Supported CuCe (Ox) / ZSM-5 molecular sieve catalyst as well as preparation method and application thereof

The CuCe(O)/ZSM-5 catalyst addresses the challenge of catalyzing chlorine-containing VOCs by optimizing Cu to Ce molar ratios, enhancing redox ability and acidity, achieving high conversion rates of toluene and chlorobenzene at low temperatures with improved stability and efficiency.

CN119056487AActive Publication Date: 2024-12-03JIANGXI AGRICULTURAL UNIVERSITY +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411334103.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Existing catalysts face challenges in achieving high catalytic activity and stability for the combustion of chlorine-containing multi-component volatile organic compounds (VOCs), particularly due to competition for active sites and differences in molecular diameter, shape, and interaction forces.

Method used

A supported CuCe(O) type x ZSM-5 molecular sieve catalyst is prepared by dispersing copper and cerium sources in ethanol, loading onto ZSM-5 molecular sieve, and calcining to form a CuCe composite metal oxide, optimizing the molar ratio of Cu to Ce for enhanced redox ability and acidity, resulting in a synergistic effect with the support.

Benefits of technology

The catalyst exhibits high catalytic activity and stability, achieving over 90% conversion of toluene and chlorobenzene at relatively low temperatures, with a simple and cost-effective preparation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056487A_ABST
    Figure CN119056487A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of environmental protection and environmental catalysis, and particularly relates to a supported CuCe (Ox) / ZSM-5 molecular sieve catalyst as well as a preparation method and application thereof. The preparation method of the supported CuCe (Ox) / ZSM-5 molecular sieve catalyst comprises the following steps: dispersing a copper source and a cerium source in absolute ethyl alcohol by adopting an ethanol dispersion method, carrying out loading by taking a ZSM-5 molecular sieve as a carrier, and carrying out solvent removal, drying and roasting to load a CuCe composite metal oxide on the ZSM-5 molecular sieve carrier, thereby obtaining the CuCe (Ox) / ZSM-5 molecular sieve catalyst. Wherein the loading amount of the CuCe composite metal oxide on the ZSM-5 molecular sieve is 15-25 wt%, and the molar ratio of Cu to Ce is (0.4-1): 1. The catalyst has high catalytic activity and stable performance when being used for chlorine-containing multi-component VOCs (Volatile Organic Compounds).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of environmental protection and environmental catalysis, specifically relating to a supported CuCe(O)2O3-O3 ...-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3-O3 x ZSM-5 molecular sieve catalysts, their preparation methods and applications. Background Technology

[0002] Volatile organic compounds (VOCs) are any carbon compounds that participate in atmospheric photochemical reactions. Most VOCs are highly toxic and carcinogenic. Furthermore, VOCs are key precursors to fine particulate matter (PM2.5) and ozone (O3) pollution.

[0003] Catalytic combustion technology involves the flameless decomposition of VOCs into CO2 and H2O on the surface of a catalyst, releasing heat simultaneously. The temperature is typically between 200 and 500°C, far lower than that of direct combustion, significantly reducing reaction energy consumption and producing fewer toxic byproducts. Li Z et al.'s research mentioned that molecular sieves are a type of support characterized primarily by acidity, possessing a large specific surface area, rich and tunable pore structure, and good thermal stability, attracting widespread attention in the field of environmental catalysis (Applied Catalysis B: Environmental, 2023, 339: 123131). Under multi-component VOCs conditions, competition for active sites, differences in molecular diameter, shape, and size, as well as the strength of interaction forces, significantly affect the adsorption behavior and process of individual VOCs on adsorbents. Furthermore, the catalytic combustion of chlorine-containing multi-component VOCs places higher demands on the catalytic activity and stability of the catalyst.

[0004] The present invention aims to provide a catalyst with high catalytic activity and stability for chlorine-containing multi-component VOCs and a method for preparing the same. Summary of the Invention

[0005] To overcome the shortcomings of existing technologies, the present invention aims to provide a supported CuCe(O) type x ZSM-5 molecular sieve catalysts, their preparation methods, and applications: high catalytic activity and stability for chlorine-containing multi-component VOCs.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: The purpose of this invention is to provide a supported CuCe(O) type xThe preparation method of CuCe(O) / ZSM-5 molecular sieve catalyst involves an ethanol dispersion method, in which copper and cerium sources are dispersed in anhydrous ethanol, and then loaded onto ZSM-5 molecular sieve as a support. After solvent removal, drying, and calcination, CuCe composite metal oxide is loaded onto the ZSM-5 molecular sieve support to obtain CuCe(O) / ZSM-5 molecular sieve catalyst. x ZSM-5 molecular sieve catalyst; The CuCe composite metal oxide has a loading of 15-25 wt% and a molar ratio of Cu to Ce of (0.4-1):1.

[0007] This invention enhances the redox ability, acidity, and quantity of the catalyst by adjusting the molar ratio of the Cu-Ce composite metal and the support. It achieves a synergistic effect between the acidity of the molecular sieve support and the defect oxygen vacancies of the Cu-Ce composite metal oxide, significantly improving the activity and stability of the catalyst. At the same time, the catalyst has a regular pore structure, high catalytic activity, stability, and CO2 selectivity.

[0008] The supported CuCe(O) prepared by this invention x The ZSM-5 molecular sieve catalyst has strong acidity and defective oxygen vacancies, which gives it a strong ability to deeply oxidize (mineralize) VOCs. It can achieve the oxidation of VOCs at lower temperatures, and the microporous structure provides a suitable environment for VOCs adsorption and desorption.

[0009] Furthermore, its preparation method includes the following steps: S1. Disperse the copper source and cerium source in anhydrous ethanol to obtain a Cu-Ce composite metal salt solution; S2. Add ZSM-5 molecular sieve to the Cu-Ce composite metal salt solution obtained in S1, and disperse it by stirring-sonication-stirring in sequence to obtain a dispersion. S3. The dispersion obtained in S2 is heated and stirred continuously to evaporate the solvent, and the solid is dried and calcined to obtain CuCe(O) x ) / ZSM-5 molecular sieve catalyst.

[0010] Furthermore, the copper source in S1 is copper acetate monohydrate, and the cerium source is cerium nitrate hexahydrate.

[0011] Furthermore, in S2, the stirring-ultrasound-stirring method involves stirring until uniform, then ultrasonically dispersing for 0.5–3 hours, followed by magnetic stirring for 1–5 hours. Preferably, the stirring-ultrasounding-stirring method in S2 involves stirring until uniform, then ultrasonically dispersing for 1 hour, followed by magnetic stirring for 2 hours.

[0012] Furthermore, in S3, the method of evaporating the solvent by heating and continuous stirring is to continuously stir and evaporate the ethanol in a water bath at 50–95°C.

[0013] Furthermore, the drying process in S3 involves drying at 70–120°C for 8–24 hours.

[0014] Furthermore, the calcination in S3 is carried out in an air atmosphere at 300–500°C for 1–6 hours.

[0015] This invention also provides a supported CuCe(O) prepared by the above preparation method. x ) / ZSM-5 molecular sieve catalyst.

[0016] This invention also provides supported CuCe(O) x Application of ZSM-5 molecular sieve catalyst in the catalytic combustion of multi-component chlorine-containing VOCs; Preferably, the multi-component chlorinated VOCs are a mixture including toluene and chlorobenzene.

[0017] Furthermore, the reaction conditions used for catalytic combustion are as follows: toluene concentration of 500–1500 ppm, chlorobenzene concentration of 100–400 ppm, and reaction space velocity of 10000–20000 mL·g. -1 ·h -1 .

[0018] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention enhances the redox capacity, acidity, and quantity of the catalyst by adjusting the molar ratio of the Cu-Ce composite metal and optimizing the support. It achieves a synergistic effect between the acidity of the molecular sieve support and the defective oxygen vacancies in the Cu-Ce composite metal oxide, significantly improving the catalyst's activity and stability. Simultaneous catalytic combustion of toluene and chlorobenzene is achieved at relatively low reaction temperatures. In a mixed atmosphere of toluene and chlorobenzene, the reaction temperatures at which toluene and chlorobenzene achieve conversion rates exceeding 90% are 240℃ and 260℃, respectively.

[0019] 2. The preparation method provided in this application is not only simple and quick to synthesize, but also requires minimal equipment, saving time and energy. At the same time, the raw materials are inexpensive, and the samples exhibit excellent stability and high catalytic activity, making it a valuable reference and research method for the catalytic oxidation of industrial chlorine-containing multi-component VOCs. Attached Figure Description

[0020] Figure 1 These are activity evaluation diagrams of Example 1, Comparative Example 1, and Comparative Example 2 in this invention; Figure 2 These are activity evaluation diagrams for Examples 1, 2, and 3 of this invention; Figure 3 These are activity evaluation diagrams of Examples 1, 3, and 4 of this invention; Figure 4 These are stability test diagrams for Examples 1, 2, and 3 of this invention; Figure 5 These are N2 adsorption-desorption isotherms of Examples 1, Comparative Example 1, and Comparative Example 2 of this invention. Detailed Implementation

[0021] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. The described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] In the following examples, copper acetate monohydrate was purchased from Maclean's Company, and cerium nitrate hexahydrate was purchased from Aladdin Shanghai Company. Unless otherwise specified, all methods described are conventional, and all raw materials are available from publicly available commercial sources.

[0023] Example 1 The Cu4Ce6(O) provided in this embodiment x The preparation method of the Cu4Ce6 / ZSM-5 catalyst (abbreviated as Cu4Ce6 / ZSM-5, Cu to Ce molar ratio 4:6) is as follows: 0.289 g of copper acetate monohydrate and 0.947 g of cerium nitrate hexahydrate were weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of ZSM-5 molecular sieve support was added, resulting in a Cu-Ce composite metal oxide loading of 20 wt%. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The resulting solution was then magnetically stirred at room temperature for 2 h to obtain a mixed solution. The solution was then continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain Cu4Ce6(O) x ) / ZSM-5 molecular sieve catalyst.

[0024] Example 2 The Cu3Ce7(O) provided in this embodiment x The preparation method of the Cu3Ce7 / ZSM-5 catalyst (abbreviated as Cu3Ce7 / ZSM-5, with a Cu to Ce molar ratio of 3:7) is as follows: 0.204 g of copper acetate monohydrate and 1.033 g of cerium nitrate hexahydrate were weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of ZSM-5 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. After stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain Cu3Ce7(O) x ZSM-5 molecular sieve catalyst with a Cu-Ce composite metal oxide loading of 20 wt%.

[0025] Example 3 The Cu5Ce5(O) provided in this embodiment x The preparation method of the Cu5Ce5 / ZSM-5 catalyst (abbreviated as Cu5Ce5 / ZSM-5, with a Cu to Ce molar ratio of 5:5) is as follows: 0.390 g of copper acetate monohydrate and 0.846 g of cerium nitrate hexahydrate were weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of ZSM-5 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. After stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain Cu5Ce5(O x The catalyst is a ZSM-5 molecular sieve with a Cu-Ce composite metal oxide loading of 20 wt%.

[0026] Comparative Example 1 The Cu4Ce6(O) provided in this comparative example x The preparation method of the ) / SAPO-34 catalyst (abbreviated as Cu4Ce6 / SAPO-34, Cu to Ce molar ratio of 4:6) is as follows: 0.289 g of copper acetate monohydrate and 0.947 g of cerium nitrate hexahydrate were weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of SAPO-34 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. After stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain Cu4Ce6(O) xThe catalyst is a 20 wt% Cu-Ce composite metal oxide with a molecular sieve loading of 20 wt%.

[0027] Comparative Example 2 The Cu4Ce6(O) provided in this comparative example x The preparation method of the Cu4Ce6 / MCM-41 catalyst (abbreviated as Cu4Ce6 / MCM-41, Cu to Ce molar ratio 4:6) is as follows: 0.289 g of copper acetate monohydrate and 0.947 g of cerium nitrate hexahydrate were weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of AlMCM-41 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. After stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain Cu4Ce6(O) x The catalyst is a Cu-Ce composite metal oxide with a loading of 20 wt% (MCM-41 molecular sieve catalyst).

[0028] Comparative Example 3 The CuO provided in this embodiment x The preparation method of Cu / ZSM-5 catalyst (abbreviated as Cu / ZSM-5) is as follows: 1.255 g of copper acetate monohydrate was weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of ZSM-5 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. Following stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain CuO. x / ZSM-5 catalyst molecular sieve catalyst, with Cu metal oxide loading of 20 wt%.

[0029] Comparative Example 4 The CeO provided in this embodiment x / ZSM-5 catalyst (abbreviated as Ce / ZSM-5) is prepared by the following method: 1.247 g of cerium nitrate hexahydrate was weighed and mixed in 30 mL of anhydrous ethanol. Then, 1.6 g of ZSM-5 molecular sieve support was added. After stirring at room temperature for 1 h, the mixture was ultrasonically dispersed at a frequency of 40 kHz for 1 h. The mixture was then magnetically stirred at room temperature for 2 h. After stirring, the mixture was continuously stirred in an 80 °C water bath to evaporate the ethanol. The resulting solid was dried at 105 °C and finally placed in a tube furnace and calcined at a heating rate of 10 °C / min to 400 °C for 4 h to obtain CeO. x / ZSM-5 molecular sieve catalyst, with a Ce metal oxide loading of 20 wt%.

[0030] Test Example 1: Catalytic Performance Test The test method is as follows: 400 mg of catalyst was loaded into a quartz fixed-bed microreactor, and the evaluation parameters were as follows: flow rate of 100 ml·min. -1 Toluene gas with an initial concentration of 1000 ppm and chlorobenzene gas with an initial concentration of 250 ppm, with an equilibrium gas composition of 80% N2 + 20% O2, were analyzed using a GC (GC-9790, Fuli) gas chromatograph at a space velocity of 15000 mL·g⁻¹. -1 ·h -1 The reaction pressure was 0.1 MPa; the concentration of water vapor was 5 vol% when introduced; and the total gas flow rate was 100 mL / min.

[0031] In this embodiment, the conversion rate = (initial concentration of (toluene / chlorobenzene) - concentration of (toluene / chlorobenzene) in the tail gas) / initial concentration of (toluene / chlorobenzene) × 100%. Test results are shown in Tables 1 and 2. Figure 1 , Figure 2 As shown: Table 1. Evaluation results of toluene removal activity in the examples and comparative examples.

[0032] Table 2. Evaluation results of dechlorination activity of the examples and comparative examples.

[0033] As shown in Tables 1 and 2, CuCe / ZSM-5 prepared in Example 1 with a molar ratio of 0.66 (4:6) preferentially achieved a toluene conversion rate of 90%. At 240°C, the conversion rates of Examples 2 and 3, and Comparative Examples 1 and 2 did not reach 50%. Example 1 preferentially achieved a chlorobenzene conversion rate of 50% and 90%. Overall, the low-temperature catalytic activity of Example 1 is superior to the other examples. The catalytic activity from high to low is as follows: Example 1 > Example 3 > Example 2 > Comparative Example 3 > Comparative Example 1 > Comparative Example 2 > Comparative Example 4.

[0034] like Figure 1 As shown, the molar ratio of the active components Cu to Ce is 0.66 (4:6). Example 1 exhibits the highest low-temperature catalytic activity throughout the entire catalytic process. (The remaining text appears to be incomplete and contains errors. A more accurate translation would require the full context.) 90 At 240℃ and 260℃ respectively, and under mixed conditions at 240℃, the toluene conversion rate was about 75% higher than that of Comparative Examples 1 and 2, and the chlorobenzene conversion rate was about 40% higher than that of Comparative Examples 1 and 2.

[0035] like Figure 2 As shown, the active component CuCe, CuCe(O) using ZSM-5 as the molecular sieve support x Both CuCe and ZSM-5 catalysts exhibit excellent catalytic activity, with a CuCe(O) molar ratio of 0.66 (4:6). x The ZSM-5 catalyst exhibits the highest low-temperature catalytic activity throughout the catalytic process. Under mixed conditions at 240°C, the toluene conversion rate is approximately 50% higher than that of Examples 2 and 3, and the chlorobenzene conversion rate is approximately 55% higher than that of Examples 2 and 3.

[0036] like Figure 3 As shown, the active component CuCe, CuCe(O) using ZSM-5 as the molecular sieve support x Both CuCe and ZSM-5 catalysts exhibit excellent catalytic activity, with a CuCe(O) molar ratio of 0.66 (4:6). x The ZSM-5 catalyst exhibits the highest low-temperature catalytic activity throughout the catalytic process. Under mixed conditions at 240°C, the toluene conversion rate is approximately 50% higher than that of Comparative Examples 3 and 4, and the chlorobenzene conversion rate is approximately 40% higher than that of Comparative Examples 3 and 4.

[0037] Test Example 2: Stability Test Stability test method: 400 mg of catalyst was loaded into a quartz fixed-bed microreactor. The evaluation parameters were as follows: flow rate 100 ml / min. -1 Toluene gas with an initial concentration of 1000 ppm and chlorobenzene gas with an initial concentration of 250 ppm, with an equilibrium gas composition of 80% N2 + 20% O2, were analyzed using a GC (GC-9790, Fuli) gas chromatograph at a space velocity of 15000 mL·g⁻¹. -1 ·h -1 The reaction pressure was 0.1 MPa; the test temperature was 240℃ for 0-90 min, and then the temperature was increased to 260℃ for 90-180 min, and then increased to 280℃ for 180-280 min.

[0038] like Figure 4 As shown, the active component CuCe, CuCe(O) using ZSM-5 as the molecular sieve support xThe ZSM-5 catalyst exhibits excellent stability at 280℃, and no deactivation was observed during long-term testing.

[0039] Experimental Example 3: N2 Adsorption-Desorption Experiment The method for N2 adsorption-desorption test: The physical adsorption and desorption of N2 was measured at -196°C using a Micromeritics ASAP 2020 instrument. Before the test, the catalyst was pretreated at 250°C for 1 h to remove surface moisture and impurities.

[0040] like Figure 5 As shown, Comparative Example 1 exhibits a typical Type I adsorption / desorption isotherm, indicating that the original SAPO-34 microporous structure is retained; Comparative Example 2 exhibits a Type IV adsorption / desorption isotherm, indicating the presence of a microporous structure. Furthermore, when P / P0 > 0.4, the isotherm rises, showing a hysteresis loop, indicating the simultaneous presence of mesopores. Cu4Ce6(O x ) / ZSM-5 exhibits a combination of Type I and Type IV isotherms, meaning it simultaneously possesses micropores and a small amount of mesoporous structure.

[0041] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and not to limit them; although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of this application or equivalent substitutions can be made to some technical features, all of which should be covered within the scope of the technical solutions claimed in this application.

Claims

1. A supported CuCe(O x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The copper source and the cerium source were dispersed in anhydrous ethanol by the ethanol dispersion method, and then loaded on the ZSM-5 molecular sieve as a carrier. After solvent removal, drying and calcination, the CuCe composite metal oxide was loaded on the ZSM-5 molecular sieve carrier to obtain CuCe(O x ) / ZSM-5 molecular sieve catalyst; The loading amount of the CuCe composite metal oxide is 15-25wt%, and the molar ratio of Cu to Ce is (0.4-1):

1.

2. A supported CuCe(O) according to claim 1 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The following steps are involved: S1, dispersing a copper source and a cerium source in anhydrous ethanol to obtain a Cu-Ce composite metal salt solution; S2, adding ZSM-5 molecular sieve to the Cu-Ce composite metal salt solution obtained in S1, and dispersing by stirring-ultrasound-stirring in sequence to obtain a dispersion; S3, the dispersion obtained in S2 is heated and stirred continuously to evaporate the solvent, and the solid is dried and calcined to obtain CuCe(O x ) / ZSM-5 molecular sieve catalyst.

3. A supported CuCe(O) according to claim 2 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The copper source in S1 is copper acetate monohydrate, and the cerium source is cerium nitrate hexahydrate.

4. A supported CuCe(O) according to claim 2 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The stirring-ultrasonic-stirring method in S2 is to stir evenly, then ultrasonically disperse for 0.5 to 3 hours, and then magnetically stir for 1 to 5 hours; Preferably, the stirring-ultrasound-stirring method in S2 is to stir evenly, then perform ultrasonic dispersion for 1 hour, and then perform magnetic stirring for 2 hours.

5. A supported CuCe(O) according to claim 2 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The method of volatilizing the solvent by heating and stirring continuously in S3 is to volatilize the ethanol by stirring continuously in a water bath at 50 to 95°C.

6. A supported CuCe(O) according to claim 2 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The drying in S3 is performed at 70 to 120° C. for 8 to 24 hours.

7. A supported CuCe(O) according to claim 2 x ) / ZSM-5 molecular sieve catalyst preparation method, characterized in that, The calcination in S3 is carried out at 300-500° C. in an air atmosphere for 1-6 hours.

8. A supported CuCe(O) prepared by the preparation method according to any one of claims 1 to 7 x ) / ZSM-5 molecular sieve catalyst.

9. The supported CuCe(II) according to claim 8 x ) / Application of ZSM-5 molecular sieve catalyst in catalytic combustion of multi-component chlorine-containing VOCs; Preferably, the multi-component chlorine-containing VOCs is a mixture of toluene and chlorobenzene.

10. The use according to claim 9, characterized in that The reaction conditions used for catalytic combustion are: toluene concentration is 500-1500 ppm, chlorobenzene concentration is 100-400 ppm, reaction space velocity is 10000-20000 mL·g -1 ·h -1 .

Citation Information

Patent Citations

  • Method for easy volatility Cl generation aromatic low temperature catalyst burning eliminable

    CN101199885A

  • Preparation method for supported catalyst for catalyzing combustion of VOCs (Volatile Organic Compounds)

    CN105879901A

  • Preparing method and application of MCM-41 supported CuO-CeO2 nanocrystalline catalyst

    CN109772444A

  • RuCe / ZSM-5 molecular sieve catalyst as well as preparation method and application thereof

    CN113797961A

  • Cauliflower-shaped LaMnO3-CuMnCeOx mixed composite oxide catalyst, preparation method and application of cauliflower-shaped LaMnO3-CuMnCeOx mixed composite oxide catalyst

    CN114849731A