Preparation method of composite material with high spectral matching degree with green vegetation

By using components such as aluminum salt, magnesium salt and anionic surfactant in hyperspectral camouflage materials to simulate the spectral characteristics of green vegetation, the problem that camouflage materials cannot be effectively integrated into the background in the prior art is solved, and hyperspectral matching and weather resistance are achieved suitable for mass production.

CN119059543APending Publication Date: 2024-12-03NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411175784.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing hyperspectral camouflage materials cannot effectively simulate the reflection spectrum of green vegetation, resulting in the inability to integrate the camouflage target into the background, and large-scale production and mechanical properties are difficult to meet the needs.

Method used

Aluminum salts and magnesium salts are used to react with anionic surfactants, organic pigment dyes and chlorophyll derivatives in deionized water to control pH value, form precipitates, wash and dry, and prepare a double-layer hydroxide composite pigment to simulate green Spectral characteristics of vegetation.

Benefits of technology

It achieves a high spectrum matching degree with green vegetation in the 400-2500nm band, achieving a similarity of 0.988, and the material has good weather resistance and thermal stability, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059543A_ABST
    Figure CN119059543A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite material having a high spectral matching degree with green vegetation, and the method comprises the following steps: (1) mixing two metal salts, an anionic surfactant, an organic pigment dye and a chlorophyll derivative in deionized water, and adding a precipitant to make the pH value of a reaction system be 9-10; (2) reacting the mixed solution obtained in the step (1) at the temperature not lower than 35 DEG C to obtain a precipitate; and (3) washing and drying the precipitate to obtain the composite material. The prepared composite material can be highly matched with green vegetation, and the spectrum similarity of the composite material is as high as 0.988.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a composite material having high spectral matching degree with green vegetation. Background Art

[0002] With the continuous development of hyperspectral detection technology, it is found that green vegetation has highly similar reflectance spectra in the 400-2500nm band. It has a special reflectance peak at 550nm, which is called the "green peak". This is mainly due to the unique conjugated large π form of chlorophyll in vegetation, which causes it to absorb very little green light. In the 680-780nm band, there is a slope with a rapid increase in reflectivity, called the "red edge", because the main body of the leaves absorbs very little in this band. The loose porous structure of the leaves causes it to have a stable reflectivity platform in the 780-1300nm range, called the "near-infrared plateau". There are two obvious absorption valleys at 1450nm and 1940nm, which are attributed to the absorption bands produced by the vibration of the OH bonds in water and are called "water absorption bands". The above characteristics of green vegetation make it impossible for simple visible light stealth materials to match the reflectance spectrum of background vegetation, so that the camouflaged target cannot be integrated into the background and fails.

[0003] Hyperspectral camouflage materials need to meet the requirements of having a highly similar reflectance spectrum to vegetation, so they need to simulate the chlorophyll, porous structure and moisture of vegetation. Yang Yujie et al. designed a three-layer bionic leaf structure, with a waterproof polyvinyl chloride film on the surface, a high-water barrier bag in the middle layer, and a loose paper structure on the bottom layer. The reflectance spectrum of the bionic material has a similarity of 0.9983 with the spectrum of vegetation. However, the structure is too complicated and the mechanical properties are not clarified, making it difficult to mass produce and apply. Guo Li et al. directly prepared a water-containing coating using water, chlorophyll, and chrome green as fillers. The spectral similarity of the material with green leaves reached 0.99, but the water retention rate was poor and difficult to apply. Wang Can et al. used Mg-Al layered hydroxide as a water-containing material and intercalated pigment groups in it to prepare a camouflage filler. The filler has strong weather resistance and thermal stability, but the filler preparation conditions are harsh and the cost of mass production is high. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a composite material having a high spectral matching degree with green vegetation. The reflectance spectrum of the composite material prepared by the method has a similarity of 0.988 with the spectrum of green vegetation.

[0005] Technical solution: The method for preparing the composite material of the present invention comprises the following steps:

[0006] (1) two metal salts, anionic surfactant, organic pigment dye and chlorophyll derivative are mixed in deionized water, and a precipitant is added thereto to make the pH of the reaction system be 9 to 10;

[0007] (2) reacting the mixed solution obtained in step (1) at a temperature not lower than 35° C. to obtain a precipitate;

[0008] (3) Washing and drying the precipitate to obtain a composite material.

[0009] Wherein, in step (1), the two metal salts are aluminum salt and magnesium salt; wherein the molar ratio of the aluminum salt to the magnesium salt is 1:3 to 3.5.

[0010] Wherein, the aluminum salt is aluminum chloride hexahydrate; and the magnesium salt is magnesium chloride hexahydrate.

[0011] Wherein, in step (1), the organic pigments are alcohol-soluble yellow and patent green; the chlorophyll derivative is sodium copper chlorophyllin; wherein the mass ratio of patent green, alcohol-soluble yellow and sodium copper chlorophyllin is 1:3 to 5:1.

[0012] The total amount of alcohol-soluble yellow, patent green and sodium copper chlorophyllin added is 3-4% of the total mass of magnesium salt and aluminum salt.

[0013] Wherein, in step (1), the anionic surfactant is SHMP (sodium hexametaphosphate); the amount of the anionic surfactant added is 1 / 10 to 1 / 15 of the total mass of the magnesium salt and the aluminum salt.

[0014] Wherein, the precipitant is NaOH solution; the concentration of the NaOH solution is 2-3 mol / L.

[0015] Wherein, in step (2), the reaction time is not less than 15 hours.

[0016] Wherein, in step (3), the precipitate is washed until the pH of the washing liquid is neutral.

[0017] Wherein, in step (3), the drying temperature is 100-110° C. and the drying time is 4-5 h.

[0018] The composite material prepared by the above method has a high spectral matching degree with green vegetation. The double-layer hydroxide composite pigment appears green, and there are "green peaks" and "red edges" in the visible light region that are highly similar to green vegetation.

[0019] Through physical stirring, AlCl3·6H2O and MgCl2·6H2O were mixed and dissolved in deionized water in a molar ratio of 1:3, and anionic surfactant SHMP was added to it. It was ionized in water to change the surface tension and free energy, leaving enough space for the reactants to promote the grain growth of double hydroxides; NaOH was used as a precipitant, and the OH generated by its ionization in water was used to generate the -The ions react with the metal ions in the metal salt. The electrostatic force between the metal ions and OH- and the interlayer anions causes the formed metal hydroxide precursor to further assemble into a layered structure, and the anion layers are stacked to form a double-layer hydroxide containing water molecules.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the composite material prepared by the present invention can be highly matched with green vegetation, and the spectral similarity in the 400-2500nm band is as high as 0.988. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The reflection spectrum curve pictures of the water-containing materials prepared in Example 1 and Comparative Examples 1 to 3 at 1000 to 2500 nm and the similarity diagram with the spectrum curve of green vegetation;

[0022] Figure 2 The SEM images of the water-containing materials LDH1-4 prepared in Example 1 and Comparative Examples 1-3;

[0023] Figure 3 X-ray diffraction patterns of water-containing materials LDH1-4 obtained in Example 1 and Comparative Examples 1-3;

[0024] Figure 4 The reflection spectrum curve pictures of the composite materials prepared in comparative examples 4 to 6 at 400 to 2500 nm and the similarity diagram with the spectrum curve of green vegetation;

[0025] Figure 5 The reflection spectrum curve pictures of the composite materials prepared in Examples 2 to 4 at 400 to 2500 nm and the similarity diagram with the spectrum curve of green vegetation;

[0026] Figure 6 This is a physical picture of the composite material prepared in Examples 1 to 4. DETAILED DESCRIPTION

[0027] Example 1

[0028] The method for preparing the water-containing material of the present invention comprises the following steps:

[0029] (1) 0.937 g of AlCl3·6H2O, 1.537 g of MgCl2·6H2O and 0.5 mmol of SHMP were dissolved in 100 mL of deionized water to obtain solution A; 5 g of NaOH was dissolved in 25 mL of deionized water to prepare a NaOH solution with a concentration of 2 mol / L; the NaOH solution was slowly added dropwise to solution A to make its pH reach 9 to 10;

[0030] (2) placing the mixed solution in a constant temperature water bath, setting the reaction temperature to 35°C, the reaction time to 15 h, and obtaining a precipitate after the reaction;

[0031] (3) The precipitate was washed until the pH of the eluate was neutral; then it was dried at 100°C for 4 hours to obtain the aqueous material LDH-4, the spectral similarity of which was 0.97876 in the 400-2500nm band; and the spectral similarity of which was 0.85734 in the 400-2500nm band.

[0032] Example 2

[0033] The method for preparing the composite material of the present invention comprises the following steps:

[0034] (1) 1.886 g of AlCl3·6H2O, 3.052 g of MgCl2·6H2O, 0.5 mmol of SHMP, 0.029 g of patent green, 0.089 g of alcohol-soluble yellow and 0.029 of sodium copper chlorophyllin were dissolved in 100 mL of deionized water to obtain solution A; 2 mol / L NaOH solution was slowly added dropwise to solution A to make its pH reach 9-10;

[0035] (2) placing the mixed solution in a constant temperature water bath, setting the reaction temperature to 35°C, the reaction time to 15 h, and obtaining a precipitate after the reaction;

[0036] (3) The precipitate was washed until the pH of the eluate was neutral; and then it was dried at 100° C. for 4 h. The spectral similarity of the composite material in the 400-2500 nm band was 0.96351.

[0037] Example 3

[0038] The method for preparing the composite material of the present invention comprises the following steps:

[0039] (1) 1.886 g of AlCl3·6H2O, 3.052 g of MgCl2·6H2O, 0.5 mmol of SHMP, 0.025 g of patent green, 0.098 g of alcohol-soluble yellow and 0.025 g of sodium copper chlorophyllin were dissolved in 100 ml of deionized water to obtain solution A; 2 mol / L NaOH solution was slowly added dropwise to solution A to adjust its pH to 9-10;

[0040] (2) placing the mixed solution in a constant temperature water bath, setting the reaction temperature to 35°C, the reaction time to 15 h, and obtaining a precipitate after the reaction;

[0041] (3) The precipitate was washed until the pH of the eluate was neutral; and then it was dried at 100° C. for 4 h. The spectral similarity of the composite material in the 400-2500 nm band was 0.97783.

[0042] Example 4

[0043] The method for preparing the composite material of the present invention comprises the following steps:

[0044] (1) 1.886 g of AlCl3·6H2O, 3.052 g of MgCl2·6H2O, 0.5 mmol of SHMP, 0.021 g of patent green, 0.106 g of alcohol-soluble yellow and 0.021 g of sodium copper chlorophyllin were dissolved in 100 ml of deionized water to obtain solution A; 2 mol / L NaOH solution was slowly added dropwise to solution A to make its pH reach 9-10;

[0045] (2) placing the mixed solution in a constant temperature water bath, setting the reaction temperature to 35°C, the reaction time to 15 h, and obtaining a precipitate after the reaction;

[0046] (3) The precipitate was washed until the pH of the eluate was neutral; and then it was dried at 100° C. for 4 h. The spectral similarity of the composite material in the 400-2500 nm band was 0.98841.

[0047] Comparative Example 1

[0048] Compared with Example 1, the process of preparing the aqueous material in Comparative Example 1 is exactly the same, the only difference is that the preparation temperature is 5°C, and the spectral similarity of the prepared aqueous material LDH-1 in the wavelength range of 1000 to 2500 nm is 0.94427.

[0049] Comparative Example 2

[0050] Compared with Example 1, the process of preparing the aqueous material in Comparative Example 2 is exactly the same, the only difference is that the preparation temperature is 15° C., and the spectral similarity of the prepared aqueous material LDH-2 in the wavelength range of 1000 to 2500 nm is 0.94248.

[0051] Comparative Example 3

[0052] Compared with Example 1, the process of preparing the aqueous material in Comparative Example 3 is exactly the same, the only difference is that the preparation temperature is 25° C., and the spectral similarity of the prepared aqueous material LDH-3 in the wavelength range of 1000 to 2500 nm is 0.95394.

[0053] pass Figures 2-3 It can be seen that as the temperature increases, the layered structure of the water-containing material becomes more obvious, the crystallinity becomes higher, and thus the spectral similarity becomes higher.

[0054] Comparative Example 4

[0055] Compared with Example 4, the process of preparing the composite material in Comparative Example 4 is exactly the same, the only difference is that a single dye alcohol-soluble yellow is selected, and the spectral similarity of the prepared composite material in the wavelength range of 400 to 2500 nm is 0.87329.

[0056] Comparative Example 5

[0057] Compared with Example 4, the process of preparing the composite material in Comparative Example 5 is exactly the same, the only difference is that a single dye patented green is selected, and the spectral similarity of the prepared composite material in the wavelength range of 400 to 2500 nm is 0.91385.

[0058] Comparative Example 6

[0059] Compared with Example 4, the process of preparing the composite material in Comparative Example 6 is exactly the same, the only difference is that a single dye sodium copper chlorophyllin is selected, and the spectral similarity of the prepared composite material in the wavelength range of 400 to 2500 nm is 0.89476.

Claims

1. A method for preparing a composite material having high spectral matching with green vegetation, characterized in that: The steps include: (1) two metal salts, anionic surfactant, organic pigment dye and chlorophyll derivative are mixed in deionized water, and a precipitant is added thereto to make the pH of the reaction system be 9 to 10; (2) reacting the mixed solution obtained in step (1) at a temperature not lower than 35° C. to obtain a precipitate; (3) Washing and drying the precipitate to obtain a composite material.

2. The preparation method according to claim 1, characterized in that: In step (1), the two metal salts are aluminum salt and magnesium salt; wherein the molar ratio of the aluminum salt to the magnesium salt is 1:3 to 3.

5.

3. The preparation method according to claim 2, characterized in that: The aluminum salt is aluminum chloride hexahydrate; the magnesium salt is magnesium chloride hexahydrate.

4. The preparation method according to claim 1, characterized in that: In step (1), the organic pigments are alcohol-soluble yellow and patent green; the chlorophyll derivative is sodium copper chlorophyllin; wherein the mass ratio of patent green, alcohol-soluble yellow and sodium copper chlorophyllin is 1:3 to 5:

1.

5. The preparation method according to claim 4, characterized in that: The total amount of alcohol-soluble yellow, patent green and sodium copper chlorophyllin added is 3-4% of the total mass of magnesium salt and aluminum salt.

6. The preparation method according to claim 1, characterized in that: In step (1), the anionic surfactant is SHMP; the amount of the anionic surfactant added is 1 / 10 to 1 / 15 of the total mass of the magnesium salt and the aluminum salt.

7. The preparation method according to claim 1, characterized in that: In step (1), the precipitant is a NaOH solution; the concentration of the NaOH solution is 2-3 mol / L.

8. The preparation method according to claim 1, characterized in that: In step (2), the reaction time is not less than 15 h.

9. The preparation method according to claim 1, characterized in that: In step (3), the precipitate is washed until the pH of the washing solution is neutral.

10. The preparation method according to claim 1, characterized in that: In step (3), the drying temperature is 100-110° C. and the drying time is 4-5 hours.