Waterproof sealing butyl rubber adhesive tape and preparation method thereof

By introducing modified brominated butyl rubber and flame-retardant butyl rubber layers into the butyl rubber adhesive tape, their flammability problems are solved, and waterproof, sealing and flame-retardant effects are achieved, which improves safety and application range.

CN119060645AInactive Publication Date: 2024-12-03JIANGSU XINYI CONSTRUCTION ENGINEERING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410996077.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Butyl rubber adhesive tape is flammable, has a fast combustion speed, and has a large amount of heat and smoke release, which endangers the safety of life and property, limiting its application.

Method used

Using a combination of a modified brominated butyl rubber layer and a flame retardant butyl rubber layer, the treatment of stearamide propyldimethyl tertiary amine, benzyl chloride, sodium montmorillonium, brominated butyl rubber, and The reaction of diethylphosphorus thioyl chloride, methyl parabenzoate, and chitosan quaternary ammonium salts forms an antibacterial, waterproof and flame-retardant adhesive tape.

Benefits of technology

The adhesive tape is waterproof, sealed and flame retardant, which enhances antibacterial and airtightness, and reduces combustion risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a waterproof sealing butyl rubber adhesive tape and a preparation method thereof, and relates to the technical field of adhesive tapes. The waterproof sealing butyl rubber adhesive tape prepared by the invention comprises a modified brominated butyl rubber layer and a flame-retardant butyl rubber layer, according to the modified brominated butyl rubber layer, stearamide propyl dimethyl tertiary amine and benzyl chloride are quaternized to generate an antibacterial monomer, the antibacterial property is improved, the modified brominated butyl rubber layer is subjected to ion exchange with Na-montmorillonite, the compatibility of montmorillonite and the antibacterial monomer is improved, the modified brominated butyl rubber layer is subjected to melt blending with rubber, long-chain-containing modified montmorillonite forms uniform nano dispersion in a rubber matrix, and a blocking layer is formed; the permeability is reduced, and the waterproof air tightness of the adhesive tape is enhanced; the flame-retardant butyl rubber layer is a flame-retardant substance which is formed by reacting diethyl thiophosphoryl chloride with methyl p-hydroxybenzoate and integrates aromatic hydrocarbon, phosphorus and sulfur elements, so that the flame retardance of the adhesive tape is improved, the flame-retardant butyl rubber layer is electrostatically combined with chitosan quaternary ammonium salt to form an ion complex, and the flame-retardant butyl rubber layer can be heated to form a carbon layer to block heat and oxygen and enhance the flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive tapes, in particular to a waterproof sealing butyl rubber adhesive tape and a preparation method thereof. Background Art

[0002] Butyl rubber adhesive tape is an environmentally friendly sealing adhesive material made from a mixture of butyl rubber and polyisobutylene, produced according to a special production formula and a special process flow. It has excellent sealing, adhesion and chemical resistance and is widely used in construction, automobiles, processing equipment and other fields.

[0003] However, butyl rubber adhesive tape is a flammable material with a fast burning speed, large heat and smoke release, and will produce molten droplets, which seriously endangers human life and property safety and greatly limits the application of butyl tape. Therefore, it is particularly important to prepare a flame-retardant, waterproof and sealing butyl rubber adhesive tape. Summary of the invention

[0004] The object of the present invention is to provide a waterproof sealing butyl rubber adhesive tape and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a waterproof sealing butyl rubber adhesive tape, wherein the waterproof sealing butyl rubber adhesive tape comprises a modified brominated butyl rubber layer and a flame retardant butyl rubber layer.

[0006] Furthermore, the modified brominated butyl rubber layer is prepared from stearamidopropyl dimethyl tertiary amine, benzyl chloride, sodium montmorillonite and brominated butyl rubber.

[0007] Furthermore, the flame retardant butyl rubber layer is made of diethyl thiophosphoryl chloride, methyl p-hydroxybenzoate and chitosan quaternary ammonium salt.

[0008] Furthermore, a method for preparing a waterproof sealing butyl rubber adhesive tape comprises the following preparation steps: (1) Stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol were mixed in a mass ratio of 5-5.3:2:7, heated to 50-80°C, stirred at 80-120 rpm for 4 h, and reduced pressure to 0.05-0.1 MPa for filtration to obtain an antibacterial monomer; sodium montmorillonite and deionized water were mixed in a mass ratio of 1:15-20, stirred at room temperature and 700-800 rpm for 8-9 h, and the mixture was allowed to stand for 15 h to allow large impurities and large particles of clay that are difficult to mix to precipitate, and the upper clay suspension was taken, heated to 60°C, and stirred at 700 rpm for 1 h. Add 1-2 times the mass of the suspension antibacterial monomer, react for 2-3 hours, let stand for 12 hours, centrifuge at 5000 rpm for 10-20 minutes, take out the solid, wash with deionized water for 3-4 times, heat to 90°C and dry for 24-30 hours to obtain organic modified clay; heat the brominated butyl rubber to 80°C and plasticize for 1 minute, add zinc oxide, stearic acid, organic modified clay, dibenzothiazole disulfide accelerator, zinc diethyl dithiocarbamate accelerator and sulfur, mix evenly for 10 minutes to obtain a rubber mix, put the rubber mix into a mold for vulcanization to obtain modified brominated butyl rubber; (2) Diethyl thiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate are mixed uniformly in a mass ratio of 1:1:2~3, heated to 95~100℃, stirred at 90~150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80℃ to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90℃ and dried for 3h to obtain a flame retardant; chitosan quaternary ammonium salt and hydrolyzed flame retardant are mixed in a mass ratio of 10:1~1.5, heated to 50℃ for reaction for 3h, centrifuged three times for 10min, removed the solid, frozen to -10℃ and dried for 15h to obtain a flame retardant; the flame retardant and butyl rubber are heated to 80℃ in a mass ratio of 17:5, mixed for 15~20min, heated to 150~160℃, vulcanized for 30~40min, and pressed into sheets to obtain flame retardant butyl rubber; (3) Cut the flame retardant butyl rubber and modified brominated butyl rubber into 18 mm × 30 m, with flame retardant butyl rubber and modified brominated butyl rubber from top to bottom, put them into the glue box of the coating machine and coat them with glue, let them stand for 24 hours, and isolate the two end disks with release paper to obtain a waterproof sealing butyl rubber adhesive tape.

[0009] Furthermore, the specific conditions for rubber vulcanization in the above step (1) are: heating temperature of 150-170° C., and vulcanization time of 20-30 min.

[0010] Furthermore, in the above step (1): by weight, 100 parts of plasticized brominated butyl rubber, 2-5 parts of zinc oxide, 1-3 parts of stearic acid, 2-4 parts of organic modified clay, 1-3 parts of dibenzothiazole disulfide accelerator, 1-3 parts of zinc diethyl dithiocarbamate accelerator, and 1-3 parts of sulfur.

[0011] Furthermore, the preparation method of the hydrolyzed flame retardant in the above step (2) is as follows: the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 1-2:0.5:1, the temperature is raised to 70°C, and the mixture is stirred at 50-60 rpm for 1.5 h. The mixture is heated to 60°C and evaporated to constant weight, deionized water of 3-4 times the mass of the flame retardant is added, the pH is adjusted to 1-2 with 1 mol / L hydrochloric acid, the mixture is stirred at 30-50 rpm for 12 h, the solid is taken out by centrifugation for 10 min, and then the solid is washed with deionized water, ethanol and methanol for 3 times respectively, and the solid is dried at 65°C.

[0012] Furthermore, in the above step (2), the chitosan quaternary ammonium salt is hydroxypropyltrimethylammonium chloride chitosan.

[0013] Furthermore, the glue in the above step (3) is polyurethane glue, and the total amount used is 125g / m 2 .

[0014] Furthermore, the specific conditions of the coating machine treatment in the above step (3) are: the heating temperature of the glue box is 150°C, the temperature of the coating die is 140°C, and the coating speed is 3-4 m / min.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The waterproof and sealing butyl rubber adhesive tape prepared by the invention comprises a modified brominated butyl rubber layer and a flame retardant butyl rubber layer to achieve the effects of waterproofing, sealing and flame retardancy.

[0016] Firstly, the present invention quaternizes stearamidopropyl dimethyl tertiary amine and benzyl chloride to generate antibacterial monomers to improve the antibacterial property of the adhesive tape, and the long-chain alkyl group of the stearamidopropyl dimethyl tertiary amine can improve the waterproof property of the adhesive tape and reduce the adhesion of bacteria on the surface, thereby increasing the antibacterial property of the adhesive tape; then, cation exchange is performed with sodium montmorillonite to improve the compatibility of the montmorillonite with the antibacterial monomer; then, the tertiary amine is melt-blended with brominated butyl rubber to form a strong interface interaction force and improve the mechanical property; the modified montmorillonite containing more long chains can form a uniform nano-dispersion in the rubber matrix to form a physical barrier layer mainly with a lamellar structure, reduce the permeability, and enhance the waterproof and airtightness of the adhesive tape.

[0017] Secondly, the present invention reacts the chlorine group of diethyl thiophosphoryl chloride with the hydroxyl group of methyl parahydroxybenzoate to form a flame retardant integrating aromatic hydrocarbons, phosphorus and sulfur elements, which synergistically improve the flame retardancy of the adhesive tape. Then, the ester group is hydrolyzed to form a carboxyl group, which is electrostatically combined with the chitosan quaternary ammonium salt to form an ion complex. The quaternary ammonium salt of chitosan can decompose under heat to form a dense carbon layer, which blocks heat and oxygen and enhances the flame retardancy. At the same time, the chitosan quaternary ammonium salt and the antibacterial monomer work together to improve the antibacterial effect of the adhesive tape. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the waterproof sealing butyl rubber adhesive tape prepared in the following examples are as follows: Antibacterial property: The antibacterial rate test of the examples and comparative examples was carried out with reference to GB / T 20944.3-2008. The examples and comparative examples were respectively placed in Erlenmeyer flasks with a test bacterial solution of a certain concentration, and oscillated at a specified temperature for a certain time. The live bacteria concentration of the bacterial solution in the Erlenmeyer flask before and after oscillation for a certain time was measured, and the antibacterial rate was calculated to evaluate the antibacterial effect of the sample. Antibacterial rate = (unmodified adhesive tape - modified adhesive tape) / unmodified adhesive tape × 100%.

[0020] Hydrophobicity: A contact angle meter was used to observe the angle between the contour of a water drop on the butyl tape and the plane of the tape to characterize its hydrophobicity. Deionized water was used and the drop volume was 2 μL.

[0021] Adhesion: The holding time of the adhesive tape under constant tension is tested using a tape holding force tester to characterize the adhesive tape's ability to resist displacement. The hanging weight is 10 kg.

[0022] Flame retardancy: The limiting oxygen index of the examples and comparative examples was determined according to GB / T 2406-93.

[0023] Air tightness: VAC-V2 manufactured by Labthink was used to monitor the values ​​on the low pressure side through the gas pressure gradient to obtain the parameters of various gas permeation parameters. The test conditions were nitrogen as the permeating gas and a temperature of 25°C. Example 1

[0024] (1) Stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol were mixed in a mass ratio of 5:2:7, heated to 50°C, stirred at 80 rpm for 4 h, and reduced pressure to 0.05 MPa for filtration to obtain the antibacterial monomer; sodium montmorillonite and deionized water were mixed in a mass ratio of 1:15, stirred at room temperature and 700 rpm for 8 h, and the mixture was allowed to stand for 15 h to allow large particles of impurities and large particles of clay that are difficult to mix to precipitate, the upper clay suspension was taken, heated to 60°C, stirred at 700 rpm for 1 h, and an antibacterial monomer of 1 times the mass of the suspension was added, reacted for 2 h, allowed to stand for 12 h, centrifuged at 5000 rpm for 10 min, the solid was taken out, and deionized water was used to remove the solid. Wash with water for 3 times, heat to 90°C and dry for 24h to obtain organic modified clay; heat the brominated butyl rubber to 80°C and plasticize for 1min, add zinc oxide, stearic acid, organic modified clay, dibenzothiazole disulfide accelerator, zinc diethyl dithiocarbamate accelerator and sulfur, wherein by weight, plasticize 100 parts of brominated butyl rubber, 2 parts of zinc oxide, 1 part of stearic acid, 2 parts of organic modified clay, 1 part of dibenzothiazole disulfide accelerator, 1 part of zinc diethyl dithiocarbamate accelerator, 1 part of sulfur, and mix evenly for 10min to obtain a rubber mix, put the rubber mix into a mold, heat to 150°C, and vulcanize for 20min to obtain modified brominated butyl rubber; (2) Diethylthiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate were mixed in a mass ratio of 1:1:2, heated to 95°C, stirred at 90 rpm for 1 h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90°C and dried for 3 h to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution were mixed in a mass ratio of 1:0.5:1, heated to 70°C, stirred at 50 rpm for 1.5 h, heated to 60°C and evaporated to constant weight, and deionized water 3 times the mass of the flame retardant was added. The pH was adjusted to 1 with 1 mol / L hydrochloric acid, stirred at 30 rpm for 12 h, centrifuged for 10 min to take out the solid, and then washed with deionized water, ethanol and methanol for 3 times respectively, heated to 65°C and dried to obtain a hydrolyzed flame retardant; chitosan quaternary ammonium salt and hydrolyzed flame retardant were mixed at a mass ratio of 10:1, heated to 50°C for reaction for 3 h, centrifuged for 10 min three times, solid was taken out, frozen to -10°C and dried for 15 h to obtain a flame retardant, the flame retardant and butyl rubber were heated to 80°C at a mass ratio of 17:5, mixed for 15 min, heated to 150°C, vulcanized for 30 min, and pressed into sheets to obtain flame-retardant butyl rubber; (3) Cut the flame retardant butyl rubber and modified brominated butyl rubber into 18mm×30m, with flame retardant butyl rubber and modified brominated butyl rubber from top to bottom, and put them into the coating machine. The heating temperature of the glue box is 150℃, the temperature of the coating die is 140℃, and the coating speed is 3m / min. Use polyurethane glue to coat, and the total amount is 125g / m2 , let it stand for 24 hours, isolate the disks at both ends with release paper, and obtain a waterproof sealing butyl rubber adhesive tape. Example 2

[0025] (1) Stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol were mixed in a mass ratio of 5.2:2:7, heated to 60°C, stirred at 100 rpm for 4 hours, and reduced pressure to 0.07 MPa for filtration to obtain the antibacterial monomer; sodium montmorillonite and deionized water were mixed in a mass ratio of 1:158, stirred at room temperature and 750 rpm for 8.5 hours, and the mixture was allowed to stand for 15 hours to allow large particles of impurities and large particles of clay that are difficult to mix to precipitate. The upper clay suspension was taken, heated to 60°C, stirred at 700 rpm for 1 hour, and 1.5 times the mass of the suspension antibacterial monomer was added, reacted for 2.5 hours, left to stand for 12 hours, centrifuged at 5000 rpm for 15 minutes, and the solid was taken out. , washed with deionized water for 3 times, heated to 90°C and dried for 28h to obtain organic modified clay; heated the brominated butyl rubber to 80°C and plasticized for 1min, added zinc oxide, stearic acid, organic modified clay, dibenzothiazole disulfide accelerator, zinc diethyl dithiocarbamate accelerator and sulfur, wherein by weight, 100 parts of brominated butyl rubber, 3 parts of zinc oxide, 2 parts of stearic acid, 3 parts of organic modified clay, 2 parts of dibenzothiazole disulfide accelerator, 2 parts of zinc diethyl dithiocarbamate accelerator, 2 parts of sulfur, and uniformly mixed for 10min to obtain a rubber mix, put the rubber mix into a mold, heated to 160°C, and vulcanized for 25min to obtain a modified brominated butyl rubber; (2) Diethylthiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate were mixed in a mass ratio of 1:1:2, heated to 100°C, stirred at 120 rpm for 1 hour, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90°C and dried for 3 hours to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution were mixed in a mass ratio of 1.5:0.5:1, heated to 70°C, stirred at 60 rpm for 1.5 hours, heated to 60°C and evaporated to constant weight, and deionized water 3 times the mass of the flame retardant was added. , adjust the pH to 1 with 1 mol / L hydrochloric acid, stir at 40 rpm for 12 hours, centrifuge for 10 minutes to take out the solid, wash it with deionized water, ethanol and methanol respectively for 3 times, heat it to 65°C and dry it to obtain a hydrolyzed flame retardant; mix the chitosan quaternary ammonium salt and the hydrolyzed flame retardant in a mass ratio of 10:1.3, heat it to 50°C to react for 3 hours, centrifuge it for 10 minutes three times, take out the solid, freeze it to -10°C and dry it for 15 hours to obtain a flame retardant, heat the flame retardant and butyl rubber in a mass ratio of 17:5 to 80°C, mix them for 18 minutes, heat it to 160°C, vulcanize it for 35 minutes, and press it into sheets to obtain a flame retardant butyl rubber; (3) Cut the flame retardant butyl rubber and modified brominated butyl rubber into 18mm×30m, with flame retardant butyl rubber and modified brominated butyl rubber from top to bottom, and put them into the coating machine. The heating temperature of the glue box is 150℃, the temperature of the coating die is 140℃, the coating speed is 3.5m / min, and the polyurethane glue is used for coating. The total amount is 125g / m 2 , let it stand for 24 hours, isolate the disks at both ends with release paper, and obtain a waterproof sealing butyl rubber adhesive tape. Example 3

[0026] (1) Stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol were mixed in a mass ratio of 5.3:2:7, heated to 80°C, stirred at 120 rpm for 4 h, and reduced pressure to 0.1 MPa for filtration to obtain the antibacterial monomer; sodium montmorillonite and deionized water were mixed in a mass ratio of 1:20, stirred at room temperature and 800 rpm for 9 h, and the mixture was allowed to stand for 15 h to allow large particles of impurities and large particles of clay that are difficult to mix to precipitate, the upper clay suspension was taken, heated to 60°C, stirred at 700 rpm for 1 h, and the antibacterial monomer twice the mass of the suspension was added, reacted for 3 h, allowed to stand for 12 h, centrifuged at 5000 rpm for 20 min, and the solid was taken out and removed by deionization. The mixture was washed with water for 4 times, heated to 90°C and dried for 30h to obtain organic modified clay; the bromobutyl rubber was heated to 80°C and plasticized for 1min, and zinc oxide, stearic acid, organic modified clay, dibenzothiazole disulfide accelerator, zinc diethyl dithiocarbamate accelerator and sulfur were added, wherein by weight, 100 parts of bromobutyl rubber, 5 parts of zinc oxide, 3 parts of stearic acid, 4 parts of organic modified clay, 3 parts of dibenzothiazole disulfide accelerator, 3 parts of zinc diethyl dithiocarbamate accelerator, 3 parts of sulfur were plasticized, and uniformly mixed for 10min to obtain a rubber mix, and the rubber mix was put into a mold, heated to 170°C, and vulcanized for 30min to obtain a modified bromobutyl rubber; (2) Diethylthiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate were mixed in a mass ratio of 1:1:3, heated to 100°C, stirred at 150 rpm for 1 hour, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90°C and dried for 3 hours to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution were mixed in a mass ratio of 2:0.5:1, heated to 70°C, stirred at 60 rpm for 1.5 hours, heated to 60°C and evaporated to constant weight, and deionized water 4 times the mass of the flame retardant was added. The pH was adjusted to 2 with 1 mol / L hydrochloric acid, stirred at 50 rpm for 12 h, centrifuged for 10 min to take out the solid, and then washed with deionized water, ethanol and methanol for 3 times respectively, heated to 65°C and dried to obtain a hydrolyzed flame retardant; chitosan quaternary ammonium salt and hydrolyzed flame retardant were mixed at a mass ratio of 10:1.5, heated to 50°C for reaction for 3 h, centrifuged for 10 min three times, solid was taken out, frozen to -10°C and dried for 15 h to obtain a flame retardant, the flame retardant and butyl rubber were heated to 80°C at a mass ratio of 17:5, mixed for 20 min, heated to 160°C, vulcanized for 40 min, and pressed into sheets to obtain flame-retardant butyl rubber; (3) Cut the flame retardant butyl rubber and modified brominated butyl rubber into 18mm×30m, with flame retardant butyl rubber and modified brominated butyl rubber from top to bottom, and put them into the coating machine. The heating temperature of the glue box is 150℃, the temperature of the coating die is 140℃, the coating speed is 4m / min, and the polyurethane glue is used for coating. The total amount is 125g / m 2 , let it stand for 24 hours, isolate the disks at both ends with release paper, and obtain a waterproof sealing butyl rubber adhesive tape.

[0027] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is only that step (1) is different. Step (1) is changed to: heating the brominated butyl rubber to 80°C and plasticizing for 1 min, adding zinc oxide, stearic acid, sodium montmorillonite, dibenzothiazole disulfide accelerator, zinc diethyldithiocarbamate accelerator and sulfur, wherein, by weight, 100 parts of brominated butyl rubber, 5 parts of zinc oxide, 3 parts of stearic acid, 4 parts of sodium montmorillonite, 3 parts of dibenzothiazole disulfide accelerator, 3 parts of zinc diethyldithiocarbamate accelerator, and 3 parts of sulfur are plasticized, and uniformly mixed for 10 minutes to obtain a rubber mix, which is placed in a mold, heated to 170°C, and vulcanized for 30 minutes to obtain a modified brominated butyl rubber.

[0028] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is only the difference in step (1), and step (1) is changed to: stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol are mixed in a mass ratio of 5.3:2:7, heated to 80°C, stirred at 120rpm for 4h, and reduced to 0.1MPa by filtration to obtain an antibacterial monomer; brominated butyl rubber is heated to 80°C and plasticized for 1min, zinc oxide, stearic acid, antibacterial monomer, dibenzothiazole disulfide are added to promote The invention discloses a novel modified bromobutyl rubber preparation method, wherein the modified bromobutyl rubber is prepared by mixing 100 parts of bromobutyl rubber, 5 parts of zinc oxide, 3 parts of stearic acid, 4 parts of antibacterial monomer, 3 parts of dibenzothiazole disulfide accelerator, 3 parts of zinc diethyldithiocarbamate accelerator and 3 parts of sulfur. The mixture is uniformly mixed for 10 minutes to obtain a rubber mixture, and the mixture is put into a mold, heated to 170°C and vulcanized for 30 minutes to obtain a modified bromobutyl rubber.

[0029] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is only that step (2) is different. Step (2) is changed to: diethyl thiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate are mixed uniformly in a mass ratio of 1:1:3, heated to 100°C, stirred at 150 rpm for 1 hour, cooled to room temperature, filtered to obtain a clarified filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water three times respectively, heated to 90°C and dried for 3 hours to obtain a flame retardant; chitosan quaternary ammonium salt and flame retardant are mixed in a mass ratio of 10:1.5, heated to 50°C for reaction for 3 hours, centrifuged three times for 10 minutes, took out the solid, frozen to -10°C and dried for 15 hours to obtain a flame retardant, and the flame retardant and butyl rubber are heated to 80°C in a mass ratio of 17:5, mixed for 20 minutes, heated to 160°C, vulcanized for 40 minutes, and vulcanized and pressed into sheets to obtain flame retardant butyl rubber.

[0030] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is only that step (2) is different. Step (2) is changed to: diethyl thiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate are mixed uniformly in a mass ratio of 1:1:3, heated to 100°C, stirred at 150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to take out the precipitate, washed with anhydrous ethanol and deionized water three times respectively, heated to 90°C and dried for 3h to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 2:0.5:1, heated to 70°C, stirred at 60rpm for 1.5h, heated to 60°C and rotary evaporated to constant weight , add deionized water 4 times the mass of the flame retardant, adjust the pH to 2 with 1 mol / L hydrochloric acid, stir at 50 rpm for 12 hours, centrifuge for 10 minutes to take out the solid, wash it with deionized water, ethanol and methanol respectively for 3 times, heat it to 65°C and dry it to obtain a hydrolyzed flame retardant; mix chitosan and hydrolyzed flame retardant in a mass ratio of 10:1.5, heat it to 50°C to react for 3 hours, centrifuge it three times for 10 minutes, take out the solid, freeze it to -10°C and dry it for 15 hours to obtain a flame retardant, heat the flame retardant and butyl rubber in a mass ratio of 17:5 to 80°C, mix them for 20 minutes, heat it to 160°C, vulcanize it for 40 minutes, and vulcanize it into sheets to obtain flame-retardant butyl rubber.

[0031] Comparative Example 5 The difference between Comparative Example 5 and Example 3 is only that step (2) is different. Step (2) is changed to: diethyl thiophosphoryl chloride and methyl p-hydroxybenzoate are mixed in a mass ratio of 1:3, heated to 100°C, stirred at 150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90°C and dried for 3h to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 2:0.5:1, heated to 70°C, stirred at 60rpm for 1.5h, heated to 60°C and evaporated to constant weight, and the flame retardant is added. The mass of the substance was 4 times of deionized water, the pH was adjusted to 2 with 1 mol / L hydrochloric acid, the mixture was stirred at 50 rpm for 12 h, the solid was taken out by centrifugation for 10 min, and then washed with deionized water, ethanol and methanol for 3 times respectively, and the mixture was heated to 65 °C and dried to obtain a hydrolyzed flame retardant; the chitosan quaternary ammonium salt and the hydrolyzed flame retardant were mixed in a mass ratio of 10:1.5, the mixture was heated to 50 °C and reacted for 3 h, the mixture was centrifuged for 10 min three times, the solid was taken out, frozen to -10 °C and dried for 15 h to obtain a flame retardant, the flame retardant and butyl rubber were heated to 80 °C in a mass ratio of 17:5, mixed for 20 min, heated to 160 °C, vulcanized for 40 min, and vulcanized and pressed into sheets to obtain a flame retardant butyl rubber.

[0032] Comparative Example 6 The difference between Comparative Example 6 and Example 3 is only the difference in step (2). Step (2) is changed to: diethyl thiophosphoryl chloride and tetrahydrofuran are mixed in a mass ratio of 1:1, heated to 100°C, stirred at 150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water three times respectively, heated to 90°C and dried for 3h to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 2:0.5:1, heated to 70°C, stirred at 60rpm for 1.5h, heated to 60°C and evaporated to constant weight, and the flame retardant is added. 4 times the amount of deionized water, adjust the pH to 2 with 1 mol / L hydrochloric acid, stir at 50 rpm for 12 h, centrifuge for 10 min to take out the solid, then wash it with deionized water, ethanol and methanol for 3 times respectively, heat it to 65 ° C and dry it to obtain a hydrolyzed flame retardant; mix the chitosan quaternary ammonium salt and the hydrolyzed flame retardant in a mass ratio of 10:1.5, heat it to 50 ° C to react for 3 h, centrifuge it three times for 10 min, take out the solid, freeze it to -10 ° C and dry it for 15 h to obtain a flame retardant, heat the flame retardant and butyl rubber in a mass ratio of 17:5 to 80 ° C, mix them for 20 min, heat it to 160 ° C, vulcanize it for 40 min, and vulcanize it into sheets to obtain flame-retardant butyl rubber.

[0033] Comparative Example 7 The difference between Comparative Example 7 and Example 3 is only the difference in step (2). Step (2) is changed to: tetrahydrofuran and methyl paraben are mixed in a mass ratio of 1:3, heated to 100°C, stirred at 150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80°C to remove the precipitate, washed with anhydrous ethanol and deionized water three times respectively, heated to 90°C and dried for 3h to obtain a flame retardant; the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 2:0.5:1, heated to 70°C, stirred at 60rpm for 1.5h, heated to 60°C and evaporated to constant weight, and the flame retardant is added. 4 times the amount of deionized water, adjust the pH to 2 with 1 mol / L hydrochloric acid, stir at 50 rpm for 12 h, centrifuge for 10 min to take out the solid, then wash it with deionized water, ethanol and methanol for 3 times respectively, heat it to 65 ° C and dry it to obtain a hydrolyzed flame retardant; mix the chitosan quaternary ammonium salt and the hydrolyzed flame retardant in a mass ratio of 10:1.5, heat it to 50 ° C to react for 3 h, centrifuge it three times for 10 min, take out the solid, freeze it to -10 ° C and dry it for 15 h to obtain a flame retardant, heat the flame retardant and butyl rubber in a mass ratio of 17:5 to 80 ° C, mix them for 20 min, heat it to 160 ° C, vulcanize it for 40 min, and vulcanize it into sheets to obtain flame-retardant butyl rubber.

[0034] Effect example Table 1 below shows the performance analysis results of the waterproof sealing butyl rubber adhesive tapes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.

[0035]

[0036] By comparing the antibacterial rate experimental data of the embodiment and the comparative example in Table 1, it can be found that stearamidopropyl dimethyl tertiary amine and benzyl chloride are used to quaternize to generate antibacterial monomers to improve the antibacterial property of the adhesive tape, and the long-chain alkyl group carried by stearamidopropyl dimethyl tertiary amine can reduce the adhesion of bacteria on the surface, thereby increasing the antibacterial property of the adhesive tape; from the comparison of the water contact angle and air permeability coefficient experimental data of the embodiment and the comparative example, it can be found that the long-chain alkyl group carried by stearamidopropyl dimethyl tertiary amine can improve the waterproofness of the adhesive tape, and the organic modified clay and brominated butyl rubber are melt-blended to form a strong interfacial interaction force, thereby improving the mechanical properties, and the modified montmorillonite containing more long chains will be in the rubber matrix. A uniform nano-dispersion is formed, and a physical barrier layer with a mainly lamellar structure is formed, which reduces the permeability and enhances the waterproof and airtightness of the adhesive tape. From the comparison of the limiting oxygen index experimental data of the embodiment and the comparative example, it can be found that the chlorine group of diethyl thiophosphoryl chloride reacts with the hydroxyl group of methyl parahydroxybenzoate to form a flame retardant integrating aromatic hydrocarbons, phosphorus and sulfur elements, which synergistically improve the flame retardancy of the adhesive tape. Then, the ester group is hydrolyzed to form a carboxyl group, which is electrostatically combined with the chitosan quaternary ammonium salt to form an ion complex, which can be decomposed by heat to form a dense carbon layer, which blocks heat and oxygen and enhances the flame retardancy. At the same time, the chitosan quaternary ammonium salt and the antibacterial monomer work together to improve the antibacterial effect of the adhesive tape.

[0037] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A waterproof sealing butyl rubber adhesive tape, characterized in that: The waterproof sealing butyl rubber adhesive tape comprises a modified brominated butyl rubber layer and a flame retardant butyl rubber layer.

2. The waterproof sealing butyl rubber adhesive tape according to claim 1, characterized in that: The modified brominated butyl rubber layer is prepared from stearamidopropyl dimethyl tertiary amine, benzyl chloride, sodium montmorillonite and brominated butyl rubber.

3. The waterproof sealing butyl rubber adhesive tape according to claim 1, characterized in that: The flame retardant butyl rubber layer is prepared from diethyl thiophosphoryl chloride, methyl p-hydroxybenzoate and chitosan quaternary ammonium salt.

4. A method for preparing a waterproof sealing butyl rubber adhesive tape, characterized in that: The method comprises the following preparation steps: (1) Stearamidopropyl dimethyl tertiary amine, benzyl chloride and anhydrous ethanol were mixed in a mass ratio of 5-5.3:2:7, heated to 50-80°C, stirred at 80-120 rpm for 4 h, and reduced pressure to 0.05-0.1 MPa for filtration to obtain an antibacterial monomer; sodium montmorillonite and deionized water were mixed in a mass ratio of 1:15-20, stirred at room temperature and 700-800 rpm for 8-9 h, and the mixture was allowed to stand for 15 h to allow large impurities and large particles of clay that are difficult to mix to precipitate, and the upper clay suspension was taken, heated to 60°C, and stirred at 700 rpm for 1 h. Add 1-2 times the mass of the suspension antibacterial monomer, react for 2-3 hours, let stand for 12 hours, centrifuge at 5000 rpm for 10-20 minutes, take out the solid, wash with deionized water for 3-4 times, heat to 90°C and dry for 24-30 hours to obtain organic modified clay; heat the brominated butyl rubber to 80°C and plasticize for 1 minute, add zinc oxide, stearic acid, organic modified clay, dibenzothiazole disulfide accelerator, zinc diethyl dithiocarbamate accelerator and sulfur, mix evenly for 10 minutes to obtain a rubber mix, put the rubber mix into a mold for vulcanization to obtain modified brominated butyl rubber; (2) Diethyl thiophosphoryl chloride, tetrahydrofuran and methyl parahydroxybenzoate are mixed uniformly in a mass ratio of 1:1:2~3, heated to 95~100℃, stirred at 90~150rpm for 1h, cooled to room temperature, filtered to obtain a clear filtrate, heated to 80℃ to remove the precipitate, washed with anhydrous ethanol and deionized water for 3 times respectively, heated to 90℃ and dried for 3h to obtain a flame retardant; chitosan quaternary ammonium salt and hydrolyzed flame retardant are mixed in a mass ratio of 10:1~1.5, heated to 50℃ for reaction for 3h, centrifuged three times for 10min, removed the solid, frozen to -10℃ and dried for 15h to obtain a flame retardant; the flame retardant and butyl rubber are heated to 80℃ in a mass ratio of 17:5, mixed for 15~20min, heated to 150~160℃, vulcanized for 30~40min, and pressed into sheets to obtain flame retardant butyl rubber; (3) Cut the flame retardant butyl rubber and modified brominated butyl rubber into 18 mm × 30 m, with flame retardant butyl rubber and modified brominated butyl rubber from top to bottom, put them into the glue box of the coating machine and coat them with glue, let them stand for 24 hours, and isolate the two end disks with release paper to obtain a waterproof sealing butyl rubber adhesive tape.

5. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: The specific conditions for rubber vulcanization in the above step (1) are: heating temperature of 140-160° C., and vulcanization time of 20-30 min.

6. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: In the above step (1), the following are prepared by weight: 100 parts of plasticized brominated butyl rubber, 2 to 5 parts of zinc oxide, 1 to 3 parts of stearic acid, 2 to 4 parts of organic modified clay, 1 to 3 parts of dibenzothiazole disulfide accelerator, 1 to 3 parts of zinc diethyldithiocarbamate accelerator, and 1 to 3 parts of sulfur.

7. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: The preparation method of the hydrolyzed flame retardant in the above step (2) is as follows: the flame retardant, tetrahydrofuran and 1.8 mol / L sodium hydroxide aqueous solution are mixed in a mass ratio of 1-2:0.5:1, the temperature is raised to 70°C, and the mixture is stirred at 50-60 rpm for 1.5 h. The mixture is heated to 60°C and rotary evaporated to constant weight, deionized water of 3-4 times the mass of the flame retardant is added, the pH is adjusted to 1-2 with 1 mol / L hydrochloric acid, the mixture is stirred at 30-50 rpm for 12 h, the solid is taken out by centrifugation for 10 min, and then the solid is washed with deionized water, ethanol and methanol for 3 times respectively, and the solid is dried after being heated to 65°C.

8. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: The chitosan quaternary ammonium salt in the above step (2) is hydroxypropyltrimethylammonium chloride chitosan.

9. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: The glue in step (3) above is polyurethane glue, with a total amount of 125g / m 2 .

10. The method for preparing a waterproof sealing butyl rubber adhesive tape according to claim 4, characterized in that: The specific conditions of the coating machine treatment in the above step (3) are: the heating temperature of the glue box is 150°C, the temperature of the coating die is 140°C, and the coating speed is 3~4m / min.

Citation Information

Patent Citations

  • Flame-retardant insulating electrical adhesive tape and preparation method thereof

    CN113930168A

  • Flame-retardant type strong cross film self-adhesion waterproof coiled material

    CN213924635U