external terminal 12, the negative electrode connection portion 12a and the negative electrode collector plate 24.
[0033] In order to electrically insulate the positive electrode collector plate 44, the negative electrode collector plate 24, the positive electrode external terminal 14, and the negative electrode external terminal 12 from the battery cover 6, respectively, a gasket 5 is provided between each of the positive electrode external terminal 14 and the negative electrode external terminal 12 and the battery cover 6, and an insulating plate 7 is provided between each of the positive electrode collector plate 44 and the negative electrode collector plate 24 and the battery cover 6. Examples of the raw materials of the insulating plate 7 and the gasket 5 include insulating resin materials such as polybutylene terephthalate, polyphenylene sulfide, and perfluoroalkoxy fluorine resin.
[0034] The battery can 1 contains the electrolyte EL and the winding group 3. The electrolyte EL is injected into the battery can 1 from the injection port 9. Figure 3 As shown, the winding group 3 has a negative electrode 32, a positive electrode 34 and two separators 33 and 35. The separator 35, the negative electrode 32, the separator 33 and the positive electrode 34 are sequentially overlapped and wound into a flat shape. The separator 35 is located at the outermost periphery of the winding group 3, and the negative electrode 32 is located on the inner side of the separator 35. The two separators 33 and 35 electrically insulate the positive electrode 34 and the negative electrode 32.
[0035] The winding group 3 has a pair of end faces 3a and 3b that are perpendicular to the winding axis and a side face 3c between the pair of end faces 3a and 3b. The side face 3c has a pair of curved portions that are opposite to each other and have a semicircular cross section and a flat portion that is continuously formed between the pair of curved portions. The winding group 3 is arranged in the battery can 1 so that the flat portion of the side face 3c is substantially parallel to the wide side face 1b of the battery can 1.
[0036] Hereinafter, the main parts of the lithium ion secondary battery 100 of the embodiment will be described with the positive electrode 34, the negative electrode 32 and the electrolyte EL as the center. In addition, the "positive electrode mixture layer" is equivalent to the "positive electrode active material layer" of the present invention, and the "negative electrode mixture layer" is equivalent to the "negative electrode active material layer" of the present invention.
[0037] <Positive electrode>
[0038] The positive electrode 34 includes a positive electrode current collector 34a and a positive electrode mixture layer 34b (positive electrode active material layer) provided on at least one surface, preferably both surfaces, of the positive electrode current collector 34a. In the description of the positive electrode, the "positive electrode current collector" may be simply referred to as "current collector".
[0039] The positive electrode collector 34a is formed of any material that has high conductivity and does not alloy with lithium ions. The positive electrode collector 34a can have a plate-like (sheet-like) shape. As the positive electrode collector 34a, for example, a positive electrode foil can be used, specifically, a metal foil such as aluminum foil can be used. A portion 34c (hereinafter referred to as "positive electrode collector exposed portion") that is not covered by the positive electrode mixture layer 34b is provided at an end portion on one side in the width direction of the positive electrode collector 34a. The positive electrode collector exposed portion 34c is provided at the end face 3a of the winding group 3 and its vicinity. The positive electrode collector exposed portion 34c is opposite to and electrically connected to the positive electrode side connection end portion 42 of the positive electrode collector plate 44.
[0040] The positive electrode mixture layer 34b contains a positive electrode active material. As the positive electrode active material, for example, a ternary material containing at least nickel, cobalt and manganese is included. Specifically, a composite oxide of nickel, cobalt and manganese can be used. In addition, as the positive electrode active material, a ternary lithium-containing composite oxide represented by the following composition formula (1) is used as one of the preferred methods.
[0041] Li 1+X M A O2(1)
[0042] (Where X satisfies -0.15≤X≤0.15, M A It represents an element group containing at least one selected from Mn and Al, Ni and Co. )
[0043] The ternary lithium-containing composite oxide represented by the general composition formula (1) has high thermal stability and stability in a high potential state, and the use of this oxide can improve the safety and various battery characteristics of lithium-ion secondary batteries.
[0044] The positive electrode mixture layer 34 b may further contain at least one of a conductive additive and a binder, and preferably contains both.
[0045] As the conductive auxiliary agent, there is no particular limitation, for example, a carbon-based material can be used. The carbon-based material can be crystalline carbon, amorphous carbon, or a mixture thereof. As an example of crystalline carbon, artificial graphite, natural graphite (e.g., flaky graphite), or a mixture thereof can be cited. As an example of amorphous carbon, carbon black (e.g., acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, or a mixture thereof) can be cited.
[0046] The binder is not particularly limited, and for example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyethylene, polystyrene, polybutadiene, polyacrylonitrile, polyvinyl fluoride, polypropylene fluoride, polychloroprene fluoride, butyl rubber, nitrile rubber, styrene butadiene rubber (SBR), polysulfide rubber, nitrocellulose, cyanoethyl cellulose, various latexes, acrylic resins, or mixtures thereof can be used.
[0047] The positive electrode 34 can be formed, for example, as follows. The positive electrode active material and at least one of the arbitrarily selected conductive aids and binders are dispersed in a solvent (for example, N-methyl-2-pyrrolidone (NMP), water) to prepare a paste or slurry positive electrode mixture composition. The positive electrode mixture composition is applied to the surface (one side or both sides) of the positive electrode collector 34a, dried, and calendered as needed to form a positive electrode mixture layer 34b. Thus, the positive electrode 34 is obtained. However, the positive electrode is not necessarily limited to the positive electrode formed by the above method, and may also be a positive electrode formed by other methods.
[0048] <Negative electrode>
[0049] The negative electrode 32 includes a negative electrode current collector 32a and a negative electrode mixture layer 32b (negative electrode active material layer) provided on at least one side, preferably both sides, of the negative electrode current collector 32a. In the description of the negative electrode, the "negative electrode current collector" is sometimes referred to as simply "current collector".
[0050] The negative electrode current collector 32a is formed of any material that has high conductivity and does not alloy with lithium ions. A portion 32c (hereinafter referred to as "negative electrode current collector exposed portion") not covered by the negative electrode mixture layer 32b is provided at one end portion in the width direction of the negative electrode current collector 32a. The negative electrode current collector exposed portion 32c is provided at and near the end surface 3b of the winding group 3. The negative electrode current collector exposed portion 32c is opposite to and electrically connected to the negative electrode side connection end portion 22 of the negative electrode current collector plate 24.
[0051] The portion of the negative electrode 32 coated with the negative electrode mixture layer 32b is larger in the width direction than the portion of the positive electrode 34 coated with the positive electrode mixture layer 34b, and thus, the portion coated with the positive electrode mixture layer 34b is preferably configured to be sandwiched by the portion coated with the negative electrode mixture layer 32b. One of the preferred methods is to bundle the positive electrode collector exposed portion 34c and the negative electrode collector exposed portion 32c in the plane portion and connect them by welding or the like. In addition, the separators 33 and 35 are wider in the width direction than the portion coated with the negative electrode mixture layer 32b, but because they are wound around the positions where the collectors are exposed at the ends of the positive electrode collector exposed portion 34c and the negative electrode collector exposed portion 32c, they will not become obstacles when bundling and welding.
[0052] The negative electrode mixture layer 32b includes a negative electrode active material containing graphite particles and amorphous carbon particles. As the negative electrode active material, there is no particular limitation as long as it contains graphite particles and amorphous carbon particles, but it is preferred that the amorphous carbon particles are supported on the graphite particles, wherein the graphite particles preferably contain graphite particles (A) and graphite particles (B) supported with the amorphous carbon particles.
[0053] In addition to the negative electrode active material, the negative electrode mixture layer 32b may also contain at least one of a negative electrode additive and a binder, preferably both. In one embodiment, the negative electrode mixture layer 32b contains a negative electrode active material containing graphite particles (A) and graphite particles (B) carrying amorphous carbon particles, and the number of amorphous carbon particles per unit area in the graphite particles (B) carrying amorphous carbon particles is 0.4 particles / μm 2 In another embodiment, the negative electrode mixture layer 32b includes a negative electrode active material and a binder for retaining the negative electrode active material, and the negative electrode active material includes graphite particles and amorphous carbon particles. In addition, the negative electrode mixture layer 32b may further include a negative electrode additive including copper oxide.
[0054] The graphite particles are not particularly limited, and for example, natural graphite particles and artificial graphite particles can be cited, preferably natural graphite particles. As natural graphite, for example, flaky graphite, blocky graphite, and earthy graphite can be cited. The graphite particles constituting the graphite particles (A) and the graphite particles (B) carrying amorphous carbon particles can be the same type of graphite particles or different types of graphite particles.
[0055] Examples of negative electrode active materials other than graphite include carbon-based materials such as hardly graphitizable carbon (hard carbon) and easily graphitizable carbon (soft carbon).
[0056] Graphite can also use graphite obtained by coating the graphite surface with amorphous carbon. By coating with amorphous carbon, it is possible to prevent reaction with an excessive amount of electrolyte. As amorphous carbon, for example, asphalt can be cited. That is, the graphite particles constituting the graphite particles (A) and the graphite particles (B) carrying amorphous carbon particles are preferably graphite particles coated with amorphous carbon, more preferably particles of asphalt-coated graphite. In addition, the graphite particles constituting the graphite particles (A) and the graphite particles (B) carrying amorphous carbon particles are particularly preferably natural graphite particles coated with amorphous carbon.
[0057] The amorphous carbon particles carried by the graphite particles (B) carrying amorphous carbon particles are not particularly limited, and examples thereof include carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black. In addition, the amorphous carbon particles carried refer to particles of amorphous carbon dispersed on the surface of the graphite particles, which are different from the amorphous carbon coated graphite particles as described above. The amorphous carbon coated graphite particles refers to amorphous carbon covering all or part of the surface of the graphite particles.
[0058] In the graphite particles (B) carrying amorphous carbon particles, the number of amorphous carbon particles per unit area is 0.4 particles / μm 2 The number of amorphous carbon particles per unit area is preferably 0.4 particles / μm 2 ~2.4 / μm 2 The number of amorphous carbon particles per unit area is more preferably 0.8 particles / μm 2 ~2.0 / μm 2 In addition, when the graphite particles carry a small amount of amorphous carbon particles, that is, the number of amorphous carbon particles per unit area is less than 0.4 particles / μm 2 When the number of amorphous carbon particles per unit area is less than 0.4 / μm, the graphite particles carrying amorphous carbon particles do not belong to the graphite particles (B). 2 When the graphite particles (A) are used, graphite particles carrying amorphous carbon fine particles may also be used.
[0059] The average particle size of the graphite particles (A) is preferably 4 μm or more and 12 μm or less, and more preferably 5 μm or more and 10 μm or less.
[0060] The average particle size of the graphite particles (B) carrying amorphous carbon particles is preferably 4 μm to 12 μm, more preferably 5 μm to 10 μm. In addition, the average particle size of the graphite particles (A) and the average particle size of the graphite particles (B) carrying amorphous carbon particles may be the same or different.
[0061] The average particle size of the amorphous carbon particles carried by the graphite particles (B) carrying the amorphous carbon particles is preferably smaller than the average particle size of the graphite particles (A) and the average particle size of the graphite particles that constitute the graphite particles (B) carrying the amorphous carbon particles. The average particle size of the amorphous carbon particles is preferably 0.05 μm to 0.5 μm, and more preferably 0.1 μm to 0.4 μm.
[0062] As the negative electrode active material containing graphite particles (A) and graphite particles carrying amorphous carbon fine particles (B), for example, Figure 4As shown, preferably, graphite particles (A) 50 not carrying amorphous carbon particles and graphite particles (B) 52 carrying amorphous carbon particles (amorphous carbon particles 56 are carried on graphite particles 54) are present in the negative electrode active material layer in a mixed state. Figure 4 In the above description, description of components constituting the negative electrode active material layer other than the graphite particles (A) and the graphite particles (B) carrying amorphous carbon fine particles is omitted.
[0063] When the negative electrode active material contains graphite particles (A) and graphite particles (B) carrying amorphous carbon particles, their mass ratio (graphite particles (A) / graphite particles (B) carrying amorphous carbon particles) is preferably greater than 0.25 and less than 5, and more preferably greater than 0.5 and less than 2.
[0064] In addition, as the negative electrode active material, for example, a material obtained by mixing carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, etc. into a graphite material as a conductive aid, a composite material obtained by coating with amorphous carbon after mixing these conductive aids into a graphite material, or a material obtained by mixing difficult graphitization carbon (hard carbon) and easy graphitization carbon (soft carbon) into a graphite material. The shape of the negative electrode active material is not particularly limited, and for example, it can have a spherical, flaky, fibrous shape or a shape obtained by crushing them.
[0065] The inventors of the present invention have repeatedly conducted in-depth research and found that by using a negative electrode active material containing graphite particles (A) and graphite particles (B) carrying amorphous carbon particles, a lithium-ion secondary battery can ensure the capacity of the battery while reducing the internal resistance in a wide range from a low SOC region to a high SOC region, thereby having high output and good storage characteristics.
[0066] In addition, the inventors have repeatedly conducted in-depth research and found that the negative electrode active material includes a negative electrode active material containing graphite particles and amorphous carbon particles, and the negative electrode active material layer has a negative electrode active material and a binder for retaining the negative electrode active material. The lithium ion secondary battery can ensure the capacity of the battery and reduce the internal resistance in a wide range from the low SOC region to the high SOC region. Therefore, it has high output and good storage characteristics.
[0067] As the negative electrode active material layer, it is preferred to contain copper oxide as a negative electrode additive. By containing 0.5% to 15% by mass of copper oxide relative to the total 100% by mass of the negative electrode active material and copper oxide, the lithium ion secondary battery can more appropriately ensure the capacity of the battery, and at the same time can reduce the internal resistance in a wide range from the low SOC region to the high SOC region, so that it can have high output and good storage characteristics, so it is preferred.
[0068] Copper oxide is contained as a negative electrode additive. The copper oxide may be copper (I) oxide (Cu2O), copper (II) oxide (CuO), or a mixture thereof. That is, the copper oxide may be at least one copper oxide selected from Cu2O and CuO. The negative electrode additive may be granular. The shape of the granular negative electrode additive is not particularly limited, and may have, for example, a spherical, flaky, fibrous shape, or a shape obtained by crushing them. The granular negative electrode additive may be a particle containing copper (I) oxide (Cu2O), copper (II) oxide (CuO), or a mixture thereof, or may be a particle substantially composed of copper (I) oxide (Cu2O), copper (II) oxide (CuO), or a mixture thereof. These various granular negative electrode additives may be used alone or in combination.
[0069] In the negative electrode mixture layer 32b, the negative electrode active material and the negative electrode additive can exist as separate particles that are not composited with each other. As a result, the negative electrode active materials can be well electrically connected to each other without being hindered by the negative electrode additive with high resistance, and the increase in the internal resistance of the lithium-ion secondary battery can be suppressed. The negative electrode additive can have an average particle size smaller than the average particle size of the negative electrode active material, and can have an average particle size of 1μm to 10μm. As a result, the negative electrode active materials can be well electrically connected to each other without being hindered by the negative electrode additive with high resistance, and therefore, the increase in the internal resistance of the lithium-ion secondary battery can be suppressed. The average particle size of the negative electrode active material (such as graphite particles, amorphous carbon particles, etc.) and the negative electrode additive is obtained based on the SEM observation image.
[0070] As the binder of the negative electrode mixture layer 32 b , the same material as exemplified as the binder that can be used as the positive electrode mixture layer 34 b can be used.
[0071] The negative electrode mixture layer 32b may further contain a dispersant. As the dispersant, carboxymethyl cellulose (CMC) can be used.
[0072] The negative electrode 32 can be formed, for example, as follows. First, prepare a negative electrode active material and a negative electrode additive containing copper oxide, a binder, and an arbitrarily selected dispersant. The negative electrode active material and the negative electrode additive can be in a granular form. The negative electrode active material and the negative electrode additive can be separate particles that are not composited with each other. The negative electrode active material, the negative electrode additive, the binder, and an arbitrarily selected dispersant are dispersed in a solvent (for example, N-methyl-2-pyrrolidone (NMP), water) to prepare a paste or slurry-like negative electrode mixture composition. The negative electrode mixture composition is applied to the surface (one side or both sides) of the negative electrode collector 32a, dried, and subjected to a rolling treatment as needed to form a negative electrode mixture layer 32b. Thus, the negative electrode 32 is obtained. However, the negative electrode is not necessarily limited to the negative electrode formed by the above-mentioned method, and can also be a negative electrode formed by other methods.
[0073] <Electrolyte>
[0074] The electrolyte (non-aqueous electrolyte) EL of the lithium-ion secondary battery 100 contains at least a non-aqueous solvent, an electrolyte salt and an additive, and the additive contains a fluorosulfonate and a methoxysulfonate. Since the electrolyte contains a non-aqueous solvent and an electrolyte salt, and also contains a fluorosulfonate and a methoxysulfonate as additives, the protective film called SEI (Solid Electrolyte Interface) formed on the surface of the negative electrode active material of the negative electrode is strengthened, and even in a high-temperature storage environment, the side reactions caused at the interface between the electrolyte and the negative electrode active material can be suppressed. Therefore, by using the electrolyte and the above-mentioned negative electrode in combination, it is possible to take into account both the improvement of the output characteristics in the low SOC region and the improvement of the high-temperature storage characteristics.
[0075] Hereinafter, the additives, electrolyte salt, and non-aqueous solvent according to the embodiment will be described in detail.
[0076] 1. Additives
[0077] The additive contains fluorosulfonate and methoxysulfonate. Here, fluorosulfonate and methoxysulfonate are described.
[0078] a. Fluorosulfonate
[0079] The fluorosulfonate is represented by the following general composition formula (2).
[0080] X1(FSO3) n (2)
[0081] (Wherein, X1 represents the counter cation of the fluorosulfonate, and n represents the valence of the counter cation.)
[0082] The counter cation of the fluorosulfonate is not particularly limited, and examples thereof include lithium, sodium, and potassium.
[0083] Specific examples of fluorosulfonates include lithium fluorosulfonate (FSO3Li), sodium fluorosulfonate, potassium fluorosulfonate, and the like, with lithium fluorosulfonate being particularly preferred. Lithium fluorosulfonate is represented by the following structural formula (2-1).
[0084]
[0085] Fluorosulfonate can be used alone or in combination of two or more in any ratio. The content of fluorosulfonate contained in the electrolyte is, for example, 0.001% by mass or more, preferably 0.1% by mass or more, and more preferably 0.3% by mass or more. In addition, the content of fluorosulfonate contained in the electrolyte is, for example, 3% by mass or less, preferably 2% by mass or less, and more preferably 1.5% by mass or less. If it is within this range, it is easy to show the effect of improving the high temperature storage characteristics of the lithium ion secondary battery, and the expansion of the battery caused by the increase in gas generation can be avoided.
[0086] b. Methoxysulfonate
[0087] The methoxysulfonate is represented by the following general composition formula (3).
[0088] X2(CH3OSO3) m (3)
[0089] (Wherein, X2 represents the counter cation of methoxysulfonate, and m represents the valence of the counter cation.)
[0090] The counter cation of the methoxysulfonate is not particularly limited, and examples thereof include lithium, sodium, and potassium.
[0091] Specific examples of methoxysulfonates include lithium methoxysulfonate (CH3OSO3Li), sodium methoxysulfonate, potassium methoxysulfonate, and the like, with lithium methoxysulfonate being particularly preferred. Lithium methoxysulfonate is represented by the following structural formula (3-1).
[0092]
[0093] Methoxysulfonate can be used alone or in combination of two or more in any ratio. The content of methoxysulfonate (e.g., lithium methoxysulfonate) contained in the electrolyte is, for example, 0.001% by mass or more, preferably 0.1% by mass or more. In addition, the content of methoxysulfonate (e.g., lithium methoxysulfonate) contained in the electrolyte is, for example, 1% by mass or less, preferably 0.8% by mass or less, more preferably 0.5% by mass or less. If it is such a range, it is easy to show the improvement effect of the high temperature storage characteristics of the lithium ion secondary battery, and it can be uniformly dissolved in the electrolyte.
[0094] c. Others
[0095] The additive is not particularly limited as long as it contains a fluorosulfonate and a methoxysulfonate, but preferably further contains a lithium borate and a difluorophosphate, and particularly preferably further contains a vinylene carbonate compound.
[0096] (a) Lithium borate
[0097] Specific types of lithium borates include lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), etc., and LiBOB is particularly preferred. Lithium bis(oxalatoborate) (LiBOB) is represented by the following structural formula (4-1). Lithium difluorooxalatoborate (LiDFOB) is represented by the following structural formula (4-2).
[0098]
[0099] Lithium borate can be used alone or in combination of two or more in any ratio. The content of lithium borate contained in the electrolyte is, for example, 0.001% by mass or more, preferably 0.1% by mass or more, and more preferably 0.4% by mass or more. In addition, the content of lithium borate contained in the electrolyte is, for example, 3% by mass or less, preferably 2% by mass or less, and more preferably 1% by mass or less. If it is within this range, it is easy to show the effect of improving the high temperature storage characteristics of the lithium ion secondary battery, and the increase in negative electrode resistance caused by excessive addition can be avoided.
[0100] (b) Difluorophosphate
[0101] The difluorophosphate is represented by the following general composition formula (5).
[0102] X3(F2PO2) k (5)
[0103] (Wherein, X3 represents the counter cation of the fluorosulfonate, and k represents the valence of the counter cation.)
[0104] The counter cation of the difluorophosphate is not particularly limited, and examples thereof include lithium, sodium, and potassium.
[0105] Specific examples of difluorophosphates include lithium difluorophosphate (LiPO2F2), sodium difluorophosphate, potassium difluorophosphate, and the like, with lithium difluorophosphate being particularly preferred. Lithium difluorophosphate is represented by the following structural formula (5-1).
[0106]
[0107] Difluorophosphate can be used alone or in combination of two or more in any ratio. The content of difluorophosphate contained in the electrolyte is, for example, 0.001% by mass or more, preferably 0.1% by mass or more, and more preferably 0.5% by mass or more. In addition, the content of difluorophosphate contained in the electrolyte is, for example, 3% by mass or less, preferably 2% by mass or less, and more preferably 1% by mass or less. If this range, it is easy to show the improvement effect of the high temperature storage characteristics of the lithium ion secondary battery.
[0108] (c) Vinylene carbonate compounds
[0109] Specific types of the vinylene carbonate compound include, for example, vinylene carbonate (1,3-dioxol-2-one), methyl vinylene carbonate (4-methyl-1,3-dioxol-2-one), and ethyl vinylene carbonate (4-ethyl-1,3-dioxol-2-one).
[0110] The vinylene carbonate compound can be used alone or in combination of two or more in any ratio. Among them, vinylene carbonate (C3H2O3) can obtain excellent effects and is therefore particularly preferred. Vinylene carbonate is represented by the following structural formula (6-1).
[0111]
[0112] The content of the vinylene carbonate compound contained in the electrolyte is, for example, more than 0.001 mass %, preferably more than 0.1 mass %, more preferably more than 0.4 mass %. In addition, the content of the vinylene carbonate compound contained in the electrolyte is, for example, below 3 mass %, preferably below 2 mass %, more preferably below 1 mass %. If this scope, then easily show the raising effect of the high temperature storage characteristic of lithium ion secondary battery, can avoid the expansion of the battery caused by the increase of gas generation amount.
[0113] 2. Electrolyte Salts
[0114] In the electrolyte, at least one electrolyte salt is dissolved in a non-aqueous solvent. The electrolyte salt is a lithium salt, and as the lithium salt, for example, a lithium salt containing fluorine (fluorine-containing lithium salt) is preferred. As specific types of fluorine-containing lithium salts, inorganic anion salts such as lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4), organic anion salts such as lithium trifluoromethanesulfonate (LiCF3SO3), etc. can be cited, among which LiPF6 is particularly preferred.
[0115] The lithium salt may be used alone or in combination of two or more in any ratio. The content of the lithium salt contained in the electrolyte is, as long as it does not significantly damage the effect of the present invention, for example, 0.01% by mass or more, preferably 0.1% by mass or more. In addition, the content of the lithium salt contained in the electrolyte is, for example, 30% by mass or less, preferably 20% by mass or less.
[0116] 3. Non-aqueous solvents
[0117] The electrolyte solution contains at least one non-aqueous solvent. Specific examples of the non-aqueous solvent include cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates.
[0118] As the specific type of cyclic carbonate, for example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) etc. can be mentioned. As the specific type of fluorine-containing cyclic carbonate, for example, fluoroethylene carbonate (FEC) etc. can be mentioned. As the specific type of linear carbonate, for example, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) etc. can be mentioned.
[0119] The non-aqueous solvent can be used alone or in combination of two or more in any ratio. From the perspective of the dielectric constant of the electrolyte and the balance of viscosity, it is preferred that the non-aqueous solvent contains at least a cyclic carbonate and a linear carbonate. Specifically, it is preferred that the non-aqueous solvent contains at least one solvent of the cyclic carbonate and at least one solvent of the linear carbonate. In this case, the ratio of the cyclic carbonate and the linear carbonate contained in the non-aqueous solvent is preferably 10:90 to 50:50 by volume. Furthermore, as the non-aqueous solvent, it is preferred to contain ethylene carbonate as the cyclic carbonate, and contain ethyl methyl carbonate and dimethyl carbonate as the linear carbonate.
[0120] <Other>
[0121] The separators 33 and 35 have an insulating function to prevent a short circuit between the positive electrode 34 and the negative electrode 32, and a function to retain the electrolyte. The separators 33 and 35 are not particularly limited, and for example, a porous sheet made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, polyamide, or a laminated sheet thereof (for example, a three-layer structure sheet of PP / PE / PP) can be used.
[0122] A layer containing an inorganic material (e.g., alumina particles) and an adhesive may also be provided on one or both sides of the separator 33, 35. Thus, even when the lithium-ion secondary battery 100 is used in an abnormal state (e.g., when the temperature of the lithium-ion secondary battery rises to 160°C or more due to overcharging or crushing), the separator 33, 35 can be prevented from melting and the insulation function can be maintained. Therefore, the safety of the lithium-ion secondary battery 100 is improved.
[0123] If necessary, a core (not shown) may be disposed at the innermost periphery of the winding group 3. As the core, a resin sheet having a higher bending rigidity than any of the positive electrode collector, the negative electrode collector, and the separators 33 and 35 may be used.
[0124] An insulating protective film (not shown) may be optionally wound on the winding group 3. The insulating protective film is not particularly limited, and is composed of, for example, a sheet or a plurality of film members made of a synthetic resin such as PP (polypropylene), and has a length that allows it to be wound with a direction parallel to the flat surface of the winding group 3 and perpendicular to the winding axis direction as the winding center.
[0125] Example
[0126] Hereinafter, the present invention will be specifically described by way of Examples, but the present invention is not limited to these Examples.
[0127] [Example 1]
[0128] First, prepare Li as the positive electrode active material. 1.0 Ni 0.33 Co 0.33 Mn 0.33 O2 powder, acetylene black as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder.
[0129] Next, the positive electrode active material, the conductive aid, and the binder were mixed at a mass ratio of 90:5:5. N-methyl-2-pyrrolidone (NMP) was added to the obtained mixture to adjust the viscosity, thereby obtaining a positive electrode slurry (a positive electrode mixture composition in a slurry form).
[0130] Next, as the positive electrode current collector 34a, an aluminum foil with a thickness of 15 μm was prepared. Next, the uncoated portion that became the welding portion (positive electrode current collector exposed portion 34c) was left on both sides of the positive electrode current collector 34a, and the positive electrode slurry was used in a slot die coating method to form a layer of positive electrode slurry by double-layer simultaneous coating. Next, the layer of positive electrode slurry was dried and pressed to form a positive electrode mixture layer 34b, and a positive electrode mixture layer 34b was prepared. Figure 3 The positive electrode 34 is shown.
[0131] Next, as negative electrode active materials, natural graphite particles coated with amorphous carbon (negative electrode active material A) and natural graphite particles coated with amorphous carbon carrying amorphous carbon particles (negative electrode active material B) are prepared, styrene butadiene rubber (SBR) is prepared as a binder, and carboxymethyl cellulose (CMC) is prepared as a dispersant.
[0132] Next, the negative electrode active material A and the negative electrode active material B, the binder, and the dispersant are mixed in a mass ratio of 98:1:1 of the total of the negative electrode active material A and the negative electrode active material B: the binder: the dispersant. The contents of the negative electrode active material A and the negative electrode active material B (a total of 98% by mass) and the specifications are shown in Table 1 below. Ion exchange water is added to the obtained mixture to adjust the viscosity to obtain a negative electrode slurry (a negative electrode mixture composition in a slurry state).
[0133] Next, a copper foil with a thickness of 10 μm is prepared as the negative electrode current collector 32a. Next, the negative electrode slurry is applied by slit die coating, with the uncoated portion (negative electrode current collector exposed portion 32c) remaining on both sides of the negative electrode current collector 32a, and a negative electrode slurry layer is formed by double-layer simultaneous coating. Next, the negative electrode slurry layer is dried and pressed to form a negative electrode mixture layer 32b, and a negative electrode mixture layer 32b is produced. Figure 3 The negative electrode 32 is shown.
[0134] Next, separators 33 and 35 are sandwiched between the positive electrode 34 and the negative electrode 32. Figure 3 The winding group 3 is made of the structure shown in the figure. The positive electrode collector plate 44 and the positive electrode side connection end 42 and the negative electrode side connection end 22 of the negative electrode collector plate 24 connected to the battery cover 6 are welded to the uncoated part (positive electrode collector exposed part 34c, negative electrode collector exposed part 32c) of the winding group 3, and the winding group 3 is covered with an insulating protective film (not shown), and the winding group 3 is sealed in the battery can 1, and the battery cover 6 and the battery can 1 are welded (refer to Figure 1 and Figure 2 ).
[0135] Next, a non-aqueous solvent containing cyclic carbonate (ethylene carbonate (EC)) and chain carbonate (ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC)) is prepared, and the ratio of the cyclic carbonate to the chain carbonate is 30:70 by volume ratio. Next, an electrolyte solution is prepared by dissolving LiPF6 as an electrolyte salt, FSO3Li (fluorosulfonate), CH3OSO3Li (methoxysulfonate), LiBOB (lithium borate), LiPO2F2 (difluorophosphate) and VC (vinylene carbonate (C3H2O3)) as additives in the non-aqueous solvent. At this time, as shown in Table 1 below, the content of LiPF6 (electrolyte salt) contained in the electrolyte was 1.2 mol / L, the content of FSO3Li contained in the electrolyte was 1.0 mass%, the content of CH3OSO3Li contained in the electrolyte was 0.5 mass%, the content of LiBOB contained in the electrolyte was 0.4 mass%, the content of LiPO2F2 contained in the electrolyte was 1.0 mass%, and the content of VC contained in the electrolyte was 0.4 mass%. Next, the prepared electrolyte was injected into the battery can 1 from the injection port 9 of the battery cover 6, and the injection port 9 was sealed with the injection plug 11 to produce the lithium ion secondary battery 100.
[0136] [Examples 2 and 3 and Comparative Examples 1 and 2]
[0137] A lithium ion secondary battery 100 was produced by the same method as in Example 1 except that the content of each additive contained in the electrolytic solution was changed as shown in Table 1 below.
[0138] [evaluate]
[0139] The lithium ion secondary batteries prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were initialized by charge and discharge, and then evaluated for various characteristics by the following methods. The evaluation results are shown in Table 2 below.
[0140] <Obtaining SOC-Open Circuit Voltage (OCV) Curve>
[0141] In a lithium-ion secondary battery placed in a thermostatic chamber at 25°C, the battery capacity was discharged from 4.2V to 5% of the battery capacity at a discharge current of 1C, and the voltage after 1 hour of discharge was set as OCV to obtain a SOC-open circuit voltage (OCV) curve.
[0142] <Evaluation of output characteristics in the low SOC region at low temperatures>
[0143] First, in a lithium-ion secondary battery placed in a constant temperature chamber at 25°C, constant voltage-constant current charging (CC-CV charging) is performed from SOC0% to SOC25% with a charging current of 1C according to the relationship of the SOC-OCV curve. Next, the lithium-ion secondary battery is left to stand in a constant temperature chamber at -10°C for 5 hours. Then, the lithium-ion secondary battery is discharged at a constant current of 9C for 10 seconds, and the voltage drop value caused by the discharge is measured. Then, the discharge DC resistance (DCR) at SOC25% is obtained based on the measured voltage drop value. The DCR (relative value) at SOC25% of the lithium-ion secondary battery of each embodiment and each comparative example, in which the DCR of the lithium-ion secondary battery of Comparative Example 1 at SOC25% is standardized to 100, is shown in the following Table 2. In addition, the smaller the value of DCR, the better. The smaller the value of DCR at SOC25%, the lower the internal resistance of the lithium-ion secondary battery in the low SOC region.
[0144] <Evaluation of characteristics before and after high-temperature storage>
[0145] First, in a lithium ion secondary battery placed in a thermostatic chamber at 25°C, CC-CV charging was performed for 2.5 hours at a charging current of 1C until the battery voltage reached 4.2V. Then, after a 30-minute pause, constant current discharge (CC discharge) was performed at a discharge current of 1C until the battery voltage reached 2.8V, and the capacity (initial capacity) before high-temperature storage was obtained. The capacity (relative value) before high-temperature storage of the lithium ion secondary battery of each embodiment and each comparative example, with the capacity (initial capacity) before high-temperature storage of the lithium ion secondary battery of Comparative Example 1 being standardized to 100, is shown in the following Table 2. Furthermore, in a lithium ion secondary battery placed in a thermostatic chamber at 25°C, CC-CV charging was performed at a charging current of 1C from SOC0% to SOC50% according to the relationship of the SOC-OCV curve. Then, after a 30-minute pause, the lithium ion secondary battery was discharged at a constant current of 30C for 10 seconds, and the voltage drop value caused by the discharge was measured. The DCR at SOC50% before high-temperature storage was obtained based on the measured voltage drop value. Table 2 below shows the DCR (relative value) at SOC 50% of the lithium ion secondary batteries of each Example and each Comparative Example before high-temperature storage, with the DCR at SOC 50% of the lithium ion secondary battery of Comparative Example 1 before high-temperature storage being normalized to 100.
[0146] Next, in the lithium-ion secondary battery placed in a constant temperature chamber at 25°C, CC-CV charging is performed at a charging current of 1C from SOC0% to SOC80% according to the relationship of the SOC-OCV curve. Next, the lithium-ion secondary battery is moved to a constant temperature chamber at 70°C and kept for 100 days, and then the lithium-ion secondary battery is taken out of the constant temperature chamber at 70°C and moved to a constant temperature chamber at 25°C. Then, constant current discharge (CC discharge) is performed with a discharge current of 1C until the battery voltage reaches 2.8V. On this basis, in the lithium-ion secondary battery placed in a constant temperature chamber at 25°C, CC-CV charging is performed for 2.5 hours with a charging current of 1C until the battery voltage reaches 4.2V. Then, after pausing for 30 minutes, constant current discharge (CC discharge) is performed with a discharge current of 1C until the battery voltage reaches 2.8V, and the capacity after high-temperature storage is obtained. The capacity (relative value) of the lithium ion secondary battery after high temperature storage of each embodiment and each comparative example is standardized as 100. Furthermore, in the lithium ion secondary battery arranged in a constant temperature chamber at 25°C, CC-CV charging is performed at a charging current of 1C from SOC0% to SOC50% according to the relationship of the SOC-OCV curve. Then, after pausing for 30 minutes, the lithium ion secondary battery is discharged at a constant current of 30C for 10 seconds, and the voltage drop value caused by the discharge is measured. The DCR at SOC50% after high temperature storage is obtained from the measured voltage drop value. The DCR (relative value) of the lithium ion secondary battery after high temperature storage of each embodiment and each comparative example is standardized as 100. The DCR at SOC50% after high temperature storage of each embodiment and each comparative example is shown in the following Table 2.
[0147] [Table 1]
[0148]
[0149] [Table 2]
[0150]
[0151] <Investigation>
[0152] The composition and evaluation results of the electrolyte of the lithium ion secondary battery of each embodiment and each comparative example are shown in Table 1 and Table 2. As shown in Table 1 and Table 2, in Embodiments 1 and 2, it is taught that both the reduction of DCR in the low SOC region and the improvement of high temperature storage characteristics (capacity retention rate and DCR retention rate) can be achieved. On the other hand, in Comparative Examples 1 and 2, the high temperature storage characteristics are reduced, and it is believed that the reduction of DCR in the low SOC region and the improvement of high temperature storage characteristics cannot be achieved.
[0153] Therefore, by using the electrolyte solution of the present invention as the electrolyte solution of a lithium ion secondary battery, it is possible to provide a lithium ion secondary battery having high output in a low SOC region and excellent high temperature storage characteristics.
[0154] As long as one is skilled in the art, the above description can be used to maximize the use of the present invention. It should be understood that the scope of the claims and the embodiments disclosed in this specification are only illustrative and exemplary, and do not limit the scope of the present invention in any sense. With the assistance of the present invention, the details of the above embodiments can be changed without departing from the basic principles of the present invention. In other words, various changes and improvements to the embodiments specifically disclosed in the above description are within the scope of the present invention.
[0155] Description of Reference Numerals
[0156] 1: Battery can; 1a: Opening; 1b: Wide side; 1c: Narrow side; 1d: Bottom; 3: Winding group; 5: Sealing gasket; 6: Battery cover; 7: Insulating plate; 9: Liquid filling port; 10: Gas discharge valve; 11: Liquid filling plug; 12: Negative external terminal; 12a: Negative connection; 14: Positive external terminal; 14a: Positive connection; 21: Negative collector plate base; 22: Negative side connection end; 23: Negative side opening hole; 24: Negative collector plate; 26: Negative side through hole; 32: Negative electrode; 32a: Negative collector ; 32b: negative electrode mixture layer; 32c: exposed portion of negative electrode collector; 33: diaphragm; 34: positive electrode; 34a: positive electrode collector; 34b: positive electrode mixture layer; 34c: exposed portion of positive electrode collector; 35: diaphragm; 41: positive electrode collector plate base; 42: positive electrode side connecting end; 43: positive electrode side opening hole; 44: positive electrode collector plate; 46: positive electrode side through hole; 50: graphite particles (A); 52: graphite particles carrying amorphous carbon particles (B); 54: graphite particles; 56: amorphous carbon particles; 100: lithium-ion secondary battery.
Claims
1. A lithium ion secondary battery, characterized in that: It has a positive electrode, a negative electrode and an electrolyte. The negative electrode comprises a current collector and a negative electrode active material layer provided on at least one surface of the current collector. The negative electrode active material layer includes a negative electrode active material including graphite particles and amorphous carbon particles. The electrolyte contains at least a non-aqueous solvent, an electrolyte salt and an additive. The additives contain fluorosulfonate and methoxysulfonate.
2. The lithium ion secondary battery according to claim 1, wherein: The additive also contains lithium borate and difluorophosphate.
3. The lithium ion secondary battery according to claim 2, characterized in that: The lithium borate is lithium bis(oxalatoborate) (LiBOB), and the difluorophosphate is lithium difluorophosphate.
4. The lithium ion secondary battery according to claim 2 or 3, characterized in that: The additive further contains a vinylene carbonate compound.
5. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The non-aqueous solvent contains at least a cyclic carbonate and a chain carbonate, and the content ratio of the cyclic carbonate to the chain carbonate contained in the non-aqueous solvent is 10:90 to 50:50 in terms of volume ratio.
6. The lithium ion secondary battery according to claim 5, characterized in that: The nonaqueous solvent contains ethylene carbonate as the cyclic carbonate, and contains ethyl methyl carbonate and dimethyl carbonate as the chain carbonate.
7. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The electrolyte salt is lithium hexafluorophosphate.
8. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The content of the fluorosulfonate contained in the electrolyte is 0.3 mass % to 1.5 mass %.
9. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The content of the methoxysulfonate salt contained in the electrolytic solution is 0.5 mass % or less.
10. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The amorphous carbon particles are supported on the graphite particles.
11. The lithium ion secondary battery according to claim 10, characterized in that: The negative electrode active material contains graphite particles (A) and graphite particles (B) carrying the amorphous carbon fine particles as the graphite particles.
12. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The average particle size of the amorphous carbon fine particles is 0.05 μm or more and 0.5 μm or less.
13. The lithium ion secondary battery according to any one of claims 1 to 3, characterized in that: The positive electrode comprises a current collector and a positive electrode active material layer provided on at least one surface of the current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a ternary material containing at least nickel, cobalt, and manganese.