Continuous synthesis method of polysuccinate
Through the five-step continuous process of succinic anhydride and polyol, the problems of small molecules and poor quality in polysuccinate synthesis are solved, and high-efficiency and low-cost high-quality polysuccinate production are achieved, which improves the Melt strength and product controllability.
Patent Information
- Application Number
- CN202411269483.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The existing polysuccinate synthesis method produces a large number of small molecules by-products, resulting in low raw material utilization, poor quality and performance of polyester products, high production costs, and intermittent operations lead to uneven product quality and poor batch controllability. .
The esterification efficiency and molecular weight are improved through five continuous processes: normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum finalization. , reduce acid value and chromaticity, and enhance melt strength.
Achieve high-quality polysuccinate production efficiently and at low cost, reducing production costs, improving the molecular weight and melt strength of the product, ensuring the quality uniformity and controllability of the product, reducing environmental pollution and follow-up treatment costs .
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material synthesis, and in particular relates to a continuous synthesis method of polysuccinate. Background Art
[0002] Polyester is an extremely important polymer material with a wide range of applications in aerospace, biomedicine, agriculture and daily life. It has become an indispensable basic material for the national economy and modern life. Polysuccinates such as polyethylene succinate (PES) and polybutylene succinate (PBS) are a large class of materials with special properties and application scenarios in polyesters. They have become the focus of public attention. my country will have a huge demand for them in the future, so it is urgent to develop advanced and low-cost large-scale continuous production technology for polysuccinates.
[0003] The existing methods for synthesizing polysuccinates mainly include direct esterification and transesterification. The direct esterification method uses succinic acid and polyols as monomers, first esterifies to generate oligomers and water of two times the molar amount of monomer succinic acid, and then the oligomers are prepolymerized and finally polycondensed under high temperature and high vacuum conditions to generate high molecular weight polyester. The transesterification method uses succinic acid diester (methyl ester or ethyl ester) and polyols as monomers, first generates oligomers and alcohol of two times the molar amount of monomer succinic acid diester through transesterification, and then the oligomers are prepolymerized and finally polycondensed to obtain polysuccinates. However, the above two methods all produce a large number of small molecules as byproducts, resulting in low raw material utilization, low polyester product yield, and the generation of a large number of small molecules is not conducive to improving polymer molecular weight, polyester product quality and performance are poor, and finally, the recovery and treatment of a large number of small molecules will increase environmental protection treatment costs, indirectly increasing production costs.
[0004] Adopt succinic anhydride to replace succinic acid or succinic diester and polyol through ring-opening polycondensation can effectively avoid the above problems, because the reaction process only produces the water of monomer succinic anhydride equimolar amount, can greatly reduce the consumption of raw materials, improve product yield, with succinic anhydride, polyester yield reaches more than 90wt% (succinic acid method route with succinic acid product yield is no more than 72wt%, succinic diester route with succinic diester yield is no more than 65%). And, there is no chemical equilibrium in the ring-opening process, can greatly improve reaction efficiency, and improve product molecular weight, mechanical property and thermal property of products obtained therefrom also significantly improve. However, the report of preparing polysuccinic esters by succinic anhydride and polyol is less. For example, patent CN102964581A discloses a method for preparing polyester polyols by two-step esterification reaction using succinic anhydride and aliphatic diols such as 1,4-butanediol, ethylene glycol, and diethylene glycol through gradient heating. The polyester polyols obtained by this method are used as polymerization monomers or intermediates, and usually have a low molecular weight and cannot be used directly as materials. Patents CN101880377A, CN104130381B, CN104130382B, etc. reported the use of succinic anhydride and aliphatic diols through three-step reactions of ring-opening esterification, negative pressure prepolymerization, and vacuum polycondensation to prepare aliphatic polyesters. The weight-average molecular weight of the obtained polyesters is more than 100,000, and can reach up to 300,000. However, since this method only uses a one-step ring-opening esterification process, the esterification reaction is incomplete, especially the acid value of the esterified product is high, which increases the side reactions, and ultimately leads to a high acid value of the product (generally above 50 mol / t), poor chromaticity, and even yellowing. In addition, the increase of side reactions will also reduce the molecular weight of polyester and increase the molecular weight distribution, which will affect the final use of the product. For example, the PBS product disclosed in the above patent has poor melt strength, and the melt index is generally between 30 and 50 g / 10 min, and its blow molding processing ability is poor. A large number of studies have shown that the melt strength of polyesters formed by polyols (3 yuan and above) or rigid structure diols is usually high and can be used as blow molding products, but the above patents do not involve this. At present, the synthesis of polysuccinates by ring-opening polycondensation of succinic anhydride and polyols mostly adopts intermittent operation. The disadvantage of this method is that it will lead to uneven product quality, poor controllability of batch products, and will also affect the quality of the product.
[0005] The applicant team previously disclosed in patents CN114920916A, CN114015026B and CN113980252B that succinic anhydride, tetrahydrofuran and modifier are used as monomer raw materials, and the technology of preparing high molecular weight, high performance polybutylene succinate (PBS) or modified PBS through three reaction steps of ring-opening esterification, negative pressure prepolymerization and vacuum final polymerization. Recently, we unexpectedly found that adding reaction steps such as ring-opening or pressurized esterification can significantly reduce the acid value and melt index of the product. In view of this, comparative analysis of the polymerization of succinic anhydride and polyols found that when only one-step ring-opening esterification is used, the esterification will be incomplete due to low ring-opening efficiency and low utilization rate of alcohol, thereby affecting the quality of the final product. Therefore, adding the ring-opening step alone can improve the ring-opening efficiency of polyols and succinic anhydride, and obtain the ring-opening product in a directional manner. Subsequently, increasing the pressurized esterification operation can effectively avoid the volatilization or decomposition of the remaining alcohol, improve its utilization rate, and further improve the esterification rate by reduced pressure esterification after the esterification rate reaches a certain degree, so that the esterification is close to complete. The above steps can effectively solve the problem of incomplete esterification, thereby solving the technical problems brought about thereby, and further by using polyols (3 yuan and above) or rigid structure diols to significantly improve the melt strength of the product, expand its application range. In view of this, the present invention develops an advanced continuous polymerization technology for preparing polysuccinates using succinic anhydride and polyols as polymerization raw materials in five steps of normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization, and solves the above technical problems in a targeted manner. Summary of the invention
[0006] In order to solve the shortcomings of the prior art, the present invention provides a continuous synthesis method of polysuccinate, which uses succinic anhydride and polyols as polymerization monomers, and continuously and low-cost produces high-quality polysuccinate materials with uniform quality through five steps of normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization and vacuum final polymerization. The method mainly overcomes the problems of high acid value, poor chromaticity, poor melt strength, high production cost and intermittent operation of products in the prior art.
[0007] The objective of the present invention is achieved through the following technical solutions:
[0008] A continuous synthesis method of polysuccinate is to use succinic anhydride and polyol as monomer raw materials, and to continuously synthesize polysuccinate through five steps including normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization, and specifically comprises the following steps:
[0009] (1) continuously conveying the monomer raw material succinic anhydride and part of the polyol to a ring-opening reaction device, performing a ring-opening reaction at a temperature of 60 to 120° C., under normal pressure, and for a residence time of 5 to 120 minutes to obtain a normal pressure ring-opening product;
[0010] (2) continuously feeding the ring-opening product obtained in step (1) into a pressure esterification reaction device, and continuously adding the remaining polyol and esterification catalyst, and performing a pressure esterification reaction at a temperature of 100 to 220° C., a pressure of 0.10 to 1.0 MPa (A), and a residence time of 30 to 300 min to obtain a pressure esterification product;
[0011] (3) continuously feeding the pressurized esterification product obtained in step (2) into a reduced pressure esterification reaction device, removing small molecules under reduced pressure at a temperature of 140 to 240° C., a pressure of 10 to 80 kPa (A), and a residence time of 30 to 180 min to obtain a reduced pressure esterification product;
[0012] (4) continuously feeding the vacuum esterification product obtained in step (3) into a prepolymerization reaction device, mixing it with a polymerization catalyst, and then performing a prepolymerization reaction at a temperature of 180 to 240° C., a pressure of 1 to 60 kPa(A), and a residence time of 20 to 180 min to obtain a vacuum prepolymerization product;
[0013] (5) The prepolymer product obtained in step (4) is continuously fed into a final polymerization reaction device, and a vacuum final polymerization reaction is carried out at a temperature of 200 to 280° C., a pressure of 5 to 200 Pa (A), and a residence time of 30 to 240 min to obtain polysuccinate. The obtained polysuccinate is continuously discharged and pelletized and dried underwater to obtain a polyester pellet product.
[0014] Furthermore, in step (1), the ring-opening reaction conditions are a temperature of 70 to 100° C., a pressure of normal pressure, and a residence time of 20 to 90 min.
[0015] Furthermore, in step (1), the conditions for the ring-opening reaction are a temperature of 70 to 90° C., a pressure of normal pressure, and a residence time of 30 to 60 min.
[0016] Furthermore, in step (2), the pressurized esterification reaction conditions are a temperature of 150 to 200° C., a pressure of 0.2 to 0.7 MPa, and a residence time of 60 to 240 min.
[0017] Furthermore, in step (2), the pressurized esterification reaction conditions are a temperature of 170-190° C., a pressure of 0.3-0.5 MPa and a residence time of 90-180 min.
[0018] Furthermore, in step (3), the reduced pressure esterification reaction conditions are a temperature of 160 to 210° C., a pressure of 20 to 60 kPa, and a residence time of 60 to 150 min.
[0019] Furthermore, in step (3), the reduced pressure esterification reaction conditions are a temperature of 180 to 200° C., a pressure of 30 to 50 kPa, and a residence time of 90 to 120 min.
[0020] Furthermore, in step (4), the negative pressure prepolymerization reaction conditions are a temperature of 190 to 230° C., a pressure of 2 to 30 kPa, and a residence time of 45 to 150 min.
[0021] Furthermore, in step (4), the pre-polycondensation reaction conditions are a temperature of 200 to 220° C., a pressure of 3 to 15 kPa, and a residence time of 60 to 120 min.
[0022] Furthermore, in step (5), the vacuum polymerization reaction conditions are temperature 210-260° C., pressure 10-150 Pa and residence time 60-210 min.
[0023] Furthermore, in step (5), the vacuum polymerization reaction conditions are temperature 230-250° C., pressure 30-80 Pa and residence time 90-180 min.
[0024] Furthermore, the molar ratio of the monomer raw materials is succinic anhydride:polyol=1.00:(1.00-2.00), preferably 1.00:(1.10-1.45).
[0025] Furthermore, in step (1), the molar ratio of succinic anhydride:polyol is 1.00:(1.00-1.10), preferably 1.00:(1.00-1.05), and the remaining part of the polyol is continuously added in the pressurized esterification reaction in step (2).
[0026] Furthermore, the amount of the esterification catalyst is 0.01 to 2.00% of the molar amount of succinic anhydride, preferably 0.05 to 0.20%.
[0027] Furthermore, the amount of the polymerization catalyst is 0.01 to 1.00% of the molar amount of succinic anhydride, preferably 0.05 to 0.20%.
[0028] Furthermore, the esterification catalyst is selected from one or more of methanesulfonic acid, p-toluenesulfonic acid, p-toluenesulfonic acid hydrate, trifluoromethanesulfonic acid, trifluoroacetic acid and trichloroacetic acid; and the polymerization catalyst is selected from one or more of titanium, tin, antimony and germanium compounds.
[0029] Further, the polymerization catalyst is titanium dioxide, titanium silicon composite, titanium trichloride, titanium tetrachloride, tributoxytitanium chloride, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetraisooctyl titanate, tetrahydroxyethyl titanate, diethylene glycol titanate, tetrahydroxypropyl titanate, dipropylene glycol titanate, tetrahydroxybutyl titanate or dibutyl titanate, or tin dichloride, tin tetrachloride, stannous succinate, stannous octoate, stannous benzoate, dioctyltin oxide, tetrabutyltin, dibutyltin acetate, or antimony pentoxide, antimony trioxide, antimony trichloride, antimony pentachloride, ethylene glycol antimony or butanediol antimony, or one or more of germanium dioxide, germanium tetrachloride, tetrabutoxygermanium, tetramethylgermanium or tetraethylgermanium.
[0030] Furthermore, the polymerization catalyst is at least one of tetrabutyl titanate, diethylene glycol titanate, tetrahydroxybutyl titanate, dibutylene glycol titanate and antimony ethylene glycol.
[0031] Furthermore, the polyol is one or more of aliphatic polyols, aromatic polyols, heterocyclic polyols, polyaliphatic alcohol ether polyols, polyaromatic alcohol ether polyols, polyaromatic phenol ether polyols, polyheterocyclic alcohol ether polyols, polyfatty acid ester polyols, polyaromatic acid ester polyols and polyheterocyclic acid ester polyols.
[0032] Furthermore, the molecular weight Mn of the polyfatty alcohol ether polyol is 300-10000 g / mol, the molecular weight Mn of the polyaromatic alcohol ether polyol is 500-5000 g / mol, the molecular weight Mn of the polyaromatic phenol ether polyol is 500-5000 g / mol, the molecular weight Mn of the polyheterocyclic alcohol ether polyol is 500-5000 g / mol, the molecular weight Mn of the polyfatty acid ester polyol is 400-10000 g / mol, the molecular weight Mn of the polyaromatic acid ester polyol is 300-10000 g / mol, and the molecular weight Mn of the polyheterocyclic acid ester polyol is 300-10000 g / mol.
[0033] Further, the fatty polyols include 1,2-ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,2-propylene glycol, 1,2-butylene glycol, 2-methyl-1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, 2,2,4 4-tetramethyl-1,3-cyclobutanediol, glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, lactitol, glucose, fructose, chitosan, starch or more; the aromatic polyols include phenyl glycol, terephthalic alcohol, o-terephthalic alcohol, isophthalic alcohol, terephthalic alcohol, o-terephthalic alcohol, isophthalic alcohol, o-chlorophenyl glycol, 4,4'-dihydroxymethyl biphenyl or more; the heterocyclic polyols include 2,5-furan dimethanol, tetrahydro-2-methyl-2H-pyran-3,4-diol, hydroxypropyl tetrahydropyrantriol, 2,6-pyridine dimethanol, 2,3-thiophene The polyaliphatic alcohol ether polyol includes ethylene glycol or ethylene oxide, 1,2-propylene glycol or propylene oxide, 1,4-butanediol or tetrahydrofuran, 1,2-butanediol or 1,2-butylene oxide, 2,3-butanediol or 2,3-butylene oxide, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol or cyclohexene oxide, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, glycerol or glycidol or epichlorohydrin and polyethers thereof with polyols The polyols are selected from the group consisting of one or more copolymers of polyols, the polyaromatic alcohol ether polyols include one or more polyethers of terephthalylinol, isophthalylinol, o-phthalylinol, styrene oxide or phenyl glycol and copolymers thereof with polyols, the polyaromatic phenol ether polyols include one or more copolymers of hydroquinone, resorcinol and / or o-phthalylinol and polyethers thereof with polyols, the polyheterocyclic alcohol ether polyols include one or more polyethers of 2,5-furan dimethanol, 2,6-pyridine dimethanol, 2,3-thiophenedimethanol, 3,4-thiophenediol and 3,4-tetrahydrothiophenediol and copolymers thereof with polyols, the polyfatty acid ester polyols include poly C 1 ~C 10One or more of fatty polyacid polyols, polyhydroxy acid esters, and polyhydroxy acid ester polyols; the polyaromatic acid ester polyols include one or more of polyphthalic acid polyols, polytricarboxylic acid polyols, and polynaphthalic acid polyols; the polyheterocyclic acid ester polyols include one or more of poly-2,5-furandicarboxylate polyols, poly-2,6-pyridinedicarboxylate polyols, and poly-2,3-thiophenedicarboxylate polyols.
[0034] Further, the fatty polyol includes one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, 1,2-propylene glycol, 1,2-butanediol, 2-methyl-1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, and lactitol, and the aromatic polyol includes one or more of terephthalic acid, isophthalic acid, 4-terephthalic acid, 1,2-butylene glycol, 1,2-methyl-1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, and lactitol. ,4'-dihydroxymethyl biphenyl, the heterocyclic polyol includes one or more of 2,5-furan dimethanol, 2,6-pyridine dimethanol, 2,3-thiophenedimethanol and 3,4-thiophenediol, the poly fatty alcohol ether polyol includes one or more of ethylene glycol, 1,2-propylene glycol, poly 1,4-butylene glycol, poly 1,4-cyclohexanediol, poly 1,4-cyclohexanedimethanol, polyethylene glycol glycerol ether, polypropylene glycol glycidyl ether, poly 1,2-cyclohexanediol ethylene glycol ether and poly 1,4-butylene glycol pentaerythritol ether, the poly aromatic alcohol ether polyol includes poly p-phenylene glycol, poly m-phenylene glycol, polyoxyethylene glycol The polyols are selected from the group consisting of polyols of polyethylene glycol, polyethylene glycol ether, polyethylene oxide glycerol ether, polyols of polyethylene glycol ether, polyethylene glycol ether, polyethylene glycol ether, polyols of ... The invention relates to a polyol comprising one or more of lactide diol, poly(glycolide-lactide) diol, polylactide diol, polyglycolic acid glyceride, polyhydroxybutyric acid, polycaprolactone diol, and polyhydroxycaproic acid glyceride; the polyaromatic acid ester polyol comprises one or more of polyethylene terephthalate diol, polyethylene isophthalate diol, polyethylene trimesic acid triol, and polyethylene naphthalate diol; the polyheterocyclic acid ester polyol comprises one or more of polyethylene 2,5-furandicarboxylic acid-ethylene glycol ester diol, poly-2,5-furandimethylol ester diol, and polyethylene 2,6-pyridinedicarboxylic acid glycol ester diol.
[0035] Further, the fatty polyol includes one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,4-cyclohexanediol, glycerol, trimethylolpropane, pentaerythritol, erythritol or sorbitol, the aromatic polyol is terephthalic acid, the heterocyclic polyol is 2,5-furan dimethanol, the poly fatty alcohol ether polyol is one of polyethylene glycol, poly 1,2-propylene glycol, poly 1,4-butanediol, polyethylene glycol glycerol ether, polypropylene glycol glycidyl ether and poly 1,4-butanediol pentaerythritol ether, the poly aromatic alcohol ether polyol is polyoxystyrene glycerol ether, and the poly aromatic phenol ether polyol is polyhydroquinone glycol ether or polyhydroquinone condensation. The polyheterocyclic alcohol ether polyol is poly-2,5-furan dimethanol ether or poly-2,5-furan dimethanol ethylene glycol ether, the poly fatty acid ester polyol is polyethylene oxalate glycol ester diol, polybutylene succinate glycol ester diol, polyhexamethylene adipate glycol ester diol, polyethylene adipate glycol ester diol, polyglycolide diol, poly(glycolide-lactide) diol, polylactide diol, polyhydroxybutyric acid or polycaprolactone diol, the polyaromatic acid ester polyol is polyethylene terephthalate diol, polyethylene isophthalate diol or polyethylene trimesic acid triol, and the polyheterocyclic acid ester polyol is polyethylene 2,5-furan dicarboxylate diol or poly-2,5-furan dicarboxylic acid-2,5-furan dimethanol ester diol.
[0036] Furthermore, the polyol is a combination of at least one of ethylene glycol, 1,3-propylene glycol, pentaerythritol, aromatic diols, polyethylene glycol and 1,4-butanediol.
[0037] Furthermore, the polyol is a composition of 1,4-butanediol and one of 1,3-propylene glycol, pentaerythritol, aromatic diols, polyethylene glycol, wherein the molar amount of 1,4-butanediol in the composition is not less than the molar amount of other alcohols; preferably, the molar ratio of 1,4-butanediol to any other alcohol in the composition is (50-95): (50-5).
[0038] The present invention also provides a polysuccinate prepared by the above-mentioned continuous synthesis method of polysuccinate.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] (1) The use of succinic anhydride and polyol ring-opening polycondensation can improve reaction efficiency, improve raw material utilization, and increase product molecular weight and quality, and can significantly reduce raw material costs. Because the efficiency of the ring-opening reaction of succinic anhydride and polyol is high, and the amount of small molecules generated by esterification is small, it is easy to remove them in vacuum, thereby increasing the molecular weight of the polymer; at the same time, the energy consumption of vacuum removal of small molecules is also greatly reduced, and the emission of environmental pollutants is also greatly reduced, which not only makes the production process cleaner, but also reduces the cost of subsequent treatment.
[0041] (2) The five-step operation, especially the ring-opening and two-step esterification units, can significantly improve the esterification rate, making the esterification reaction close to completion, the acid value of the esterified product is low, and the acid-catalyzed side reactions during polymerization are reduced, thereby making the acid value of the product low, which is conducive to storage and transportation, and the product has good color, excellent performance and high quality.
[0042] (3) The continuous polymerization process is adopted, the material concentration and temperature are uniform and the residence time is short, which avoids the thermal depolymerization of polyester in the high temperature stage, so that the synthesized product has a high degree of polymerization and good quality, and can be mass-produced continuously with uniform quality polysuccinate products. In addition, the continuous polymerization process is conducive to reducing production costs.
[0043] (4) The raw materials and process of the present invention are flexible to adjust. By flexibly changing the types and proportions of polyols and process conditions, a variety of products with different properties and grades can be produced. In particular, the use of polyols (trihydric and above) or rigid structure diols can obtain polyester products with high melt strength to meet the needs of specific downstream users. DETAILED DESCRIPTION
[0044] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples. Obviously, the described examples are only part of the embodiments of the present invention, not all. Based on the examples in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0045] Examples 1 to 9
[0046] Polybutylene succinate (PBS) was prepared by a five-step continuous reaction process of normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization using succinic anhydride (SAA) and 1,4-butanediol (BDO) as monomer raw materials. The preparation process is as follows:
[0047] (1) Succinic anhydride and 1,4-butanediol are continuously transported to a ring-opening reaction kettle at a molar ratio of anhydride:alcohol = 1.00:(1.00-1.10), and a normal pressure ring-opening reaction is carried out at a temperature of 60-120° C., a normal pressure, and a residence time of 5-120 min to obtain a normal pressure ring-opening product;
[0048] (2) the normal pressure ring-opening product is then continuously fed into a pressure esterification reactor, and the remaining polyol (in an amount of 0.01 to 0.90 times the molar amount of succinic anhydride) and an esterification catalyst (in an amount of 0.01 to 2.0% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and a pressure esterification reaction is carried out at a temperature of 100 to 220° C., a pressure of 0.11 to 1.0 MPa, and a residence time of 30 to 300 min to obtain a pressure esterification product;
[0049] (3) continuously feeding the pressurized esterification product into a vacuum esterification reactor, removing small molecules under reduced pressure at a temperature of 140 to 240° C., a pressure of 10 to 80 kPa, and a residence time of 30 to 180 min, thereby further improving the esterification rate and obtaining a vacuum esterification product;
[0050] (4) continuously feeding the vacuum esterification product into a vacuum prepolymerization reactor, and mixing it with a polymerization catalyst (the amount used is 0.01-1.00% of the molar amount of succinic anhydride), and then performing a prepolymerization reaction at a temperature of 180-240° C., a pressure of 1-60 kPa, and a residence time of 20-180 min to obtain a vacuum prepolymerization product;
[0051] (5) The negative pressure prepolymerization product is continuously fed into the final polymerization reactor, and vacuum final polymerization is carried out at a temperature of 200-280°C, a pressure of 5-200Pa and a residence time of 30-240min to obtain polybutylene succinate, and the material is continuously discharged and underwater pelletized and dried to obtain a PBS pellet product. The specific formulas and process conditions of Examples 1-9 are shown in Tables 1 and 2, wherein Table 1 shows the total ratio of succinic anhydride to 1,4-butanediol monomer, the feed ratio in the ring-opening reactor, and the type and amount of catalyst, and Table 2 shows the process conditions of each stage corresponding to each embodiment. Table 3 shows the molecular weight and performance indicators of the polymers prepared in the specific embodiments.
[0052] Table 1 Raw material ratio, catalyst type and dosage conditions for the synthesis of PBS by ring-opening polymerization of SAA and BDO
[0053]
[0054] Table 2 Process conditions for the synthesis of PBS by ring-opening polymerization of succinic anhydride and 1,4-butanediol
[0055]
[0056] Table 3 Molecular weight and main performance indicators of the obtained polymer
[0057]
[0058]
[0059] It can be seen from the results of each embodiment given in Table 3 that a PBS product with a higher molecular weight can be obtained by adopting the ratio, catalyst and dosage, and process conditions described in the present invention. Under relatively optimized conditions (Examples 1 to 7), the molecular weight of the obtained PBS is higher, between 210,000 and 310,000, which is higher than the molecular weight of PBS obtained by the esterification method and the ester exchange method under the optimized conditions, and the molecular weight distribution Mw / Mn is 1.39 to 1.87, which is relatively narrow. In addition, the PBS acid value is low, which is 19 to 29 mol / t, the color quality is very good, the L value is above 88, and the melt index can reach 8.5 to 15.7 g / 10 min, generally below 20 g / 10 min, which significantly improves its melt strength and improves its processing performance.
[0060] The above results show that the five-step continuous operation can significantly increase the molecular weight of the polymer by increasing the esterification rate, reduce the molecular weight distribution, and make its performance better, especially greatly reduce the acid value and improve the melt index, thereby significantly improving the quality of PBS products and expanding its application field.
[0061] Comparative Example 1
[0062] Compared with Example 1, the difference is that succinic acid and 1,4-butanediol are used as monomer raw materials to prepare the PBS product by esterification method, and the similar operation steps of ring-opening polycondensation are followed: succinic acid and 1,4-butanediol are continuously transported to a pressure reactor at a molar ratio of succinic acid: alcohol = 1.00:1.35 and an esterification catalyst (the amount used is 0.05% of the molar amount of succinic acid) to carry out a pressure esterification reaction at a temperature of 170° C., a pressure of 0.3 MPa and a residence time of 100 min; then, the mixture is continuously transported to a reduced pressure esterification reactor at a temperature of 190° C., a pressure of 45k The small molecules are removed under reduced pressure at 400° C. and a residence time of 110 min to further improve the esterification rate; the mixture is then continuously fed into a prepolymerization reactor, mixed with a polymerization catalyst (the dosage is 0.05% of the molar amount of succinic acid), and a prepolymerization reaction is carried out at a temperature of 200° C., a pressure of 4 kPa, and a residence time of 80 min to obtain a negative pressure prepolymerization product; the mixture is finally continuously fed into a final polymerization reactor, and a vacuum final polymerization reaction is carried out at a temperature of 235° C., a pressure of 50 Pa, and a residence time of 120 min to obtain polybutylene succinate, which is continuously discharged and underwater pelletized and dried to obtain a PBS pellet product.
[0063] After testing, the molecular weight of the obtained polymer is 144,000, the molecular weight distribution is 2.13, and the acid value is relatively large, which is 58.7 mol / t, the L value is about 74, and the melt index is 36g / 10min. It can be seen that compared with the ring-opening polycondensation method, the product obtained by the esterification method has a lower molecular weight, a larger molecular weight distribution, a higher acid value, poorer quality, and a higher melt index.
[0064] Comparative Example 2
[0065] Compared with Example 1, the difference is that dimethyl succinate and 1,4-butanediol are used as monomer raw materials to prepare the PBS product by ester exchange method, and the similar operation steps of ring-opening polycondensation are followed: dimethyl succinate and 1,4-butanediol are continuously transported to a pressure reactor at a molar ratio of dimethyl succinate: alcohol = 1.00:1.35 and an esterification catalyst (the amount used is 0.05% of the molar amount of dimethyl succinate) to carry out a pressure esterification reaction at a temperature of 170°C, a pressure of 0.3 MPa and a residence time of 100 min; then continuously sent to a reduced pressure esterification reactor, at a temperature of 190°C, a pressure of 0.3 MPa and a residence time of 100 min. The small molecules are removed under reduced pressure at a pressure of 45 kPa and a residence time of 110 min to further improve the esterification rate; then the mixture is continuously fed into a prepolymerization reactor and mixed with a polymerization catalyst (the dosage is 0.05% of the molar amount of dimethyl succinate), and then a negative pressure prepolymerization reaction is carried out at a temperature of 200° C., a pressure of 4 kPa and a residence time of 80 min to obtain a negative pressure prepolymerization product; finally, the mixture is continuously fed into a final polymerization reactor, and a vacuum final polymerization reaction is carried out at a temperature of 235° C., a pressure of 50 Pa and a residence time of 120 min to obtain polybutylene succinate, and the mixture is continuously discharged and underwater pelletized and dried to obtain a PBS pellet product.
[0066] After testing, the molecular weight of the obtained polymer is 183,000, the molecular weight distribution is 1.98, and the acid value is relatively large, which is 33.4 mol / t, the L value is about 89, and the melt index is 30g / 10min. Although compared with the esterification method, the molecular weight and product quality have improved, but it is still lower than the ring-opening polycondensation method, especially the melt index is significantly higher than the ring-opening polycondensation method.
[0067] Comparative Example 3
[0068] Compared with Example 1, the difference is that the PBS product is prepared by the PBS transesterification method in which SAA and BDO are subjected to three steps of ring-opening esterification, negative pressure prepolymerization, and vacuum polycondensation. The specific steps are as follows:
[0069] Succinic anhydride and 1,4-butanediol are added to a ring-opening esterification reaction kettle at a molar ratio of anhydride:alcohol=1.00:1.35, mixed with p-toluenesulfonic acid (the amount is 0.05% of the molar amount of succinic anhydride), and subjected to a ring-opening esterification reaction at a temperature of 190°C, a pressure of 45 kPa and a residence time of 110 min; then continuously fed into a prepolymerization kettle, mixed with a polymerization catalyst tetrabutyl titanate (the amount is 0.05% of the molar amount of succinic anhydride), and subjected to a prepolymerization reaction at a temperature of 200°C, a pressure of 4 kPa and a residence time of 80 min to obtain a negative pressure prepolymerization product; finally continuously fed into a final polymerization reaction kettle, subjected to a vacuum final polymerization reaction at a temperature of 235°C, a pressure of 50 Pa and a residence time of 120 min to obtain polybutylene succinate, and continuously discharged and underwater pelletized and dried to obtain a polyester pellet product.
[0070] After testing, the molecular weight of the obtained polymer is 178,000, the molecular weight distribution is 1.94, and the acid value is relatively large, which is 41 mol / t, the L value is about 83, and the melt index is 37 g / 10 min. It can be seen that the three-step method has a high acid value, poor quality, and a high melt index due to incomplete esterification.
[0071] Comparative Example 4
[0072] Compared with Example 1, the difference is that the PBS product is prepared by reacting SAA and BDO in four steps of normal pressure ring opening, pressurized esterification, negative pressure prepolymerization, and vacuum final polymerization. Comparative Example 4 removes the reduced pressure esterification process in Example 1, and the other operations are consistent with Example 1, that is, it is changed to a four-step operation. After testing, the molecular weight of the obtained polymer is 143,000, the molecular weight distribution is 2.04, the acid value is 46 mol / t, the L value is about 80, and the melt index is 44 g / 10min. It can be seen that due to the reduction of the reduced pressure esterification process, the esterification process is incomplete, so both the polymer molecular weight and the product quality are poor, significantly lower than the results of Example 1, and even lower than the three-step method results of Comparative Example 3.
[0073] Comparative Example 5
[0074] Compared with Example 1, the difference is that PBS is prepared by reacting SAA and BDO in four steps: normal pressure ring opening, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization.
[0075] Comparative Example 5 removes the pressurized esterification process in Example 1, and the other operations are consistent with Example 1, that is, it is changed to a four-step operation. After testing, the molecular weight of the obtained polymer is 203,000, the molecular weight distribution is 1.68, the acid value is 42 mol / t, the L value is about 82, and the melt index is 18g / 10min. It can be seen that the pressurized esterification process is reduced, resulting in a decrease in monomer utilization, making the actual alcohol-acid ratio much smaller than the feed ratio. Therefore, the acid value of the product will increase significantly and the chromaticity will also be poor. However, due to the presence of the reduced pressure esterification operation, this step can increase the esterification rate, and ultimately has little effect on the molecular weight and melt index of the polymer. In summary, Comparative Example 5 shows that the presence of the pressurized esterification operation is very beneficial to the acid value and chromaticity of the product.
[0076] Comparative Example 6
[0077] Compared with Example 1, the difference is that PBS is prepared by reacting SAA and BDO through four steps of reduced pressure esterification, pressurized esterification, negative pressure prepolymerization and vacuum final polymerization.
[0078] Comparative Example 6 removes the normal pressure ring-opening process in Example 1, and the other operations are consistent with Example 1, that is, it is changed to a four-step operation. After testing, the molecular weight of the obtained polymer is 213,000, the molecular weight distribution is 1.79, the acid value is 38 mol / t, the L value is about 90, and the melt index is 17g / 10min. It can be seen that the ring-opening process is reduced. Since there is no directional ring-opening product, the ring-opening and esterification are carried out simultaneously, so that the molecular weight distribution of the polymer will become wider and the acid value will increase slightly. However, due to the presence of pressurized esterification and reduced pressure esterification operations, this step can increase the esterification rate, and ultimately has little effect on the molecular weight, chromaticity and melt index of the polymer. Therefore, Comparative Example 6 shows that the normal pressure ring-opening step is beneficial.
[0079] Comparative Example 7
[0080] Compared with Example 1, Comparative Example 7 is an intermittent operation, in order to compare the quality of 5 batches of products obtained by intermittent operation and continuous operation, thereby verifying the advantages of continuous operation.
[0081] The intermittent operation is as follows: succinic anhydride and 1,4-butanediol are added to a reaction kettle at a molar ratio of succinic anhydride: alcohol = 1.00:1.01, and then the temperature is raised to 70°C. After reacting for 30 minutes at normal pressure, p-toluenesulfonic acid (0.05% of the molar amount of succinic anhydride) and the remaining 1,4-butanediol (0.34 times the molar amount of succinic anhydride) are added, the temperature is raised to 170°C, and the reaction is carried out at a pressure of 0.3 MPa for 10 minutes. 0min, then reduce the pressure to 45kPa, and raise the temperature to 190℃, react for 110min, introduce nitrogen after the reaction, add polymerization catalyst tetrabutyl titanate (0.05% of the molar amount of succinic anhydride) through the upper end of the reactor, and carry out negative pressure prepolymerization at a temperature of 200℃ and a pressure of 4kPa. After the reaction for 80min, raise the temperature to 235℃, and reduce the pressure to 50Pa, and continue the vacuum final polymerization for 120min. After the final polymerization is completed, the material in the reactor is kept warm and pressurized and discharged through the bottom valve, and then water-cooled into strips and pelletized. Collect the pellets for performance testing. Repeat 5 times. The experimental results are shown in Table 4.
[0082] Table 4 Comparison of product quality obtained by intermittent operation and continuous operation
[0083]
[0084] As can be seen from the results in Table 4, the product quality obtained by continuous operation of Example 1 is more stable (sampling evaluation 5 times), the molecular weight, molecular weight distribution, melt index, and acid value are very controllable, and the product chromaticity and performance are better. However, the product quality obtained by intermittent operation of Comparative Example 7 is unstable, and the results of 5 times fluctuate greatly, which is mainly caused by the instability of intermittent operation and thermal decomposition.
[0085] Examples 10 to 29
[0086] The preparation of polysuccinates by a five-step continuous reaction process of normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization of succinic anhydride and other diols or polyols as monomer raw materials was investigated. The alcohols selected in Examples 10 to 29 are shown in Table 5, and the preparation steps are as follows:
[0087] Succinic anhydride and alcohol are continuously conveyed to a ring-opening reactor in a molar ratio of succinic anhydride:alcohol=1.00:1.05, and a ring-opening reaction is carried out at a temperature of 80±20°C, a pressure of normal pressure and a residence time of 60±10min to obtain a normal-pressure ring-opening product; then the mixture is continuously conveyed to a pressurized esterification reactor, and the remaining polyol (the amount is 0.25 to 0.45 times the molar amount of succinic anhydride) and an esterification catalyst p-toluenesulfonic acid (the amount is 0.1% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and a pressurized esterification reaction is carried out at a temperature of 170±20°C, a pressure of 0.5±0.1MPa and a residence time of 120±30min to obtain a pressurized esterification product; then the mixture is continuously conveyed to a reduced-pressure esterification reactor In the process, the small molecules are removed under reduced pressure at a temperature of 190±10°C, a pressure of 30±10kPa and a residence time of 90±20min to further improve the esterification rate; then it is continuously fed into a prepolymerization reactor and mixed with a polymerization catalyst tetrabutyl titanate (the amount is 0.12% of the molar amount of succinic anhydride), and then a pre-polycondensation reaction is carried out at a temperature of 210±20°C, a pressure of 5±2kPa and a residence time of 90±20min to obtain a negative pressure prepolymerization product; finally, it is continuously fed into a final polycondensation reactor, and a vacuum final polymerization reaction is carried out at a temperature of 240±15°C, a pressure of 70±20Pa and a residence time of 120±30min to obtain polysuccinate, which is continuously discharged and underwater pelletized and dried to obtain a polyester pellet product. The molecular weight information and chromaticity information of the obtained product are shown in Table 5.
[0088] Table 5 Polysuccinates prepared by polymerization of succinic anhydride with diols and polyols
[0089]
[0090]
[0091] According to the experimental results in Table 5, it can be seen that the polysuccinate products obtained in Examples 10 to 29 have a relatively high molecular weight, Mw between 150,000 and 310,000, and a relatively narrow molecular weight distribution Mw / Mn between 1.4 and 2.0, and a very good color quality, L is basically above 88, and the acid value is generally low, generally below 30 mol / t. This also shows that the five-step continuous operation can obtain a polysuccinate product with a higher molecular weight and better performance.
[0092] It is particularly noteworthy that the use of trivalent and higher polyols (Examples 17-19) and rigid structural diols (Examples 20-25) significantly reduces the melt index of the product (usually <10g / 10min), and can be used as a blow molding material to make various blow molding products. Therefore, through the flexible adjustment of monomer types, polyester products with different performances, different application scenarios and different grades can be developed.
[0093] Embodiment 30
[0094] Succinic anhydride is polymerized with 1,3-propylene glycol and 1,4-butanediol to prepare polysuccinate, and the preparation steps are as follows: the raw materials are continuously transported to a ring-opening reactor in a molar ratio of succinic anhydride: alcohol = 1.00:1.15 (and the molar ratio of 1,3-propylene glycol to 1,4-butanediol is 0.3:0.7), and the ring-opening reaction is carried out at a temperature of 90° C., a pressure of normal pressure and a residence time of 45 min to obtain a normal-pressure ring-opening product; then the raw materials are continuously transported to a pressurized esterification reactor, and the remaining polyol (the amount is 0.35 times the molar amount of succinic anhydride) and an esterification catalyst trichloroacetic acid (the amount is 0.05% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and the temperature is 180° C., the pressure is 0.3 MPa and the residence time is 90 min for pressure esterification reaction to obtain an esterification product; then continuously feeding it into a reduced pressure esterification kettle, removing small molecules under reduced pressure at a temperature of 180° C., a pressure of 55 kPa and a residence time of 100 min, and further improving the esterification rate; then continuously feeding it into a prepolymerization reactor, and after being mixed with a polymerization catalyst diethylene glycol titanate (the amount used is 0.15% of the molar amount of succinic anhydride), a pre-polycondensation reaction is carried out at a temperature of 200° C., a pressure of 8 kPa and a residence time of 100 min to obtain a negative pressure prepolymerization product; finally continuously feeding it into a final polycondensation reactor, carrying out a vacuum final polymerization reaction at a temperature of 245° C., a pressure of 90 Pa and a residence time of 100 min to obtain polysuccinate, and continuously discharging and underwater pelletizing and drying to obtain a polyester pellet product.
[0095] The molecular weight M of the obtained polysuccinate (similar to modified polybutylene succinate) product is w The molecular weight distribution is 198,000, the melt index is 22g / 10min, the acid value is 24mol / t, and the elongation at break is as high as 760%, while the elongation at break of polybutylene succinate products is usually between 200 and 300%. It can be seen that adding a small amount of aliphatic diol to modify polybutylene succinate can significantly improve its tensile properties.
[0096] Embodiment 31
[0097] Succinic anhydride is polymerized with 1,4-butanediol and terephthalic acid diol to prepare polysuccinate, and the preparation steps are as follows: the raw materials are continuously transported to a ring-opening reactor in a molar ratio of succinic anhydride: alcohol = 1.00:1.10 (the molar ratio of 1,4-butanediol to terephthalic acid diol is 0.75:0.25), and the ring-opening reaction is carried out at a temperature of 120° C., a pressure of normal pressure and a residence time of 80 min to obtain a normal pressure ring-opening product; then the raw materials are continuously transported to a pressurized esterification reactor, and the remaining polyol (the amount is 0.5 times the molar amount of succinic anhydride) and the esterification catalyst p-toluenesulfonic acid (the amount is 0.15% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and the temperature is 190° C., the pressure is 0.2 MPa and the residence time is 90 m in for a pressure esterification reaction to obtain an esterification product; then continuously feeding it into a reduced pressure esterification kettle, removing small molecules under reduced pressure at a temperature of 200° C., a pressure of 25 kPa and a residence time of 120 min, and further improving the esterification rate; then continuously feeding it into a prepolymerization reactor, and mixing it with a polymerization catalyst tetraisopropyl titanate (the amount used is 0.10% of the molar amount of succinic anhydride), and performing a pre-polycondensation reaction at a temperature of 230° C., a pressure of 2 kPa and a residence time of 110 min to obtain a negative pressure prepolymerization product; finally continuously feeding it into a final polycondensation reactor, performing a vacuum final polymerization reaction at a temperature of 245° C., a pressure of 40 Pa and a residence time of 160 min to obtain polysuccinate, and continuously discharging and underwater pelletizing and drying to obtain a polyester pellet product.
[0098] The molecular weight M of the obtained polysuccinate (similar to rigid diol-modified polybutylene succinate) product is w It is 168,000, the molecular weight distribution is 1.39, the acid value is 18 mol / t, the elongation at break is as high as 560%, and the melt index can be below 10 (7.9 g / 10 min). Compared with polybutylene succinate, the elongation at break is significantly increased. In addition, its melt strength and blow molding processing ability are also significantly improved.
[0099] Embodiment 32
[0100] Succinic anhydride is polymerized with 1,4-butanediol and pentaerythritol to prepare polysuccinate, and the preparation steps are as follows: the raw materials are continuously transported to a ring-opening reactor in a molar ratio of succinic anhydride: alcohol = 1.00:1.06 (the molar ratio of 1,4-butanediol to pentaerythritol is 0.95:0.05), and the ring-opening reaction is carried out at a temperature of 90° C., a pressure of normal pressure and a residence time of 30 minutes to obtain a normal-pressure ring-opening product; then the raw materials are continuously transported to a pressurized esterification reactor, and the remaining polyol (the amount is 0.5 times the molar amount of succinic anhydride) and the esterification catalyst p-toluenesulfonic acid monohydrate (the amount is 0.08% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and the temperature is 160° C., the pressure is 0.1 MPa and the residence time is 9 0min, a pressure esterification reaction is carried out to obtain an esterification product; then it is continuously fed into a reduced pressure esterification kettle, and small molecules are removed under reduced pressure at a temperature of 180°C, a pressure of 55kPa and a residence time of 120min, so as to further improve the esterification rate; then it is continuously fed into a prepolymerization reactor, and after being mixed with a polymerization catalyst tetrabutyl titanate (the amount used is 0.08% of the molar amount of succinic anhydride), a pre-condensation reaction is carried out at a temperature of 210°C, a pressure of 9kPa and a residence time of 60min to obtain a negative pressure prepolymerization product; finally, it is continuously fed into a final polycondensation reactor, and a vacuum final polymerization reaction is carried out at a temperature of 245°C, a pressure of 100Pa and a residence time of 70min to obtain polysuccinate, and the material is continuously discharged and underwater pelletized and dried to obtain a polyester pellet product.
[0101] The molecular weight M of the obtained polysuccinate (similar to polyol-modified polybutylene succinate) product is w It is 298,000 and the molecular weight distribution is 2.29, which means that the addition of a small amount of polyol can significantly increase the molecular weight of polyester. In addition, the acid value of the product is 19 mol / t and the melt index can be below 10 (3.9 g / 10 min), which significantly improves the polymer melt strength and blow molding processing ability.
[0102] Embodiment 33
[0103] Succinic anhydride is polymerized with 1,4-butanediol and polyethylene glycol (Mn=2000g / mol) to prepare polysuccinate, and the preparation steps are as follows: the raw materials are continuously transported to a ring-opening reactor in a molar ratio of succinic anhydride: alcohol=1.00:1.10 (the molar amount of 1,4-butanediol and polyethylene glycol is 0.7:0.3), and the ring-opening reaction is carried out at a temperature of 110°C, a pressure of normal pressure and a residence time of 60min to obtain a normal pressure ring-opening product; then the raw materials are continuously transported to a pressurized esterification reactor, and the remaining polyol (the amount is 0.30 times the molar amount of succinic anhydride) and the esterification catalyst p-toluenesulfonic acid (the amount is 0.10% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and the temperature is 180°C, the pressure is 0.2MPa and the residence time is 15min. The reaction mixture was subjected to a pressure esterification reaction at a temperature of 190° C., a pressure of 40 kPa and a residence time of 120 min to obtain an esterification product; the reaction mixture was then continuously fed into a reduced pressure esterification kettle, and small molecules were removed under reduced pressure at a temperature of 190° C., a pressure of 40 kPa and a residence time of 120 min to further improve the esterification rate; the reaction mixture was then continuously fed into a prepolymerization reactor, and mixed with a polymerization catalyst tin tetrachloride (the dosage was 0.20% of the molar amount of succinic anhydride), and then subjected to a precondensation reaction at a temperature of 220° C., a pressure of 5 kPa and a residence time of 75 min to obtain a negative pressure prepolymerization product; the reaction mixture was finally continuously fed into a final polycondensation reactor, and a vacuum final polymerization reaction was carried out at a temperature of 245° C., a pressure of 70 Pa and a residence time of 180 min to obtain polysuccinate, and the product was continuously discharged and pelletized and dried underwater to obtain a polyester pellet product.
[0104] The molecular weight M of the obtained polysuccinate product w The molecular weight distribution is 1.65, the melt index is 31g / 10min, the acid value of the product is 21mol / t, the chromaticity is good, the L value is 91, the a value is 3.7, and the b value is 1.9.
[0105] Embodiment 34
[0106] Succinic anhydride is polymerized with three alcohols, ethylene glycol, 1,3-propylene glycol and 1,4-butanediol, to prepare polysuccinate, and the preparation steps are as follows: the raw materials are continuously transported to a ring-opening reactor in a molar ratio of succinic anhydride:alcohol=1.00:1.02 (the molar amounts of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol are 0.25:0.25:0.50), and the ring-opening reaction is carried out at a temperature of 70°C, a pressure of normal pressure and a residence time of 45 minutes to obtain a normal-pressure ring-opening product; then the raw materials are continuously transported to a pressurized esterification reactor, and the remaining polyol (the amount is 0.33 times the molar amount of succinic anhydride) and an esterification catalyst p-toluenesulfonic acid monohydrate (the amount is 0.10% of the molar amount of succinic anhydride) are continuously added through a raw material tank, and the temperature is 180°C and the pressure is 0.25M The product was continuously fed into a vacuum esterification kettle, and small molecules were removed under reduced pressure at a temperature of 200° C., a pressure of 70 kPa, and a residence time of 120 min, so as to further improve the esterification rate; the product was continuously fed into a prepolymerization kettle, and mixed with a polymerization catalyst diethylene glycol titanate (the dosage was 0.06% of the molar amount of succinic anhydride), and then a precondensation reaction was carried out at a temperature of 210° C., a pressure of 6 kPa, and a residence time of 60 min to obtain a negative pressure prepolymerization product; the product was continuously fed into a final polycondensation kettle, and a vacuum final polymerization reaction was carried out at a temperature of 240° C., a pressure of 110 Pa, and a residence time of 150 min to obtain polysuccinate, and the product was continuously discharged and pelletized and dried underwater to obtain a polyester pellet product.
[0107] The molecular weight M of the obtained polysuccinate product w It is 257,000, the molecular weight distribution is 1.58, the melt index is 18g / 10min, the product acid value is 27mol / t, the chromaticity is good, the L value is 89, the a value is 1.7, the b value is 3.9, and the elongation at break of the product is 640%.
[0108] It can be seen from Examples 30 to 34 that, through the flexible adjustment and application of monomer types and ratios, polyester products with different performances and grades can be developed to meet different downstream application scenarios.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A continuous synthesis method of polysuccinate, It is characterized in that The method uses succinic anhydride and polyol as monomer raw materials, and continuously synthesizes polysuccinate through five steps including normal pressure ring opening, pressurized esterification, reduced pressure esterification, negative pressure prepolymerization, and vacuum final polymerization. The specific steps include the following: (1) continuously conveying the monomer raw material succinic anhydride and part of the polyol to a ring-opening reaction device, performing a ring-opening reaction at a temperature of 60 to 120° C., normal pressure, and a residence time of 5 to 120 minutes to obtain a normal pressure ring-opening product; (2) continuously feeding the ring-opening product obtained in step (1) into a pressure esterification reaction device, and continuously adding the remaining polyol and esterification catalyst, and performing a pressure esterification reaction at a temperature of 100 to 220° C., a pressure of 0.10 to 1.0 MPa (A), and a residence time of 30 to 300 min to obtain a pressure esterification product; (3) continuously feeding the pressurized esterification product obtained in step (2) into a reduced pressure esterification reaction device, removing small molecules under reduced pressure at a temperature of 140 to 240° C., a pressure of 10 to 80 kPa (A), and a residence time of 30 to 180 min to obtain a reduced pressure esterification product; (4) continuously feeding the vacuum esterification product obtained in step (3) into a prepolymerization reaction device, mixing it with a polymerization catalyst, and then performing a prepolymerization reaction at a temperature of 180 to 240° C., a pressure of 1 to 60 kPa(A), and a residence time of 20 to 180 min to obtain a vacuum prepolymerization product; (5) The prepolymer product obtained in step (4) is continuously fed into a final polymerization reaction device, and a vacuum final polymerization reaction is carried out at a temperature of 200 to 280° C., a pressure of 5 to 200 Pa (A), and a residence time of 30 to 240 min to obtain polysuccinate.
2. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that In step (2), the pressurized esterification reaction conditions are a temperature of 150-200° C., a pressure of 0.2-0.7 MPa, and a residence time of 60-240 min; preferably, the pressurized esterification reaction conditions are a temperature of 170-190° C., a pressure of 0.3-0.5 MPa, and a residence time of 90-180 min.
3. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that In step (3), the reduced pressure esterification reaction conditions are temperature 160-210° C., pressure 20-60 kPa and residence time 60-150 min; preferably, the reduced pressure esterification reaction conditions are temperature 180-200° C., pressure 30-50 kPa and residence time 90-120 min.
4. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that In step (1), the ring-opening reaction conditions are a temperature of 70 to 100° C., a pressure of normal pressure, and a residence time of 20 to 90 min; preferably, the ring-opening reaction conditions are a temperature of 70 to 90° C., a pressure of normal pressure, and a residence time of 30 to 60 min; In step (4), the prepolymerization reaction conditions are a temperature of 190 to 230° C., a pressure of 2 to 30 kPa, and a residence time of 45 to 150 min; preferably, the prepolymerization reaction conditions are a temperature of 200 to 220° C., a pressure of 3 to 15 kPa, and a residence time of 60 to 120 min; In step (5), the vacuum final polymerization reaction conditions are temperature 210-260° C., pressure 10-150 Pa and residence time 60-210 min; preferably, the vacuum final polymerization reaction conditions are temperature 230-250° C., pressure 30-80 Pa and residence time 90-180 min.
5. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that The molar ratio of the monomer raw materials is succinic anhydride:polyol=1.00:(1.00-2.00), preferably 1.00:(1.10-1.45); wherein, in step (1), succinic anhydride:polyol=1.00:(1.00-1.10), and the remaining part of the polyol is continuously added in the pressurized esterification reaction in step (2).
6. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that The esterification catalyst is selected from one or more of methanesulfonic acid, p-toluenesulfonic acid, p-toluenesulfonic acid hydrate, trifluoromethanesulfonic acid, trifluoroacetic acid and trichloroacetic acid, and the amount of the esterification catalyst is 0.01 to 2.00% of the molar amount of succinic anhydride, preferably 0.05 to 0.20%; The polymerization catalyst is selected from one or more of titanium, tin, antimony and germanium compounds, and the amount of the polymerization catalyst is 0.01-1.00% of the molar amount of succinic anhydride, preferably 0.05-0.20%.
7. A continuous synthesis method of polysuccinate according to claim 6, It is characterized in that The polymerization catalyst is titanium dioxide, titanium silicon composite, titanium trichloride, titanium tetrachloride, tri-butoxy titanium chloride, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetraisooctyl titanate, tetrahydroxyethyl titanate, diethylene glycol titanate, tetrahydroxypropyl titanate, dipropylene glycol titanate, tetrahydroxybutyl titanate or dibutyl titanate, or tin dichloride, tin tetrachloride, stannous succinate, stannous octoate, stannous benzoate, dioctyl tin oxide, tetrabutyl tin, dibutyl tin acetate, or antimony pentoxide, antimony trioxide, antimony trichloride, antimony pentachloride, ethylene glycol antimony or butanediol antimony, or one or more of germanium dioxide, germanium tetrachloride, tetrabutoxygermanium, tetramethyl germanium or tetraethyl germanium.
8. A continuous synthesis method of polysuccinate according to claim 1, It is characterized in that The polyol is one or more of aliphatic polyols, aromatic polyols, heterocyclic polyols, polyaliphatic alcohol ether polyols, polyaromatic alcohol ether polyols, polyaromatic phenol ether polyols, polyheterocyclic alcohol ether polyols, polyfatty acid ester polyols, polyaromatic acid ester polyols and polyheterocyclic acid ester polyols; Preferably, the fatty polyols include 1,2-ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,2-propylene glycol, 1,2-butylene glycol, 2-methyl-1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, glycerol, trimethylol The aromatic polyols include one or more of phenyl glycol, terephthalic acid, o-terephthalic acid, isophthalic acid, terephthalic acid, o-terephthalic acid, isophthalic acid, o-chlorophenyl glycol, and 4,4'-dihydroxymethyl biphenyl; the heterocyclic polyols include one or more of 2,5-furan dimethanol, tetrahydro-2-methyl-2H-pyran-3,4-diol, hydroxypropyl tetrahydropyrantriol, 2,6-pyridine dimethanol, 2,3-thiophenedimethanol, 3,4-thiophene diol, and 3,4-tetrahydrothiophene diol; the poly fatty alcohol ether polyols include one or more of The alcohol includes one or more of ethylene glycol or ethylene oxide, 1,2-propylene glycol or propylene oxide, 1,4-butanediol or tetrahydrofuran, 1,2-butanediol or 1,2-butylene oxide, 2,3-butanediol or 2,3-butylene oxide, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol or cyclohexene oxide, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, glycerol or glycidol or epichlorohydrin polyether and copolymers thereof with polyols; the polyaromatic alcohol ether polyol includes terephthalyl alcohol, isophthalic alcohol, o-phthalic alcohol, styrene oxide or phenyl glycol polyether and copolymers thereof with polyols; The polyaromatic phenol ether polyol includes one or more copolymers of hydroquinone, resorcinol and / or catechol and their polyethers with polyols; the polyheterocyclic alcohol ether polyol includes one or more polyethers of 2,5-furan dimethanol, 2,6-pyridine dimethanol, 2,3-thiophenedimethanol, 3,4-thiophenediol and 3,4-tetrahydrothiophenediol and their copolymers with polyols; the polyfatty acid ester polyol includes one or more of poly C1-C10 fatty acid polyol, polyhydroxy acid ester, polyhydroxy acid ester polyol; the polyaromatic acid ester polyol includes one or more of polyphthalic acid polyol, polyphthalic acid polyol and polynaphthalic acid polyol;The polyheterocyclic acid ester polyol includes one or more of poly-2,5-furandicarboxylate polyol, poly-2,6-pyridinedicarboxylate polyol and poly-2,3-thiophenedicarboxylate polyol. ; 9. A continuous synthesis method of polysuccinate according to claim 8, It is characterized in that The fatty polyols include one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, 1,2-propylene glycol, 1,2-butylene glycol, 2-methyl-1,3-propylene glycol, 2,2-dimethyl-1,3-propylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,2,4-trimethyl-1,3-pentanediol, glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, and lactitol; the aromatic polyols include one or more of terephthalate, isophthalate, 4,4'-dihydroxymethane The heterocyclic polyol includes one or more of 2,5-furan dimethanol, 2,6-pyridine dimethanol, 2,3-thiophenedimethanol and 3,4-thiophenediol; the poly fatty alcohol ether polyol includes polyethylene glycol, poly 1,2-propylene glycol, poly 1,4-butylene glycol, poly 1,4-cyclohexanediol, poly 1,4-cyclohexanedimethanol, polyethylene glycol glycerol ether, polypropylene glycol glycidyl ether, poly 1,2-cyclohexanediol glycol ether and poly 1,4-butylene glycol pentaerythritol ether; the poly aromatic alcohol ether polyol includes poly (p-phenylene glycol), poly (m-phenylene glycol), poly (styrene oxide), poly (p-phenylene glycol). One or more of dimethylol glycol ether, polyoxystyrene glycerol ether; the polyaromatic phenol ether polyol includes one or more of polyhydroquinone glycol ether and polyhydroquinone glycidyl ether; the polyheterocyclic alcohol ether polyol includes one or more of poly-2,5-furan dimethanol, poly-2,6-pyridine dimethanol, poly-3,4-thiophene diol and poly-2,5-furan dimethanol glycol ether; the polyfatty acid ester polyol includes polyethylene oxalate glycol ester glycol, polyethylene adipate glycol ester glycol, polybutylene succinate glycol ester glycol, polyhexanediol adipate glycol, polyhexanediol sebacate glycol, polyethylene cyclohexanedicarboxylate glycol, One or more of polyglycolide diol, poly(glycolide-lactide) diol, polylactide diol, polyglycolic acid glyceride, polyhydroxybutyric acid, polycaprolactone diol, and polyhydroxycaproic acid glyceride; the polyaromatic acid ester polyol includes one or more of polyethylene terephthalate diol, polyethylene isophthalate diol, polyethylene trimesic acid triol, and polyethylene naphthalate diol; the polyheterocyclic acid ester polyol includes one or more of poly-2,5-furandicarboxylic acid-ethylene glycol ester diol, poly-2,5-furandimethylol ester diol, and poly-2,6-pyridinedicarboxylic acid ethylene glycol ester diol.
10. A polysuccinate prepared by the continuous synthesis method of polysuccinate according to any one of claims 1 to 9.
Citation Information
Patent Citations
Continuous production method of modified poly (butylene succinate)
CN113980252A
Method for synthesizing poly (1, 4-butanediol succinate) through ring-opening polymerization
CN114015026A
Preparation method of binary acid and dihydric alcohol modified poly (butylene succinate) copolyester
CN117050281A
Preparation method of poly (butylene succinate)
CN118047937A
Continuous synthesis method and production system of high-viscosity PBS / PBAT degradable polyester
CN118562114A