Cooking container and method for manufacturing cooking container

By forming two protective layers on the inner surface of the cooking container and removing impurities, the problem of unstable connection of multiple non-stick coatings is solved, which significantly improves the durable non-stickness and initial non-stickness, and improves the use effect of the container.

CN119055094APending Publication Date: 2024-12-03JOYOUNG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411364838.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The connection between the multi-layer non-stick coatings of existing cooking containers is not stable enough, resulting in insufficient non-stickness. Especially when external objects such as spatulas are impacted, the surface layer is prone to fall off, affecting the long-lasting non-stickness.

Method used

By forming two protective layers on the inner surface of the cooking container, a direct bonding connection is made between the first protective layer and the second protective layer, and removing impurities in the cleaning step to improve adhesion stability, ensuring that between the two protective layers close contact.

Benefits of technology

Improves the long-lasting non-stickness and initial non-stickness of the cooking container, reduces the fall of the non-stick coating, and significantly improves the service life and non-stick effect of the container.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119055094A_ABST
    Figure CN119055094A_ABST
Patent Text Reader

Abstract

The invention discloses a cooking container and a manufacturing method of the cooking container. A cooking cavity of the cooking container is covered with a protective layer, and the protective layer comprises a first protective layer connected to the surface of the cooking cavity; the second protection layer covers the first protection layer, the projection parts of the second protection layer and the first protection layer on the normal plane of the thickness direction of the pot body are overlapped, and the second protection layer corresponding to the projection overlapping part is directly attached and connected with the first protection layer. The manufacturing method of the cooking container comprises a forming step, a roughening step, a first spraying step, a curing step, a cleaning step, a second spraying step and an integral curing step. By arranging the cleaning step, the first protection layer and the second protection layer can be in direct contact and connected, so that the connection firmness of the first protection layer and the second protection layer is improved, and the lasting non-stickiness of the cooking container is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of cooking utensils, and in particular to a cooking container and a manufacturing method thereof. Background Art

[0002] Cooking containers (such as woks, frying pans, pressure cooker inner pots, steamers, etc.) are commonly used tools in the kitchen cooking process. Food is processed by putting food into the cooking cavity and then stir-frying it. Based on the demand for non-stick cooking containers, the current common practice in the industry is to spray a layer of non-stick coating on the surface of the cooking container, so that the food directly contacts the non-stick coating during cooking to achieve non-stick.

[0003] Although non-stick coatings have good non-stick properties, they are generally prone to partial detachment, especially during cooking, when they are easily impacted by a spatula and fall off. After the non-stick coating falls off, the non-stick properties of the cooking container will be significantly reduced. Once partial detachment occurs, the overall structural stability of the non-stick coating is destroyed, causing the remaining non-stick coating to fall off more easily. To alleviate this problem, the prior art chooses to spray more than two layers of non-stick coating on the surface of the cooking container. This solution allows the inner layer of the non-stick coating to continue to exert its non-stick properties after the non-stick coating on the surface of the cooking container falls off, thereby helping to improve the long-lasting non-stick properties of the cooking container.

[0004] However, the long-lasting non-stick properties of current cooking containers with more than two layers of non-stick coating are still not ideal and cannot meet the needs of consumers. After analysis, one of the important reasons for this problem is that the connection between the non-stick layers is not stable enough. When impacted by foreign objects such as spatulas and steel wool, the surface non-stick layer is easy to fall off, resulting in the surface non-stick layer not actually playing its role for a long time. In order to solve this problem, the main research direction of the current existing technology is to improve the composition of non-stick coatings to make the connection between the non-stick layers more reliable. However, the research on coating composition is a relatively complex research project, which is not only costly and slow, but also has unsatisfactory results. Summary of the invention

[0005] In view of the above problems, the present application provides a cooking container and a manufacturing method, starting from the structural and process perspectives, in order to improve the adhesion effect between multiple layers of non-stick coatings.

[0006] On the one hand, the present application provides a cooking container, which includes a pot body with a cooking cavity, wherein the side surface of the pot body facing the cooking cavity is an inner surface; the inner surface is covered with a protective layer, and the protective layer includes: a first protective layer, connected to the inner surface and covering a portion of the inner surface; a second protective layer, the second protective layer covers the first protective layer, the second protective layer and the first protective layer overlap in their projections on the normal surface in the thickness direction of the pot body, and the second protective layer corresponding to the overlapping projection portion is directly bonded and connected to the first protective layer.

[0007] It should be noted that the first protective layer may completely cover the inner surface or partially cover the inner surface.

[0008] On the one hand, the cooking container has a second protective layer covering the entire inner surface, so that it has good initial non-stick properties. Moreover, the second protective layer and the first protective layer are directly attached to the overlapping part of the projection, ensuring that there is no gap between the two, and no impurities that separate the first protective layer and the second protective layer, so that the second protective layer and the first protective layer have good connection stability. At the same time, when the second protective layer is transparent, there is no accumulation of impurities, which can also make the appearance of the cooking cavity more beautiful.

[0009] On the other hand, the present application also provides a method for manufacturing a cooking container, which is used to manufacture the cooking container as described above; the method for manufacturing a cooking utensil comprises the following steps: a molding step: processing the raw materials into a pot blank having a cooking cavity; a roughening step: roughening the inner surface of the pot blank facing the cooking cavity to form a rough surface; a first spraying step: spraying a non-stick coating on the inner surface to form a first protective layer; a curing step: drying and curing the first protective layer; a cleaning step: cleaning the surface of the first protective layer to remove impurities on the surface of the first protective layer; a second spraying step: spraying a non-stick coating on the surface of the first protective layer to form a second protective layer covering the first protective layer; an overall curing step: sintering and curing the second protective layer to form the cooking container.

[0010] After research and analysis, it was found that one of the reasons for the poor adhesion of the second protective layer on the surface is that after the first spraying, the surface of the first protective layer often has more impurities. When the second protective layer is subsequently sprayed, the force generated by the spraying on the surface of the pot will push the impurities and cause them to accumulate somewhere, making it impossible for the second protective layer to directly contact and adhere to the first protective layer in the area where the impurities are accumulated. Instead, it directly contacts the impurities, which directly affects the bonding stability of the second protective layer and the first protective layer.

[0011] In the above embodiment, the cleaning step can effectively reduce the amount of impurities on the surface of the first protective layer, thereby effectively alleviating the problem of low adhesion stability between the second protective layer and the first protective layer due to impurity accumulation, and improving the connection stability between the first protective layer and the second protective layer, thereby helping to improve the long-lasting non-stick properties of the cooking container.

[0012] In some embodiments, the outer surface of the first protective layer may be polished before the cleaning step to remove the uneven areas on the outer surface of the first protective layer, thereby alleviating the problem that impurities are easily accumulated in the uneven areas. In addition, the uneven areas may hinder the normal movement of impurities in the cleaning step, causing the impurities to accumulate in the uneven areas. Therefore, polishing the outer surface of the first protective layer can also improve the cleaning effect of the subsequent cleaning step.

[0013] In some embodiments, the cleaning step includes: spraying high-pressure air onto the surface of the first protective layer to remove surface impurities; and physically wiping the surface of the first protective layer to remove residual impurities.

[0014] In these embodiments, since high-pressure air generally does not contain solid impurities, no more impurities will be added to the surface of the first protective layer. The subsequent physical wiping step can be performed with a dry rag or the like to remove the more stubborn residual impurities on the surface of the first protective layer to ensure the cleaning effect. After cleaning, the surface of the first protective layer can be wiped once with a light-colored paper towel and the color change of the paper towel can be observed to confirm whether the impurities have been removed. If there is no obvious color change on the surface of the paper towel, it proves that the cleaning effect is good; if there is obvious color change on the paper towel, it proves that the cleaning should continue.

[0015] In some embodiments, the spraying pressure P of the high-pressure air is ≥ 0.5 kPa, and the distance between the spraying position of the high-pressure air and the first protective layer is less than 50 mm.

[0016] In these embodiments, the airflow has a greater pressure when it reaches the surface of the first protective layer, and a better cleaning effect can be obtained. Only one spray around the first protective layer is required to achieve a good cleaning effect with high efficiency, and after spraying the high-pressure air, only a little wiping is required to remove the remaining impurities.

[0017] In some embodiments, the cleaning step includes: spraying high-pressure liquid onto the surface of the first protective layer to remove surface impurities; drying the pot blank, and the drying temperature is W1; wherein the drying and curing temperature of the first protective layer is W2, W1<W2.

[0018] Through testing experiments, it is found that the cleaning effect of high-pressure liquid is better than that of high-pressure gas, and impurities can be removed without physical wiping after cleaning. The subsequent drying step is mainly used to evaporate the liquid so that there is no liquid residue on the surface of the first protective layer, which is convenient for subsequent spraying. Considering that too high drying temperature may affect various properties of the first protective layer, such as causing bubbles in the first protective layer, the drying temperature for evaporating the cleaning liquid in this solution is set as W1, and the drying and curing temperature of the first protective layer is W2, where W2 is a determined temperature set based on the raw materials of the first protective layer and combined with industrial production experience, and it is limited that W1 < W2. This is because subsequent process steps still need to continue spraying, and the first protective layer is only in a surface-dry state rather than a fully cured state in the previous steps. If the curing is excessive, it will affect the bonding stability of the second protective layer to be sprayed subsequently. Therefore, setting W1 < W2 can尽可能地使液体烘干步骤不会使第一保护层固化过度,从而尽可能地降低影响后续喷涂的效采。例如,如果某实施方案中第一保护层的材质为陶瓷涂料,基于行业标准,一般陶瓷涂料不粘层所需的烘干固化温度W2为100℃-150℃,则此实施方案中设定W1小于100℃,例如可以是70℃、80℃或90℃等。

[0019] In some embodiments, the cleaning step includes: repeatedly wiping the surface of the first protective layer with a wiping cloth; after repeated wiping, wiping the surface of the first protective layer with a light-colored tissue paper once. If the color change of the tissue paper surface is obvious, continue to repeatedly wipe with the wiping cloth until there is no obvious color change on the tissue paper surface.

[0020] This embodiment has low requirements for equipment and can be achieved by manual labor, which helps to reduce the difficulty of promoting the solution.

[0021] In some embodiments, the surface of the pot blank has several outwardly protruding portions; the first spraying step further includes: after spraying, the first protective layer covers the surface of the cooking cavity; a polishing step is further included between the curing step and the cleaning step, and the polishing step includes: performing surface polishing on the first protective layer to remove the first protective layer at the top of the protruding portion, so that the top of the protruding portion protrudes from the first protective layer; the second spraying step further includes: the second protective layer covers the protruding portion.

[0022] It should be noted that there seems to be an incomplete or inaccurate expression in the original text "尽可能地使液体烘干步骤不会使第一保护层固化过度,从而尽可能地降低影响后续喷涂的效采", which has been translated as accurately as possible while maintaining the original meaning. You may want to check and correct this part if necessary.Since the top of the raised portion protrudes from the first protective layer, when the second protective layer falls off and the raised portion is exposed, the raised portion can provide physical protection for the first protective layer, making it difficult for the first protective layer to directly contact the spatula, thereby reducing the probability of the first protective layer falling off. In other words, the first protective layer can be more durably attached to the inner surface, and can continue to provide protection for the pot body even when the second protective layer falls off, so that the cooking container has better long-term non-stick properties. The second protective layer covers the raised portion and the first protective layer, so in the initial state, the entire inner surface of the cooking container has a non-stick coating, that is, the cooking container has good initial non-stick properties.

[0023] In some embodiments, the surface of the cooking cavity includes a plurality of first parts and a plurality of second parts, wherein the first parts are higher than the adjacent second parts; the second spraying step also includes: by spraying, forming a plurality of first parts and a plurality of second parts on the surface of the second protective layer, wherein the first parts protrude from the adjacent second parts.

[0024] As a further optional solution, the first part is located above the raised part. Since the raised part is in an upwardly protruding form, the paint does not occupy space and is more likely to accumulate above the raised part, thereby more easily forming the first part protruding upward. Of course, other conceivable solutions can also be used to form the first part, such as covering a part of the first protective layer with a tool and spraying the unshielded part, which can also form the first part protruding upward.

[0025] In some embodiments, the height of the upward protrusion of the first part relative to the adjacent second part is h, and the value of h can be any value between 50μm-200μm, for example, it can be 50μm, 70μm, 85μm, 100μm, 125μm, 150μm, 180μm, 190μm, 195μm, 199μm, etc. The minimum value of h is defined so that the protrusion has a sufficient protrusion height, that is, the receiving groove has a sufficient depth, which helps to store more cooking oil and makes it more difficult for the food to directly contact the bottom of the receiving groove. After experiments, when h≥50μm, the cooking utensil has a good non-stick effect. Defining the maximum value of h helps to reduce the sense of jamming caused by the spatula scratching the surface of the cooking cavity and improve the user experience.

[0026] In addition, since the bonding between the protective layers of the cooking container produced by the embodiment is relatively stable, even if h has a larger value (for example, greater than 150 μm), the second protective layer is less likely to fall off than the cooking container produced by the prior art process, so a larger h value can be selected to obtain a better non-stick effect. Moreover, since a portion of the surface of the raised portion will be thrown away in the previous process, spraying the second protective layer can also make up for the height lost by the raised portion, so that the cooking container finally manufactured meets the requirements for the h value. Similarly, the third protective layer can also make up for the lost height.

[0027] In some embodiments, a third spraying step is further included between the second spraying step and the overall curing step: spraying a non-stick coating on the surface of the second protective layer to form a third protective layer covering the second protective layer; wherein the first protective layer has a color; the second protective layer is translucent; the third protective layer is transparent, and the third protective layer includes a first part and a second part, and a surface of the first part facing the cooking cavity is higher than a surface of the adjacent second part facing the cooking cavity.

[0028] In these embodiments, the color of the first protective layer can be various colors, such as gold, black or white, etc., and it is only necessary to add a slurry with a specified color to the raw materials of the first protective layer. The second protective layer is translucent. On the one hand, it allows users to directly see the color of the first protective layer, so that the cooking container has a better appearance. Moreover, translucent means a state in which light can still pass through with a certain color, for example, it can present an atomized effect. Therefore, the second protective layer can also modify and improve the visual effect of the color of the first protective layer, making the visual effect presented on the inner surface more diverse and beautiful. The third protective layer is transparent. On the one hand, after the third protective layer falls off, the second protective layer provides a non-stick effect, and the third protective layer can further enhance the durable anti-stick effect. On the other hand, compared with colored coatings, users have a higher acceptance of non-colored coatings, thereby avoiding the cognitive bias that colored equals toxic.

[0029] Furthermore, in the case of a raised portion, debris is easily accumulated at the raised portion. When the second protective layer and the third protective layer are translucent or transparent, the accumulated debris is visually obvious, which seriously affects the appearance of the raised portion and thus affects the visual effect of the cooking container. Therefore, the polishing and cleaning step also has the function of maintaining the appearance of the raised portion, so that the cooking container can have a desired visual effect.

[0030] In addition, configuring the protective layer to be transparent is also a relatively mature technology for the industry. For example, for conventional coatings such as fluorine coatings or ceramic coatings, it is relatively easy to configure them to be transparent. Therefore, configuring the second and third protective layers to be transparent or translucent will not complicate the process.

[0031] In some embodiments, the protrusion is in an enclosed form.

[0032] In these embodiments, the raised portions can surround the first protective layer, and the raised portions around each first protective layer provide protection for the first protective layer, thereby providing a better protective effect for the first protective layer and further reducing the probability of the first protective layer falling off.

[0033] In addition, the raw material of the non-stick coating can be ceramic non-stick coating. On the one hand, the curing temperature of ceramic non-stick coating is relatively low, and it can generally be cured at 100℃-150℃. In contrast, the curing temperature of fluorine coating is around 400℃. Obviously, ceramic non-stick coating has lower requirements for curing conditions and is easy to sinter and cure; on the other hand, with the development of technology, it is found that fluorine coating is easy to decompose at high temperature to produce substances that are harmful to health, while ceramic coating has no such risk. Therefore, ceramic coating can also have the advantage of being healthier while being non-sticky. In addition, there are basically no impurities between the first protective layer and the second protective layer, so that there is good adhesion stability between the first protective layer and the second protective layer.

[0034] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, which can be implemented according to the contents of the specification, and to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0036] Figure 1 A schematic flow chart of a method for manufacturing a cooking container provided in one embodiment of the present application;

[0037] Figure 2 A half-section view of a cooking container manufactured by the method for manufacturing a cooking container provided by an embodiment;

[0038] Figure 3 It is a schematic structural diagram of each protective layer of the first embodiment of the cooking container;

[0039] Figure 4It is a schematic diagram of the structure of the cooking container after one-time spraying and polishing;

[0040] Figure 5 It is a schematic diagram of the structure of the cooking container after secondary spraying;

[0041] Figure 6 is a schematic structural diagram of each protective layer of a second embodiment of a cooking container;

[0042] Figure 7 It is a schematic diagram of a partial structure of the cooking cavity surface of the third embodiment of the cooking container;

[0043] Figure 8 is a schematic diagram of a partial structure of the cooking cavity surface of a fourth embodiment of a cooking container;

[0044] Fig. 9 is a schematic diagram of a partial structure of the cooking cavity surface of the fifth embodiment of the cooking container;

[0045] Fig.10 A schematic diagram of the cooking cavity surface effect of a cooking container manufactured without a cleaning step;

[0046] Fig.11 A schematic diagram of the surface effect of the cooking cavity of the cooking container manufactured by the cleaning step;

[0047] The reference numerals in the specific implementation manner are as follows:

[0048] 1. pot body; 10. cooking cavity; 11. raised part; 12. recessed part;

[0049] 2. The first protective layer;

[0050] 30. Notch portion; 31. Second protective layer; 32. Third protective layer; 321. First portion; 322. Second portion; 33. Accommodating groove; 34. Protruding point portion. DETAILED DESCRIPTION

[0051] In order to more clearly illustrate the overall concept of the present application, a detailed description is given below in an illustrative manner in conjunction with the accompanying drawings.

[0052] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0053] In addition, the technical terms "first", "second", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0054] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0055] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0056] The research on the non-stick properties of cooking containers has always been a key research direction in the industry. The non-stick properties of cooking containers generally include initial non-stick properties and lasting non-stick properties. Initial non-stick properties refer to the non-stick properties of the cooking container when it is first used, and lasting non-stick properties refer to the non-stick properties of the cooking container after a certain period of use. In the prior art, a non-stick coating with good non-stick properties can be formed on the surface of the pot blank by spraying non-stick coating on the pot blank, thereby obtaining good initial non-stick properties. However, the non-stick coating is easy to fall off. As the coating falls off, the non-stick properties of the cooking container will be significantly reduced, that is, it is not easy for the cooking container to have good lasting non-stick properties.

[0057] In order to improve the long-lasting non-stick properties of cooking containers, one method is to form a multi-layer non-stick coating by spraying the pot blank multiple times. When the non-stick coating on the surface falls off, the inner non-stick coating is exposed and continues to provide a non-stick effect. However, based on actual tests and usage experience, in the case of multi-layer non-stick coatings, the non-stick coating attached to the non-stick coating is easier to fall off than the non-stick coating attached to the surface of the pot blank. Therefore, although in theory multi-layer non-stick coatings can effectively improve long-lasting non-stick properties, since the non-stick coating attached to the non-stick coating is easier to fall off, the actual effect of improving long-lasting non-stick properties is not obvious.

[0058] At present, in response to the above problems, some technical solutions choose to start from the components of the non-stick coating to seek to improve the connection stability between the non-stick coatings. However, the research progress of the material alone is relatively slow, the cost is high, and the results are relatively few.

[0059] Fig.10 This is a test sample of an etched pot. The sample includes two protective layers sprayed on the pot blank, of which the surface protective layer is transparent so that the etched pattern can be seen; the internal protective layer is black. However, the samples generally have the following problems: the bottom of the etched pattern on the inner wall of the sample (for example, the area indicated by the arrow) has an unknown silver stain layer, and the stain cannot be removed by wiping the surface of the pot. Analysis found that the stain is located under the surface protective layer, that is, these stains are sandwiched between the surface protective layer and the internal protective layer. For this reason, by adjusting the process, the stains between the two protective layers were removed in subsequent samples, and the results were obtained. Fig.11Samples with the appearance shown. When testing the samples after the process adjustment, it was discovered by chance that the long-lasting non-stick properties of the etching pot were improved to a certain extent after the stains were removed. After further analysis, it was found that it was precisely because these stains would accumulate between the surface protective layer and the internal protective layer that the two protective layers at the stain accumulation location could not fit properly, and because the composition of the stains was quite different from that of the protective layer, it was difficult to stably bond the surface protective layer and the internal protective layer, resulting in some areas between the surface protective layer and the internal protective layer not being stably bonded and connected, resulting in unreliable connection between the two protective layers.

[0060] Based on this, the present application proposes an optimized method for manufacturing a cooking container, which improves the adhesion strength between the two protective layers by removing impurities between the two protective layers.

[0061] Based on the test and analysis results, the present application provides a method for manufacturing a cooking container, and the process steps included in the optional embodiment can be referred to Figure 1 The specific embodiments of each step are as follows:

[0062] The forming step is to form the raw material into a pot blank of a predetermined shape by die casting, stretching, spinning or any other commonly used process. The shape of the pot blank is not limited, and can be a frying pan, a steamer, an inner pot or other conventional cooking container shapes, which can be determined according to specific needs. For example, the forming step adopted in a certain embodiment is: a plate made of composite steel is selected as the raw material. The composite steel includes three layers, wherein the first layer is made of 304 stainless steel or 316 stainless steel, the second layer is made of thermal conductive aluminum, and the third layer is made of 430 stainless steel with magnetic conductivity, and the second layer is sandwiched between the first layer and the third layer. The composite steel plate is formed into a pot blank by a stretching process. After stretching, the surface of the first layer faces the cooking cavity of the pot blank, and the surface of the third layer faces the outside of the pot blank. In other embodiments, the composite steel may also include only two layers, the first layer is made of 304 stainless steel or 316 stainless steel, and the second layer is made of thermal conductive aluminum. After stretching, the surface of the first layer faces the cooking cavity of the pot blank, and the surface of the second layer faces the outside of the pot blank.

[0063] The roughening step refers to roughening the surface of the side of the pot blank facing the cooking cavity by a process such as sandblasting, so that the roughness of the surface of the side of the pot blank facing the cooking cavity is increased, so as to increase the contact area with the coating. For example, the roughening step adopted by a certain exemplary embodiment is: after the pot blank is formed, an alkaline, acidic or neutral solvent is sprayed on the surface of the pot blank to remove tiny debris on the surface of the pot blank to prevent the debris from affecting the subsequent sandblasting process. This method of removing debris can also be called an oiling process, which is a conventional debris removal process in the industry. The specific process parameters, solvent composition and principle are not repeated here. After removing the debris, a high-speed sand flow is used to impact the surface of the pot blank facing the cooking cavity, that is, the inner surface of the pot blank, so that the inner surface of the pot blank forms an uneven plane, so that the protective layer formed by the first spraying can be stably attached. The abrasive used in the sandblasting process can be a mixture of 60 mesh and 80 mesh brown corundum or white corundum, or other sandblasting process conditions can be used, as long as the roughness of the inner surface of the pot blank obtained after treatment meets the expectations. After sandblasting, the roughness of the inner surface of the pot blank is Ra2.5μm-4.0μm, and the overall surface is relatively uniform.

[0064] The first spraying step is to spray a non-stick coating on the inner surface of the pot blank, thereby forming a first protective layer 2 attached to the inner surface of the pot blank. The non-stick coating can be a fluorine coating, a ceramic non-stick coating, or other coatings that can be applied to the field of cooking containers. The specific components of the coating are not specifically limited. In some embodiments, the sandblasted pot blank is first dusted before spraying to remove impurities remaining after sandblasting, and then the pot blank is preheated before spraying, and the pot blank is preheated to 50°C-60°C for standby use. The first spraying step adopted in the embodiment is: the coating used in this example is a ceramic coating. Specifically, the ceramic coating is a siloxane-based ceramic coating containing silica sol, siloxane, an acidic solvent and a pigment slurry. The ceramic coating is sprayed with a spray gun, and the caliber of the spray gun is set to 1.0mm-2.0mm. For example, the caliber of the spray gun can be 1mm, 1.5mm or 2mm; the spraying pressure of the spray gun is set to 2kg / cm 2 -3kg / cm 2 , for example, it can be 2kg / cm 2 , 2.5kg / cm 2 or 3kg / cm 2 . Under this working condition, the thickness of the first protective layer formed after one spraying is about 20μm-40μm, which meets the basic thickness requirement of non-stick coatings, and under this spraying pressure, the first protective layer can fit tightly to the inner surface of the pot blank, which helps to improve the bonding strength between the first protective layer and the pot blank after curing.

[0065] The purpose of preheating is to suppress the problem of rapid cooling and curing of the coating in contact with the low-temperature pot body 1, especially to alleviate the problem of rapid cooling and curing of the silicon-based ceramic coating, thereby helping to improve the connection stability between the first protective layer 2 and the pot body 1. On the other hand, if the temperature of the pot body is too low, the coating may scatter due to the large temperature difference after contacting the pot body, thereby forming a number of solid particles that cannot be stably attached to the pot body. The solid particles, as impurities, will affect the adhesion of the coating to the pot body.

[0066] The curing step refers to drying and curing the surface of the first protective layer so that the first protective layer forms a solid surface with a certain hardness, so that the first protective layer can be processed in the subsequent process steps. For example, the curing step adopted in a certain embodiment is: sintering and curing the cooking container after the first spraying in a sintering furnace. In the example where the coating is a ceramic coating, the sintering temperature in the furnace is maintained at 100°C-150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C or 150°C; the sintering and curing time is 5 minutes-20 minutes, for example, it can be 5 minutes, 7 minutes, 10 minutes, 13 minutes, 15 minutes, 18 minutes or 20 minutes. In other embodiments, when the coating composition changes, it is only necessary to adjust the curing temperature and curing time according to the actual situation. For example, the curing temperature of the fluorine coating is about 400°C. The specific working conditions can be selected according to the conventional technical means of the industry, and will not be described one by one here.

[0067] The polishing step refers to polishing the surface of the first protective layer 2 after the first spraying. The purpose of polishing is to make the surface of the first protective layer 2 flat, limit the problem of impurities accumulating in the pits and being difficult to remove in the subsequent process, and make the surface of the first protective layer 2 neat and beautiful.

[0068] The specific method of polishing can refer to the prior art, for example, the surface of the first protective layer 2 can be smoothed using sandpaper, and then large debris left over from polishing can be removed using a scouring pad. Alternatively, other conventional polishing techniques in the prior art can be used, which will not be described in detail here.

[0069] The cleaning step refers to cleaning the surface of the first protective layer 2 after the first spraying to remove impurities on the surface of the first protective layer 2. It is required that after the impurities are removed, there is basically no visible accumulation of impurities on the surface of the first protective layer 2 that can be easily removed by wiping. After the cleaning step is completed, the method for testing whether there are residual impurities can be to wipe the surface of the first protective layer 2 with a white paper towel. If the surface of the white paper towel is obviously discolored, it proves that the impurities are not completely removed, and it is necessary to continue cleaning to remove the impurities until the white paper towel does not change color or only changes color very slightly. The main purpose of removing impurities is to reduce the interference of impurities with the spraying effect, that is, to enable the second protective layer 31 sprayed subsequently to directly contact and fit with the first protective layer 2. In addition, removing impurities can also eliminate the interference of impurities on the appearance of the cooking container.

[0070] Here are three cleaning examples that can be selected based on actual process conditions:

[0071] Cleaning Example 1:

[0072] Use high-pressure air to remove impurities on the surface of the first protective layer. Specifically, spray high-pressure air directly onto the surface of the first protective layer 2, and use the high-pressure air to blow the impurities directly out of the accommodation cavity. Then use a lint-free towel or paper towel to repeatedly wipe the surface of the first protective layer 2 several times to remove the remaining impurities.

[0073] The effect of using high-pressure air to remove impurities is that there are generally fewer solid impurities entrained in the air, and it is not easy to continue to increase impurities on the surface of the first protective layer 2 that affect the mutual adhesion of the first protective layer 2 and the second protective layer 31. Basically, no subsequent treatment is required, and the impurity removal effect is better.

[0074] Specifically, the spray pressure of the high-pressure air is set to P≥0.5kpa, and the distance between the spray position of the high-pressure air and the first protective layer 2 is less than 50mm. For example, a high-pressure air gun can be used for cleaning, and the jet pressure of the high-pressure air gun is set to 0.5kpa, or 0.8kpa or 1kpa, etc., and the muzzle of the high-pressure air gun is set to a position about 30mm above the surface of the first protective layer 2, or 20mm, 39mm, 40mm, etc. The high-pressure air gun sprays high-pressure gas at an angle directly facing the surface of the first protective layer 2 to blow away impurities on the surface of the first protective layer 2. Based on experiments, when the above process parameters are used for spraying and removing impurities, the paper towel will only change color slightly or not change color after wiping it with a paper towel, and the spray gun distance is greater than 50mm or the air pressure is less than 0.5kpa, which will cause the paper towel to change color more obviously, that is, the cleaning effect is not ideal.

[0075] Cleaning Example 2:

[0076] Use high-pressure water flow to clean debris, and dry the residual liquid after cleaning. Specifically, a high-pressure water gun can be used to rinse the surface of the first protective layer 2, and then the cooking container can be dried to remove the residual liquid after rinsing. Compared with gas, the rinsing effect of high-pressure liquid is better. Generally, after rinsing once, physical wiping is not required again to meet the cleaning requirements. The drying temperature can be controlled below the curing and drying temperature of the first protective layer, that is, the drying temperature for removing the cleaning liquid is W1, and the drying and curing temperature of the first protective layer is W2, where W1 < W2. This temperature is relatively low compared to the temperature of the curing step. Drying within this temperature range helps reduce the risk of cracking of the first protective layer 2 and prevent over-curing of the first protective layer 2 as much as possible.

[0077] Cleaning Example Three:

[0078] Directly use a wiping cloth to repeatedly wipe the surface of the first protective layer 2 to remove the attached impurities. The method for testing the wiping result can also be to wipe with a white paper towel. When the paper towel does not change color significantly, it can be considered that there are no impurities on the surface of the first protective layer 2.

[0079] In Cleaning Experimental Example Three, note that the wiping cloth should be a non-shedding flannel to avoid further increasing impurities.

[0080] The above three cleaning examples can also be used simultaneously or in pairs to obtain a better cleaning effect.

[0081] The second spraying step refers to continuing to spray the inner wall of the pot body 1 with a coating to form a second protective layer 31. The coating used in the second spraying step is a transparent non-stick coating. The main components of this coating can be the same as or different from those of the coating of the first protective layer 2. For example, in a certain exemplary embodiment, the second spraying step is as follows: use a spray gun with a caliber of 1.0 mm - 2.0 mm for spraying, and set the spraying pressure to 1.5 kg / cm 2 - 2.5 kg / cm 2 , for example, the spraying pressure can be 1.5 kg / cm 2 、2 kg / cm 2 or 2.5 kg / cm 2 . After spraying, a second protective layer 31 with a thickness slightly thinner than that of the first protective layer 2 can be formed. The thickness of the second protective layer 31 formed under the working conditions of this embodiment is about 3 μm - 12 μm. The thickness of the second protective layer 31 is relatively thin. Based on tests, on the one hand, the thinner the second protective layer 31, the less likely it is to fall off after being impacted; on the other hand, the second protective layer 31 with this thickness can have a primary non-stickiness of level 1 and a persistent non-stickiness of level 2 after vibration testing based on GB / T 32388 when combined with the first protective layer 2. Therefore, the non-stickiness can also meet the requirements, that is, the second protective layer 31 within this range can balance the connection stability and non-stickiness.

[0082] In addition, in certain further embodiments, the interval time between the first spraying step and the second spraying step is required to be H, 1 hour ≤ H ≤ 100 hours. If the interval time is greater than 100 hours, the first protective layer may be completely cured, and the completely cured first protective layer and the uncured second protective layer may have the defect of being difficult to stably combine, thereby affecting the bonding stability of the first protective layer and the second protective layer; and if the interval time is less than 1 hour, the interval time is too short and the surface of the first protective layer may not be completely cured, resulting in the polishing step and the cleaning step being difficult to proceed normally. After experimental verification, controlling the interval time between the first spraying step and the second spraying step to 1 hour-100 hours can take into account both the requirements that the first protective layer will not be completely cured and the surface of the first protective layer is dry and cured, and the time arrangement is reasonable, which is convenient for the connection of each process.

[0083] The third spraying step refers to spraying the pot body 1 having the second protective layer 31 for the third time to form a third protective layer 32. Similar to the second protective layer 31, the coating used to form the third protective layer 32 can be the same as the main component of the coating of the first protective layer 2, or different, and the third protective layer 32 is transparent. The specific method adopted in the third spraying step can also refer to the second spraying step. The formed third protective layer 32 can further enhance the lasting non-stickiness on the one hand, and can complement the appearance of the second protective layer 31 on the other hand. For example, the second protective layer 31 and the third protective layer 32 are both transparent protective layers with a certain base color. When the two are superimposed, a new appearance style can be formed, thereby improving the aesthetics.

[0084] The overall curing step refers to sintering and curing the first protective layer 2, the second protective layer 31 and the third protective layer 32. The specific process flow and parameters of the overall curing step can refer to the aforementioned curing step or the prior art, and only the second protective layer 31 and the third protective layer 32 need to be cured.

[0085] In addition, in some optional embodiments, the following process is used for overall curing: first, the pot body is placed in an environment of 80°C-150°C for 5 minutes-18 minutes, for example, it can be placed in an environment of 80°C for 18 minutes, an environment of 100°C for 15 minutes, an environment of 120°C for 10 minutes, or an environment of 140°C for 8 minutes. The specific temperature or time can be adjusted according to the actual situation. If the curing is not complete, it can be considered to increase the temperature or extend the placement time within the range. After that, the environment is heated to 200°C-250°C, such as 200°C, 220°C, 240°C, etc., and continue to be placed for 5 minutes-28 minutes. The heating process can make the curing effect more complete, so that the part below the surface can also be effectively cured, and the occurrence of cracking of the protective layer can be suppressed. After two drying treatments, the first protective layer 2, the second protective layer 31 and the third protective layer 32 are completely dried and tightly combined and not easy to fall off.

[0086] After the overall solidification, the surface of the cooking cavity 10 of the pot body 1 can be polished as needed, so that the surface of the cooking cavity 10 presents a style that meets the requirements.

[0087] In some other embodiments, the method for manufacturing a cooking utensil is used to produce a cooking container having an etched pattern. Figure 2 The cooking container produced includes a pot body 1, a first protective layer 2, a second protective layer 31 and a third protective layer 32, wherein the surface of the cooking cavity 10 facing the pot body 1 has a plurality of protrusions 11, and the protrusions 11 form etching lines with a certain pattern on the surface of the pot body 1. The highest point of the first protective layer 2 is lower than the highest point of the protrusions 11, so that the first protective layer 2 is located in the concave portion 12 formed between adjacent protrusions 11 and is concave relative to the protrusions 11, so that the protrusions 11 can make it difficult for foreign objects such as spatulas to directly contact the first protective layer 2, play a role in protecting the first protective layer 2, and the etching line pattern formed by the protrusions 11 can be seen. The second protective layer 31 is formed on the surface of the first protective layer 2, and the second protective layer 31 covers both the first protective layer 2 and the protrusions 11, that is, the highest point of the protrusions 11 is located inside the second protective layer 31. Since the second protective layer 31 covers the protrusion 11, the food will not directly contact the protrusion 11 if the second protective layer 31 is not detached, which helps to improve the anti-stickiness of the pot body 1. The third protective layer 32 covers the second protective layer 31, which helps to increase the overall thickness of the protective layer, thereby further improving the non-stickiness of the cooking container.

[0088] The manufacturing method of the cooking utensil for producing a cooking container with etching lines comprises Figure 1 The steps shown in the embodiment further include the following steps compared with the above embodiment:

[0089] The raw material used in the forming step is a composite plate that has been etched, and a plurality of protrusions 11 have been formed on the composite plate.

[0090] The structure after the polishing step can be referred to Figure 4 In the polishing step, it is necessary to completely remove the first protective layer 2 on the surface of the raised portion 11, so that the highest point of the raised portion 11 protrudes from the first protective layer 2. On the one hand, only when the raised portion 11 protrudes relative to the first protective layer 2 can it effectively play a protective effect. On the other hand, the etching lines formed by the raised portion 11 have a certain appearance style, and the first protective layer 2 is a colored protective layer. Therefore, in order to make the etching lines visible, the first protective layer 2 on the surface of the raised portion 11 needs to be completely removed. In addition, after this step, the surface of the cooking cavity 11 presents an uneven style, which is conducive to increasing the contact area with the second protective layer 31 and also facilitates the subsequent attachment of the second protective layer 31.

[0091] The structure after the second spraying step can be referred to Figure 5 It should be noted that the sprayed second protective layer 31 needs to completely cover the first protective layer 2 and the protrusion 11 to provide a good initial non-stick effect.

[0092] Specifically, an optional embodiment of a method for manufacturing a cooking utensil is provided, which is used to produce a cooking container with an etched pattern, and specifically comprises the following steps:

[0093] The raw materials of the pot body 1 are selected from a composite plate with an outer layer of 430 magnetic conductive plate, an intermediate layer of aluminum heat conductive plate, and an inner layer of 304 or 316L with etched patterns; the coating of the protective layer is selected from a ceramic coating containing silica sol, siloxane, acidic solvent and pigment slurry. Since the sintering temperature of ceramic coating is lower than that of fluorine coating, the ceramic coating can be set thicker to improve the non-stickiness. Moreover, the sintering temperature of fluorine coating is relatively high, and fluorine coating is easy to decompose at high temperature, and the sintering temperature of fluorine coating is close to the high-temperature decomposition temperature of fluorine coating, so it is possible that the fluorine coating will decompose and produce harmful substances during sintering. When using ceramic coating, ceramic coating will not produce harmful substances at the sintering temperature, thereby avoiding the unhealthy phenomenon caused by fluorine coating.

[0094] The pot body 1 is formed by a stretching process using a composite plate that has been etched.

[0095] After stretching, the surface of the pot body 1 is degreased by spraying an alkaline, acidic or neutral solvent onto the pot body 1 to remove the larger impurities.

[0096] After degreasing, the inner surface of the pot body 1 is sandblasted to clean and roughen the inner surface of the pot body 1 by the impact of high-speed sand flow. The sandblasting uses a mixture of 60 and 80 mesh brown corundum or white corundum. Sandblasting can increase the surface tension, provide physical and chemical bonding strength for the combination of the coating and the substrate, extend the durability of the coating, facilitate the leveling of the coating, and strengthen the direct bonding between the base oil layer of the ceramic coating and the pot blank. After sandblasting, the inner surface roughness of the pot body 1 is Ra2.5μm~4.0μm, and the inner surface of the pot body 1 is uniform everywhere.

[0097] Preheat the pot body 1 after sandblasting: The pot body temperature should be preheated to 50℃~60℃ before the pot body is sent to the spray room for primer spraying. The reason for preheating is that, on the one hand, the temperature difference between the pot body and the paint is too large, and the paint may solidify quickly after contacting the surface of the pot body due to the large temperature difference, affecting the normal adhesion of the paint to the pot body and the stability of the connection between the two; on the other hand, if the temperature of the pot body is too low, the paint may scatter due to the large temperature difference after contact, thus forming a number of solid particles that cannot be stably attached to the pot body. The solid particles, as impurities, will affect the adhesion of the paint to the pot body. After the pot body is preheated, the above problems can be effectively suppressed.

[0098] After preheating, spray the first protective layer 2: adjust the spray gun diameter to 1.0mm~1.5mm, and adjust the atomization pressure to 2.5Kg / cm 2 ~3.0Kg / cm 2 The thickness of the first protective layer 2 after spraying is 20 μm to 25 μm.

[0099] After spraying the first protective layer 2, it is dried for subsequent polishing: After spraying the first protective layer 2, it is dried in a sintering furnace at 100° C. to 110° C. for 7 to 15 minutes. The main purpose of this drying step is to solidify the surface of the first protective layer 2 for subsequent polishing.

[0100] Polishing is performed after drying: the pot body 1 is placed in the mold and kept rotating, and the first protective layer 2 is removed from the etched raised part and the part near the pot mouth without etched lines with 180-grit sandpaper, and then wiped with a scouring pad to remove large impurities.

[0101] After polishing, cleaning and dust removal are performed to remove the remaining small impurities to prevent the impurities from affecting the adhesion of the second protective layer 31 .

[0102] After cleaning, the pot body 1 is preheated for the second time: before spraying the second protective layer 31 , the surface temperature of the pot body 1 is raised to 30° C. to 50° C.

[0103] The purpose of the secondary preheating is to avoid the problem of rapid solidification of the second protective layer 31 during the secondary spraying, and it is also beneficial to reduce the impurities generated after the second protective layer 31 is sprayed, and improve the bonding stability of the third protective layer 32 and the second protective layer 31. In addition, considering that the first protective layer 2 has been formed before the secondary preheating, the highest temperature of the pot body after the secondary preheating needs to be less than or equal to the lowest temperature after preheating, that is, less than or equal to 50°C, so as to avoid the problem of the first protective layer 2 changing in shape due to the high temperature of the pot body after preheating.

[0104] Spray the second protective layer 31: adjust the spray gun diameter to 1.0mm-1.5mm, and the atomization pressure to 2.0Kg / cm 2 ~2.5Kg / cm 2 The ceramic coating is sprayed to form a second protective layer 31, and the thickness of the second protective layer 31 is 3 μm to 5 μm. The second protective layer 31 is in a semi-transparent state, that is, the second protective layer 31 is a transparent protective layer with a certain color.

[0105] Spray the third protective layer 32 immediately after spraying the second protective layer 31: adjust the spray gun diameter to 1.0mm-1.5mm, and the atomization pressure to 2.0Kg / cm 2 ~2.5Kg / cm 2 , spraying ceramic coating to form a third protective layer 32, the thickness of the third protective layer 32 is 5μm to 7μm. The spraying process of the second protective layer 31 and the third protective layer 32 is completed continuously in a spray room, and a wet-spray-wet mode is adopted, that is, the third protective layer 32 is sprayed immediately before the second protective layer 31 is cured, so that the second protective layer 31 is bonded to the third protective layer 32 in a partially liquid form.

[0106] After spraying, the whole is cured: the pot body 1 is kept in an environment of 80°C to 150°C for 8 minutes to 15 minutes, and then the ambient temperature is raised to 220°C to 250°C and maintained for another 8 minutes to 15 minutes to complete the overall curing of the first protective layer 2, the second protective layer 31 and the third protective layer 32.

[0107] Final polishing: Use 180-grit sandpaper to remove the ceramic coating from the area without etching on the pot mouth of the pot body 1, and then wipe it with a towel to make the mouth of the cooking container smooth. Generally speaking, consumers do not have a non-stick requirement for the pot mouth, and the pot mouth is prone to bumps. Removing the ceramic coating from the pot mouth will not have a significant adverse effect on the performance of the cooking container, and it will also help reduce the risk of coating shedding due to abnormal actions such as bumps and knocks.

[0108] Table 1 shows the effect comparison between three embodiments manufactured by the manufacturing method of the above cooking container and comparative example 1, wherein experimental example 1 uses a high-pressure air gun for cleaning and dust removal; experimental example 2 uses a high-pressure water gun for cleaning and dust removal and drying; experimental example 3 uses manual wiping for cleaning and dust removal; comparative example 1 does not perform cleaning and dust removal. In view of the fact that the second protective layer 31 and the third protective layer 32 are transparent, it is difficult to accurately judge whether they have fallen off by direct observation in some cases. Therefore, the non-stickiness of the cooking container after the simulated cooking test is used as an indirect evaluation method. If the non-stickiness decreases, it means that the coating has partially fallen off. Among them, the steps of the simulated cooking test refer to the national standard GB / T32095.4 Food Simulation Test Specifications and Evaluation Methods for cyclic cooking tests, and the non-stickiness test rating refers to the fried egg non-stick rating item of GB / T32388. The test results are as follows:

[0109] Table 1

[0110]

[0111] It can be seen that the non-stickiness of Comparative Example 1 dropped to Level 2 after one cycle, and the coating had obviously fallen off after three cycles, indicating that the coating connection stability of Comparative Example 1 was not good. However, Experimental Examples 1, 2, and 3, which were cleaned and dusted, still maintained Level 1 non-stickiness after one cycle, and the protective layer did not obviously fall off after five cycles. Obviously, the bonding strength of the non-stick coating was enhanced after cleaning and dusting.

[0112] The manufacturing method of the cooking container can also be made into Figure 6 Cookware shown. Figure 2 Similar to the embodiment shown, the cooking container of this embodiment includes a pot body 1, which is bent to form a cooking cavity 10, wherein the side surface of the pot body 1 facing the cooking cavity 10 is the inner surface, and the inner surface is provided with a plurality of protrusions 11 and recesses 12, wherein the recesses 12 are formed between the protrusions 11, and the recesses 12 are in a concave form relative to the protrusions 11. The protrusions 11 and the recesses 12 can be formed by various existing processes, for example, by chemical etching, rolling or physical hammering, etc., and the forming method is not limited here. The inner surface of the pot body is covered with a protective layer for providing a non-stick effect, and the protective layer includes at least a first protective layer 2 and a second protective layer 31, and in some embodiments, a third protective layer 32 may also be included. The first protective layer 2 is arranged in the recess 12 and covers the recess 12, that is, the highest point of the surface of the first protective layer 2 facing the cooking cavity 10 is lower than the protrusion 11, and the protrusion 11 is in a convex form toward the cooking cavity 10 side relative to the first protective layer 2. The second protective layer 31 entirely covers the first protective layer 2 and the protruding portion 11 , that is, the first protective layer 2 and the protruding portion 11 are both located in the second protective layer 31 . Figure 6 Examples and Figure 3The difference between the embodiments is that, in the direction shown in the figure, the highest point of the second protective layer 31 located at the raised portion 11 is higher than the highest point of the second protective layer 31 located in the recessed portion 12, that is, the surface of the second protective layer 31 facing the cooking cavity 10 corresponds to the portion located at the raised portion 11, and is in a form of protruding toward the cooking cavity 10.

[0113] In the above embodiment, the raised portion 11 is covered by the formed second protective layer 31, so the position of the surface of the cooking cavity 10 corresponding to the raised portion 11 also has non-stick properties. And because the second protective layer 31 at the raised portion 11 is also in a convex form, when the second protective layer 31 directly contacts the food, it helps to reduce the contact area between the surface of the protective layer and the surface of the food, so that the protective layer has better non-stick properties.

[0114] In some other embodiments, the second protective layer 31 may also only cover the protrusion 11 , and the other areas of the cooking cavity surface are provided with a non-stick effect by the first protective layer 2 .

[0115] Considering that the material of the raised portion 11 is generally metal such as stainless steel or aluminum, and the second protective layer 31 is generally thin, the raised portion 11 may still be corroded by food. Therefore, in some embodiments, at least one of the corrosion-resistant components such as titanium, titanium dioxide, titanium nitride or titanium carbide can be added to the second protective layer 31. Specifically, in the second protective layer 31, the total mass proportion of one or more of titanium, titanium dioxide or titanium nitride is Z, and Z>2%. For example, the value of Z can be 5%, 10%, 15%, 20%, etc. Mixing a small amount of corrosion-resistant components such as titanium, titanium dioxide or titanium nitride into the coating can improve the corrosion resistance of the formed second protective layer 31, making the raised portion 11 less susceptible to corrosion. However, in the embodiment, the value of Z should not be too large. For example, when it is greater than 20%, the use of a general spraying process may affect the bonding ability of the second protective layer 31, and the spraying process needs to be adjusted, resulting in an increase in cost. Therefore, the value of Z is controlled to be below 20%.

[0116] Considering that the second protective layer 31 contains corrosion-resistant components such as titanium, titanium dioxide or titanium nitride, the first protective layer 2 may also contain corrosion-resistant components, which on the one hand provides corrosion resistance and on the other hand makes the components of the first protective layer 2 and the second protective layer 31 similar, which is beneficial to the combination of the first protective layer 2 and the second protective layer 31.

[0117] Table 2 shows the test data obtained after subjecting the above-mentioned embodiments and comparative examples to salt spray tests. Among them, the physical structures of comparative examples 2, 3, experimental examples 4, 5, and 6 are similar, and the material of the raised parts is 304 stainless steel. The difference is that in comparative example 2, the surface of the raised part is directly exposed; in comparative example 3, the protective layer on the surface of the raised part does not contain corrosion-resistant components such as titanium, titanium dioxide or titanium nitride, and the difference between the protective layer of comparative example 3 and the protective layer of the above-mentioned embodiment is that it does not contain corrosion-resistant components; in experimental example 4, the mass proportion of the corrosion-resistant component is 1%; in experimental example 5, the mass proportion of the corrosion-resistant component is 2%; in experimental example 6, the mass proportion of the corrosion-resistant component is 5%. The salt spray test can be carried out in accordance with the national standards, which are not limited here.

[0118] Table 2

[0119] Example No. Mass ratio of corrosion resistant components State of raised part Salt spray test results Comparative Example 2 0% Exposed bulge 2 hours rust Comparative Example 3 0% The raised part is covered 18 hours rust Embodiment 4 1% The raised part is covered 20 hours rust Experimental Example 5 2% The raised part is covered 24 hours no rust Experimental Example 6 5% The raised part is covered 24 hours no rust

[0120] It can be seen that in Comparative Examples 2 and 3, which do not contain corrosion-resistant components, the cooking containers cannot meet the test standard of no rust in the salt spray test for 24 hours; and in Experimental Example 4, due to the low mass proportion of the corrosion-resistant component, the test requirements cannot be met. When the mass proportion of the corrosion-resistant component reaches more than 2%, the cooking container can meet the test standard of no rust in 24 hours. Therefore, when the mass proportion of the corrosion-resistant component reaches more than 2%, the protective layer can effectively protect the protrusion 11.

[0121] Reference Figure 6 and Figure 7 , the third protective layer 32 is attached to the second protective layer 31, and the third protective layer 32 covers the second protective layer 31. Among them, the first protective layer 2 has a predetermined color, such as white, black, medical stone color and gold, etc. The method of obtaining the predetermined color is to add a slurry of the corresponding color to the raw material of the first protective layer 2, which belongs to the prior art and is not repeated here; the second protective layer 31 is translucent, which can adjust the appearance of the first protective layer 2, so that the visual effect presented on the surface of the cooking cavity 10 is more in line with the requirements; the third protective layer 32 is fully transparent, and has no obvious effect on the appearance.

[0122] In other embodiments, the second protective layer 31 may be transparent and the third protective layer 32 may be translucent. Furthermore, the third protective layer 32 may be added with ingredients such as pearlescent powder to make it shiny. Due to the complex ingredients of the coating, in some cases, it is difficult to adjust the protective layer to a fully transparent effect. Therefore, the third protective layer 32 located on the outermost side is set to a translucent state with a certain color, and the second protective layer 31 is set to a transparent state. On the one hand, it can ensure that the translucent effect and pearlescent effect of the third protective layer 32 can be effectively recognized by consumers; on the other hand, since the color of the first protective layer 2 is darker, even if the second protective layer 31 cannot present a completely transparent effect and thus has problems such as fogging and whitish, its fogging and whitish effect will be covered by the dark color of the first protective layer 2, so that the appearance will not be significantly affected.

[0123] The third protective layer 32 includes a first portion 321 and a second portion 322, wherein the first portion 321 is correspondingly located on the raised portion 11, and the second portion 322 is correspondingly located on the recessed portion 12. Along the thickness direction of the pot body, the surface of the first portion 321 facing the cooking cavity 10 is higher than the surface of the adjacent second portion 322 facing the cooking cavity 10, that is, along the thickness direction of the pot body 1, the first portion 321 is in the form of convexity upward (that is, toward the side of the cooking cavity 10) relative to the adjacent second portion 322. The first portions 321 are mutually enclosed, so that the first portions 321 and the second portions 322 jointly form a plurality of receiving grooves 33, the first portions 321 constitute the side walls of the receiving grooves 33, and the second portions 322 enclosed in the first portions 321 constitute the bottom walls of the receiving grooves 33.

[0124] The first portion 321, as the side wall of the receiving groove 33, can limit the outflow of cooking oil from the receiving groove 33, so that after pouring cooking oil into the cooking container during cooking, a portion of cooking oil can be retained in each receiving groove 33 even during operations such as flipping the pan, thereby helping to improve the non-stickiness of the cooking container during cooking.

[0125] The shape formed by the first portion 321 and the receiving groove 33 can be a hexagonal honeycomb as shown in the figure, or can be other shapes, and the shape is not particularly limited here.

[0126] Furthermore, the raised portions 11 also surround each other, so that the recess 12 is surrounded by raised portions 11 .

[0127] The raised portions 11 intersect and enclose the recessed portion 12 so that the recessed portion 12 is surrounded by raised portions 11 . Thus, no matter from which angle the spatula impacts the surface of the cooking cavity 10 , the raised portions 11 can provide protection for the recessed portion 12 .

[0128] exist Figure 6 and Figure 7In the second embodiment shown in FIG. 1 , the reference diagrams of the layered structures of the second embodiment can also be referred to as Figure 2 The area in the cooking container where the protective layer is provided is the cooking area B. In the illustrated embodiment, the bottom surface of the cooking cavity and the side surface connected to the bottom surface together constitute the cooking area B (i.e. Figure 2 The cooking cavity surface below the dotted line is shown in the figure below the dotted line to make the diagram clear. Figure 2 The structure of the receiving groove 33 is omitted in the cooking zone B), and the ratio of the projection of the receiving groove 7 on the cooking zone B to the area of ​​the cooking zone B is greater than or equal to 85%. For example, it can be 85%, 86%, 88%, 89%, 90%, 91%, 94%, 95%, 97%, 98%, 99%, 99.5%, etc. Since the receiving groove 33 is arranged in most areas of the cooking zone B, the receiving groove 33 can store part of the edible oil, so that the cooking zone B can be filled with edible oil as much as possible, thereby obtaining an ideal non-stick effect.

[0129] Reference Figure 6 and Figure 7 In the second embodiment shown, the maximum spacing between the side walls of the receiving groove 33 is L mm, that is, for each receiving groove 33, the maximum spacing between the first parts 321 constituting the receiving groove 33 is L mm. Figure 7 In the embodiment of , L is the diagonal length of the hexagonal receiving groove 33. The depth of the receiving groove 33 is h mm. Among them, 0.06≤hh / L≤0.5.

[0130] Among them, the larger the h is, the deeper the depth of the receiving groove 33 is, and the less likely the food is to contact the bottom surface of the receiving groove 33; and the smaller the L is, the easier it is for the food to be lifted up by more adjacent first parts 321, so that the food is not easy to enter the receiving groove 33. It can be seen that the larger the value of h / L is, the less likely the food is to contact the bottom surface of the receiving groove 33, that is, the better the physical non-stick effect is. However, the value of h / L cannot be increased indefinitely. On the one hand, if the h value is too large, it will affect the cooking feel. On the other hand, if the L value is too small, the opening of the receiving groove 33 will be too small, making it difficult for the oil to flow in, resulting in poor oil storage effect. Moreover, if the L value is too small, it is also difficult to clean. After comprehensive consideration, within the value range of 0.06≤h / L≤0.5, the oil storage effect, physical non-occupancy and cooking feel can be taken into account.

[0131] exist Figure 7In the illustrated embodiment, the spacing between the diagonal points of the side walls of each regular hexagonal receiving groove 33 is 8 mm, that is, the maximum spacing between the side walls of the receiving groove 33 is 8 mm. Of course, the spacing can also be 5 mm, 6.5 mm, 7 mm, 10 mm, 12 mm, etc., as long as L is less than or equal to 12. Under this size, the spacing between the side walls of the receiving groove 33 is small, and after edible oil is adsorbed, the oil beads in the receiving groove 33 can be continuously distributed, so that the oil can be distributed more evenly in the receiving groove 33. In addition, the minimum value of L is 3, so that the oil storage tank can store oil normally.

[0132] In some embodiments, the thickness of the first protective layer 2 may be 15 μm-30 μm, for example, 15 μm, 16 μm, 20 μm, 24 μm, 25 μm, 28 μm, and 30 μm. Within this thickness range, on the one hand, the first protective layer 2 has a sufficient thickness so that the first protective layer has good non-stickiness; on the other hand, the thickness value is adapted to the height of the protrusion 11 formed by the conventional process, so that the thickness of the first protective layer 2 will not be greater than the height of the protrusion 11, so as to meet the purpose of the protrusion 11 being higher than the first protective layer 2. The thickness of the second protective layer 31 is 3 μm-8 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, or 8 μm. Since the second protective layer 31 is located between the first protective layer 2 and the third protective layer 32, the second protective layer 31 can be set thinner accordingly, which is beneficial to material saving on the one hand, and the thinner second protective layer 31 is also convenient for sintering and curing. The thickness of the third protective layer 32 is 3 μm-10 μm, such as 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, so that the total thickness of the third protective layer 32 and the second protective layer 31 is larger, so that the protrusion 11 has a good non-stick effect.

[0133] In some embodiments, the third protective layer 32 can be thicker than the second protective layer 31, so that the total thickness of the third protective layer 32 and the second protective layer 31 is larger, thereby providing better protection for the pot body 1; and the second protective layer 31 is thinner and less likely to be foggy or white. Moreover, the thinner second protective layer 31 is also easier to dry as a whole later.

[0134] Specifically, the thickness ratio of the second protective layer 31 to the third protective layer 32 is Q, and 0.7≤Q<1, which can make the drying and curing more complete.

[0135] In some embodiments, the thickness of the first protective layer 2 is greater than the thickness of the third protective layer 32 and greater than the thickness of the second protective layer 31. Since the first protective layer 2 is protected by the protrusion 11, it is not easy to fall off even if it is thick, so the first protective layer 2 can be set thicker accordingly to obtain a better non-stick effect.

[0136] exist Figure 8 In another embodiment shown, the second part 322 is provided with a plurality of convex points 34, and the convex points 34 are in the form of upward protrusion relative to the bottom surface of the surrounding receiving grooves 33, that is, the surface of the second part 322 corresponding to the area located at the convex points 34 is higher than the surface of the adjacent second part 322. The convex points 34 are provided to further reduce the contact area between the food and the surface of the cooking cavity, thereby improving the non-stickiness. The convex points 34 can be formed by providing a plurality of convex points on the substrate, and after spraying the coating, the coating covers the convex points, and the convex points 34 can be naturally formed.

[0137] The main material of the protective layer in the above embodiment except for the corrosion-resistant component can be ceramic coating. Ceramic coating is a common non-stick coating in the field of cooking utensils. Since ceramic coating has a lower sintering and curing temperature, it is more suitable for the above embodiment with a thicker total thickness of the protective layer. That is, the use of ceramic coating is more convenient for sintering and curing during production, so that the protective layer has an adhesion firmness that meets the requirements.

[0138] For the pot body 1, one embodiment of the pot body 1 includes an outer layer, a heat-conductive middle layer and an inner layer, wherein the material of the outer layer is the existing 430 magnetic stainless steel, the material of the heat-conductive middle layer is aluminum, and the material of the inner layer is 304 stainless steel or 316L stainless steel. 430 magnetic stainless steel can make the pot body 1 suitable for induction cookers; aluminum has good thermal conductivity, so the heat-conductive middle layer can transfer the heat of the outer layer to the inner layer; the inner layer has good anti-rust performance. The inner layer refers to a layer of the layered structure of the pot body 1 facing the cooking cavity 10, the outer layer refers to a layer of the layered structure of the pot body 1 facing the outside of the pot body 1, and the heat-conductive middle layer is a layered structure sandwiched between the inner layer and the outer layer.

[0139] In another embodiment of the pot body 1, only an outer layer and an inner layer are included, wherein the outer layer is made of aluminum, and the inner layer is made of 304 stainless steel or 316L stainless steel, so as to be suitable for open flame scenes, and the overall weight of the pot body 1 is relatively light.

[0140] Fig. 9 The embodiment shown is Figure 2 and Figure 8 The structures of the embodiments shown are basically the same, except that: Fig.10 The first middle portion 321 is provided with a plurality of notches 30 , which allow adjacent receiving grooves 33 to communicate with each other, thereby facilitating the mutual circulation of edible oil in each receiving groove and further facilitating the uniform distribution of edible oil.

[0141] The non-stickiness comparison results of the embodiment and the comparative example provided in this application can be referred to Table 3. The structure of Experimental Example 7 in Table 3 can be referred to Figure 2 and Figure 6The pot body 1 of the embodiment includes an outer layer made of 430 magnetic conductive stainless steel, a heat conductive middle layer made of aluminum, and an inner layer made of 304 stainless steel. Figure 3 The honeycomb-shaped raised portion 11 is shown, and the raised portion 11 surrounds the recess 12. The surface of the inner layer is attached with a protective layer formed by spraying ceramic coating, and the protective layer includes a first protective layer 2, a second protective layer 31 and a third protective layer 32, wherein the first protective layer 2 covers the recess 12, the second protective layer 31 covers the raised portion 11 and the recess 12, and the third protective layer 32 covers the second protective layer 31, and the third protective layer 32 forms a first part 321 at a position corresponding to the raised portion 11, and the third protective layer 32 forms a second part 322 at a position corresponding to the recess 12, the first part 321 protrudes outward relative to the adjacent second part 322, and the first part 321 intersects with each other, and together with the second part 322, forms a receiving groove 33. In addition, a plurality of protruding convex points 34 are formed on the bottom surface of the receiving groove 33.

[0142] The structure of the pot body 1 of comparative example 4 is the same as that of the embodiment, and the only difference is that the comparative example only includes a protective layer covering the recessed portion 12, that is, the surface of the raised portion 11 of comparative example 1 has no protective layer.

[0143] The overall structure of Comparative Example 5 is the same as that of Comparative Example 4, but the difference is that the protective layer material of Comparative Example 5 is fluorine coating.

[0144] The test methods are based on the national standard GB / T32388 fried egg test for initial non-stickiness, and the national standard GB / T32388 vibration wear test followed by a fried egg test to verify long-term non-stickiness.

[0145] The test results are shown in Table 3:

[0146] Table 3

[0147] Initial non-stickiness Long-lasting non-stickiness Experimental Example 7 Level 1 Level 2 Comparative Example 4 Level 3 Level 3 Comparative Example 5 Level 2 Level 2

[0148] It can be seen that compared with comparative example 4, the initial non-stickiness and the lasting non-stickiness of experimental example 7 are significantly improved, which shows that providing a protective layer on the surface of the raised portion 11 can significantly improve the initial non-stickiness and the lasting non-stickiness of the cooking container; and compared with comparative example 5, experimental example 7 has better initial non-stickiness and basically equivalent lasting non-stickiness. It can be seen that after providing multiple protective layers, the protective layer of the ceramic coating can have a non-stick effect equivalent to that of the fluorine coating, and the use of ceramic coating can also avoid the disadvantage of fluorine coating that toxic substances are easily volatilized at high temperatures, making the cooking container healthier.

[0149] In addition, refer to Fig.10 and Fig.11 , Fig.10 A comparative example of a cooking container without a cleaning step, Fig.11The surface appearance of the cooking cavity of the cooking container manufactured by the manufacturing method of the cooking container including the cleaning step is compared with Fig.10 , Fig.11 It can be clearly seen from the embodiment that after the impurities are removed, there is no obvious accumulation of stains on the bottom of the first portion 321 (i.e., the bottom of the raised portion 11), and the appearance of the surface of the cooking cavity is more neat and beautiful. In addition, in combination with the above experimental results, in the absence of stain accumulation, the long-lasting non-stickiness of the cooking container is improved.

[0150] It should be noted that the cooking containers in this application refer to various utensils used for cooking food, such as woks, frying pans, pressure cooker inner pots and steamers, including utensils that come into direct contact with open flames, utensils that are heated by electromagnetic means, etc., and also include utensils used for holding food in household appliances such as rice cookers, electric pressure cookers, soy milk makers, and food processors.

[0151] Anything not described in this application can be achieved by adopting or drawing on existing technologies.

[0152] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0153] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A cooking container, characterized in that: The cooking container comprises a pot body having a cooking cavity, wherein a side surface of the pot body facing the cooking cavity is an inner surface; The inner surface is covered with a protective layer, and the protective layer comprises: A first protective layer connected to the inner surface and covering a portion of the inner surface; The second protective layer covers the first protective layer, the second protective layer and the first protective layer overlap in projection on the normal surface in the thickness direction of the pot body, and the second protective layer corresponding to the overlapping projection part is directly bonded and connected to the first protective layer.

2. A method for manufacturing a cooking utensil, characterized in that: Used to manufacture the cooking container as claimed in claim 1; The manufacturing method of the cooking utensil comprises the following steps: Forming step: processing the raw materials into a pot blank with a cooking cavity; Roughening step: roughening the inner surface of the pot blank facing the cooking cavity to form a rough surface; The first spraying step: spraying a non-stick coating onto the inner surface to form a first protective layer; Curing step: drying and curing the first protective layer; Cleaning step: cleaning the surface of the first protective layer to remove impurities on the surface of the first protective layer; Second spraying step: spraying a non-stick coating onto the surface of the first protective layer to form a second protective layer covering the first protective layer; Overall curing step: sintering and curing the second protective layer to form the cooking container.

3. The method for manufacturing a cooking utensil according to claim 2, wherein: The cleaning step comprises: Spraying high-pressure air onto the surface of the first protective layer to remove surface impurities; Physically wipe the surface of the first protective layer to remove residual impurities.

4. The method for manufacturing a cooking utensil according to claim 3, wherein: The spraying pressure P of the high-pressure air is ≥ 0.5 kpa, and the distance between the spraying position of the high-pressure air and the first protective layer is less than 50 mm.

5. The method for manufacturing a cooking utensil according to claim 2, wherein: The cleaning step comprises: Spraying high-pressure liquid onto the surface of the first protective layer to remove surface impurities; Drying the pot blank at a drying temperature of W1; The drying and curing temperature of the first protective layer is W2, W1 <W2。 6. The method for manufacturing a cooking utensil according to claim 2, wherein: The cleaning step comprises: Repeatedly wipe the surface of the first protective layer with a wiping cloth; After repeated wiping, wipe the surface of the first protective layer with a light-colored paper towel. If the color of the surface of the paper towel changes significantly, continue to wipe it repeatedly with the wiping cloth until there is no obvious color change on the surface of the paper towel.

7. The method for manufacturing a cooking utensil according to claim 2, wherein: The roughening step and the first spraying step also include: Preheating step: preheating the pot blank to 50°C-70°C; And / or, between the cleaning step and the second spraying step, the following steps are also included: Second preheating step: preheat the cleaned pot blank to 30°C-50°C.

8. The method for manufacturing a cooking utensil according to any one of claims 2 to 7, characterized in that: The surface of the pot blank has a plurality of protrusions protruding outwards; The first spraying step further comprises: the first protective layer covers the surface of the cooking cavity after spraying; A polishing step is further included between the curing step and the cleaning step, and the polishing step includes: performing surface polishing on the first protective layer to remove the first protective layer at the top of the protrusion so that the top of the protrusion protrudes from the first protective layer; The second spraying step further includes: the second protective layer covers the protrusion.

9. The method for manufacturing a cooking utensil according to claim 8, wherein: A third spraying step is also included between the second spraying step and the overall curing step: spraying a non-stick coating on the surface of the second protective layer to form a third protective layer covering the second protective layer; The first protective layer has color; the second protective layer is translucent; the third protective layer is transparent, and the third protective layer includes a first part and a second part, and the surface of the first part facing the cooking cavity is higher than the surface of the adjacent second part facing the cooking cavity.

10. The method for manufacturing a cooking utensil according to claim 8, wherein: The second spraying step further includes: forming a plurality of first parts and a plurality of second parts on the surface of the second protective layer by spraying, wherein the first part protrudes from the adjacent second part.

Citation Information

Patent Citations

  • Non-sticking cooker and manufacturing method thereof

    CN104887060A

  • Pot and cooking utensil with same

    CN110859518A

  • Manufacturing method of pot body made of surface-layer hard root-planting non-stick pot material

    CN111685605A

  • Manufacturing method of cookware and cookware

    CN115624275A

  • Cooking utensil

    CN212698557U