Heterogeneous catalyst for advanced oxidation of wastewater, preparation method of heterogeneous catalyst and advanced oxidation method
By using activated carbon, γ-Al2O3 and graphene composites as catalysts in Fenton Advanced oxidation method, combined with advanced oxidation and salting treatment, the problems of sludge generation and low COD removal rate in high-concentration PVA wastewater treatment were solved, and the problem of low COD removal rate was achieved. Efficient removal and catalyst regeneration.
Patent Information
- Application Number
- CN202411010300.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing Fenton Advanced oxidation method will produce a large amount of sludge and high catalyst usage when treating wastewater with high concentrations of PVA, and the COD removal rate is low, making it difficult to effectively reduce the viscosity of the wastewater and affect the treatment effect.
Using a composite containing activated carbon, γ-Al2O3 and graphene as a heterogeneous catalyst, combined with advanced oxidation and salting treatment, degradation of PVA through hydroxyl radicals, reducing the viscosity of wastewater, and forming a mesh whole through borax to perform PVA and COD. Remove.
The oxidation efficiency and salting treatment of advanced oxidation treatment are improved, the sludge generation and catalyst usage are reduced, and the high concentration of PVA and COD are effectively removed, secondary pollution is avoided, and the catalyst recycling and recycling are promoted.
Smart Images

Figure CN119056432A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wastewater advanced oxidation catalysts, and in particular to a wastewater advanced oxidation heterogeneous catalyst, a preparation method thereof and an advanced oxidation method. Background Art
[0002] Polyvinyl alcohol (PVA) is a water-soluble polymer with good adhesion, mechanical properties and stability. As an important industrial raw material, it is widely used in the production of coatings, adhesives, paper processing agents, emulsifiers, dispersants and films. Its application range covers textiles, food, medicine, construction, wood processing, papermaking, printing, agriculture, steel, polymer chemicals and other industries. PVA is a typical biodegradable polymer. The COD (Chemical Oxygen Demand) of wastewater containing PVA is high and its biodegradability is poor. Direct discharge will seriously pollute the water body, so it is necessary to treat the wastewater containing PVA.
[0003] There are many existing methods for treating PVA-containing wastewater. The main current methods for treating PVA-containing wastewater are introduced in a tabular form below. See Table 1 for details. As can be seen from Table 1, in the current treatment process for PVA-containing wastewater, the PVA concentration of PVA-containing wastewater is mostly below 5g / L. It is understood that the current treatment method for PVA-containing wastewater with a PVA concentration of more than 30g / L (referred to as "high-concentration PVA-containing wastewater" in the present invention) is still very rare and lacks data and technical support.
[0004]
[0005] The applicant of the present invention is faced with the problem of treating wastewater containing high concentration of PVA. After research, an attempt was made to use a method based on chemical coagulation (salting out treatment). Because the salting out treatment method can treat wastewater with relatively high PVA concentration, and can simultaneously reduce the concentration of PVA and COD, unlike the Fenton advanced oxidation method, the removal rate of COD will decrease after degrading PVA, and unlike the biological method, there are problems of long treatment time and high cost. In addition, compared with the membrane separation method, the cost can be greatly reduced. However, experiments have found that the effect of using salting out treatment alone to treat wastewater containing high concentration of PVA is not ideal. Further research found that: due to the high viscosity of wastewater containing high concentration of PVA, the salting out agent is difficult to disperse evenly during the process of adding wastewater containing high concentration of PVA, resulting in the salting out effect is not obvious.
[0006] Based on the above research, a method for treating wastewater containing high concentration of PVA was further developed, which method comprises: first, subjecting the high concentration of PVA wastewater to advanced oxidation treatment; then, subjecting the wastewater after the advanced oxidation treatment to salting-out treatment to simultaneously remove the remaining PVA and COD in the wastewater. The main mechanism of action of the above advanced oxidation treatment is to promote the generation of hydroxyl radicals of hydrogen peroxide through the contact reaction between the catalyst and hydrogen peroxide. In the above method for treating wastewater containing high concentration of PVA, the significance of combining the advanced oxidation treatment with the salting-out treatment is that the viscosity of the wastewater can be reduced by degrading PVA with hydroxyl radicals having strong oxidizing properties, thereby greatly improving the effect of the salting-out treatment. In addition, for wastewater containing high concentration of PVA, the concentration of COD will increase after the advanced oxidation treatment degrades PVA, while the main mechanism of salting-out treatment is to combine PVA molecules to form a network through the special chemical properties of borax, and then remove the water in them by adding salting-out agent and coagulant, so as to achieve the recovery of PVA and the removal of COD and PVA in wastewater. In other words, salting-out treatment not only removes PVA, but also reduces the content of COD in the water. Therefore, salting-out treatment just makes up for the defect of low COD removal rate of advanced oxidation treatment.
[0007] However, advanced oxidation treatment is currently mainly based on the Fenton advanced oxidation process, which uses an iron salt homogeneous catalytic system and produces a large amount of sludge, causing secondary pollution. In addition, the Fenton advanced oxidation process uses a large amount of catalyst and the utilization rate of hydrogen peroxide is not high. Summary of the invention
[0008] The purpose of the present invention is to provide a heterogeneous catalyst for advanced oxidation of wastewater, a preparation method thereof and an advanced oxidation method, and to solve the technical problems mentioned in the above background technology that the Fenton advanced oxidation method using an iron salt homogeneous catalytic system will produce a large amount of sludge causing secondary pollution and a large amount of catalyst is required.
[0009] In the first aspect, a heterogeneous catalyst for advanced oxidation of wastewater is provided, comprising: a carrier, wherein the carrier is a composite comprising activated carbon, γ-Al2O3 and graphene, wherein the γ-Al2O3 comes from hydrotalcite in the carrier preparation raw material, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; a metal oxide, wherein the metal oxide is a composite metal oxide comprising manganese and cerium, the atomic number ratio of manganese to cerium in the composite metal oxide is (1-3):1; and the loading mass fraction of manganese element in the metal oxide in the heterogeneous catalyst for advanced oxidation of wastewater is 4%-20%.
[0010] In the carrier of the wastewater advanced oxidation heterogeneous catalyst, the activated carbon has a large surface area and good adsorption performance, which can provide a carrier for the metal oxide and improve the activity of the catalyst. γ-Al2O3 has high thermal stability and mechanical strength, which can provide support for the activated carbon to prevent its deformation and breakage. The mass ratio of activated carbon to γ-Al2O3 is (1-5):1, so the activated carbon is the main component in the carrier, which can play its adsorption role and improve the adsorption capacity of the catalyst for pollutants, and the addition of γ-Al2O3 is mainly to improve the thermal stability and mechanical strength of the carrier, thereby realizing the regeneration and recycling of the wastewater advanced oxidation heterogeneous catalyst.
[0011] In the carrier of the wastewater advanced oxidation heterogeneous catalyst, the main role of graphene is to enhance the conductivity of the catalyst and improve the electron transfer efficiency of the catalyst surface. This is crucial in the advanced oxidation process because it can promote the generation of active oxidation species (such as hydroxyl radicals) and improve oxidation efficiency. Better conductivity can also enhance the interaction between the catalyst and the pollutant and improve the overall catalytic efficiency. In addition, graphene can further enhance the mechanical properties of the composite, thus providing conditions for further increasing the specific surface area of activated carbon. The significance of setting the content of graphene in the composite to 0.5wt%-2wt% is that when the content of graphene in the composite is above 0.5wt%, the conductivity of the wastewater advanced oxidation heterogeneous catalyst can be significantly improved; setting the content of graphene to less than 2wt% is conducive to controlling costs and avoiding graphene agglomeration during the preparation of the wastewater advanced oxidation heterogeneous catalyst.
[0012] The composite metal oxide of the wastewater advanced oxidation heterogeneous catalyst is composed of two metal oxides, manganese and cerium, which can play a synergistic catalytic role and improve the activity of the catalyst. The ratio of the number of manganese atoms to cerium atoms is (1-3): 1. Therefore, the manganese element plays a major role in the catalyst. Its redox potential is low, and it can effectively activate hydrogen peroxide to produce hydroxyl radicals; and the cerium element can promote the redox cycle of the manganese element and improve the catalytic activity. The loading amount of the manganese element is one of the important factors affecting the catalytic activity. Too low loading amount will lead to insufficient catalytic activity, while too high loading amount will cause the metal oxide particles to agglomerate and reduce the catalytic activity. It is more appropriate to set the loading mass fraction of the manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst to 4%-20%.
[0013] In the second aspect, a method for preparing a heterogeneous catalyst for advanced oxidation of wastewater is provided, comprising: fully mixing carbon powder, hydrotalcite, graphene powder, a binder and an acid solution and forming them into granules, and then activating the granules. The conditions of the activation treatment are: using an inert gas as a carrier of water vapor, a water-carbon ratio of 0.4 ml / g-0.8 ml / g, a reaction temperature of 500°C-700°C, a reaction time of 50 minutes-80 minutes, and obtaining a carrier, wherein the carrier is a composite comprising activated carbon and γ-Al2O3, wherein the activated carbon and the pressurized carbon in the composite are The mass ratio of γ-Al2O3 calculated based on hydrotalcite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; a manganese metal salt solution and a cerium metal salt solution are mixed in a manganese to cerium atomic ratio of (1-3):1 to form a mixed solution, and then the carrier is immersed in the mixed solution, and after immersion, the carrier is taken out, washed with deionized water, and calcined at 400°C-500°C for 2 hours-6 hours to obtain a wastewater advanced oxidation heterogeneous catalyst, wherein the loading mass fraction of manganese element in the wastewater advanced oxidation heterogeneous catalyst is 4%-20%.
[0014] In a third aspect, a method for advanced oxidation of wastewater is provided, wherein the wastewater is set to have a wastewater advanced oxidation heterogeneous catalyst content of 7g / L-20g / L and is under continuous stirring, and hydrogen peroxide is added in an amount of 1mL / L-1L / L to carry out an oxidation reaction, wherein the wastewater advanced oxidation heterogeneous catalyst comprises a carrier and a metal oxide loaded on the carrier, the carrier comprises a composite of activated carbon, γ-Al2O3 and graphene, wherein the γ-Al2O3 comes from hydrotalcite in the carrier preparation raw material, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; the metal oxide is a composite metal oxide comprising manganese and cerium, the ratio of the number of manganese atoms to cerium atoms in the composite metal oxide is (1-3):1, and the loading mass fraction of manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst is 4%-20%.
[0015] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. Additional aspects and advantages provided by the present invention will be partially given in the following description, partially become apparent from the following description, or be learned through practice. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings constituting a part of the present invention are used to assist the understanding of the present invention. The contents provided in the drawings and their related descriptions in the present invention can be used to explain the present invention, but do not constitute improper limitations on the present invention.
[0017] Figure 1This is a schematic diagram of a method for treating high-concentration PVA wastewater according to an embodiment of the present invention.
[0018] Figure 2 for Figure 1 Schematic diagram of the regeneration tank.
[0019] Figure 3 This is the XRD pattern of Mn-Ce / γ-Al2O3-AC numbered A6.
[0020] Figure 4 This is the XRD pattern of Mn-Ce / γ-Al2O3-AC-graphene numbered A9. DETAILED DESCRIPTION
[0021] The present invention is described clearly and completely below in conjunction with the accompanying drawings. A person skilled in the art will be able to implement the present invention based on these descriptions. Before describing the present invention in conjunction with the accompanying drawings, it should be particularly noted that: The technical solutions and technical features provided in each section, including the following description, can be combined with each other without conflict. In addition, where possible, these technical solutions, technical features and related combinations can be assigned specific technical themes and protected by relevant patents.
[0022] The embodiments of the present invention involved in the following description are generally only a part of the embodiments rather than all the embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work should fall within the scope of patent protection.
[0023] The terms "include", "comprising" and any variations thereof in this specification and the corresponding claims and related parts are intended to cover non-exclusive inclusions. Other related terms and units can be reasonably interpreted based on the relevant contents provided by the present invention.
[0024] Figure 1 Schematic diagram of a method for treating high-concentration PVA wastewater according to an embodiment of the present invention. Figure 1 As shown, the method for treating high-concentration PVA wastewater is used to treat high-concentration PVA wastewater with a PVA concentration in the concentration range of 30g / L-120g / L and above the upper limit of the concentration range, comprising: first, performing advanced oxidation treatment on the high-concentration PVA wastewater in an advanced oxidation tank 11; then, performing salting-out treatment on the wastewater after the advanced oxidation treatment in a salting-out tank 12 to simultaneously remove the remaining PVA and COD in the wastewater.
[0025] The PVA concentration of the high-concentration PVA wastewater may be greater than 30 g / L. In some cases, the PVA concentration of the high-concentration PVA wastewater is above 50 g / L, for example, the PVA concentration of the high-concentration PVA wastewater is 50 g / L-100 g / L. In some cases, the PVA concentration of the high-concentration PVA wastewater may be greater than 120 g / L.
[0026] The main mechanism of action of the above-mentioned advanced oxidation treatment is to promote the generation of hydroxyl radicals of hydrogen peroxide through the contact reaction between the catalyst and hydrogen peroxide. In the above-mentioned treatment method of wastewater containing high concentration of PVA, the significance of combining the advanced oxidation treatment with the salting-out treatment is that the viscosity of the wastewater can be reduced by degrading PVA with hydroxyl radicals having strong oxidizing properties, thereby greatly improving the effect of the salting-out treatment.
[0027] The significance of combining advanced oxidation treatment with salting-out treatment is that for wastewater containing high-concentration PVA, the COD concentration will increase after the advanced oxidation treatment degrades PVA, and the main mechanism of salting-out treatment is to combine PVA molecules to form a network through the special chemical properties of borax, and then remove the water in them by adding salting-out agents and coagulants, so as to achieve the recovery of PVA and the removal of COD and PVA in wastewater. In other words, salting-out treatment removes PVA and reduces the COD content in the water. Therefore, salting-out treatment just makes up for the defect of low COD removal rate of advanced oxidation treatment.
[0028] Advanced oxidation treatment is currently mainly based on the Fenton advanced oxidation process, which uses an iron salt homogeneous catalytic system and produces a large amount of sludge, causing secondary pollution. In addition, the Fenton advanced oxidation process uses a large amount of catalyst and the utilization rate of hydrogen peroxide is not high.
[0029] In order to avoid the above-mentioned defects when using the Fenton advanced oxidation method, the specific method used in the above-mentioned advanced oxidation treatment is: in the advanced oxidation tank 11, the high-concentration PVA wastewater is set at a pH value of 6-8, a temperature of 70°C-90°C, the wastewater advanced oxidation heterogeneous catalyst content is 7g / L-20g / L and is under continuous stirring, and hydrogen peroxide is added in an amount of 1mL / L-1L / L to carry out an oxidation reaction, wherein the wastewater advanced oxidation heterogeneous catalyst comprises a carrier and a metal oxide loaded on the carrier, the carrier comprises a composite of activated carbon and γ-Al2O3, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, the metal oxide is a composite metal oxide comprising manganese and cerium, the ratio of the number of manganese atoms to cerium atoms in the composite metal oxide is (1-3):1, and the loading mass fraction of manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst is 4%-12%.
[0030] The above-mentioned advanced oxidation treatment uses a novel wastewater advanced oxidation heterogeneous catalyst, which can be efficiently separated from the wastewater by filtration after use, and then recycled after regeneration. Therefore, the problem of secondary pollution caused by a large amount of sludge generated by the Fenton advanced oxidation process is solved.
[0031] In the wastewater advanced oxidation heterogeneous catalyst: the activated carbon has a large surface area and good adsorption performance, which can provide a carrier for the metal oxide and improve the activity of the catalyst. γ-Al2O3 has high thermal stability and mechanical strength, which can provide support for the activated carbon to prevent its deformation and breakage. The mass ratio of activated carbon to γ-Al2O3 is (1-5):1, so the activated carbon is the main component in the carrier, which can play its adsorption role and improve the adsorption capacity of the catalyst for pollutants, while the addition of γ-Al2O3 is mainly to improve the thermal stability and mechanical strength of the carrier, thereby realizing the regeneration and recycling of the wastewater advanced oxidation heterogeneous catalyst. The composite metal oxide is composed of two metal oxides, manganese and cerium, which can play a synergistic catalytic role and improve the activity of the catalyst. The atomic number ratio of manganese to cerium is (1-3):1, so the manganese element plays a major role in the catalyst, and its redox potential is low, which can effectively activate hydrogen peroxide to produce hydroxyl radicals; and the cerium element can promote the redox cycle of the manganese element and improve the catalytic activity. The loading amount of manganese element is one of the important factors affecting catalytic activity. Too low loading amount will lead to insufficient catalytic activity, while too high loading amount will cause metal oxide particles to agglomerate and reduce catalytic activity. It is more appropriate to set the loading mass fraction of manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst to 4%-12%.
[0032] Since a heterogeneous catalyst for advanced oxidation of wastewater is used, in the above-mentioned method for treating wastewater containing high-concentration PVA, a filter 13 is used to filter the wastewater after the advanced oxidation treatment, the filtered wastewater advanced oxidation heterogeneous catalyst is regenerated, and then the regenerated wastewater advanced oxidation heterogeneous catalyst is returned to the advanced oxidation treatment, and the filtered wastewater is subjected to the salting-out treatment.
[0033] The above-mentioned heterogeneous catalyst for advanced oxidation of wastewater can be further improved as follows: the heterogeneous catalyst for advanced oxidation of wastewater comprises: a carrier, wherein the carrier is a composite comprising activated carbon, γ-Al2O3 and graphene, wherein the γ-Al2O3 comes from hydrotalcite in the raw material for preparing the carrier, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; a metal oxide, wherein the metal oxide is a composite metal oxide comprising manganese and cerium, and the atomic number ratio of manganese to cerium in the composite metal oxide is (1-3):1; and the loading mass fraction of manganese element in the metal oxide in the heterogeneous catalyst for advanced oxidation of wastewater is 4%-20%.
[0034] Since graphene is added to the composite, the main function of graphene is to enhance the conductivity of the catalyst and improve the electron transfer efficiency on the catalyst surface. This is very important in the advanced oxidation process because it can promote the generation of active oxidative species (such as hydroxyl radicals) and improve the oxidation efficiency. Better conductivity can also enhance the interaction between the catalyst and the pollutant and improve the overall catalytic efficiency. In addition, graphene can further enhance the mechanical properties of the composite, thus providing conditions for further increasing the specific surface area of the activated carbon, so that the loading amount of the metal oxide can be increased. The significance of setting the content of graphene in the composite to 0.5wt%-2wt% is that when the content of graphene in the composite is above 0.5wt%, the conductivity of the heterogeneous catalyst for advanced oxidation of wastewater can be significantly improved; setting the content of graphene to below 2wt% is conducive to controlling costs and avoiding graphene agglomeration during the preparation of heterogeneous catalyst for advanced oxidation of wastewater.
[0035] In the above-mentioned method for treating high-concentration PVA wastewater, regeneration treatment can be performed through the regeneration tank 14, and the regeneration treatment comprises: placing the wastewater advanced oxidation heterogeneous catalyst in running water at a temperature of 50°C-80°C for more than 90 minutes.
[0036] Figure 2 for Figure 1 Schematic diagram of the regeneration tank. Figure 2As shown, the regeneration tank 14 adopts a stepped regeneration tank composed of a plurality of flow-type regeneration tanks 141 connected end to end in sequence and arranged obliquely. The inclination angles of these flow-type regeneration tanks 141 and the roughness of the contact surface with the wastewater advanced oxidation heterogeneous catalyst are specially designed so that the wastewater advanced oxidation heterogeneous catalyst passes through the stepped regeneration tank from top to bottom along with the water flow (the wastewater advanced oxidation heterogeneous catalyst is put into the step-type regeneration tank from the top and discharged from the bottom of the step-type regeneration tank) within a set time (such as 90 minutes).
[0037] During operation, the wastewater advanced oxidation heterogeneous catalyst slowly moves downward with the water flow and passes through the flow-type regeneration tanks 141 at each level in sequence. The residence time of the wastewater advanced oxidation heterogeneous catalyst in the stepped regeneration tank is precisely controlled to ensure that the regeneration is completed within the set time. The regenerated wastewater advanced oxidation heterogeneous catalyst is discharged from the bottom of the stepped regeneration tank and returned to the advanced oxidation tank 11, and the upper part of the stepped regeneration tank is continuously replenished with new wastewater advanced oxidation heterogeneous catalyst and water, so that the regeneration process is continuous. In addition, since the wastewater advanced oxidation heterogeneous catalyst is in full contact with the water flow, the regeneration effect is ideal.
[0038] Generally speaking, the salting-out treatment includes: setting the wastewater at a pH value of 6-8 and a temperature of 50°C-90°C, adding a cross-linking agent, a salting-out agent, and a coagulant aid to react, wherein the cross-linking agent is borax, and the amount of borax added is 1g / L-10g / L, the salting-out agent is sodium sulfate, and the amount of sodium sulfate added is 10g / L-20g / L, and the coagulant aid is sodium bicarbonate, and the amount of sodium bicarbonate added is 0.8g / L to 2g / L.
[0039] Experimental example 1. Heterogeneous catalysts for advanced oxidation of wastewater and their preparation 1.1 Preparation method of heterogeneous catalyst for advanced oxidation of wastewater (Implementation plan 1) First, carbon powder, hydrotalcite, a binder (specifically coal tar) and nitric acid are fully mixed and formed into pellets, and then the pellets are activated. The activation treatment conditions are: using inert gas as a carrier of water vapor, a water-to-carbon ratio of 0.4 ml / g, a reaction temperature of 600°C, and a reaction time of 65 minutes to obtain a carrier, which is a composite of activated carbon and γ-Al2O3.
[0040] Then, a manganese nitrate solution and a cerium nitrate solution are mixed to form a mixed solution, and then the carrier is immersed in the mixed solution. After the immersion, the carrier is taken out, washed with deionized water, and then calcined at 450° C. for 4 hours to obtain a wastewater advanced oxidation heterogeneous catalyst (hereinafter represented by Mn-Ce / γ-Al2O3-AC).
[0041] In order to ensure the impregnation effect, when the carrier is immersed in the mixed solution, it is shaken at 35° C. for 10 h to 16 h by a constant temperature oscillator.
[0042] The carbon powder is specifically made by cutting fresh square bamboo into pieces, drying them, and then carbonizing them at 450°C.
[0043] The above-mentioned nitric acid may also be replaced by hydrochloric acid, acetic acid or the like; the above-mentioned manganese nitrate solution may also be replaced by manganese sulfate solution or manganese acetate solution; the above-mentioned cerium nitrate solution may also be replaced by cerium chloride solution.
[0044] The above-mentioned molding is specifically extrusion molding. Mn-Ce / γ-Al2O3-AC is a granular material, and the granular material is specifically a cylinder with a length of 1cm-2cm and a diameter of 2mm-6mm.
[0045] 1.2 Preparation method of heterogeneous catalyst for advanced oxidation of wastewater (Implementation Plan 2) First, carbon powder, graphene powder (single-layer graphene, prepared by chemical vapor deposition), hydrotalcite, a binder (specifically coal tar) and nitric acid are fully mixed and formed into granules, and then the granules are activated. The conditions of the activation treatment are: using inert gas as a carrier of water vapor, a water-to-carbon ratio of 0.8 ml / g, a reaction temperature of 600°C, and a reaction time of 65 minutes to obtain a carrier, which is a composite of activated carbon, γ-Al2O3 and graphene.
[0046] Then, a manganese nitrate solution and a cerium nitrate solution were mixed to form a mixed solution, and then the carrier was immersed in the mixed solution. After the immersion, the carrier was taken out, washed with deionized water, and then calcined at 450° C. for 4 hours to obtain a wastewater advanced oxidation heterogeneous catalyst (hereinafter represented by Mn-Ce / γ-Al2O3-AC-graphene).
[0047] In order to ensure the impregnation effect, when the carrier is immersed in the mixed solution, it is shaken at 35° C. for 10 h to 16 h by a constant temperature oscillator.
[0048] The carbon powder is specifically made by cutting fresh square bamboo into pieces, drying them, and then carbonizing them at 450°C.
[0049] The above-mentioned nitric acid may also be replaced by hydrochloric acid, acetic acid or the like; the above-mentioned manganese nitrate solution may also be replaced by manganese sulfate solution or manganese acetate solution; the above-mentioned cerium nitrate solution may also be replaced by cerium chloride solution.
[0050] The above-mentioned molding is specifically extrusion molding. Mn-Ce / γ-Al2O3-AC-graphene is a granular material, and the granular material is specifically a cylinder with a length of 1 cm-2 cm and a diameter of 2 mm-6 mm.
[0051] 1.3 Numbering and corresponding properties of heterogeneous catalysts for wastewater advanced oxidation Different Mn-Ce / γ-Al2O3-AC and Mn-Ce / γ-Al2O3-AC-graphene were prepared by the above preparation method, and their numbers and corresponding properties are shown in Table 2.
[0052]
[0053] The XRD pattern of Mn-Ce / γ-Al2O3-AC numbered A6 is shown in Figure 3 The XRD pattern of Mn-Ce / γ-Al2O3-AC-graphene numbered A9 is shown in Figure 4 shown.
[0054] 2. High concentration PVA wastewater treatment experiment 2.1 Experimental method for treatment of high-concentration PVA wastewater 1L of high-concentration PVA wastewater with a concentration of 100g / L was placed in a catalytic oxidation experimental container, and then a buffer solution was slowly added to adjust the pH value to neutral, and then 10g / L of Mn-Ce / γ-Al2O3-Ac or Mn-Ce / γ-Al2O3-Ac-graphene was added, and then the temperature in the catalytic oxidation experimental container was adjusted, and the stirring device was turned on to keep the solution stirred at a uniform speed, and finally 1mL / L of hydrogen peroxide was added to react for 2h, and the liquid and Mn-Ce / γ-Al2O3-AC or Mn-Ce / γ-Al2O3-Ac-graphene were obtained after filtration.
[0055] Then, 500 mL of the above liquid was placed in a salting-out experiment container, the liquid temperature in the salting-out experiment container was adjusted and the pH was adjusted to neutral by a buffer solution, and then a cross-linking agent, a salting-out agent and a coagulant were added to the salting-out recovery pool, respectively, and after reacting for 1 hour, the supernatant was taken to determine the remaining COD and PVA content, thereby calculating the removal rate of COD and PVA. The cross-linking agent is borax, the salting-out is sodium sulfate, and the coagulant is sodium bicarbonate.
[0056] 2.2 Numbers and corresponding attributes of high-concentration PVA wastewater treatment experiments The numbers and corresponding attributes of the high-concentration PVA wastewater treatment experiments are shown in Table 3.
[0057]
[0058] 3. Mn-Ce / γ-Al2O3-AC regeneration experiment 3.1 Experimental method of Mn-Ce / γ-Al2O3-AC regeneration 1L of PVA-containing wastewater with a concentration of 10g / L was placed in a catalytic oxidation experimental container, and a buffer solution was slowly added to adjust the pH value to neutral. Then 10g / L of Mn-Ce / γ-Al2O3-AC (No. A6) was added, and then the temperature in the catalytic oxidation experimental container was adjusted to 80°C, and the stirring device was turned on to keep the solution stirred at a uniform speed. Finally, 1mL / L of hydrogen peroxide was added to react for 2h, and the liquid and Mn-Ce / γ-Al2O3-AC were obtained after filtration.
[0059] The PVA of the liquid is tested. The PVA determination method is as follows: According to the spectrophotometric method for determining the content of polyvinyl alcohol in wastewater, take 1 mL of the test liquid, dilute it to 20 mL, add 10 mL of boric acid solution, then add 1 mL-2 mL of water, add 2 mL of iodine solution, and finally make the volume to 50 mL; take the solution and measure the absorbance at 680 nm to calculate the removal rate.
[0060] Take the filtered Mn-Ce / γ-Al2O3-AC and put it into the regeneration reaction test container. Pass running water of a certain temperature at a flow rate of 100mL / min. After leaving it for a certain period of time, take out the regenerated Mn-Ce / γ-Al2O3-AC and place it in an oven at 105℃ for drying. Use it again to calculate the regeneration rate.
[0061]
[0062] Wherein: β is the regeneration rate, unit is %, P1 is the PVA degradation rate after the first use, unit is %, and P2 is the PVA degradation rate after the second use, unit is %.
[0063] The results of the regeneration experiment are shown in Table 4.
[0064]
[0065] 4. Strength comparison experiment between Mn-Ce / γ-Al2O3-AC and Mn-Ce / γ-Al2O3-AC-graphene Twenty pieces of Mn-Ce / γ-Al2O3-AC numbered A6 and 20 pieces of Mn-Ce / γ-Al2O3-AC-graphene numbered A9 were taken, and the compressive strength and wear resistance of the samples were tested in the following ways.
[0066] a. Compression strength test: Place 10 samples of each type on an activated carbon compression strength tester (manufactured in accordance with the requirements of GB / T30202.3-2013), increase the pressure at a constant rate (1mm / min) until the sample breaks, record the maximum pressure when it breaks, repeat the test for all samples, and calculate the average value.
[0067] b. Wear resistance test: Place 10 samples of each type into a standard wear resistance test device (rotating drum), rotate at a fixed speed for 30 minutes, take out the samples, sieve them with a standard sieve (mm sieve), weigh the mass of the remaining samples on the sieve, calculate the wear rate, and calculate the average value.
[0068] The average compressive strength of Mn-Ce / γ-Al2O3-AC numbered A6 is 2.4 MPa, and the average compressive strength of Mn-Ce / γ-Al2O3-AC-graphene numbered A9 is 2.6 MPa.
[0069] The above is a description of the relevant contents of the present invention. A person skilled in the art will be able to implement the present invention based on these descriptions. Based on the above contents of this specification, all other embodiments obtained by a person skilled in the art without making creative work should fall within the scope of the present invention.
Claims
1. A heterogeneous catalyst for advanced oxidation of wastewater, characterized in that: include: A carrier, wherein the carrier is a composite comprising activated carbon, γ-Al2O3 and graphene, wherein the γ-Al2O3 comes from hydrotalcite in the carrier preparation raw material, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; a metal oxide, wherein the metal oxide is a composite metal oxide comprising manganese and cerium, the atomic number ratio of manganese to cerium in the composite metal oxide is (1-3):1; and the loading mass fraction of manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst is 4%-20%.
2. The wastewater advanced oxidation heterogeneous catalyst according to claim 1, characterized in that: The mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is 3:
1.
3. The wastewater advanced oxidation heterogeneous catalyst according to claim 1, characterized in that: The granular material is a cylinder with a length of 1 cm to 2 cm and a diameter of 2 mm to 6 mm.
4. A method for preparing a heterogeneous catalyst for advanced oxidation of wastewater, characterized in that: include: After carbon powder, hydrotalcite, graphene powder, adhesive and acid solution are fully mixed and formed into pellets, the pellets are activated. The activation treatment conditions are as follows: inert gas is used as a carrier of water vapor, the water-carbon ratio is 0.4 ml / g-0.8 ml / g, the reaction temperature is 500°C-700°C, and the reaction time is 50 minutes-80 minutes to obtain a carrier, which is a composite of activated carbon and γ-Al2O3, wherein the mass of the activated carbon and γ-Al2O3 in the composite is 0.1% to 0.1% of the γ-Al2O3 calculated as hydrotalcite. The ratio is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; a manganese metal salt solution and a cerium metal salt solution are mixed in a manganese to cerium atomic ratio of (1-3):1 to form a mixed solution, and then the carrier is immersed in the mixed solution, and after immersion, the carrier is taken out, washed with deionized water, and then calcined at 400°C-500°C for 2 hours-6 hours to obtain a wastewater advanced oxidation heterogeneous catalyst, wherein the loading mass fraction of manganese element in the wastewater advanced oxidation heterogeneous catalyst is 4%-20%.
5. The method for preparing a heterogeneous catalyst for advanced oxidation of wastewater according to claim 4, characterized in that: When the carrier is immersed in the mixed solution, it is shaken at 25° C.-45° C. for 10 h-16 h by a constant temperature oscillator; and / or, the acid solution is nitric acid, hydrochloric acid or acetic acid.
6. The method for preparing a heterogeneous catalyst for advanced oxidation of wastewater according to claim 4, characterized in that: The mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is 3:
1.
7. A wastewater advanced oxidation process, characterized in that: The wastewater is set to have a content of 7g / L-20g / L of a wastewater advanced oxidation heterogeneous catalyst and is in a state of continuous stirring, and then hydrogen peroxide is added in an amount of 1mL / L-1L / L to carry out an oxidation reaction, wherein the wastewater advanced oxidation heterogeneous catalyst comprises a carrier and a metal oxide loaded on the carrier, the carrier comprises a composite of activated carbon, γ-Al2O3 and graphene, wherein the γ-Al2O3 comes from hydrotalcite in the carrier preparation raw material, the mass ratio of activated carbon to γ-Al2O3 calculated as hydrotalcite in the composite is (1-5):1, and the content of graphene in the composite is 0.5wt%-2wt%; the metal oxide is a composite metal oxide comprising manganese and cerium, the atomic number ratio of manganese to cerium in the composite metal oxide is (1-3):1, and the loading mass fraction of manganese element in the metal oxide in the wastewater advanced oxidation heterogeneous catalyst is 4%-20%.
8. The wastewater advanced oxidation method according to claim 7, characterized in that: The wastewater is PVA-containing wastewater; the PVA-containing wastewater is set at a pH value of 6-8 and a temperature of 70° C.-90° C. to carry out the oxidation reaction.
9. The wastewater advanced oxidation method according to claim 7, characterized in that: The wastewater after the advanced oxidation treatment is filtered, the filtered wastewater advanced oxidation heterogeneous catalyst is regenerated, and then the regenerated wastewater advanced oxidation heterogeneous catalyst is returned to the advanced oxidation treatment.
10. The wastewater advanced oxidation method according to claim 9, characterized in that: The regeneration treatment comprises: placing the wastewater advanced oxidation heterogeneous catalyst into running water at a temperature of 50° C. to 80° C. for more than 90 minutes.