Nitrogen-oxygen separation adsorbent and preparation method thereof

By using a composite layer structure in the nitrogen-oxygen separation adsorbent, the outer adsorbent layer adsorbs carbon dioxide and water vapor, the problem of degradation of separation performance of low-silicon X molecular sieve during pressure swing adsorption is solved, and efficient nitrogen-oxygen separation is achieved.

CN119056402AActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310623006.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

During the pressure swing adsorption and separation process, the low-silicon X molecular sieve adsorbent has a strong binding ability to carbon dioxide and water vapor, which makes it difficult for these gases to desorption quickly when the system pressure is reduced, resulting in a decrease in the adsorbent separation performance or even inactivation.

Method used

The nitrogen-oxygen separation adsorbent is adopted with a composite layer structure, and the outer adsorbent layer is composed of Y molecular sieve and binder to absorb carbon dioxide and water vapor in the air, thereby preventing it from entering the inner adsorbent layer and improving the separation performance of nitrogen and oxygen.

Benefits of technology

By rapidly desorbing carbon dioxide and water vapor from the external adsorbent layer, the impact on low-silicon X molecular sieve is reduced, the nitrogen-oxygen separation performance is improved, and the service life of the adsorbent is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004255968280000011
    Figure HDA0004255968280000011
  • Figure HDA0004255968280000012
    Figure HDA0004255968280000012
  • Figure HDA0004255968280000021
    Figure HDA0004255968280000021
Patent Text Reader

Abstract

The nitrogen-oxygen separation adsorbent is characterized in that the nitrogen-oxygen separation adsorbent comprises an inner adsorbent layer and an outer adsorbent layer, the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, the outer adsorbent layer comprises a Y molecular sieve and a binder, the cation site of the low-silicon X molecular sieve is occupied by Li, and the cation site of the Y molecular sieve is occupied by at least one of Na or K. The adsorbent is used for pressure swing adsorption separation of nitrogen and oxygen in air and preparation of oxygen-rich gas, and has good separation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a nitrogen-oxygen separation adsorbent and a preparation method thereof, in particular to a nitrogen-oxygen separation adsorbent with an X molecular sieve as an active component and a preparation method thereof. Background Art

[0002] Oxygen can be widely used in many fields such as metallurgy, chemical industry, and environmental protection. By using pressure swing adsorption (PSA) technology to separate nitrogen from other gases in the air, oxygen-rich gas with an oxygen concentration of more than 90% can be obtained. The active component of the pressure swing adsorption separation adsorbent is usually X molecular sieve. The X molecular sieve and clay are mixed evenly in a certain proportion, and the adsorbent balls are obtained after rolling, drying, and roasting.

[0003] CN1146374A discloses an adsorbent for a cyclic pressure swing adsorption process, the adsorbent containing a framework SiO2 / Al2O3 molar ratio of 2.0 to 2.4 and 60 to 89% (equivalent) Ca ++ Cation, 10-40% (equivalent) Na + Cations and 0-10% (equivalent) K + Cationic zeolite X, Ca ++ 、Na + and K + Providing a total cation equivalent of at least 90%, this X-type zeolite is much more effective as an adsorbent for air separation in a pressure swing adsorption process at 50-20°C and 5-506.5 kPa (0.05-5.0 atm) than the same X-type zeolite which has been calcium exchanged to a greater or lesser extent.

[0004] CN101708456A discloses a molecular sieve adsorbent for oxygen production by pressure swing adsorption air separation and a preparation method thereof. The active component of the adsorbent is Ca2O3 with SiO2 / Al2O3=2.0-2.1. 2+ Exchanged low silicon X-type molecular sieve, in which Ca 2+ The exchange degree is 80-100%. Since the exchange of calcium-type X molecular sieve with high exchange degree is difficult and costly, calcium chloride solution is used to exchange low-silicon X molecular sieve to reduce the cost.

[0005] CN1158139C discloses an improved binder zeolite adsorbent, whose active component is a deep lithium exchanged X molecular sieve with a Si / Al atomic ratio of 1. Multiple exchanges with lithium chloride solution can obtain a higher lithium exchange rate and nitrogen adsorption capacity.

[0006] CN1291907A discloses an improved PSA adsorbent whose active component is LiX zeolite material. The intrinsic mass transfer rate of the PSA adsorbent is improved by using an appropriate amount of agglomerated binder that can be converted into zeolite by alkali cooking ("CD") and adding combustible fibers or particulate materials during the molding process to improve the macroporous structure.

[0007] CN104138741A discloses a rare earth modified lithium low silicon molecular sieve adsorbent and a preparation method thereof. The method can significantly improve the hydrothermal stability and help prolong the service life by introducing rare earth elements into the cavity structure of the lithium low silicon molecular sieve.

[0008] During the pressure swing adsorption separation process, carbon dioxide, water vapor, etc. in the air will also be adsorbed by the low-silicon X-ray distillation molecular sieve adsorbent. However, due to the strong binding ability of carbon dioxide and water vapor with the low-silicon X-ray distillation molecular sieve, these gases are difficult to desorb quickly when the system pressure is reduced, resulting in a significant decrease in the separation performance of the adsorbent or even deactivation. Summary of the invention

[0009] The purpose of the present invention is to provide a nitrogen and oxygen separation adsorbent based on the prior art, which is used for pressure swing adsorption separation of nitrogen and oxygen in the air to produce high-concentration oxygen and has high nitrogen and oxygen separation performance.

[0010] The nitrogen-oxygen separation adsorbent provided by the present invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises a Y molecular sieve and a binder, wherein the cation position of the low-silicon X molecular sieve is occupied by Li, and the cation position of the Y molecular sieve is occupied by at least one of Na or K.

[0011] The present invention also provides a method for preparing a nitrogen-oxygen separation adsorbent, comprising the following steps:

[0012] (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as an inner adsorbent layer, and then a powder of Y molecular sieve and binder mixed in a mass ratio of 50-79:21-50 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening;

[0013] (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours;

[0014] (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

[0015] The present invention also provides a method for preparing oxygen from air using the nitrogen-oxygen separation adsorbent of the present invention or the nitrogen-oxygen separation adsorbent prepared by the method provided by the present invention.

[0016] The nitrogen-oxygen separation adsorbent provided by the present invention adopts a composite layer structure. During the adsorption process, the outer adsorbent layer adsorbs carbon dioxide and water vapor in the air that can be adsorbed, thereby preventing the carbon dioxide and water vapor from entering the inner adsorbent layer and affecting the separation performance of the low-silicon X molecular sieve for nitrogen and oxygen. Since the outer adsorbent layer has a weak adsorption capacity for carbon dioxide and water vapor, the carbon dioxide and water vapor adsorbed by the outer adsorbent layer during the pressure reduction and purge process can be quickly removed, reducing the influence of the carbon dioxide and water vapor on the low-silicon X molecular sieve, thereby improving the nitrogen-oxygen separation performance of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of pressure swing adsorption device.

[0018] Figure 2 This is a scanning electron microscope (SEM) photograph of the low silicon X molecular sieve in Example 1.

[0019] Figure 3 This is a scanning electron microscope (SEM) photograph of the Y molecular sieve in Example 1. DETAILED DESCRIPTION

[0020] The nitrogen-oxygen separation adsorbent provided by the present invention is rolled into two batches, and a mixture of a low-silicon X molecular sieve with a high nitrogen adsorption capacity and a binder is first rolled into small balls as an inner adsorbent layer, and then a mixture of a Y molecular sieve and a binder is added and rolled to form an outer adsorbent layer to form a composite layer adsorbent. During pressure swing adsorption, during the pressure increase process, the Y molecular sieve of the outer adsorbent layer first adsorbs carbon dioxide and water vapor in the air to prevent them from entering the inner adsorbent layer. After the remaining air enters the inner adsorbent layer, nitrogen is selectively adsorbed, and the remaining gas passes through the adsorbent bed and is discharged to obtain oxygen-rich gas; during the pressure reduction process, the nitrogen previously adsorbed by the low-silicon X molecular sieve of the inner adsorbent layer is desorbed. At the same time, since the Y molecular sieve of the outer adsorbent layer has a high silicon oxide / aluminum oxide molar ratio, the adsorption of carbon dioxide and water vapor is relatively weak, and the adsorbed carbon dioxide and water vapor can be quickly removed and discharged together with the nitrogen desorbed from the inner adsorbent layer. The adsorbent provided by the present invention effectively solves the problem that the nitrogen and oxygen separation performance of the low-silicon X molecular sieve decreases due to the adsorption of carbon dioxide and water vapor, and increases the concentration of the obtained oxygen, thereby improving the nitrogen and oxygen separation performance of the composite layer adsorbent as a whole.

[0021] The nitrogen-oxygen separation adsorbent provided by the present invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises a Y molecular sieve and a binder, wherein the cation position of the low-silicon X molecular sieve is occupied by Li, and the cation position of the Y molecular sieve is occupied by at least one of Na or K.

[0022] The nitrogen oxygen separation adsorbent provided by the present invention comprises: the inner adsorbent layer comprises 50-79 mass % of low silicon X molecular sieve and 21-50 mass % of binder, based on the total amount of the inner adsorbent layer; and the outer adsorbent layer comprises 50-79 mass % of Y molecular sieve and 21-50 mass % of binder, based on the total amount of the outer adsorbent layer.

[0023] In the nitrogen oxygen separation adsorbent provided by the present invention, the silicon oxide / aluminum oxide molar ratio of the low silicon X molecular sieve is 1.90-2.05, the content of the low silicon X molecular sieve is 90-96% by mass of the total amount of the molecular sieve in the adsorbent, the grain size of the low silicon X molecular sieve is 0.4-10 microns, and the Li2O content in the low silicon X molecular sieve is greater than or equal to 10% by mass.

[0024] In the nitrogen-oxygen separation adsorbent provided by the present invention, the silicon oxide / aluminum oxide molar ratio of the Y molecular sieve is 3.2 to 5.5, and the crystal particle size of the Y molecular sieve is 0.1 to 0.8 microns.

[0025] In the nitrogen-oxygen separation adsorbent provided by the present invention, the binder is selected from one of kaolin, halloysite and attapulgite.

[0026] The water content of the nitrogen and oxygen separation adsorbent provided by the present invention is less than or equal to 0.6% by mass.

[0027] The nitrogen-oxygen separation adsorbent provided by the present invention is preferably in the form of small spheres, and the average particle size of the small spheres is 300 to 850 microns.

[0028] The preparation method of the nitrogen-oxygen separation adsorbent provided by the present invention comprises the following steps:

[0029] (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as an inner adsorbent layer, and then a powder of Y molecular sieve and binder mixed in a mass ratio of 50-79:21-50 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening;

[0030] (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours;

[0031] (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

[0032] Wherein, the cation position of the low silicon X molecular sieve described in step (1) is occupied by Li, the cation position of the Y molecular sieve is occupied by at least one of Na or K, and the content of the low silicon X molecular sieve is 90-96% by mass of the total amount of the low silicon X molecular sieve and the Y molecular sieve; the low silicon X molecular sieve and the Y molecular sieve are prepared by conventional methods in the art, which will not be described in detail here. The equipment for rolling ball forming can be a turntable, a sugar coating pan or a drum. When rolling ball forming, the uniformly mixed solid raw materials are placed in a rotating device, and water is sprayed while rolling to make the solid powder adhere and agglomerate into small balls. The amount of water added during rolling ball forming is 5-16% of the total mass of the solid, preferably 8-12%. The small balls after rolling into balls are sieved to obtain small balls with a particle size of 300-850 microns.

[0033] In the preparation method of the nitrogen oxygen separation adsorbent provided by the present invention, in step (2), the small balls obtained in step (1) are spread flat to form a bed layer with uniform thickness, and the thickness of the bed layer is preferably less than or equal to 20 mm. During the drying process, air needs to continuously pass through the bed layer to quickly take away the water vapor. In order to avoid high-temperature water vapor from destroying the molecular sieve in the small balls, the air stays in the adsorbent bed layer for less than or equal to 20 seconds, preferably less than or equal to 15 seconds.

[0034] In the preparation method of the nitrogen-oxygen separation adsorbent provided by the present invention, in step (3), the small balls obtained in step (2) are laid flat to form a bed layer with uniform thickness, the thickness of the bed layer is preferably less than or equal to 15 mm, and the calcination is carried out in 4 stages, the calcination temperature is preferably 160-200°C, 270-300°C, 370-400°C, 460-500°C, the constant temperature calcination time of each stage is preferably 2-3 hours, 2-3 hours, 2-3 hours, 5-6 hours, the heating rate is 0.5-5°C / min, preferably 1-3°C / min, during the calcination process, air needs to continuously pass through the bed layer to quickly take away the water vapor, in order to avoid high-temperature water vapor from destroying the molecular sieve in the small ball, the air stays in the adsorbent bed layer for less than or equal to 20 seconds, preferably less than or equal to 15 seconds. After the calcination process is completed, the adsorbent small ball is cooled to room temperature under vacuum conditions.

[0035] The adsorbent provided by the present invention is suitable for separating nitrogen and oxygen in the air by pressure swing adsorption to produce high-concentration oxygen. The pressure swing adsorption can be carried out in a double-column or multi-column manner, or by using a rotary valve or a solenoid valve group to realize the pressure swing adsorption process. The operating pressure is 0.2-0.5MPa, and the operating temperature is 5-50°C.

[0036] A double-column pressure swing adsorption device is used to evaluate the adsorbent performance. The schematic diagram of the pressure swing adsorption device is shown in Figure 1 As shown in the figure, the device consists of a pressure gauge, an adsorption column, a solenoid valve, etc. The four steps of boosting, adsorption, depressurization, and purging are performed by opening or closing the solenoid valves V1, V2, V3, V5, V6, V7, and V8 to achieve continuous generation of oxygen-rich gas. About 370 mL of adsorbent is loaded in adsorption columns A and B respectively, and the adsorption is set to 3s, and the depressurization, purging, and boosting are set to 3s in total. The maximum pressure of the adsorption column is 0.25MPa, the operating temperature is 35°C, and the oxygen-rich gas generation rate is 4.5L / h. After 50 consecutive cycles, the oxygen volume concentration in the product is analyzed using an oxygen concentration meter.

[0037] Method for determining the moisture content of the adsorbent: place an adsorbent with a mass of m1 in a crucible and calcine it at 600°C for 2 hours. After calcination, quickly take out the crucible and place it in a dryer to cool to room temperature. Weigh the mass of the adsorbent after calcination as m2, and the moisture content of the adsorbent C = (m1-m2) / m1.

[0038] The present invention is further described below by way of examples, but the present invention is not limited thereto.

[0039] The following examples are used to prepare the adsorbents described in the present invention.

[0040] The preparation method of low silicon X molecular sieve and Y molecular sieve in the examples of the present invention is as follows:

[0041] Low silicon X molecular sieve: 4.66kg sodium hydroxide, 7.23kg potassium hydroxide, 35.74kg deionized water, 47.57kg low alkalinity sodium aluminate solution (Al2O3 mass fraction of 11.0%, Na2O mass fraction of 15.1%) and 36.72kg water glass are added to the reactor, stirred and mixed to form a molecular sieve synthesis system. The total molar ratio of each material in the molecular sieve synthesis system is: SiO2 / Al2O3=2.40, M2O / SiO2=2.25, H2O / SiO2=45, where M is K and Na, K / (K+Na)=0.23. The above molecular sieve synthesis system is transferred to the reactor, aged at 70°C for 6 hours, hydrothermally crystallized at 95°C for 12 hours, filtered, and the obtained solid is washed with deionized water until the filtrate pH is 8-9, and dried at 80°C for 12 hours to obtain a low silicon X molecular sieve.

[0042] A 1.5 mol / L lithium chloride solution was prepared, and the pH was adjusted to 8-10 with lithium hydroxide. The lithium chloride solution and the low silicon X molecular sieve were mixed at a liquid-to-solid ratio of 5 L / kg, and exchanged at 80°C for 1 hour, and repeated 7 times. The exchanged low silicon X molecular sieve was dried at 40°C for 10 hours to obtain a low silicon X molecular sieve with lithium cation.

[0043] The molar ratio and Li2O content of the low silicon X molecular sieve can be adjusted by adjusting the molar ratio of SiO2 / Al2O3 in the molecular sieve synthesis system, the concentration of the lithium chloride solution, and the liquid-solid ratio of the lithium chloride solution to the low silicon X molecular sieve.

[0044] Y molecular sieve: 4.02 kg of sodium hydroxide, 10.15 kg of deionized water, 2.97 kg of low-alkalinity sodium aluminate solution and 23.24 kg of water glass were added into a reactor, stirred and mixed evenly and aged at 30°C for 20 hours to obtain a directing agent.

[0045] 66.29kg of deionized water, 8.11kg of low-alkalinity sodium aluminate solution, 4.36kg of aluminum sulfate solution, 31.53kg of water glass and 2.65kg of directing agent were added to the reactor, stirred and mixed evenly to form a molecular sieve synthesis system. The total molar ratio of each material in the molecular sieve synthesis system is: SiO2 / Al2O3=6.5, Na2O / SiO2=0.5, H2O / SiO2=50. The above molecular sieve synthesis system was transferred to the reactor, hydrothermally crystallized at 95°C for 12 hours, filtered, and the obtained solid was washed with deionized water until the filtrate pH=8-9, and dried at 80°C for 12 hours to obtain Y molecular sieve.

[0046] Example 1

[0047] (1) Molding: 75 kg of low silicon X molecular sieve with a particle size of about 0.5 μm (SEM photo see Figure 2, silicon oxide / alumina molar ratio of 2.03, Li2O content of 11.9 mass%) and 25kg kaolin were mixed evenly, put into a turntable and rolled while spraying water to make the solid aggregate into small balls as the inner adsorbent layer, and then 3.95kg Y molecular sieve with a particle size of about 0.6μm was added (SEM photo see Figure 3 , the molar ratio of silicon oxide to aluminum oxide is 3.91, the cation is Na) and 1.32 kg of kaolin powder, continue to spray water and roll to form an outer adsorbent layer, and after sieving, small balls with a particle size of 300 to 850 microns are obtained.

[0048] (2) Drying: The beads prepared in step (1) were evenly spread to a bed thickness of 10 mm, and dried at 100°C in a flowing air atmosphere with the air staying in the adsorbent bed for 15 seconds. The drying was performed for 10 hours.

[0049] (3) Calcination: The small balls obtained after drying in step (2) are evenly spread out to a bed thickness of 8 mm and calcinated in a flowing air atmosphere. The air stays in the adsorbent bed for 8 seconds. The balls are treated at 200°C for 3 hours, 300°C for 3 hours, 400°C for 3 hours, and 500°C for 6 hours, with a heating rate of 2°C / min. After calcination, the temperature is cooled to room temperature under vacuum to obtain nitrogen oxygen separation adsorbent A.

[0050] The water content and separation performance of adsorbent A are shown in Table 1.

[0051] Example 2

[0052] The nitrogen-oxygen separation adsorbent B was prepared according to the method of Example 1, except that the bed thickness in step (2) was 18 mm and the drying temperature was 100° C. The bed thickness in step (3) was 15 mm and the heating rate was 3° C. / min.

[0053] The water content and separation performance of adsorbent B are shown in Table 1.

[0054] Example 3

[0055] The nitrogen-oxygen separation adsorbent C was prepared according to the method of Example 1, except that in step (2), it was dried at 100°C for 8 hours, and in step (3), it was treated at 180°C for 2 hours, 280°C for 2 hours, 380°C for 2 hours, and 470°C for 5 hours.

[0056] The water content and separation performance of adsorbent C are shown in Table 1.

[0057] Example 4

[0058] The nitrogen-oxygen separation adsorbent D was prepared according to the method of Example 1, except that in step (1), 60 kg of low-silicon X molecular sieve with a particle size of about 0.5 μm and 40 kg of attapulgite were mixed evenly, placed in a turntable and rolled while spraying water to aggregate the solids into small balls as the inner adsorbent layer, and then 5.22 kg of a mixed powder of Y molecular sieve with a particle size of about 0.6 μm and 3.48 kg of attapulgite were added, and water spraying and rolling were continued to form an outer adsorbent layer. After sieving, small balls with a particle size of 300 to 850 μm were obtained.

[0059] The water content and separation performance of adsorbent D are shown in Table 1.

[0060] Example 5

[0061] The nitrogen-oxygen separation adsorbent E was prepared according to the method of Example 4, except that in step (1), a low-silicon X molecular sieve with a particle size of about 4 μm (a silicon oxide / aluminum oxide molar ratio of 1.93, a Li2O content of 10.7 mass %) and a Y molecular sieve with a particle size of about 0.8 μm (a silicon oxide / aluminum oxide molar ratio of 4.62, a cation K) were used.

[0062] The water content and separation performance of adsorbent E are shown in Table 1.

[0063] Comparative Example 1

[0064] The nitrogen-oxygen separation adsorbent F was prepared according to the method of Example 1, except that (1) molding was performed by uniformly mixing 75 kg of low-silicon X molecular sieve (silicon oxide / aluminum oxide molar ratio of 2.03, Li2O content of 11.9 mass %) with a particle size of about 0.5 μm and 25 kg of kaolin, and placing the mixture in a rotating disk while rolling and spraying water to aggregate the solid into small balls. After screening, small balls with a particle size of 300 to 850 μm were obtained.

[0065] The water content and separation performance of adsorbent F are shown in Table 1.

[0066] Comparative Example 2

[0067] Adsorbent G was prepared according to the method of Example 1, except that the bed thickness in step (2) was 35 mm and the residence time of air in the adsorbent bed was 25 seconds.

[0068] The water content and separation performance of adsorbent G are shown in Table 1.

[0069] Comparative Example 3

[0070] Adsorbent H was prepared according to the method of Example 1, except that the bed thickness in step (3) was 35 mm and the residence time of air in the adsorbent bed was 25 seconds.

[0071] The water content and separation performance of adsorbent H are shown in Table 1.

[0072] Comparative Example 4

[0073] Adsorbent I was prepared according to the method of Example 1, except that the heating rate in step (3) was 10°C / min.

[0074] The water content and separation performance of adsorbent I are shown in Table 1.

[0075] Comparative Example 5

[0076] Adsorbent J was prepared according to the method of Example 1, except that step (3) did not use staged calcination, but directly raised the temperature to 500° C. and calcined for 6 h.

[0077] The water content and separation performance of adsorbent J are shown in Table 1.

[0078] Comparative Example 6

[0079] Adsorbent K was prepared according to the method of Example 1, except that in step (3), the adsorbent was treated at 200°C for 1 hour, 300°C for 1 hour, and 400°C for 1 hour.

[0080] The water content and separation performance of adsorbent K are shown in Table 1.

[0081] Table 1

[0082] Instance number Adsorbent No. Water content, mass% Oxygen volume concentration, % 1 A 0.32 95.1 2 B 0.35 93.5 3 C 0.56 94.2 4 D 0.30 92.3 5 E 0.34 94.5 Comparative Example 1 F 0.33 83.6 Comparative Example 2 G 0.26 78.2 Comparative Example 3 H 0.15 41.3 Comparative Example 4 I 0.25 76.5 Comparative Example 5 J 0.22 66.9 Comparative Example 6 K 3.66 85.5

[0083] It can be seen from Table 1 that the oxygen volume concentration obtained by separating air using the adsorbents described in Comparative Examples 1 to 6 is lower than that of the adsorbents described in Examples 1 to 5.

[0084] The adsorbent described in Comparative Example 1 does not contain an outer adsorbent layer, and carbon dioxide and water vapor in the air are adsorbed by the low-silicon X molecular sieve, resulting in a decrease in its nitrogen and oxygen separation performance.

[0085] In Comparative Example 2, when preparing the adsorbent G, due to the thicker bed thickness in step (2), the air stays in the adsorbent bed for a longer time, resulting in excessive contact time between water vapor and the adsorbent during the drying process, which destroys the structure of the molecular sieve and reduces the separation performance of the adsorbent. At the same time, since the molecular sieve structure is destroyed, the water absorption capacity of the adsorbent is reduced, and therefore the water content of the adsorbent is low.

[0086] In comparative example 3, when preparing the adsorbent H, the bed thickness in step (3) is relatively thick, and the air stays in the adsorbent bed for a long time, resulting in excessive contact time between water vapor and the adsorbent during the roasting process, which destroys the structure of the molecular sieve, reduces the separation performance of the adsorbent, and reduces the water content.

[0087] In comparative example 4, when preparing the adsorbent I, the heating rate in step (3) was too fast, which resulted in the destruction of the molecular sieve structure, reduced separation performance of the adsorbent, and decreased water content.

[0088] In comparative example 5, when preparing the adsorbent J, step (3) does not use staged calcination, resulting in too fast a heating rate, which leads to the destruction of the molecular sieve structure, the decrease of the separation performance of the adsorbent, and the reduction of the water content.

[0089] In Comparative Example 6, when preparing the adsorbent K, the calcination time was too short and the maximum temperature was too low, resulting in a higher water content in the adsorbent and a decrease in the adsorption and separation performance.

Claims

1. A nitrogen-oxygen separation adsorbent, characterized in that: The invention comprises an inner adsorbent layer and an outer adsorbent layer, wherein the inner adsorbent layer comprises a low-silicon X molecular sieve and a binder, and the outer adsorbent layer comprises a Y molecular sieve and a binder, wherein the cation position of the low-silicon X molecular sieve is occupied by Li, and the cation position of the Y molecular sieve is occupied by at least one of Na and K.

2. The adsorbent according to claim 1, characterized in that The inner adsorbent layer comprises 50-79 mass % of low-silicon X molecular sieve and 21-50 mass % of binder, based on the total amount of the inner adsorbent layer.

3. The adsorbent according to claim 1, characterized in that The outer adsorbent layer comprises 50-79 mass % of Y molecular sieve and 21-50 mass % of binder, based on the total amount of the outer adsorbent layer.

4. The adsorbent according to claim 1, characterized in that The silicon oxide / aluminum oxide molar ratio of the low silicon X molecular sieve is 1.90-2.05, and the silicon oxide / aluminum oxide molar ratio of the Y molecular sieve is 3.2-5.

5.

5. The adsorbent according to claim 1, characterized in that The content of the low silicon X molecular sieve in the adsorbent is 90-96% by mass of the total amount of the molecular sieve in the adsorbent.

6. The adsorbent according to claim 1, characterized in that The crystal grain size of the low-silicon X molecular sieve is 0.4 to 10 microns.

7. The adsorbent according to claim 1, characterized in that The content of Li2O in the low-silicon X molecular sieve is greater than or equal to 10 mass %.

8. The adsorbent according to claim 1, characterized in that The crystal grain size of the Y molecular sieve is 0.1 to 0.8 microns.

9. The adsorbent according to claim 1, characterized in that The binder is selected from one of kaolin, halloysite and attapulgite.

10. The adsorbent according to claim 1, characterized in that The water content of the adsorbent is less than or equal to 0.6% by mass.

11. A method for preparing the nitrogen-oxygen separation adsorbent according to claim 1, characterized in that: The following steps are involved: (1) low silicon X molecular sieve and binder are mixed uniformly in a mass ratio of 50-79:21-50, placed in a rotating disk and rolled while spraying water to aggregate the solid into small balls as an inner adsorbent layer, and then a powder of Y molecular sieve and binder mixed in a mass ratio of 50-79:21-50 is added, and water is continued to be sprayed and rolled to form an outer adsorbent layer, and small balls with a particle size of 300-850 μm are obtained after screening; (2) laying the pellets obtained in step (1) flat to a bed thickness of less than or equal to 30 mm, and drying them in a flowing air atmosphere at a temperature of 60 to 120° C., preferably 80 to 100° C., for 6 to 12 hours; (3) The dried pellets obtained in step (2) are spread out to a bed thickness of less than or equal to 20 mm, and are calcined in a flowing air atmosphere in stages, successively at 150-220° C. for 1-3 hours, 250-320° C. for 1-3 hours, 350-420° C. for 1-3 hours, and 450-540° C. for 4-8 hours.

12. The method according to claim 11, characterized in that In step (1), the total amount of water added for rolling into balls is 5 to 16% by weight of the total amount of solid powder.

13. The method according to claim 11, characterized in that In step (2) or (3), the residence time of air in the adsorbent bed is less than or equal to 20 seconds.

14. The method according to claim 11, characterized in that The staged calcination in step (3) has a heating rate of 0.5 to 5°C / min, preferably 1 to 3°C / min.

15. A method for preparing oxygen from air using the nitrogen-oxygen separation adsorbent according to claims 1 to 10 or the nitrogen-oxygen separation adsorbent prepared by the method of claims 11 to 14.

Citation Information

Patent Citations

  • A para-xylene adsorbent and a preparing method thereof

    CN108525643A

  • Core-shell molecular sieve, synthesis method and application thereof

    CN112694101A

  • Preparing method for adsorbeng for selectively adsorbing and separating aromatic isomer

    CN1339334A

  • High purity oxygen production by presssure swing adsorption

    US20020144596A1

  • Performance stability in shallow beds in pressure swing adsorption systems

    US20080083332A1