Coating / dipping composition, preparation method thereof and copper-clad plate prepared from coating / dipping composition

A novel coating/impregnation composition with fluoropolymer and polyimide emulsion, along with surface-modified nanoparticles, addresses the poor peel strength issue in copper-clad laminates, achieving enhanced bonding and thermal stability for 5G applications.

CN119060588APending Publication Date: 2024-12-03SHANGHAI 3F NEW MATERIAL TECH CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411176258.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing copper-clad laminates using fluorine-containing resins face poor peel strength due to weak affinity between polytetrafluoroethylene resin and glass fiber cloth, and high melt viscosity leading to poor bonding during hot pressing, which is inadequate for 5G technology requirements.

Method used

A coating/impregnation composition comprising fluoropolymer emulsion, polyimide emulsion, surface-modified inorganic nanoparticles, and a photoinitiator, with specific weight ratios and surfactants, is used to enhance bonding between copper foil and substrate.

Benefits of technology

The composition achieves peel strengths greater than 3.0 N/mm, maintaining high peel strength even under thermal stress, suitable for 5G copper-clad laminate applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060588A_ABST
    Figure CN119060588A_ABST
Patent Text Reader

Abstract

The invention provides a coating / dipping composition, a preparation method thereof and a copper-clad plate prepared from the coating / dipping composition. The composition comprises a component A), a component B) and a component C), wherein the component A) comprises fluorine-containing polymer emulsion; component B): polyimide emulsion; component C): a dispersion liquid of surface-modified inorganic nanoparticles; and component D): a photoinitiator; wherein the weight ratio of the component A) to the component B) is 200: 1 to 5: 1; the ratio of the total weight of the component A) and the component B) to the weight of the component C) is 5: 1 to 1: 1. The composition disclosed by the invention is suitable for manufacturing the copper-clad plate, extremely high peel strength between a copper foil and a substrate in the copper-clad plate can be realized through a uniquely designed formula, and meanwhile, the substrate also realizes extremely excellent dielectric property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of materials, and more specifically to a coating / impregnation composition, which can be used to prepare a copper clad laminate, such as a copper clad laminate used in the 5G field, and achieve excellent peel strength in the copper clad laminate. Background Art

[0002] Copper clad laminates are usually composed of a lower substrate and an upper copper foil (copper foil). They are widely used in mobile phones, computers, vending machines, communication base stations, satellites, wearable devices, driverless cars, drones, and intelligent robots. They are one of the key basic materials in the electronic communications and information industries. For printed circuit boards in such applications, the peel strength between the copper foil and the substrate material is a key issue. In addition, with the rapid development of 5G technology, higher and higher requirements are placed on the peel strength between the copper foil and the substrate material in this field.

[0003] Fluorine-containing resins represented by polytetrafluoroethylene (PTFE) have many excellent properties that other polymer resins cannot match, such as low dielectric constant, low dielectric loss, high thermal stability and chemical stability. They are an ideal copper-clad laminate substrate material. The copper-clad laminate made by laminating fluoropolymers with copper foil has low loss characteristics and is the best choice as a millimeter-wave band printed circuit board substrate. On the one hand, due to the molecular inertness and strong non-polarity of the fluororesin itself, the affinity between polytetrafluoroethylene resin and glass fiber cloth and copper foil is weak. On the other hand, due to the high melt viscosity and poor fluidity of the fluororesin, the polytetrafluoroethylene macromolecules are not easy to penetrate into the glass fiber or combine with the metal copper foil during the hot pressing process, resulting in poor peel strength of the copper-clad laminate prepared with traditional fluororesins, which cannot meet the processing requirements of the later printed circuit boards. Therefore, improving the peel strength between the copper foil and the fluororesin substrate is the core technology for preparing 5G copper-clad laminate printed circuit boards.

[0004] In order to solve the above problems, a lot of energy and resources have been invested in research in this field, such as trying to improve the composition of fluorine-containing polymer emulsions, adding different types of modifiers and additives, and making various special designs for the process parameters of dipping, coating or heating techniques. However, these studies still cannot achieve truly satisfactory peel strength. Therefore, how to develop a simple and low-cost new technology to achieve excellent peel strength between the copper foil and the substrate of the copper clad laminate is a technical problem that needs to be urgently solved in this field. Summary of the invention

[0005] In view of the above problems, the inventors of the present application conducted in-depth research and successfully developed a novel composition formula, thereby effectively solving the long-standing problem in the prior art that needs to be solved.

[0006] The first aspect of the present application provides a coating / impregnation composition, the composition comprising:

[0007] Component A): a fluoropolymer emulsion, wherein the fluoropolymer emulsion comprises 30-60 wt % of fluoropolymer particles dispersed in water, based on the total weight of the fluoropolymer emulsion;

[0008] Component B): a polyimide emulsion, wherein the polyimide emulsion comprises 20-40 wt % of polyimide particles dispersed in water, based on the total weight of the polyimide emulsion;

[0009] Component C): a dispersion comprising 10-30 wt % of surface-modified inorganic nanoparticles dispersed in water, based on the weight of the dispersion;

[0010] Component D): photoinitiator;

[0011] Wherein, the weight ratio of component A) to component B) is 200:1 to 5:1;

[0012] The weight ratio of the total weight of component A) and component B) to component C) is 5:1 to 1:1.

[0013] According to one embodiment of the first aspect of the present application, the fluorine-containing polymer is selected from at least one of the following: polytetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), modified polytetrafluoroethylene (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), and combinations thereof.

[0014] According to another embodiment of the first aspect of the present application, the polyimide particles are prepared from the following raw materials: furfuryl alcohol, N-methylpyrrolidone, and N,N-dimethylacetamide.

[0015] According to another embodiment of the first aspect of the present application, at least one of the component A) and the component B) comprises a first anionic surfactant, a nonionic surfactant, or a combination thereof.

[0016] According to another embodiment of the first aspect of the present application, when an anionic surfactant is included, the content of the anionic surfactant is 800-2500 ppm, based on the total weight of the component A) and the component B).

[0017] According to another embodiment of the first aspect of the present application, when a nonionic surfactant is included, the content of the nonionic surfactant is 4-8 wt % based on the total weight of the component A) and the component B).

[0018] According to another embodiment of the first aspect of the present application, the surface-modified inorganic nanoparticles are prepared by treating inorganic nanoparticles with a second anionic surfactant, and the inorganic nanoparticles are selected from: Al 2 O 3 Nanoparticles, ZrO 2 Nanoparticles, SiO 2 Nanoparticles, CaCO 3 Nanoparticles, TiO 2 Nanoparticles, carbon nanoparticles, metal nanoparticles, ceramic nanoparticles, glass nanoparticles, and combinations thereof.

[0019] According to another embodiment of the first aspect of the present application, the first anionic surfactant and the second anionic surfactant are each independently selected from: partially fluorinated or perfluorinated polyether carboxylic acid anionic surfactant, partially fluorinated or perfluorinated polyether sulfonic acid anionic surfactant, partially fluorinated or perfluorinated epoxysulfonic acid anionic surfactant, partially fluorinated or perfluorinated alkane carboxylic acid anionic surfactant, partially fluorinated or perfluorinated alkane sulfonic acid anionic surfactant, partially fluorinated or perfluorinated alkane carboxylic acid-sulfonic acid anionic surfactant, or a combination thereof.

[0020] According to another embodiment of the first aspect of the present application, the nonionic surfactant is selected from: polyether nonionic surfactants, polyoxyethylene alkyl alcohol amide nonionic surfactants, polyoxyethylene alkylamine nonionic surfactants, fatty acid polyoxyethylene ester nonionic surfactants, alkylphenol polyoxyethylene ether nonionic surfactants, long-chain fatty alcohol polyoxyethylene ether nonionic surfactants, and combinations thereof.

[0021] According to another embodiment of the first aspect of the present application, the photoinitiator is selected from: dimethylbenzene photoinitiators, alkyl ketone photoinitiators, diketone photoinitiators, acetylbenzene photoinitiators, and combinations thereof. According to another embodiment of the first aspect of the present application, the photoinitiator is selected from at least one of the following: benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, diphenylacetophenone, α,α-dimethoxy-α-phenylacetophenone, α,α-diethoxyacetophenone, α-hydroxyalkylphenone, α-aminoalkylphenone, aromatic phosphine oxide, bisbenzoylphenylphosphine oxide, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-2-methyl-1-phenylacetone, 1-hydroxycyclohexylphenyl ketone, 2-methyl- 2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, methyl benzoylformate, benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, and combinations thereof.

[0022] According to another embodiment of the first aspect of the present application, based on the total weight of the coating / impregnation composition, the content of the photoinitiator is 0.3-1 wt %.

[0023] The second aspect of the present application provides a method for preparing the coating / impregnation composition of the present invention, characterized in that the method comprises:

[0024] Step 1: treating the inorganic nanoparticles with a second anionic surfactant to obtain the surface-modified inorganic nanoparticles;

[0025] Step 2: Mix the component A), component B), component C), component D), optional water and optional additives to prepare the coating / impregnation composition.

[0026] The third aspect of the present application provides a copper-clad laminate, comprising at least one copper layer and at least one substrate layer, wherein the substrate layer is prepared using the coating / impregnation composition of the present invention.

[0027] According to one embodiment of the third aspect of the present application, the substrate layer is a coating, and the coating is made from the coating / impregnation composition of the present invention.

[0028] According to one embodiment of the third aspect of the present application, the substrate layer comprises a fiber material and an impregnating material, and the impregnating material is derived from the coating / impregnating composition of the present invention.

[0029] The fourth aspect of the present application provides a method for preparing the copper clad laminate of the present invention, the method comprising coating the coating / impregnation composition of the present invention on a copper foil, and drying and curing the composition to form a copper clad laminate.

[0030] According to another embodiment of the fourth aspect of the present invention, a method for preparing the copper clad laminate of the present invention is provided, the method comprising impregnating a fabric substrate with the coating / impregnation composition of the present invention, stacking the impregnated fabric substrate on a copper foil, and performing a hot press curing operation to form a copper clad laminate. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In the following paragraphs, various embodiments of the present application are discussed in conjunction with the accompanying drawings. However, it should be noted that the embodiments shown in the accompanying drawings and described in detail below are only some preferred embodiments of the present application, and the protection scope of the present application is defined by the claims, but not limited to these preferred embodiments.

[0032] Figure 1 A cross-sectional view of a copper clad laminate prepared according to one embodiment of the present invention is shown, wherein a substrate layer is formed by a coating method;

[0033] Figure 2 A cross-sectional view of a copper clad laminate prepared according to another embodiment of the present invention is shown, in which a substrate layer is formed by an immersion method. DETAILED DESCRIPTION

[0034] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0035] In this application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations.

[0036] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.

[0037] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0038] In this application, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.

[0039] like Figure 1 and Figure 2 As shown, the copper clad laminate may include at least one layer of copper foil and at least one layer of substrate, and the composition developed in the present application may be used to form the substrate, or to form a part of the substrate. Figure 1 In one embodiment shown, a coating is applied on a copper foil by coating using the composition of the present invention, and then the coating is dried and / or cured to form a substrate layer derived from the composition. Figure 2 Another embodiment is shown, using the composition of the present invention to impregnate another substrate (such as glass fiber cloth, non-woven fabric, etc.), and then the impregnated substrate is stacked with copper foil, and a copper clad laminate can be obtained by operations such as hot pressing and sintering. Figure 2 It can be seen that the substrate layer of the copper clad laminate includes a substrate (such as glass fiber cloth, non-woven fabric, etc.) and a sintered material of the composition impregnated in the substrate, and the composition of the present invention constitutes a part of the substrate layer.

[0040] According to one embodiment of the present application, in the copper clad laminate prepared using the composition of the present invention, there is a very high peel strength between the copper foil and the substrate, for example, the peel strength can be greater than 3.0N / mm, for example ≥3.2N / mm, or ≥3.3N / mm, or ≥3.4N / mm, or ≥3.5N / mm, or ≥3.6N / mm, or ≥3.7N / mm, or ≥3.8N / mm. According to another embodiment of the present invention, the copper clad laminate of the present invention can still maintain a very high peel strength after experiencing the applied thermal stress, for example, after experiencing the thermal stress, the peel strength is still greater than 3.0N / mm, for example ≥3.1N / mm, or ≥3.2N / mm, or ≥3.3N / mm, or ≥3.4N / mm, or ≥3.5N / mm, or ≥3.6N / mm, or ≥3.7N / mm, or ≥3.8N / mm. The peel strength can be tested using techniques generally accepted in the art, for example, the national standard GB 4722-2017 method can be used for testing.

[0041] According to one embodiment of the present invention, the composition of the present invention comprises:

[0042] Component A): fluorinated polymer emulsion;

[0043] Component B): a polyimide emulsion, wherein the polyimide emulsion comprises 20-40 wt % of polyimide particles dispersed in water, based on the total weight of the polyimide emulsion;

[0044] Component C): a dispersion comprising 10-30 wt % of surface-modified inorganic nanoparticles dispersed in water, based on the weight of the dispersion;

[0045] Component D): Photoinitiator.

[0046] According to one embodiment of the present invention, based on the total weight of the fluoropolymer emulsion of component A), the fluoropolymer emulsion contains 30-60wt% of fluoropolymer particles dispersed in water, for example, the content may be 32-58wt%, or 35-55wt%, or 38-52wt%, or 40-50wt%, or 42-48wt%, or 45-45wt%, or within the range of values ​​obtained by combining any two of the above end values.

[0047] According to another embodiment of the present invention, the fluorine-containing polymer comprises a material selected from the group consisting of polytetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), modified polytetrafluoroethylene (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), and combinations thereof.

[0048] According to one embodiment of the present invention, the molecular weight of the fluorine-containing polymer is 400-80000, such as 800-50000, or 1000-20000, or 2000-15000, or 3000-1000. According to another embodiment of the present invention, the average particle size of the fluorine-containing polymer particles in the fluorine-containing polymer emulsion can be 2 nanometers to 1 micrometer, such as 5 nanometers to 500 nanometers, or 10-200 nanometers.

[0049] According to another embodiment of the present application, the fluorine-containing polymer emulsion can be an emulsion prepared by the inventor himself or a commercial product purchased commercially that meets the conditions specified in the present invention, such as FR302W (PTFE emulsion), FR305W, FR463W (FEP emulsion) produced by Shanghai Huayi Sanaifu New Materials Co., Ltd.

[0050] According to another embodiment of the present application, the weight ratio of the component A) to the component B) polyimide emulsion is 200:1 to 5:1, for example, 150:1 to 8:1, or 120:1 to 10:1, or 100:1 to 11:1, or 90:1 to 15:1, or 80:1 to 20:1, or 60:1 to 30:1, or 50:1 to 40:1, or within the numerical range obtained by combining any two of the above end values.

[0051] According to another embodiment of the present application, based on the total weight of the component B) polyimide emulsion, the polyimide emulsion contains 20-40wt% of polyimide particles dispersed in water, for example, its content can be 22-35wt%, or can be 24-30wt%, or can be 25-27wt%, or can be within the numerical range obtained by combining any two of the above end values. According to another embodiment of the present invention, the polyimide particles are made from the following raw materials: furfuryl alcohol, N-methylpyrrolidone, N,N-dimethylacetamide. According to one embodiment of the present invention, the molecular weight of the polyimide is 500-20000, for example, 1000-10000. According to another embodiment of the present invention, the average particle size of the polyimide particles in the polyimide emulsion can be 5-800 nanometers, for example, 10-500 nanometers, or 20-300 nanometers.

[0052] According to another embodiment of the present application, the polyimide emulsion may be an emulsion prepared by the inventors themselves or a commercial product purchased from commercial suppliers that meets the conditions defined in the present invention.

[0053] According to one embodiment of the present application, component A) and component B) are first mixed in the proportions described above to form a composite emulsion, and then the composite emulsion is mixed with component C) to form a slurry, and then the slurry is mixed with component D) a photoinitiator, and optional additives and optional water. The formed mixed material can be used for coating on copper foil, or for impregnating fabrics, and then laminated with copper foil.

[0054] According to one embodiment of the present application, in the operation of mixing the composite emulsion with component C), the weight ratio of the total weight of component A) and component B) to component C) is 5:1 to 1:1, for example, 4:1 to 1.5:1, or 3:1 to 2:1, or 2.8:1 to 1.2:1, or 2.5:1 to 1.5:1, or 2.2:1 to 1.8:1, or can be within the numerical range obtained by combining any two of the above end values.

[0055] According to one embodiment of the present application, in at least one of the component A) and the component B), a first anionic surfactant and / or a nonionic surfactant may be included. According to one embodiment of the present invention, when the component A) and / or the component B) contain an anionic surfactant, the content of the anionic surfactant is 800-2500ppm, for example, 900-2400ppm, or 1000-2200ppm, or 1200-2000ppm, or 1500-1800ppm, or 1600-1700ppm, based on the total weight of the component A) and the component B), or within the numerical range obtained by combining any two of the above end values. According to another embodiment of the present invention, when component A) and / or component B) contains a nonionic surfactant, the content of the nonionic surfactant is 4-8% by weight, for example 4.3-7.7% by weight, 4.5-7.5% by weight, or 4.8-7.2% by weight, or 5-7% by weight, or 5.5-6.5% by weight, or 5.8-6% by weight, based on the total weight of the component A) and the component B). Or within the numerical range obtained by combining any two of the above end values.

[0056] According to one embodiment of the present application, the component C) is a dispersion, and the dispersion contains 10-30% by weight of surface-modified inorganic nanoparticles dispersed in water, based on the weight of the dispersion. For example, the content of surface-modified inorganic nanoparticles in the dispersion can be 12-28% by weight, or 16-28% by weight, or 15-25% by weight, or 18-22% by weight, or 20-21% by weight, or can be within the numerical range obtained by combining any two of the above end values. The surface-modified inorganic nanoparticles are prepared by treating inorganic nanoparticles with a second anionic surfactant. According to one embodiment of the present application, a certain amount of a second anionic surfactant is added to a dispersion (e.g., a suspension) containing inorganic nanoparticles, and the above treatment is completed by mixing and stirring to obtain surface-modified inorganic nanoparticles. According to one embodiment of the present application, during the surface modification process, the second anionic surfactant is mixed with the inorganic nanoparticles in a ratio of 1:400-600, stirred at a temperature of 2-6°C in an aqueous solution for 20-40 hours, and then washed and dried. Component C) is thus obtained.

[0057] According to one embodiment of the present application, the particle size D90 of the inorganic nanoparticles is less than 100 nanometers, for example, less than 95 nanometers, or less than 90 nanometers, or 10-80 nanometers, or 20-70 nanometers, or 30-60 nanometers, or 40-50 nanometers, or can be within the numerical range obtained by combining any two of the above end values.

[0058] According to one embodiment of the present application, the inorganic nanoparticles are selected from: Al 2 O 3 Nanoparticles, ZrO 2 Nanoparticles, SiO 2 Nanoparticles, CaCO 3 Nanoparticles, TiO 2 Nanoparticles, carbon nanoparticles, metal nanoparticles, ceramic nanoparticles, glass nanoparticles, and combinations thereof.

[0059] According to one embodiment of the present application, the first anionic surfactant and the second anionic surfactant are each independently selected from: partially fluorinated or perfluorinated polyether carboxylic acid anionic surfactants, partially fluorinated or perfluorinated polyether sulfonic acid anionic surfactants, partially fluorinated or perfluorinated epoxysulfonic acid anionic surfactants, partially fluorinated or perfluorinated alkane carboxylic acid anionic surfactants, partially fluorinated or perfluorinated alkane sulfonic acid anionic surfactants, partially fluorinated or perfluorinated alkane carboxylic acid-sulfonic acid anionic surfactants, or a combination thereof.

[0060] In one embodiment of the present invention, the anionic surfactant is a fluorinated surfactant, for example, it can be selected from:

[0061] In one example of the present invention, the anionic surfactant is a fluorinated surfactant, for example, it can be selected from the following anionic surfactants:

[0062] (a)CF 3 -(OCF) m O-CF 2 -X(I)

[0063] wherein m is an integer from 1 to 6; X represents a carboxylic acid group or a salt thereof;

[0064] (b)CF 3 -O-(CF 2 ) 3 -(OCF(CF 3 )-CF 2 ) z OLY(II)

[0065] Wherein z is an integer from 0 to 3; L represents a compound selected from -CF(CF 3 )-,-CF 2 -and-CF 2 CF 2 - a divalent linking group; Y represents a carboxylic acid group or a salt thereof;

[0066] (c)

[0067]

[0068] Among them, X' 1 and X' 2 Each is the same or different from each other and is independently selected from H, F and C 1-6 (Per)fluoroalkyl, optionally containing one or more catenary or non-catenary oxygen atoms; R F It is fluorinated C 1-3 The divalency of the bridging group;

[0069] (d) anionic surfactants selected from the group consisting of:

[0070] A 2 O 2 SOCF 2 (CF 2 OCF(CF 3 )) n-1 COOA, CF 3 CF 2 (CF 2 OCF(CF 3 )) n-1 COOA, H 3 COOCF 2 (CF 2 OCF(CF 3 )) n-1 COOA, or a mixture of two or more thereof;

[0071] Where: n = 1 to 4, A is a hydrogen atom, an alkali metal or NH 4 + ;

[0072] (e) an anionic surfactant represented by the following formula:

[0073] XC 2 CF 2 (O) a CF 2 CF 2 OCF 2 COOA

[0074] Where X is a hydrogen atom or a fluorine atom, and A is a hydrogen atom, an alkali metal or NH 4+ , a is an integer from 0 to 1, and combinations thereof.

[0075] According to one embodiment of the present application, the nonionic surfactant is selected from: polyether nonionic surfactants, polyoxyethylene alkyl alcohol amide nonionic surfactants, polyoxyethylene alkylamine nonionic surfactants, fatty acid polyoxyethylene ester nonionic surfactants, alkylphenol polyoxyethylene ether nonionic surfactants, long-chain fatty alcohol polyoxyethylene ether nonionic surfactants, and combinations thereof.

[0076] According to one embodiment of the present application, the photoinitiator is selected from: dimethylbenzene photoinitiators, alkyl ketone photoinitiators, diketone photoinitiators, acetylbenzene photoinitiators, and combinations thereof; or the photoinitiator is selected from at least one of the following: benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, diphenylacetophenone, α,α-dimethoxy-α-phenylacetophenone, α,α-diethoxyacetophenone, α-hydroxyalkylphenone, α-aminoalkylphenone, aromatic phosphine oxide, bisbenzoylphenylphosphine oxide, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-2-methyl-1 -phenylacetone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, methyl benzoylformate, benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, and combinations thereof. According to another embodiment of the present application, based on the total weight of the coating / impregnation composition, the content of the photoinitiator is 0.3-1% by weight, for example, 0.5-0.8% by weight, or 0.6-0.7% by weight.

[0077] When the above components A), B), C) and D) are mixed, other components may be optionally added as needed. Examples of the other components include: adhesives, dispersants, gelling agents, plasticizers, anti-aging agents, crosslinking agents, thickeners or mixtures thereof.

[0078] According to one embodiment of the present invention, the composition of the present invention further contains 1-6%, preferably 3.5-5.5%, and more preferably 4-5% of an adhesive, based on the total weight of the composition of the present invention. The applicable adhesive is not particularly limited and can be a conventional adhesive known in the art. According to one embodiment of the present invention, the adhesive comprises a polyacrylate water-based adhesive.

[0079] According to one embodiment of the present invention, the composition of the present invention further contains 0.2-0.5%, preferably 0.25-0.45%, and more preferably 0.3-0.4% of a dispersant, based on the total weight of the composition of the present invention. The applicable dispersant is not particularly limited and can be a conventional dispersant known in the art. According to one embodiment of the present invention, the dispersant includes ammonium polyacrylate.

[0080] According to one embodiment of the present invention, based on the total weight of the composition of the present invention, it further contains 0.2-0.5%, preferably 0.25-0.45%, and more preferably 0.3-0.4% of a gelling agent. The applicable gelling agent is not particularly limited and can be a conventional gelling agent known in the art. According to one embodiment of the present invention, the gelling agent includes agarin.

[0081] According to one embodiment of the present invention, based on the total weight of the composition of the present invention, it further contains 0.05-0.2%, preferably 0.08-0.18%, and more preferably 0.1-0.15% of a plasticizer. The applicable plasticizer is not particularly limited and can be a conventional plasticizer known in the art. According to one embodiment of the present invention, the plasticizer includes di(2-ethylhexyl)phthalate.

[0082] According to one embodiment of the present invention, based on the total weight of the composition of the present invention, it further contains 0.05-0.2%, preferably 0.08-0.18%, and more preferably 0.10-0.15% of an anti-aging agent. The applicable anti-aging agent is not particularly limited and can be a conventional anti-aging agent known in the art. According to one embodiment of the present invention, the anti-aging agent includes 2-hydroxy-4-n-octyloxybenzophenone.

[0083] According to one embodiment of the present invention, based on the total weight of the composition of the present invention, 0.05-0.2%, preferably 0.08-0.18%, and more preferably 0.10-0.15% of a crosslinking agent is additionally contained. There is no particular limitation on the applicable crosslinking agent, and it can be a conventional crosslinking agent known in the art. According to one embodiment of the present invention, the crosslinking agent includes trimethylolpropane tripropionate.

[0084] According to one embodiment of the present invention, based on the total weight of the composition of the present invention, 0.1-0.5%, preferably 0.15-0.45%, and more preferably 0.2-0.4% of a thickener is contained. There is no particular limitation on the applicable thickener, and it can be a conventional thickener known in the art. According to one embodiment of the present invention, the thickener includes sodium carboxymethyl cellulose.

[0085] According to one embodiment of the present application, the mixed raw material prepared above is evenly coated on the surface of the copper plate, and the coating film and the copper plate are compacted by a pressing device to obtain a wet composite film, which is then dried and irradiated with ultraviolet light for 3-5 minutes to obtain a copper clad laminate.

[0086] The method for coating the mixed raw material on the surface of the copper plate to obtain the composite film is not particularly limited, and can be a conventional method known in the art, for example, the raw material can be brushed on the copper foil, dried at 50-70°C and pressed, and the above operation is repeated until a fluoropolymer layer of a desired thickness is obtained. Then, the obtained composite film is dried at 50-70°C for 10-60 minutes.

[0087] The method of the present invention comprises the step of photocuring the obtained composite film, for example, irradiating the composite film with ultraviolet light for 3-5 minutes, preferably 3.5-4.5 minutes, more preferably 3.8-4.2 minutes, to obtain the final copper clad laminate.

[0088] There is no particular limitation on the suitable ultraviolet light source for irradiation, and it can be any ultraviolet light source for photocuring known in the art.

[0089] The present invention specially designs the composition formula and finds that the composition containing the above components A) to D) can increase the bonding force between the fluoropolymer and the copper foil, the bonding force between the fluoropolymer and the glass fiber cloth, and the bonding force between the copper foil and the glass fiber cloth-PTFE film, thereby improving the peel strength performance between the copper foil and the substrate layer in copper clad laminates of various structures.

[0090] The present application is described below in the form of specific examples, and its purpose is to better understand the content of the present application. It should be understood that these examples are merely illustrative and non-restrictive. The reagents used in the examples are conventionally purchased from the market unless otherwise specified. The methods and conditions used in the examples are conventional methods and conditions unless otherwise specified.

[0091] Example

[0092] Preparation of test specimens

[0093] The fluorine-containing polymer mixed raw material prepared in each example or comparative example is coated on a release liner, dried, compacted, and then heat-cured. The release liner is carefully removed to obtain a fluorine-containing polymer sheet for testing.

[0094] Test dielectric constant

[0095] The dielectric properties (dielectric constant / dielectric loss) of the cured fluoropolymer sheet were tested at 10 GHz using a split cylindrical resonance (SPDR) method.

[0096] Test peel strength

[0097] Using various embodiments and comparative examples, copper clad laminates were prepared according to GB 4722-2017 Test Method for Rigid Copper Clad Laminates for Printed Circuits and the peel strength between the copper foil layer and the substrate layer of the copper clad laminate was measured.

[0098] Example 1

[0099] (1) Fluorinated surfactant CF 3 -OCF 2 O-CF 2 -COONa and Al 2 O 3 The nanomaterials were mixed in a mass ratio of 1:500 and added to deionized water to form a dispersion, which was stirred at 4°C for 24 hours, then washed with deionized water and dried at 80°C for 3 hours to obtain surface-modified nanoparticles. The surface-modified nanoparticles were dispersed in deionized water to form a dispersion with a solid concentration of 20% by weight for later use.

[0100] (2) A PTFE emulsion (FR302W, purchased from Shanghai Huayi San Ai Fu New Materials Co., Ltd., 60 wt %) containing a non-ionic surfactant TMN content of 4% was mixed with a polyimide aqueous emulsion at a weight ratio of 90:10, and the two were stirred to mix evenly. The obtained composite emulsion was mixed with the surface-modified Al prepared in step (1) above. 2 O 3 The dispersions of the nanoparticles were mixed at a weight ratio of 3:1 and stirred sufficiently to obtain a mixed slurry.

[0101] (3) Weigh the raw materials according to the following weight ratio: 20% of mixed slurry, 3% of polyacrylate water-based adhesive, 0.2% of ammonium polyacrylate, 0.2% of agarin, 0.05% of di(2-ethylhexyl) phthalate, 0.05% of 2-hydroxy-4-n-octyloxybenzophenone, 0.05% of trimethylolpropane tripropionate, 0.1% of sodium carboxymethyl cellulose, 0.3% of xylene ketone, and the balance is deionized water. All the raw materials are fully mixed to prepare a raw material mixture for use.

[0102] (4) The raw material mixture is evenly coated on the surface of the copper foil with a brush, and the coating film and the copper foil are compacted by a pressing device to form a composite film. The composite film is dried at 50° C. for 30 minutes, and the composite film after drying is irradiated with an ultraviolet light reactor for 3 minutes to obtain a copper clad laminate, which is recorded as the copper clad laminate of Example 1.

[0103] The samples were tested as described above, and their peel strength, dielectric constant, and dielectric loss were determined. The results are shown in Table 1.

[0104] Example 2

[0105] (1) Fluorinated surfactant CF 3 -OCF 2 O-CF 2 -COONa and Al 2 O 3 The nanomaterials were mixed in a mass ratio of 1:500 and added to deionized water to form a dispersion, which was stirred at 4°C for 24 hours, then washed with deionized water and dried at 80°C for 3 hours to obtain surface-modified nanoparticles. The surface-modified nanoparticles were dispersed in deionized water to form a dispersion with a solid concentration of 20% by weight for later use.

[0106] (2) A PTFE emulsion (FR302W, purchased from Shanghai Huayi San Ai Fu New Materials Co., Ltd., 60 wt % concentration) containing a non-ionic surfactant TMN content of 4% was mixed with a polyimide aqueous emulsion at a weight ratio of 95:5, and the two were stirred to mix evenly. The obtained composite emulsion was mixed with the surface-modified Al prepared in step (1) above. 2 O 3 The dispersions of the nanoparticles were mixed at a weight ratio of 3:1 and stirred sufficiently to obtain a mixed slurry.

[0107] (3) Weigh the raw materials according to the following weight ratio: 20% of mixed slurry, 3% of polyacrylate water-based adhesive, 0.2% of ammonium polyacrylate, 0.2% of agarin, 0.05% of di(2-ethylhexyl) phthalate, 0.05% of 2-hydroxy-4-n-octyloxybenzophenone, 0.05% of trimethylolpropane tripropionate, 0.1% of sodium carboxymethyl cellulose, 0.3% of xylene ketone, and the balance is deionized water. All the raw materials are fully mixed to prepare a raw material mixture for use.

[0108] (4) The raw material mixture is evenly coated on the surface of the copper foil with a brush, and the coating film and the copper foil are compacted by a pressing device to form a composite film. The composite film is dried at 50° C. for 30 minutes, and the dried composite film is irradiated with an ultraviolet light reactor for 3 minutes to obtain a copper clad laminate, which is recorded as the copper clad laminate of Example 2.

[0109] The samples were tested as described above, and their peel strength, dielectric constant, and dielectric loss were determined. The results are shown in Table 1.

[0110] Example 3

[0111] (1) Fluorinated surfactant CF 3 -OCF 2 O-CF 2 -COONa and SiO 2The nanomaterials were mixed in a mass ratio of 1:500 and added to deionized water to form a dispersion. The dispersion was stirred at 4°C for 24 hours, washed with deionized water, and dried at 80°C for 3 hours to obtain surface-modified nanoparticles. The surface-modified nanoparticles were dispersed in deionized water to form a dispersion with a solid concentration of 18% by weight for later use.

[0112] (2) Using fluorinated anionic surfactant (CF 3 -(OCF) 2 O-CF 2 PFA emulsion (model FR305, concentration 50%, purchased from Shanghai Huayi San Ai Fu New Materials Co., Ltd.) with a content of 800 ppm of -COONa was added to the surface-modified SiO 2 The dispersions of the nanoparticles were mixed at a weight ratio of 1:1 and stirred sufficiently to obtain a mixed slurry.

[0113] (3) Weigh the raw materials according to the following weight ratio: 30% of mixed slurry, 4% of polyacrylate water-based adhesive, 0.3% of ammonium polyacrylate, 0.4% of agarin, 0.1% of di(2-ethylhexyl) phthalate, 0.1% of trimethylolpropane tripropionate, 0.3% of sodium carboxymethyl cellulose, 1% of acetylbenzene, and the balance is deionized water. All the raw materials are fully mixed to prepare a raw material mixture for use.

[0114] (4) The raw material mixture is evenly coated on the surface of the copper foil with a brush, and the coating film and the copper foil are compacted by a pressing device to form a composite film. The composite film is heated at 370° C. for 6 hours to obtain a copper clad laminate, which is recorded as the copper clad laminate of Example 3.

[0115] The samples were tested as described above, and their peel strength, dielectric constant, and dielectric loss were determined. The results are shown in Table 1.

[0116] Comparative Example 1

[0117] In this comparative example 1, the steps of example 1 were repeated, except that no polyimide aqueous emulsion was added.

[0118] The samples were tested as described above, and their peel strength, dielectric constant, and dielectric loss were determined. The results are shown in Table 1.

[0119] Comparative Example 2

[0120] The steps of Example 1 were repeated, except that 0.05% of the photoinitiator 2-hydroxy-4-n-octyloxybenzophenone was not added, and the raw material mixture prepared in Comparative Example 2 was evenly coated on the surface of the copper foil, and the coating film and the copper foil were compacted by a compacting device to form a composite film. The composite film was then dried at 370° C. for 6 hours.

[0121] The samples were tested as described above, and their peel strength, dielectric constant, and dielectric loss were determined. The results are shown in Table 1.

[0122] Table 1

[0123]

[0124] It can be seen from the above test results that the example samples of the present invention achieve a significant improvement in the peel strength of each layer in the improved copper clad laminate, so that the obtained product can be advantageously used in, for example, high-frequency fields.

Claims

1. A coating / impregnation composition comprising: Component A): a fluoropolymer emulsion, wherein the fluoropolymer emulsion comprises 30-60 wt % of fluoropolymer particles dispersed in water, based on the total weight of the fluoropolymer emulsion; Component B): a polyimide emulsion, wherein the polyimide emulsion comprises 20-40 wt % of polyimide particles dispersed in water, based on the total weight of the polyimide emulsion; Component C): a dispersion comprising 10-30 wt % of surface-modified inorganic nanoparticles dispersed in water, based on the weight of the dispersion; Component D): photoinitiator; in, The weight ratio of component A) to component B) is 200:1 to 5:1; The weight ratio of the total weight of component A) and component B) to component C) is 5:1 to 1:

1.

2. The coating / impregnation composition according to claim 1, characterized in that The fluorine-containing polymer is at least one selected from the group consisting of polytetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), modified polytetrafluoroethylene (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), and combinations thereof.

3. The coating / impregnation composition according to claim 1, characterized in that The polyimide particles are prepared from the following raw materials: furfuryl alcohol, N-methylpyrrolidone and N,N-dimethylacetamide.

4. The coating / impregnation composition according to claim 1, characterized in that At least one of component A) and component B) comprises a first anionic surfactant, a nonionic surfactant, or a combination thereof; When an anionic surfactant is included, the content of the anionic surfactant is 800-2500 ppm based on the total weight of the component A) and the component B); When a nonionic surfactant is included, the content of the nonionic surfactant is 4-8 wt % based on the total weight of the component A) and the component B).

5. The coating / impregnation composition according to claim 1, characterized in that The surface-modified inorganic nanoparticles are prepared by treating inorganic nanoparticles with a second anionic surfactant, and the inorganic nanoparticles are selected from: Al2O3 nanoparticles, ZrO2 nanoparticles, SiO2 nanoparticles, CaCO3 nanoparticles, TiO2 nanoparticles, carbon nanoparticles, metal nanoparticles, ceramic nanoparticles, glass nanoparticles, and combinations thereof.

6. The coating / impregnation composition according to claim 4 or 5, characterized in that The first anionic surfactant and the second anionic surfactant are each independently selected from: partially fluorinated or perfluorinated polyether carboxylic acid anionic surfactants, partially fluorinated or perfluorinated polyether sulfonic acid anionic surfactants, partially fluorinated or perfluorinated epoxysulfonic acid anionic surfactants, partially fluorinated or perfluorinated alkane carboxylic acid anionic surfactants, partially fluorinated or perfluorinated alkane sulfonic acid anionic surfactants, partially fluorinated or perfluorinated alkane carboxylic acid-sulfonic acid anionic surfactants, or combinations thereof; The nonionic surfactant is selected from: polyether nonionic surfactants, polyoxyethylene alkyl alcohol amide nonionic surfactants, polyoxyethylene alkylamine nonionic surfactants, fatty acid polyoxyethylene ester nonionic surfactants, alkylphenol polyoxyethylene ether nonionic surfactants, long-chain fatty alcohol polyoxyethylene ether nonionic surfactants, and combinations thereof.

7. The coating / impregnation composition according to claim 1, characterized in that The photoinitiator is selected from: xylene ketone photoinitiator, alkyl ketone photoinitiator, diketone photoinitiator, acetylbenzene photoinitiator, and combinations thereof; or the photoinitiator is selected from at least one of the following: benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, diphenylacetophenone, α,α-dimethoxy-α-phenylacetophenone, α,α-diethoxyacetophenone, α-hydroxyalkylphenone, α-aminoalkylphenone, aromatic phosphine oxide, bisbenzoylphenylphosphine oxide, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-2-methyl-1-phenylacetone, 1-Hydroxycyclohexylphenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, methyl benzoylformate, benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, and combinations thereof; The content of the photoinitiator is 0.3-1 wt % based on the total weight of the coating / impregnation composition.

8. A method for preparing a coating / impregnation composition according to claims 1 to 7, characterized in that The method comprises: Step 1: treating the inorganic nanoparticles with a second anionic surfactant to obtain the surface-modified inorganic nanoparticles; Step 2: Mix the component A), component B), component C), component D), optional water and optional additives to prepare the coating / impregnation composition.

9. A copper-clad laminate comprising at least one copper foil and at least one substrate layer, wherein the substrate layer is prepared using the coating / impregnation composition according to any one of claims 1 to 7.

10. The method for preparing the copper clad laminate according to claim 9, characterized in that: The method comprises coating the coating / impregnation composition according to any one of claims 1 to 7 on a copper foil, and drying and curing the composition; or The method comprises impregnating a fabric substrate with the coating / impregnation composition according to any one of claims 1 to 7, laminating the impregnated fabric substrate on a copper foil, and performing a heat-press curing operation.

Citation Information

Patent Citations

  • Fluorine material flexible copper-clad plate with low water absorption rate and preparation method thereof

    CN113619224A

  • Adhesive composition, cured product, adhesive sheet, copper foil with resin, copper-clad laminate, and printed wiring board

    CN114621723A

  • Fluorine-containing polymer emulsion copper-clad plate and preparation method thereof

    CN114644846A