Method for preparing tellurium dioxide from lead anode slime

Through the three-stage process of constant temperature vacuum distillation-oxidation regulation-change temperature vacuum distillation, tellurium dioxide is separated by composite oxidant, which solves the low direct yield and environmental pollution of tellurium in lead anode mud, and achieves high-efficiency and green tellurium resources use.

CN119059556AActive Publication Date: 2024-12-03KUNMING UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411279537.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-03
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing lead anode mud recovery process has problems such as long process flow, cumbersome operation, low metal direct yield and long recovery cycle. In addition, the environmental pollution is serious, the direct yield of tellurium is less than 40%, making it difficult to achieve green and efficient extraction.

Method used

The three-stage process of constant temperature vacuum distillation-oxidation regulation-variable temperature vacuum distillation is adopted. The oxidation regulation of the composite oxidant (lead dioxide and hydrogen peroxide) is carried out to separate and prepare tellurium dioxide, which increases the direct yield of tellurium and reduces reagent consumption.

Benefits of technology

The efficient direct yield of tellurium is achieved, with the direct yield of tellurium reaching 96.32% to 98.01%, reducing reagent consumption and harmless separation of arsenic antimony, simplifying process design, promoting resource utilization, and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059556A_ABST
    Figure CN119059556A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing tellurium dioxide from lead anode slime, and relates to the field of comprehensive recycling of scattered metal. According to the method disclosed by the invention, the characteristics of gasification volatilization, migration condensation and oxidative transformation of each component in the lead anode slime are utilized, and based on the advantages of a fire-wet combined process, tellurium enters tellurium-containing dust through first constant-temperature vacuum distillation to be separated from valuable metal elements such as gold, silver and copper; according to the method, arsenic, antimony and tellurium elements are all oxidized into arsenic trioxide, antimony trioxide and tellurium dioxide by adding a composite oxidizing agent (lead dioxide and hydrogen peroxide), and then two-section temperature gradient is controlled through secondary variable-temperature vacuum distillation, so that excessive moisture, arsenic trioxide, antimony trioxide and other impurities are removed from tellurium-containing dust subjected to oxidation regulation and control; tellurium dioxide powder with the tellurium dioxide content larger than 15% is obtained in residues, and the direct recovery rate of tellurium in the whole process is larger than 95%. The method is favorable for efficiently preparing tellurium dioxide from the lead anode slime, and is suitable for clean low-carbon recovery of tellurium in the comprehensive recovery and utilization process of scattered metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of comprehensive recycling of rare metals, and specifically to a method for preparing tellurium dioxide from lead anode mud. Background Art

[0002] Tellurium is a key rare metal material for safeguarding national security, promoting national economic development, and promoting the progress of high-precision and advanced technologies. Its importance in emerging fields such as national defense, aerospace, atomic energy, biomedicine, electronic information, and new energy continues to emerge. It is known as "the vitamin of modern industry, national defense, and cutting-edge technology, and the bridge to create miracles on earth" and "the supporting material of contemporary high-tech advanced materials". The efficient use of tellurium resources and the innovative development of new tellurium products have fundamental and leading strategic significance and are highly valued by the state and governments at all levels. Resources, energy, and environment are the main challenges facing modern nonferrous metallurgy. The smelting level of tellurium is an important indicator of the development level of a country's nonferrous metal industry. Clean, efficient, and short-process refining is a development goal that is constantly pursued. Tellurium in the earth's crust mainly exists in minerals such as lead, copper, nickel, gold, and silver in an associated form. There is almost no single primary mineral that can directly extract tellurium. Therefore, the main sources of tellurium are copper anode mud, lead anode mud, and nickel byproducts, and the potential sources of tellurium are tellurium bismuth ore and tellurium gold ore.

[0003] At present, more than 90% of tellurium comes from anode mud produced in the process of lead and copper electrolytic refining, and the rest comes from flue dust produced during the smelting of bismuth, nickel and copper ore, as well as tellurium bismuth ore and tellurium gold ore. In 2023, the country's lead and copper smelting enterprises will produce 430 tons of refined tellurium, accounting for about 67.19% of the global tellurium production. Lead and copper anode mud is increasingly becoming the main raw material for extracting tellurium. The traditional tellurium extraction process of lead and copper anode mud requires high-temperature smelting, slagging, leaching, purification, roasting, liquid making, electrolysis and other processes. Strong acids or alkalis such as sodium hydroxide and hydrochloric acid need to be added during refining, and a large amount of chemical reagents such as sodium sulfite and sodium sulfide and energy auxiliary materials such as heavy oil and natural gas are consumed at the same time. The generation of a large amount of wastewater, waste slag and waste gas causes serious pollution to the environment, and there are common problems such as long process flow, cumbersome operation, low metal direct recovery rate and long recovery cycle. Many bottlenecks restrict the sustainable development of tellurium extraction. The more prominent problem is that tellurium is dispersed in smelting slag, oxidation slag, refining slag, smoke and other metals, and the direct recovery rate of tellurium is less than 40%. Therefore, developing new technologies for green and efficient extraction of tellurium, cleanly utilizing tellurium resources in lead anode mud, streamlining separation process design, and improving resource utilization limits are urgent needs for the integration of lead metallurgy and tellurium refining, and are also the scientific and technological pillars for the ecological development of the industry. Summary of the invention

[0004] The present invention aims at the common problems of long process flow, complicated operation, low metal direct recovery rate and long recovery cycle in the existing lead anode mud tellurium recovery process, and proposes a method for preparing tellurium dioxide from lead anode mud from the perspectives of improving the direct recovery rate of tellurium, reducing reagent consumption, and harmlessly separating arsenic and antimony. The tellurium in the lead anode mud is separated and prepared in the form of tellurium dioxide through a three-stage process of constant temperature vacuum distillation-oxidation regulation-variable temperature vacuum distillation. The specific steps are as follows:

[0005] (1) Fresh lead anode mud is placed in a vacuum furnace for constant temperature vacuum distillation to obtain tellurium-containing dust.

[0006] (2) adding the tellurium-containing dust obtained in (1) to a composite oxidant for oxidation regulation, wherein the composite oxidant is lead dioxide and hydrogen peroxide.

[0007] (3) The tellurium-containing dust regulated by oxidation in (2) is placed in a vacuum furnace for variable temperature vacuum distillation to obtain tellurium dioxide powder and arsenic antimony oxide.

[0008] Preferably, the constant temperature vacuum distillation conditions in step (1) are: vacuum degree 1-50 Pa, distillation temperature 500-800° C., and distillation time 60-210 min.

[0009] Preferably, in step (2), the mass ratio of tellurium-containing dust, lead dioxide and hydrogen peroxide is (0.1-1):(0.3-1):2.

[0010] Preferably, the concentration of hydrogen peroxide in step (2) is 30%.

[0011] Preferably, the oxidation regulation time in step (2) is 60 to 240 minutes.

[0012] Preferably, the conditions for variable temperature vacuum distillation in step (3) are: vacuum degree 1-50 Pa, first heating to 100-200° C., keeping warm for 20-60 min, then heating to 300-660° C., and keeping warm for 30-180 min.

[0013] Preferably, a vertical vacuum furnace is used for vacuum distillation in step (1) and step (3). BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0015] The technical solutions in the embodiments of the present invention are described in further detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] Example 1

[0017] A method for efficiently preparing tellurium dioxide from lead anode mud (see Figure 1 ), the specific steps are as follows:

[0018] The lead anode mud used in this example is produced by the lead refining system of a lead smelter, and its composition is shown in Table 1.

[0019] Table 1 Lead anode mud composition

[0020] element As Sb Pb Bi Te Cu Ag Au Content (wt / %) 13.05 36.29 15.74 10.24 0.13 2.01 3.02 0.0012

[0021] (1) 10 kg of fresh lead anode mud was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled at 3 Pa and the temperature was 800 °C. After distillation for 60 min, 4.35 kg of tellurium-containing dust was obtained from the volatiles.

[0022] (2) 0.435 kg of lead dioxide and 6.53 kg of 30% hydrogen peroxide were added to the tellurium-containing dust obtained in step (1) and placed in a glass reactor for oxidation regulation. The reaction time was 240 min.

[0023] (3) The tellurium-containing dust regulated by oxidation in step (2) is placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace is controlled at 25 Pa. The temperature is first raised to 110° C. and kept at this temperature for 40 min to distill away excess hydrogen peroxide and moisture. The temperature is then raised to 660° C. and kept at this temperature for 180 min to obtain 88 g of tellurium dioxide powder from the residue.

[0024] The tellurium dioxide powder was tested and the tellurium dioxide content was 17.68% and the tellurium direct yield was 96.32%.

[0025] Example 2

[0026] A method for efficiently preparing tellurium dioxide from lead anode mud (see Figure 1 ), the specific steps are as follows:

[0027] The composition of the lead anode mud used in Example 2 of the present invention is the same as that in Example 1, and the composition is shown in Table 1.

[0028] (1) 10 kg of fresh lead anode mud was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled at 50 Pa and the temperature was 700 °C. After distillation for 180 min, 3.85 kg of tellurium-containing dust was obtained from the volatiles.

[0029] (2) The tellurium-containing dust obtained in step (1) was placed in a glass reactor together with 0.77 kg of lead dioxide and 4.24 kg of 30% hydrogen peroxide for oxidation regulation. The reaction time was 60 min.

[0030] (3) The tellurium-containing dust regulated by oxidation in step (2) is placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace is controlled to be 1 Pa. The temperature is first raised to 180° C. and kept at this temperature for 20 min to distill away excess hydrogen peroxide and moisture. The temperature is then raised to 300° C. and kept at this temperature for 150 min to obtain 100 g of tellurium dioxide powder from the residue.

[0031] The tellurium dioxide powder was tested and the tellurium dioxide content was 15.99% and the tellurium direct yield was 98.01%.

[0032] Example 3

[0033] A method for efficiently preparing tellurium dioxide from lead anode mud (see Figure 1 ), the specific steps are as follows:

[0034] The composition of the lead anode mud used in Example 3 of the present invention is the same as that in Example 1, and the composition is shown in Table 1.

[0035] (1) 10 kg of fresh lead anode mud was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled at 25 Pa and the temperature was 500 °C. After distillation for 210 min, 4.69 kg of tellurium-containing dust was obtained from the volatiles.

[0036] (2) The tellurium-containing dust obtained in step (1) was placed in a glass reactor together with 1.407 kg of lead dioxide and 9.38 kg of 30% hydrogen peroxide for oxidation regulation. The reaction time was 120 min.

[0037] (3) The tellurium-containing dust oxidized and regulated in step (2) was placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace was controlled at 50 Pa. The temperature was first raised to 200° C. and kept at this temperature for 60 min to distill away excess hydrogen peroxide and moisture. The temperature was then raised to 550° C. and kept at this temperature for 30 min to obtain 94 g of tellurium dioxide powder from the residue.

[0038] The tellurium dioxide powder was tested and the tellurium dioxide content was 16.55% and the tellurium direct yield was 95.48%.

[0039] Comparative Example 1

[0040] For comparison, the only difference between the local ratio and Example 3 is that the treatment in step (1) is not performed, and a composite oxidant consisting of lead dioxide and hydrogen peroxide is directly added to the fresh lead anode mud. The specific steps are as follows:

[0041] (1) 10 kg of fresh lead anode mud, 1.407 kg of lead dioxide and 9.38 kg of 30% hydrogen peroxide were placed in a glass reactor for oxidation control, and the reaction time was 120 min.

[0042] (2) The lead anode mud oxidized and regulated in step (1) is placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace is controlled to be 50 Pa. The temperature is first raised to 200° C. and kept at this temperature for 60 min to distill away excess hydrogen peroxide and moisture. The temperature is then raised to 550° C. and kept at this temperature for 30 min to obtain 588 g of tellurium dioxide powder from the residue.

[0043] The tellurium dioxide powder was tested, and the tellurium dioxide content was 2.11%, and the tellurium direct recovery rate was 76.21%; the effect of this comparative example was not as good as that of Example 3, because the first stage of constant temperature vacuum distillation was not performed, and the gold, silver, copper, lead, bismuth and other elements in the lead anode mud were stored in the residual tellurium dioxide powder in large quantities and could not be separated and removed, resulting in a significant decrease in the tellurium dioxide content in the residue to 2.11%, which greatly affected the quality of the tellurium dioxide product and was not conducive to the subsequent further use of the tellurium dioxide powder. At the same time, the metal compounds formed by elements such as silver and copper will also react with the lead dioxide and hydrogen peroxide in the composite oxidant, consuming part of the composite oxidant, so that the added composite oxidant is insufficient to completely oxidize tellurium to tellurium dioxide, resulting in tellurium volatilization loss during the variable temperature vacuum distillation process, which directly caused the tellurium direct recovery rate to drop significantly from 95.48% in Example 3 to 76.21%.

[0044] Comparative Example 2

[0045] For comparison, the only difference between this comparative example and Example 3 is that only hydrogen peroxide is added in step (2), and the remaining steps are the same as those in Example 3. The specific steps are as follows:

[0046] (1) 10 kg of fresh lead anode mud was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled at 25 Pa and the temperature was 500 °C. After distillation for 210 min, 4.69 kg of tellurium-containing dust was obtained from the volatiles.

[0047] (2) The tellurium-containing dust obtained in step (1) was placed in a glass reactor together with 9.38 kg of 30% hydrogen peroxide for oxidation regulation. The reaction time was 120 min.

[0048] (3) The tellurium-containing dust oxidized and regulated in step (2) was placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace was controlled at 50 Pa. The temperature was first raised to 200° C. and kept at this temperature for 60 min to distill away excess hydrogen peroxide and moisture. The temperature was then raised to 550° C. and kept at this temperature for 30 min to obtain 178 g of tellurium dioxide powder from the residue.

[0049] The tellurium dioxide powder was tested, and the tellurium dioxide content was 7.63%, and the tellurium direct yield was 83.47%; the effect of this comparative example was not as good as that of Example 3, because only adding hydrogen peroxide in step (2) would result in the inability of the hydrogen peroxide added within the same oxidation time to completely oxidize tellurium, arsenic and antimony into tellurium dioxide, arsenic trioxide and antimony trioxide. At the same time, lead dioxide also plays a role in continuing to oxidize tellurium during the variable temperature vacuum distillation process. The lack of lead dioxide prevents the composite oxidant from playing its due role during the variable temperature vacuum distillation process. When tellurium cannot be completely converted into tellurium dioxide, it is very easy to volatilize from the tellurium dioxide powder during the variable temperature vacuum distillation process, resulting in a rapid decrease in the tellurium dioxide content in the tellurium dioxide powder and a sharp drop in the tellurium direct yield.

[0050] Comparative Example 3

[0051] For comparison, the only difference between this comparative example and Example 3 is that only constant temperature distillation is performed in step (3), and the remaining steps are the same as those in Example 3. The specific steps are as follows:

[0052] (1) 10 kg of fresh lead anode mud was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled at 25 Pa and the temperature was 500 °C. After distillation for 210 min, 4.69 kg of tellurium-containing dust was obtained from the volatiles.

[0053] (2) The tellurium-containing dust obtained in step (1) was placed in a glass reactor together with 1.407 kg of lead dioxide and 9.38 kg of 30% hydrogen peroxide for oxidation regulation. The reaction time was 120 min.

[0054] (3) The tellurium-containing dust oxidized and regulated in step (2) was placed in a vertical vacuum furnace for constant temperature vacuum distillation. The vacuum degree in the furnace was controlled to 50 Pa, the temperature was raised to 550° C., and the heat preservation time was 30 min. 174 g of tellurium dioxide powder was obtained from the residue.

[0055] The tellurium dioxide powder was tested and the tellurium dioxide content was 8.13% and the tellurium direct yield was 87.36%. The effect of this comparative example was not as good as that of Example 3 because in step (3), only constant temperature vacuum distillation was performed without removing excess hydrogen peroxide and water through a variable temperature vacuum distillation process, which would directly lead to the oxidation of elements such as arsenic and antimony into high-priced arsenic pentoxide and antimony pentoxide. The high-priced arsenic antimony oxides were difficult to volatilize and remove during the vacuum distillation process. Part of the arsenic pentoxide and antimony pentoxide remained in the tellurium dioxide powder product, resulting in a significant decrease in the tellurium dioxide content and direct yield. The harmful arsenic and antimony element residues would also greatly affect the subsequent further processing and utilization of the tellurium dioxide powder.

[0056] Comparative Example 4

[0057] For comparison, the vacuum distillation in step (1) was replaced by ordinary drying, and the remaining steps were the same as those in Example 3, specifically, the following steps:

[0058] (1) Take 10 kg of fresh lead anode mud at 500 °C and dry it for 210 min to obtain 7.46 kg of tellurium-containing dust from the volatiles.

[0059] (2) The tellurium-containing dust obtained in step (1) was placed in a glass reactor together with 1.407 kg of lead dioxide and 9.38 kg of 30% hydrogen peroxide for oxidation regulation. The reaction time was 120 min.

[0060] (3) The tellurium-containing dust regulated by oxidation in step (2) was placed in a vertical vacuum furnace for variable temperature vacuum distillation. The vacuum degree in the furnace was controlled at 50 Pa. The temperature was first raised to 200° C. and kept at this temperature for 60 min to distill away excess hydrogen peroxide and moisture. The temperature was then raised to 550° C. and kept at this temperature for 30 min to obtain 623 g of tellurium dioxide powder from the residue.

[0061] The tellurium dioxide powder was tested and the tellurium dioxide content was 1.85% and the tellurium direct recovery rate was 70.84%. The effect of this comparative example was not as good as that of Example 3 because after the vacuum distillation was replaced by ordinary drying, step (1) could only remove excess water and part of arsenic antimony oxides in the fresh lead anode mud. Similar to Comparative Example 1, a large amount of elements such as gold, silver, copper, lead, bismuth and the like in the lead anode mud entered the tellurium-containing dust and tellurium dioxide powder together with tellurium, resulting in a significant decrease in the tellurium dioxide content in the residue to 1.85%, which greatly affected the quality of the tellurium dioxide product and was not conducive to the subsequent further utilization of the tellurium dioxide powder. At the same time, metal compounds formed by elements such as silver and copper will also react with lead dioxide and hydrogen peroxide in the composite oxidant, consuming part of the composite oxidant, so that the added composite oxidant is insufficient to completely oxidize tellurium into tellurium dioxide, resulting in tellurium volatilization loss during the variable temperature vacuum distillation process, which directly leads to a significant decrease in the tellurium direct yield from 95.48% in Example 3 to 70.84%.

[0062] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for preparing tellurium dioxide from lead anode mud, It is characterized in that The specific steps are as follows: (1) placing fresh lead anode mud into a vacuum furnace for constant temperature vacuum distillation to obtain tellurium-containing dust; (2) adding the tellurium-containing dust obtained in (1) to a composite oxidant for oxidation regulation, wherein the composite oxidant is lead dioxide and hydrogen peroxide; (3) The tellurium-containing dust regulated by oxidation in (2) is placed in a vacuum furnace for variable temperature vacuum distillation to obtain tellurium dioxide powder and arsenic antimony oxide.

2. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: The constant temperature vacuum distillation conditions in step (1) are: vacuum degree 1-50 Pa, distillation temperature 500-800° C., and distillation time 60-210 min.

3. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: In step (2), the mass ratio of tellurium-containing dust, lead dioxide and hydrogen peroxide is (0.1-1):(0.3-1):

2.

4. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: The concentration of hydrogen peroxide in step (2) is 30%.

5. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: The oxidation regulation time in step (2) is 60 to 240 minutes.

6. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: The conditions of variable temperature vacuum distillation in step (3) are: vacuum degree 1-50 Pa, first heating to 100-200° C., keeping warm for 20-60 min, then heating to 300-660° C., keeping warm for 30-180 min.

7. The method for preparing tellurium dioxide from lead anode mud according to claim 1, Features: In step (1) and step (3), a vertical vacuum furnace is used for vacuum distillation.

Citation Information

Patent Citations

  • Separation and recycling method for TeO2 in cuprous telluride compound waste material

    CN107827089A

  • Method for recycling lead and tellurium from lead anode slime

    CN107868875A

  • Method for efficiently recovering noble metal from lead anode slime

    CN109097587A

  • Method for lead anode slime enhanced oxidation-low-pressure efficient enrichment of precious metal

    CN116024432A

  • Method for recovering tellurium and copper from copper telluride slag

    CN117701903A