Laser melting deposition additive manufacturing method of Ti2AlNb alloy
By using interlayer pause printing and argon gas scrubbing technology during laser melting and deposition, the problem of easy oxidation of Ti2AlNb alloy is solved, significantly improving its tensile strength and performance, and achieving higher mechanical properties.
Patent Information
- Application Number
- CN202411234863.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-03
Smart Images

Figure CN119057079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an additive manufacturing method for titanium alloy. Background Art
[0002] Ti2AlNb-based alloy is an intermetallic compound dominated by ordered orthorhombic O phase, with coexistence of metallic bonds and covalent bonds, and has the performance characteristics of both metals and ceramics. It has high melting point, low density, high elastic modulus, excellent high temperature strength and creep resistance, and is a new type of lightweight and high temperature resistant structural material. The density of Ti2AlNb-based alloy is 60% of that of nickel-based high temperature alloy, and it has broken through the "thermal barrier" of traditional titanium alloy application at 600℃, and is expected to replace nickel-based high temperature alloy to become a new generation of aerospace materials, so it has good application prospects in aerospace.
[0003] Ti2AlNb-based alloys are difficult to process. O-phase alloys are intrinsically brittle and have poor thermal deformation capabilities, making them difficult to process into parts with complex shapes. The cast alloy has a coarse structure, which is not conducive to performance improvement; if hot processing is used, it needs to be heated to a higher temperature, which is costly. These problems have brought obstacles to the application of Ti2AlNb alloys. Laser melting deposition is an additive manufacturing technology based on the discrete-accumulation principle, which controls energy sources such as lasers, electron beams, and plasma to act on powders. Compared with traditional manufacturing methods, laser melting deposition has the advantage of being able to produce parts of any complex shape, and a wide range of materials can be selected and the production cycle is short. Therefore, laser melting deposition is widely used in the production of titanium alloy aerospace parts.
[0004] However, titanium alloys are very sensitive to oxygen content during the forming process, especially Ti2AlNb-based alloys. The oxidation phenomenon during the additive process will cause the formation of continuous brittle α2 phase at the grain boundaries of the formed Ti2AlNb-based alloy, which will lead to a sharp decline in the performance of the alloy. These problems are difficult to improve through post-processing and need to be solved by optimizing the additive manufacturing process parameters and improving the additive manufacturing methods. Summary of the invention
[0005] In order to solve the problem that the existing laser melting deposition method for preparing Ti2AlNb alloy is easy to oxidize and leads to poor mechanical properties, the present invention provides a laser melting deposition additive manufacturing method for Ti2AlNb alloy.
[0006] The laser melting deposition additive manufacturing method of the Ti2AlNb alloy of the present invention is carried out in the following steps:
[0007] Step 1:
[0008] preparing a Ti2AlNb alloy rod, and using an aerosol method to prepare a powder for laser melting deposition from the Ti2AlNb alloy rod;
[0009] Step 2:
[0010] The powder for laser melting deposition prepared in step 1 is dried and then placed in a powder bin, the substrate is placed in a molding bin, and argon gas is introduced into the molding bin for washing to make the oxygen content in the molding bin <50ppm;
[0011] Step 3:
[0012] Printing parameters and printing strategies are set, and Ti2AlNb alloy is printed layer by layer on the substrate to realize laser melting deposition additive manufacturing of Ti2AlNb alloy. In the process of printing Ti2AlNb alloy layer by layer on the substrate, a pause is made after each layer is printed before printing the next layer.
[0013] The principles and beneficial effects of the present invention are:
[0014] The existing conventional laser melting deposition printing of Ti2AlNb alloy is continuous printing. During the printing process, the continuous laser energy input causes the printed part to be continuously heated, the temperature is high, and it is easy to react with oxygen elements. Oxygen elements are enriched at the grain boundaries, which aggravates the oxidation degree of the alloy and reduces the performance; at the same time, the continuous heat input heats the printed part to the α2 phase formation temperature zone, and the α2 phase is easy to form at the grain boundary. The α2 phase is a close-packed hexagonal structure with fewer slip systems and is a brittle phase, which is not conducive to the improvement of performance (where the tensile strength is about 600MPa). Therefore, the conventional continuous printing method is not conducive to the performance of Ti2AlNb alloy. The present invention adopts an interlayer pause printing method to avoid the continuous input of energy. During the pause process, the temperature of the printed alloy drops rapidly, thereby reducing the oxidation tendency of the alloy during the printing process and reducing the precipitation of the brittle phase α2 phase at the grain boundary; and during the pause process, a large number of fine and dispersed strengthening phases are precipitated in the crystal, which is conducive to the improvement of performance. Compared with the continuous printing method, the tensile strength of the Ti2AlNb alloy printed by the present invention is increased from 600MPa to 900MPa, and the tensile strength is increased by 50%. Therefore, the present invention solves the problem of poor performance of Ti2AlNb alloy printed by laser melting deposition and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The engineering stress-strain curves of the Ti2AlNb alloy obtained by the printing method with interlayer pause in Example 1 and the continuous printing method in Comparative Example 1;
[0016] Figure 2 This is a microstructure photograph of the Ti2AlNb alloy obtained by the interlayer pause printing method in Example 1;
[0017] Figure 3This is an energy spectrum element analysis photograph of the Ti2AlNb alloy obtained by the interlayer pause printing method in Example 1;
[0018] Figure 4 This is a microstructure photograph of the Ti2AlNb alloy obtained by the continuous printing method in Comparative Example 1;
[0019] Figure 5 This is a spectrum element analysis photo of the Ti2AlNb alloy obtained by the continuous printing method in Comparative Example 1;
[0020] Figure 6 This is an oxygen content analysis diagram of the Ti2AlNb alloy obtained by the interlayer pause printing method in Example 1;
[0021] Figure 7 This is an oxygen content analysis diagram of the Ti2AlNb alloy obtained by continuous printing in Comparative Example 1. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.
[0023] Specific implementation method 1: The laser melting deposition additive manufacturing method of Ti2AlNb alloy in this implementation method is carried out according to the following steps:
[0024] Step 1:
[0025] preparing a Ti2AlNb alloy rod, and using an aerosol method to prepare a powder for laser melting deposition from the Ti2AlNb alloy rod;
[0026] Step 2:
[0027] The powder for laser melting deposition prepared in step 1 is dried and then placed in a powder bin, the substrate is placed in a molding bin, and argon gas is introduced into the molding bin for washing to make the oxygen content in the molding bin <50ppm;
[0028] Step 3:
[0029] Printing parameters and printing strategies are set, and Ti2AlNb alloy is printed layer by layer on the substrate to realize laser melting deposition additive manufacturing of Ti2AlNb alloy. In the process of printing Ti2AlNb alloy layer by layer on the substrate, a pause is made after each layer is printed before printing the next layer.
[0030] This implementation has the following beneficial effects:
[0031] The conventional laser melting deposition printing of Ti2AlNb alloy is continuous printing. During the printing process, the continuous laser energy input causes the printed part to be continuously heated. The temperature is high and it is easy to react with oxygen. The oxygen element is enriched at the grain boundary, which aggravates the oxidation degree of the alloy and reduces the performance. At the same time, the continuous heat input heats the printed part to the α2 phase formation temperature zone, and the α2 phase is easy to form at the grain boundary. The α2 phase is a close-packed hexagonal structure with fewer slip systems and is a brittle phase, which is not conducive to the improvement of performance (the tensile strength is about 600MPa). Therefore, the conventional continuous printing method is not conducive to the performance of Ti2AlNb alloy. This embodiment adopts an interlayer pause printing method to avoid the continuous input of energy. During the pause process, the temperature of the printed alloy drops rapidly, thereby reducing the oxidation tendency of the alloy during the printing process and reducing the precipitation of the brittle phase α2 phase at the grain boundary. In addition, during the pause process, a large number of fine and dispersed strengthening phases are precipitated in the crystal, which is conducive to the improvement of performance. Compared with the continuous printing method, the tensile strength of the Ti2AlNb alloy printed in this embodiment is increased from 600MPa to 900MPa, and the tensile strength is increased by 50%. Therefore, this embodiment solves the problem of poor performance of Ti2AlNb alloy printed by laser melting deposition and has good application prospects.
[0032] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: in step 1, the Ti2AlNb alloy rod is composed of 10-11% Al, 41-43% Nb, 0.04-0.08% Fe and the remainder Ti in a mass ratio.
[0033] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the particle size of the powder used for laser melting deposition in step one is 75 to 150 μm.
[0034] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the material of the substrate in step 2 is TC4 or TA15; the thermal expansion coefficient of the substrate material is similar to that of Ti2AlNb, which can increase the degree of bonding between the material and the substrate.
[0035] Specific implementation method five: This implementation method is different from any one of specific implementation methods one to four in that: the flow rate of the powder feeding gas used in the powder bin in step two is 5 to 7 L / min, and the powder feeding amount is 300 to 400 g / h.
[0036] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the flow rate of argon gas introduced into the forming chamber in step 2 is 3 L / min. The introduction of argon gas for washing can reduce the oxygen content in the forming chamber and protect the alloy.
[0037] Specific implementation method 7: This implementation method is different from any one of specific implementation methods 1 to 6 in that: the temperature of the drying treatment in step 2 is 120° C. and the time is 30 minutes.
[0038] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the printing parameters in step three include: laser power of 2500-3000W, scanning speed of 480-720mm / min, spot diameter of 3mm, layer height of 0.5-0.7mm, and overlap rate of 50%. The use of laser power of 2500-3000W and 480-720mm / min can ensure the full melting of the powder and improve the metallurgical bonding degree.
[0039] Specific implementation method 9: The difference between this implementation method and any one of specific implementation methods 1 to 8 is that: the pause time after each layer of printing in step 3 is 30 to 90 seconds; the pause between layers can allow the printed alloy to cool quickly and reduce the degree of oxidation.
[0040] Specific implementation ten: This implementation differs from specific implementations one to nine in that: the scanning strategy described in step three is: the printing spot path in each layer is a zigzag, the adjacent spot paths in the same layer are rotated 180°, and the spot paths between adjacent layers are rotated 90°.
[0041] Embodiment 1:
[0042] The laser melting deposition additive manufacturing method of the Ti2AlNb alloy in this embodiment is carried out in the following steps:
[0043] Step 1:
[0044] preparing a Ti2AlNb alloy rod, and using an aerosol method to powder the Ti2AlNb alloy rod into powder for laser melting deposition;
[0045] The Ti2AlNb alloy rod is composed of 10.59% Al, 42.87% Nb, 0.06% Fe and the balance Ti in terms of mass ratio;
[0046] The particle size of the powder used for laser melting deposition is 75 to 150 μm;
[0047] Step 2:
[0048] The powder for laser melting deposition prepared in step 1 is dried and then placed in a powder bin, the substrate is placed in a molding bin, and argon gas is introduced into the molding bin for washing to make the oxygen content in the molding bin <50ppm;
[0049] The material of the substrate is TC4;
[0050] The powder feeding gas flow rate used in the powder bin is 6L / min, and the powder feeding amount is 355g / h;
[0051] The flow rate of the argon gas introduced into the forming chamber is 3L / min; introducing argon gas for washing can reduce the oxygen content in the forming chamber and protect the alloy;
[0052] The drying process is carried out at a temperature of 120°C and a time of 30 minutes;
[0053] Step 3:
[0054] Setting printing parameters and printing strategies, printing Ti2AlNb alloy layer by layer on the substrate, and realizing laser melting deposition additive manufacturing of Ti2AlNb alloy; in the process of printing Ti2AlNb alloy layer by layer on the substrate, pausing for a period of time after each layer is printed before printing the next layer;
[0055] The printing parameters include: laser power of 2900W, scanning speed of 600mm / min, spot diameter of 3mm, layer height of 0.6mm, and overlap rate of 50%;
[0056] The pause time after each layer is printed is 60 seconds; the pause between layers can allow the printed alloy to cool quickly and reduce the degree of oxidation.
[0057] The scanning strategy is: the printing spot path in each layer is zigzag, the adjacent spot paths in the same layer are rotated 180°, and the spot paths between adjacent layers are rotated 90°.
[0058] Comparative Example 1:
[0059] The laser melting deposition additive manufacturing method of the Ti2AlNb alloy in this comparative example is carried out in the following steps:
[0060] Step 1:
[0061] preparing a Ti2AlNb alloy rod, and using an aerosol method to prepare a powder for laser melting deposition from the Ti2AlNb alloy rod;
[0062] The Ti2AlNb alloy rod is composed of 10.59% Al, 42.87% Nb, 0.06% Fe and the balance Ti in terms of mass ratio;
[0063] The particle size of the powder used for laser melting deposition is 75 to 150 μm;
[0064] Step 2:
[0065] The powder for laser melting deposition prepared in step 1 is dried and then placed in a powder bin, the substrate is placed in a molding bin, and argon gas is introduced into the molding bin for washing to make the oxygen content in the molding bin <50ppm;
[0066] The material of the substrate is TC4;
[0067] The powder feeding gas flow rate used in the powder bin is 6L / min, and the powder feeding amount is 355g / h;
[0068] The flow rate of the argon gas introduced into the forming chamber is 3L / min; introducing argon gas for washing can reduce the oxygen content in the forming chamber and protect the alloy;
[0069] The drying process is carried out at a temperature of 120°C and a time of 30 minutes;
[0070] Step 3:
[0071] Setting printing parameters and printing strategies, printing Ti2AlNb alloy layer by layer on the substrate, and realizing laser melting deposition additive manufacturing of Ti2AlNb alloy;
[0072] The printing parameters include: laser power of 2900W, scanning speed of 600mm / min, spot diameter of 3mm, layer height of 0.6mm, and overlap rate of 50%;
[0073] The scanning strategy is: the printing spot path in each layer is zigzag, the adjacent spot paths in the same layer are rotated 180°, and the spot paths between adjacent layers are rotated 90°.
[0074] Figure 1 The engineering stress-strain curves of Ti2AlNb alloy obtained by the printing method with interlayer pause (Example 1) and the printing method with continuous printing (Comparative Example 1); the tensile strength of the interlayer pause printing method of the present invention is increased from 600MPa to 900MPa compared with the continuous printing method, and the tensile strength is increased by 50%; Figure 2 The microstructure photograph of the Ti2AlNb alloy obtained by the interlayer pause printing method (Example 1) shows that a large number of dispersed and fine strengthening phases are precipitated in the crystal. Figure 3 This is an energy spectrum element analysis photograph of the Ti2AlNb alloy obtained by using the interlayer pause printing method (Example 1), in which the oxygen element is evenly distributed and there is no enrichment at the grain boundary; Figure 4 The microstructure photograph of the Ti2AlNb alloy obtained by the continuous printing method (Comparative Example 1) shows that there is no precipitation phase in the crystal; Figure 5The energy spectrum element analysis photo of the Ti2AlNb alloy obtained by the continuous printing method (Comparative Example 1) shows that oxygen element is enriched at the grain boundary; the interlayer pause printing method described in the present invention can precipitate a strengthening phase in the crystal, inhibit oxidation at the grain boundary, and improve performance; Figure 6 The oxygen content statistics of the Ti2AlNb alloy obtained by the printing method with interlayer pause (Example 1); Figure 7 The oxygen content statistics of the Ti2AlNb alloy obtained by the continuous printing method (Comparative Example 1) are shown; it can be seen that the interlayer pause printing method described in the present invention can reduce the oxygen content of the Ti2AlNb alloy after printing, which shows that the interlayer pause printing method described in the present invention can inhibit the oxidation phenomenon of the laser melt-deposited Ti2AlNb alloy.
Claims
1. A laser melting deposition additive manufacturing method for Ti2AlNb alloy, characterized in that: The laser melting deposition additive manufacturing method of Ti2AlNb alloy is carried out in the following steps: Step 1: preparing a Ti2AlNb alloy rod, and using an aerosol method to prepare a powder for laser melting deposition from the Ti2AlNb alloy rod; Step 2: The powder for laser melting deposition prepared in step 1 is dried and then placed in a powder bin, the substrate is placed in a molding bin, and argon gas is introduced into the molding bin for washing to make the oxygen content in the molding bin <50ppm; Step 3: Printing parameters and printing strategies are set, and Ti2AlNb alloy is printed layer by layer on the substrate to realize laser melting deposition additive manufacturing of Ti2AlNb alloy. In the process of printing Ti2AlNb alloy layer by layer on the substrate, a pause is made after each layer is printed before printing the next layer.
2. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: Step 1: The Ti2AlNb alloy rod is composed of 10-11% Al, 41-43% Nb, 0.04-0.08% Fe and the balance Ti in terms of mass ratio.
3. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: The particle size of the powder used for laser melting deposition in step 1 is 75 to 150 μm.
4. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: In step 2, the material of the substrate is TC4 or TA15; the thermal expansion coefficient of the substrate material is similar to that of Ti2AlNb, which can increase the bonding degree between the material and the substrate.
5. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: In step 2, the powder feeding gas used in the powder bin has a flow rate of 5 to 7 L / min and a powder feeding amount of 300 to 400 g / h.
6. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: In step 2, the flow rate of argon gas introduced into the molding chamber is 3 L / min.
7. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: The temperature of the drying treatment in step 2 is 120° C. and the time is 30 minutes.
8. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: The printing parameters in step 3 include: laser power of 2500-3000 W, scanning speed of 480-720 mm / min, spot diameter of 3 mm, layer height of 0.5-0.7 mm, and overlap rate of 50%.
9. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: The pause time after each layer of printing in step 3 is 30 to 90 seconds; the pause between layers can allow the printed alloy to cool quickly and reduce the degree of oxidation.
10. The laser melting deposition additive manufacturing method of Ti2AlNb alloy according to claim 1, characterized in that: The scanning strategy described in step three is: the printing spot path in each layer is a zigzag, the spot paths of adjacent passes in the same layer are rotated 180°, and the spot paths between adjacent layers are rotated 90°.
Citation Information
Cited By
Method for inhibiting cracks in additive manufacturing of Ti2AlNb alloy with high O phase content
CN120286728A
A 750 degree celsius / 650 mpa grade ti2alnab alloy additive manufacturing method
CN120790960B
Additive preparation method of Ti2AlNb alloy with high strength and high plasticity
CN121017569A
A method for additive manufacturing of a Ti2AlNb alloy with high strength and high plasticity
CN121017569B
Ti2AlNb-based alloy ring piece and preparation method and application thereof
CN121447045A