Novel heat-insulating and heat-preserving printing ink and preparation method thereof

CN119060581APending Publication Date: 2024-12-03夏雨
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411114194.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Patent Text Reader

Abstract

The invention discloses novel thermal insulation ink and a preparation method thereof, and relates to the technical field of ink preparation. Glass beads are pretreated through alkali, so that the surfaces of the glass beads are negatively charged, the glass beads and 1-carboxyl-1-methyl ethyoxyl ammonium chloride with positive charges are subjected to electrostatic adsorption, bacterial biofilm formation is interfered, bacterial reproduction is inhibited, and the antibacterial effect is achieved; then the glass beads are coordinated and combined with cerous nitrate to weaken the thermal expansion trend of the glass beads and indirectly improve the thermal stability of the ink; then polyphenyl-ring polyurethane is formed by polymerizing isocyanato of m-xylylene dimethyl isocyanate and hydroxyl of 1, 5-hexadiene-3, 4-diol, so that the thermal decomposition temperature of the resin is greatly increased, and the thermal stability of the ink is improved; then through an alkenyl addition reaction of double bonds and vinyl trichlorosilane, silicon-oxygen groups are carried, the thermal stability and the adhesive force of the ink are improved, meanwhile, halogen atoms are introduced, the thermal stability is enhanced, and the heat resistance of the ink is further improved. And the two components are mixed to prepare the ink to realize antibacterial, heat-resistant and high-durability effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ink preparation, in particular to a new type of heat-insulating ink and a preparation method thereof. Background Art

[0002] With the development of society and the advancement of science and technology, inks are becoming more and more important in many fields, such as medical, food packaging, electronic products, etc. These inks not only need to have good antibacterial properties to prevent the growth and spread of microorganisms, but also need to have heat resistance to adapt to high temperature environments, and also need to be durable to ensure that the ink does not fade or fall off during long-term use.

[0003] At present, antibacterial inks on the market are mainly achieved by adding antibacterial agents, heat-resistant inks are prepared by using high-temperature resistant resins and pigments, and durable inks are improved by optimizing ink formulas and production processes to improve ink weather resistance and adhesion. However, these inks often have certain limitations, such as antibacterial agents may affect other properties of inks, the cost of high-temperature resistant resins and pigments is high, it is difficult to optimize ink formulas and production processes, and the existing technology only achieves the single antibacterial, heat-resistant and durable properties of inks to a certain extent. Therefore, developing a new type of antibacterial, heat-resistant and durable ink to solve the problems of the existing technology has become a technical problem that urgently needs to be solved. Summary of the invention

[0004] The purpose of the present invention is to provide a new type of thermal insulation ink and a preparation method thereof to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a new type of thermal insulation ink, wherein the new type of thermal insulation ink is made of composite glass microspheres and modified resin.

[0006] Furthermore, the composite glass microspheres are prepared from active glass microspheres, 1-carboxyl-1-methylethoxyammonium chloride and cerium nitrate.

[0007] Furthermore, the active glass microspheres are prepared from alkali solution and glass microspheres.

[0008] Furthermore, the modified resin is prepared from m-phenylenedimethyl isocyanate, 1,5-hexadiene-3,4-diol and vinyltrichlorosilane.

[0009] Furthermore, a method for preparing a novel thermal insulation ink comprises the following preparation steps:

[0010] (1) adding 16 to 24 parts of glass microspheres to 79 to 118 parts of a 0.5 mol / L alkaline aqueous solution, stirring at 30 to 40° C. and 800 rpm for 2 to 4 hours, taking out the solid, washing it three times with 64 to 96 parts of ethanol, and drying it at 60 to 70° C. for 6 to 8 hours to obtain active glass microspheres;

[0011] (2) 6 to 10 parts of active glass microspheres, 60 to 100 parts of water, and 98 to 160 parts of ethanol were ultrasonically dispersed at 40 to 60 kHz for 10 to 20 minutes, 7 to 11 parts of 1-carboxyl-1-methylethoxyammonium chloride were added, and stirred at 600 rpm for 0.5 to 1.5 hours. The solid was taken out, washed three times with 44 to 71 parts of ethanol, and dried at 50 to 60° C. for 4 to 6 hours to obtain modified glass microspheres;

[0012] (3) adding 7 to 11 parts of modified glass microspheres to 38 to 54 parts of cerium nitrate aqueous solution, ultrasonicating at 40 to 60 kHz for 20 to 30 minutes, heating to 70 to 80° C. for reaction for 4 to 6 hours, taking out the solid, washing it three times with 30 to 46 parts of ethanol, and drying it at 50 to 60° C. for 3 to 5 hours to obtain composite glass microspheres;

[0013] (4) Under a nitrogen atmosphere, 21 to 63 parts of m-phenylenedimethyl isocyanate and 1 to 3 parts of dibutyltin disilicate are dissolved in 108 to 304 parts of tetrahydrofuran, 16 to 48 parts of 1,5-hexadiene-3,4-diol are added, the temperature is raised to 60 to 80° C., the reaction is performed for 4 to 6 hours, and the mixture is concentrated at a vacuum degree of -0.1 to -0.06 MPa for 3 to 5 hours to obtain a composite resin;

[0014] (5) 19 to 25 parts of the composite resin were dissolved in 68 to 82 parts of toluene, 21 to 27 parts of vinyl trichlorosilane were added and stirred at 1000 rpm for 1 to 2 hours, 0.3 to 0.7 parts of AIBN were added and mixed evenly, half of the mixed solution was heated to 80 to 90° C. and reacted for 1 to 2 hours, and the other half of the mixed solution was added at 25 mL / min and continued to react for 3 to 5 hours, and concentrated at a vacuum degree of -0.1 to -0.06 MPa for 3 to 5 hours to obtain a modified resin;

[0015] (6) 5 to 25 parts of composite glass microspheres, 32 to 58 parts of modified resin, 1 to 3 parts of defoaming agent, 8 to 26 parts of diluent, and 5 to 15 parts of ether ester solvent are mixed evenly to prepare a new thermal insulation ink.

[0016] Furthermore, the alkaline aqueous solution in step (1) is: sodium hydroxide aqueous solution or potassium hydroxide aqueous solution.

[0017] Furthermore, the content of cerium nitrate in the cerium nitrate aqueous solution in step (3) is 0.5-1.5 wt%.

[0018] Furthermore, the defoaming agent in step (6) is a mixture of one or more of polydimethylsiloxane, GPE type polyoxyethylene polyoxypropylene glycerol ether, and GP type glycerol polyether.

[0019] Furthermore, the diluent in step (6) is a mixture of one or more of hexahydrophthalic acid diglycidyl ester, polypropylene glycol diglycidyl ether, and 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester.

[0020] Furthermore, the ether ester solvent in step (6) is a mixture of one or more of dipropylene glycol dimethyl ether, propylene glycol methyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] The present invention pre-treats glass microbeads with alkali to increase the number of oxygen-containing groups on the surface of the glass microbeads, thereby causing the surface to carry a negative charge. The positive charge of 1-carboxyl-1-methylethoxyammonium chloride is then electrostatically adsorbed on the surface of the glass microbeads, wherein the alkyl groups can interfere with the formation of bacterial biofilms, inhibit bacterial reproduction, prevent ink deterioration, and achieve an antibacterial effect. The carboxyl groups are then coordinated with cerium nitrate to weaken the thermal expansion trend of the glass microbeads, reduce volume changes, and indirectly improve the thermal stability of the ink. Finally, the ink is mixed with a modified resin to form an ink, thereby achieving antibacterial, heat-resistant, and highly durable effects.

[0023] Among them, the modified resin is made of m-phenylenedimethyl isocyanate, 1,5-hexadiene-3,4-diol, and vinyltrichlorosilane; the isocyanate of m-phenylenedimethyl isocyanate is polymerized with the hydroxyl group of 1,5-hexadiene-3,4-diol to form a polyurethane containing multiple benzene rings, which greatly increases the thermal decomposition temperature of the resin and thereby improves the thermal stability of the ink; then, the double bonds in the polymer react with the alkenyl addition reaction of vinyltrichlorosilane to give it a siloxy group, thereby improving the thermal stability and adhesion of the ink, while at the same time introducing halogen atoms to enhance thermal stability and further improve the heat resistance of the ink. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the new thermal insulation ink prepared in the following examples are as follows:

[0026] Adhesion grade: Take the same weight of the thermal insulation ink of the embodiment and the comparative example and evenly apply it on the test piece. After curing, test it according to GB / T 9286-1998.

[0027] Heat resistance and friction grade: Take the same weight of the thermal insulation and heat preservation new ink of the embodiment and the comparative example and evenly apply it on the test piece. After curing, test it in a friction meter at 1 pound pressure, 40 reciprocating frequency, and 130 degrees heat friction 100 times, and record the friction resistance grade, which increases from 0 to 5 in order of wear resistance.

[0028] Antibacterial activity value: The same weight of the thermal insulation ink of the embodiment and the comparative example was uniformly coated on a test piece, and after curing, the antibacterial activity value of the ink against Staphylococcus aureus was detected according to Japanese Industrial Standard JIS Z2801.

[0029] Example 1

[0030] (1) adding 16 parts of glass microspheres to 79 parts of 0.5 mol / L sodium hydroxide aqueous solution, stirring at 30° C. and 800 rpm for 2 h, taking out the solid, washing it three times with 64 parts of ethanol, and drying it at 60° C. for 6 h to obtain active glass microspheres;

[0031] (2) 6 parts of active glass microspheres, 60 parts of water, and 98 parts of ethanol were ultrasonically dispersed at 40 kHz for 10 min, 7 parts of 1-carboxy-1-methylethoxyammonium chloride were added, and the mixture was stirred at 600 rpm for 0.5 h. The solid was taken out, washed three times with 44 parts of ethanol, and dried at 50° C. for 4 h to obtain modified glass microspheres;

[0032] (3) adding 7 parts of modified glass microspheres to 38 parts of 0.5 wt% cerium nitrate aqueous solution, ultrasonicating at 40 kHz for 20 min, heating to 70° C. for 4 h, taking out the solid, washing it 3 times with 30 parts of ethanol, and drying it at 50° C. for 3 h to obtain composite glass microspheres;

[0033] (4) Under nitrogen atmosphere, 21 parts of m-phenylenedimethyl isocyanate and 1 part of dibutyltin diisocyanate were dissolved in 108 parts of tetrahydrofuran, 16 parts of 1,5-hexadiene-3,4-diol were added, the temperature was raised to 60° C. for reaction for 4 h, and concentrated at a vacuum degree of -0.1 MPa for 3 h to obtain a composite resin;

[0034] (5) 19 parts of the composite resin was dissolved in 68 parts of toluene, 21 parts of vinyl trichlorosilane was added and stirred at 1000 rpm for 1 hour, 0.3 parts of AIBN was added and mixed evenly, half of the mixture was heated to 80°C for reaction for 1 hour, and the other half of the mixture was added at 25 mL / min and continued to react for 3 hours, and concentrated at a vacuum degree of -0.1 MPa for 3 hours to obtain a modified resin;

[0035] (6) 5 parts of composite glass microspheres, 32 parts of modified resin, 1 part of polydimethylsiloxane, 8 parts of diglycidyl hexahydrophthalate, and 5 parts of dipropylene glycol dimethyl ether were mixed evenly to prepare a new type of thermal insulation ink.

[0036] Example 2

[0037] (1) adding 20 parts of glass microspheres to 99 parts of 0.5 mol / L sodium hydroxide aqueous solution / potassium hydroxide aqueous solution, stirring at 35° C. and 800 rpm for 3 h, taking out the solid, washing it three times with 80 parts of ethanol, and drying it at 65° C. for 7 h to obtain active glass microspheres;

[0038] (2) 8 parts of active glass microspheres, 80 parts of water, and 129 parts of ethanol were ultrasonically dispersed at 50 kHz for 15 min, 9 parts of 1-carboxy-1-methylethoxyammonium chloride were added, and the mixture was stirred at 600 rpm for 1 h. The solid was taken out, washed 3 times with 58 parts of ethanol, and dried at 55° C. for 5 h to obtain modified glass microspheres;

[0039] (3) adding 9 parts of modified glass microspheres to 46 parts of cerium nitrate aqueous solution with a content of 1.0 wt% cerium nitrate, ultrasonicating at 50 kHz for 25 min, heating to 75° C. for reaction for 5 h, taking out the solid, washing it 3 times with 38 parts of ethanol, and drying it at 55° C. for 4 h to obtain composite glass microspheres;

[0040] (4) Under nitrogen atmosphere, 42 parts of m-phenylenedimethyl isocyanate and 2 parts of dibutyltin diosilicate were dissolved in 206 parts of tetrahydrofuran, 32 parts of 1,5-hexadiene-3,4-diol were added, the temperature was raised to 70° C. for reaction for 5 h, and concentrated at a vacuum degree of -0.08 MPa for 4 h to obtain a composite resin;

[0041] (5) 22 parts of the composite resin were dissolved in 75 parts of toluene, 24 parts of vinyl trichlorosilane were added and stirred at 1000 rpm for 1.5 hours, 0.5 parts of AIBN were added and mixed evenly, half of the mixture was heated to 85°C and reacted for 1.5 hours, and the other half of the mixture was added at 25 mL / min and continued to react for 4 hours, and concentrated at a vacuum degree of -0.08 MPa for 4 hours to obtain a modified resin;

[0042] (6) 15 parts of composite glass microspheres, 45 parts of modified resin, 2 parts of GPE type polyoxyethylene polyoxypropylene glycerol ether, 17 parts of polypropylene glycol diglycidyl ether, and 10 parts of propylene glycol methyl ether acetate were mixed evenly to prepare a new type of thermal insulation ink.

[0043] Example 3

[0044] (1) adding 24 parts of glass microspheres to 118 parts of 0.5 mol / L potassium hydroxide aqueous solution, stirring at 40° C. and 800 rpm for 4 h, taking out the solid, washing it three times with 96 parts of ethanol, and drying it at 70° C. for 8 h to obtain active glass microspheres;

[0045] (2) 10 parts of active glass microspheres, 100 parts of water, and 160 parts of ethanol were ultrasonically dispersed at 60 kHz for 20 min, 11 parts of 1-carboxy-1-methylethoxyammonium chloride were added, and the mixture was stirred at 600 rpm for 1.5 h. The solid was taken out, washed three times with 71 parts of ethanol, and dried at 60° C. for 6 h to obtain modified glass microspheres;

[0046] (3) adding 11 parts of modified glass microspheres to 54 parts of cerium nitrate aqueous solution with a content of 1.5 wt% cerium nitrate, ultrasonicating at 60 kHz for 30 min, heating to 80° C. for reaction for 6 h, taking out the solid, washing it 3 times with 46 parts of ethanol, and drying it at 60° C. for 5 h to obtain composite glass microspheres;

[0047] (4) Under nitrogen atmosphere, 63 parts of m-phenylenedimethyl isocyanate and 3 parts of dibutyltin diosilicate were dissolved in 304 parts of tetrahydrofuran, 48 parts of 1,5-hexadiene-3,4-diol were added, the temperature was raised to 80° C. for reaction for 6 h, and concentrated at a vacuum degree of -0.06 MPa for 5 h to obtain a composite resin;

[0048] (5) 25 parts of the composite resin were dissolved in 82 parts of toluene, 27 parts of vinyl trichlorosilane were added and stirred at 1000 rpm for 2 hours, 0.7 parts of AIBN were added and mixed evenly, half of the mixture was heated to 90°C and reacted for 2 hours, and the other half of the mixture was added at 25 mL / min and continued to react for 5 hours, and concentrated at a vacuum degree of -0.06 MPa for 5 hours to obtain a modified resin;

[0049] (6) 25 parts of composite glass microspheres, 58 parts of modified resin, 3 parts of GP-type glycerol polyether, 26 parts of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester, and 15 parts of diethylene glycol monobutyl ether acetate were mixed evenly to prepare a new type of thermal insulation ink.

[0050] Comparative Example 1

[0051] The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (2) is changed to: 8 parts of glass microspheres, 80 parts of water, and 129 parts of ethanol are ultrasonically dispersed at 50kHz for 15 minutes, 9 parts of 1-carboxyl-1-methylethoxyammonium chloride are added, and stirred at 600rpm for 1 hour, the solid is taken out, washed 3 times with 58 parts of ethanol, and dried at 55°C for 5 hours to obtain modified glass microspheres. The remaining steps are the same as those in Example 2.

[0052] Comparative Example 2

[0053] The difference between Comparative Example 2 and Example 2 is that there are no steps (1) and (2), and step (3) is changed to: add 9 parts of 1-carboxyl-1-methylethoxy ammonium chloride to 46 parts of cerium nitrate aqueous solution with a content of 1.0wt% of cerium nitrate, ultrasonicate at 50kHz for 25min, heat to 75℃ for reaction for 5h, and concentrate at vacuum degree -0.08MPa for 4h to obtain a modifier; step (6) is changed to: mix 15 parts of modifier, 45 parts of modified resin, 2 parts of GPE type polyoxyethylene polyoxypropylene glyceryl ether, 17 parts of polypropylene glycol diglycidyl ether, and 10 parts of propylene glycol methyl ether acetate to obtain a new thermal insulation ink. The remaining steps are the same as those in Example 2.

[0054] Comparative Example 3

[0055] The difference between Comparative Example 3 and Example 2 is that there is no step (2), and step (3) is changed to: 9 parts of active glass microspheres are added to 46 parts of cerium nitrate aqueous solution with a content of 1.0wt% cerium nitrate, ultrasonicated at 50kHz for 25min, heated to 75°C for reaction for 5h, solids are taken out, washed 3 times with 38 parts of ethanol, and dried at 55°C for 4h to obtain composite glass microspheres. The remaining steps are the same as those in Example 2.

[0056] Comparative Example 4

[0057] The difference between Comparative Example 4 and Example 2 is that there is no step (3), and step (6) is changed to: 15 parts of modified glass microspheres, 45 parts of modified resin, 2 parts of GPE type polyoxyethylene polyoxypropylene glycerol ether, 17 parts of polypropylene glycol diglycidyl ether, and 10 parts of propylene glycol methyl ether acetate are mixed evenly to prepare a new thermal insulation ink. The remaining steps are the same as in Example 2.

[0058] Comparative Example 5

[0059] The difference between Comparative Example 5 and Example 2 is that there is no step (4), and step (5) is changed to: 22 parts of 1,5-hexadiene-3,4-diol are dissolved in 75 parts of toluene, 24 parts of vinyltrichlorosilane are added and stirred at 1000 rpm for 1.5 hours, 0.5 parts of AIBN are added and mixed evenly, half of the mixed solution is heated to 85° C. and reacted for 1.5 hours, and the other half of the mixed solution is added at 25 mL / min and continued to react for 4 hours, and concentrated at a vacuum degree of -0.08 MPa for 4 hours to obtain a modified resin. The remaining steps are the same as those in Example 2.

[0060] Comparative Example 6

[0061] The difference between Comparative Example 6 and Example 2 is that there is no step (4), and step (5) is changed to: 22 parts of m-phenylenedimethyl isocyanate are dissolved in 75 parts of toluene, 24 parts of vinyltrichlorosilane are added and stirred at 1000 rpm for 1.5 hours, 0.5 parts of AIBN are added and mixed evenly, half of the mixed solution is heated to 85° C. and reacted for 1.5 hours, and the other half of the mixed solution is added at 25 mL / min and continued to react for 4 hours, and concentrated at a vacuum degree of -0.08 MPa for 4 hours to obtain a modified resin. The remaining steps are the same as those in Example 2.

[0062] Comparative Example 7

[0063] The difference between Comparative Example 7 and Example 2 is that there is no step (5), and step (6) is changed to: 15 parts of composite glass microspheres, 45 parts of composite resin, 2 parts of GPE type polyoxyethylene polyoxypropylene glycerol ether, 17 parts of polypropylene glycol diglycidyl ether, and 10 parts of propylene glycol methyl ether acetate are mixed evenly to prepare a new thermal insulation ink. The remaining steps are the same as in Example 2.

[0064] Effect example

[0065] The following table shows the performance analysis results of the new thermal insulation inks of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.

[0066] Adhesion grade Heat resistance and friction grade Antimicrobial activity value Example 1 1 5 4.7 Example 2 1 5 4.9 Example 3 1 5 4.6 Comparative Example 1 4 3 3.2 Comparative Example 2 3 0 3.6 Comparative Example 3 4 2 1.4 Comparative Example 4 3 2 2.5 Comparative Example 5 2 1 3.8 Comparative Example 6 3 1 3.5 Comparative Example 7 4 1 3.1

[0067] From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 1, it can be found that the glass microspheres treated with alkali solution can increase the number of oxygen-containing groups on their surface, and then the surface has a negative charge, which provides a basic condition for the subsequent electrostatic adsorption to increase the adhesion performance; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 2, it can be found that the unique hollow structure of the glass microspheres significantly improves the heat resistance and thermal insulation effect of the ink; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 3, it can be found that the positive charge carried by 1-carboxy-1-methylethoxyammonium chloride itself can be electrostatically adsorbed on the surface of the negatively charged glass microspheres, and the alkyl group therein can interfere with the formation of bacterial biofilms, inhibit bacterial reproduction, and achieve an antibacterial effect; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 4, it can be found that cerium nitrate is coordinated with the carboxyl group of 1-carboxy-1-methylethoxyammonium chloride to include The invention relates to a novel polyurethane foam for coating glass microspheres, which is coated on the surface of glass microspheres, thereby reducing the thermal expansion tendency of glass microspheres, reducing volume changes, and indirectly improving the thermal stability of ink; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 5, it can be found that the polyurethane containing multiple benzene rings is formed by the polymerization reaction of m-phenylenedimethyl isocyanate, which can greatly increase the thermal decomposition temperature of the resin, thereby improving the thermal stability of the ink; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 6, it can be found that 1,5-hexadiene-3,4-diol can inhibit the normal anabolism of related enzymes of bacteria and play an antibacterial effect; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 7, it can be found that vinyl trichlorosilane can react with the double bonds in the polymer to make the combination more stable, effectively improve the adhesion, and at the same time make it have siloxy groups, improve the thermal stability and adhesion of the ink, and introduce halogen atoms to enhance the thermal stability and further improve the heat resistance.

[0068] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A new type of thermal insulation ink, It is characterized in that The novel heat-insulating ink is prepared from composite glass microspheres and modified resin.

2. A new type of thermal insulation ink according to claim 1, It is characterized in that The composite glass microspheres are prepared from active glass microspheres, 1-carboxyl-1-methylethoxyammonium chloride and cerium nitrate.

3. A new type of thermal insulation ink according to claim 2, It is characterized in that The active glass microbeads are prepared from alkali solution and glass microbeads.

4. A new thermal insulation ink according to claim 1, It is characterized in that The modified resin is prepared from m-phenylenedimethyl isocyanate, 1,5-hexadiene-3,4-diol and vinyl trichlorosilane.

5. A method for preparing a new type of thermal insulation ink, It is characterized in that The method comprises the following preparation steps: (1) adding 16 to 24 parts of glass microspheres to 79 to 118 parts of a 0.5 mol / L alkaline aqueous solution, stirring at 30 to 40° C. and 800 rpm for 2 to 4 hours, taking out the solid, washing it three times with 64 to 96 parts of ethanol, and drying it at 60 to 70° C. for 6 to 8 hours to obtain active glass microspheres; (2) 6 to 10 parts of active glass microspheres, 60 to 100 parts of water, and 98 to 160 parts of ethanol were ultrasonically dispersed at 40 to 60 kHz for 10 to 20 minutes, 7 to 11 parts of 1-carboxyl-1-methylethoxyammonium chloride were added, and stirred at 600 rpm for 0.5 to 1.5 hours. The solid was taken out, washed three times with 44 to 71 parts of ethanol, and dried at 50 to 60° C. for 4 to 6 hours to obtain modified glass microspheres; (3) adding 7 to 11 parts of modified glass microspheres to 38 to 54 parts of cerium nitrate aqueous solution, ultrasonicating at 40 to 60 kHz for 20 to 30 minutes, heating to 70 to 80° C. for reaction for 4 to 6 hours, taking out the solid, washing it three times with 30 to 46 parts of ethanol, and drying it at 50 to 60° C. for 3 to 5 hours to obtain composite glass microspheres; (4) Under a nitrogen atmosphere, 21 to 63 parts of m-phenylenedimethyl isocyanate and 1 to 3 parts of dibutyltin disilicate are dissolved in 108 to 304 parts of tetrahydrofuran, 16 to 48 parts of 1,5-hexadiene-3,4-diol are added, the temperature is raised to 60 to 80° C., the reaction is performed for 4 to 6 hours, and the mixture is concentrated at a vacuum degree of -0.1 to -0.06 MPa for 3 to 5 hours to obtain a composite resin; (5) 19 to 25 parts of the composite resin were dissolved in 68 to 82 parts of toluene, 21 to 27 parts of vinyl trichlorosilane were added and stirred at 1000 rpm for 1 to 2 hours, 0.3 to 0.7 parts of AIBN were added and mixed evenly, half of the mixed solution was heated to 80 to 90° C. and reacted for 1 to 2 hours, and the other half of the mixed solution was added at 25 mL / min and continued to react for 3 to 5 hours, and concentrated at a vacuum degree of -0.1 to -0.06 MPa for 3 to 5 hours to obtain a modified resin; (6) 5 to 25 parts of composite glass microspheres, 32 to 58 parts of modified resin, 1 to 3 parts of defoaming agent, 8 to 26 parts of diluent, and 5 to 15 parts of ether ester solvent are mixed evenly to prepare a new thermal insulation ink.

6. A method for preparing a novel heat insulating ink according to claim 5, It is characterized in that The alkaline aqueous solution in step (1) is: sodium hydroxide aqueous solution or potassium hydroxide aqueous solution.

7. The method for preparing a novel heat-insulating ink according to claim 5, It is characterized in that The content of cerium nitrate in the cerium nitrate aqueous solution in step (3) is 0.5-1.5wt%.

8. The method for preparing a novel heat insulating ink according to claim 5, It is characterized in that The defoaming agent in step (6) is a mixture of one or more of polydimethylsiloxane, GPE type polyoxyethylene polyoxypropylene glycerol ether, and GP type glycerol polyether.

9. The method for preparing a novel heat insulating ink according to claim 5, It is characterized in that The diluent in step (6) is a mixture of one or more of hexahydrophthalic acid diglycidyl ester, polypropylene glycol diglycidyl ether, and 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester.

10. The method for preparing a novel heat insulating ink according to claim 5, It is characterized in that The ether ester solvent in step (6) is a mixture of one or more of dipropylene glycol dimethyl ether, propylene glycol methyl ether acetate, and diethylene glycol monobutyl ether acetate.

Citation Information

Patent Citations

  • Ultrathin high-temperature-resistant thermal-insulation paint

    CN104277653A

  • Reflective slurry, preparation method and preparation method of reflective enamel glaze

    CN108707366A

  • Light-cured polyurethane primer and preparation method thereof

    CN111675961A

  • Antistatic colorful reflective fabric reflective coating and preparation method thereof