Chloride ultraviolet afterglow material

By doping Pb2+ ions in Cs2NaScCl6, the chloride ultraviolet afterglow material synthesis at low temperature hydrothermal synthesis is achieved, solving the problem of high-temperature sintering of oxide materials and the difficulty of designing chloride materials, and achieving ultraviolet afterglow emission with peak position near 385nm and Long-term attenuation has promoted the development of chloride ultraviolet afterglow materials.

CN119060731AActive Publication Date: 2024-12-03NANKAI UNIV

Patent Information

Application Number
CN202411303942.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The lattice energy of oxide ultraviolet afterglow materials leads to high temperature sintering demands, and the band gap of chloride ultraviolet afterglow materials is small and the design is difficult, which has not been explored in depth.

Method used

The chloride ultraviolet afterglow material of Cs2NaScCl6:Pb2+ is used to reduce the lattice energy by doping Pb2+ ions, and low-temperature hydrothermal synthesis is achieved, resulting in ultraviolet afterglow emission with a peak position near 385nm, with an attenuation time of more than 1 hour.

Benefits of technology

UV afterglow emission based on chloride system is achieved, the reaction temperature is reduced, the use of dangerous light sources is avoided, the gap in the academic community is filled, and the development of afterglow materials is promoted.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060731A_ABST
    Figure CN119060731A_ABST
Patent Text Reader

Abstract

The invention relates to a chloride ultraviolet afterglow material. The structural formula of the material is Cs2NaScCl6: xPb, wherein x is more than or equal to 0.005 and less than or equal to 0.1. The preparation method comprises the following steps: weighing and mixing a Cs-containing compound, a Na-containing compound, an Sc-containing compound and a Pb-containing compound, and then adding concentrated hydrochloric acid; reacting after sealing to obtain a target product. The material obtained by the invention can continuously emit ultraviolet afterglow of 380-390nm after being irradiated by a deep ultraviolet light source (254nm), and the decay time of the ultraviolet afterglow can be maintained for more than 1h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, in particular to a chloride ultraviolet afterglow material. Background Art

[0002] Afterglow materials can store external excitation light energy, and continue to emit light after the excitation light source is turned off, and continue to emit light for a period of time in the form of gradually decaying light intensity. They are widely used in optical storage, night guidance, multi-mode anti-counterfeiting and biological imaging. Among them, ultraviolet light has higher photon energy than visible light and near-infrared light, showing special application value, such as being a material excitation medium, sterilization, and promoting vitamin synthesis. Therefore, ultraviolet afterglow materials have gradually received attention and research and development, such as: Ca2Al2SiO7:Pr 3+ ,LiScGeO4:Bi 3+ ,YBO3:Pr 3+ However, the lattice energy of oxide materials is relatively high (~3000 kJ mol -1 ), which requires long-term high-temperature sintering (generally above 1300°C) and is therefore heavily dependent on electrical thermal energy.

[0003] In comparison, chloride materials based on ionic bonding have lower lattice energy (generally less than 1000 kJ mol -1 ), so it supports the liquid phase synthesis strategy under low temperature environment. In recent years, chloride afterglow materials have been gradually explored, such as Cs2Na 1-x Ag x InCl6:Mn 2+ 、Cs2NaScCl6:Tb 3+ 、Cs2NaInCl6:Ag,Bi、Cs2(Na 0.9 Ag 0.1 In) 1-x Zr x Cl6, etc. However, compared with oxides, the band gap of chloride materials is smaller and the design of ultraviolet emission is more difficult, so the ultraviolet afterglow materials based on the chloride system have not been deeply explored so far.

[0004] The present invention proposes a novel nanostructured carbon nanotube based on Cs2NaScCl6:Pb 2+ The chloride ultraviolet afterglow material can continuously emit ultraviolet afterglow with a peak position near 385nm after being irradiated by a deep ultraviolet light source (254nm), and its decay time can be maintained for more than 1h. Summary of the invention

[0005] The purpose of the present invention is to provide a chloride ultraviolet afterglow material (Cs2NaScCl6:xPb2+ , 0.005≤x≤0.1). After irradiation with deep ultraviolet light such as 254nm, the material produces ultraviolet afterglow emission with a peak at about 385nm, and the specific emission peak covers a range of about 320-450nm. After irradiation with 254nm deep ultraviolet light for 5 minutes, the ultraviolet afterglow decay time exceeds 1h.

[0006] The technical solution of the present invention is:

[0007] A chloride ultraviolet afterglow material has a structural formula of Cs2NaScCl6:xPb, 0.005≤x≤0.1.

[0008] After being charged by 254nm deep ultraviolet light, the material produces ultraviolet afterglow emission with a peak at around 385nm, and the specific emission peak covers the range of 320-450nm.

[0009] The preparation method of the chloride ultraviolet afterglow material comprises the following steps:

[0010] (1) weighing and mixing a Cs-containing compound, a Na-containing compound, a Sc-containing compound, and a Pb-containing compound in a reaction kettle lined with polytetrafluoroethylene;

[0011] Wherein, the Cs-containing compound is a chloride or carbonate of Cs; the Na-containing compound is a chloride or carbonate of Na; the Sc-containing compound is a chloride or oxide of Sc; the Pb-containing compound is a chloride or oxide of Pb;

[0012] The ratio of the above salts is based on the corresponding amount of substance in Cs2NaScCl6:xPb, that is, Cs:Na:Sc:Pb=2:1:1:x; 0.005≤x≤0.1;

[0013] (2) Add concentrated hydrochloric acid to the reaction kettle; add 4-12 mL of concentrated hydrochloric acid for every 2 mmol of CsCl;

[0014] The concentration of the concentrated hydrochloric acid is 30-38wt%.

[0015] (3) Seal the reactor and heat at 150-200 ℃ Keep warm for 3-12 hours, and then cool naturally to room temperature;

[0016] (4) washing the crystal product with anhydrous ethanol;

[0017] (5) Dry the product at 40-80°C for about 1-5 hours and grind it to obtain a powdery target product.

[0018] The essential features of the present invention are:

[0019] From the above similar literature, we can see that different luminescence properties can be obtained by doping different ions based on the Cs2NaScCl6 matrix. The band gap of the matrix is ​​relatively wide (>4.0eV), which is suitable for ultraviolet luminescence design. The present invention prepares a new material Cs2NaScCl6:Pb 2+ , by doping with Pb 2+ Introducing luminescent energy levels to induce ultraviolet luminescence properties. Due to different valence states, Pb 2+ After the doping, lattice defects are caused, which can capture and store electrons. After the excitation light is turned off, the captured electrons can be gradually released and deposited in Pb 2+ The luminescence process is completed at the point where the ultraviolet afterglow phenomenon occurs.

[0020] The beneficial effects of the present invention are:

[0021] (1) The present invention realizes ultraviolet afterglow emission based on the chloride system, fills the gap in the academic community, and promotes the development of the afterglow field.

[0022] (2) The material of the present invention can be excited by deep ultraviolet light such as 254 nm, avoiding the use of dangerous light sources such as X-rays or gamma rays.

[0023] (3) Oxides usually require a solid phase environment of >1300°C. The hydrothermal synthesis temperature of the present invention is 180°C, which greatly reduces the reaction temperature compared to oxides and reduces the consumption of electrical thermal energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the XRD spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1;

[0025] Figure 2 is the fluorescence emission spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, with an excitation wavelength of 295nm;

[0026] Figure 3 The fluorescence excitation spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, with a monitoring wavelength of 385 nm;

[0027] Figure 4 is the fluorescence emission spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, with an excitation wavelength of 265nm;

[0028] Figure 5 The fluorescence excitation spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, with a monitoring wavelength of 500nm;

[0029] Figure 6The afterglow emission spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, the charging light source is 254nm, and the charging time is 5min;

[0030] Figure 7 The afterglow decay spectrum of Cs2NaScCl6:0.03Pb obtained in Example 1, the charging light source is 254nm, the charging time is 5min, and the monitoring wavelength is 385nm;

[0031] Figure 8 is the XRD spectrum of Cs2NaScCl6:0.005Pb obtained in Example 2;

[0032] Fig. 9 The afterglow emission spectrum of Cs2NaScCl6:0.005Pb obtained in Example 2, the charging light source is 254nm, and the charging time is 5min;

[0033] Fig.10 The afterglow decay spectrum of Cs2NaScCl6:0.005Pb obtained in Example 2, the charging light source is 254nm, the charging time is 5min, and the monitoring wavelength is 380nm;

[0034] Fig.11 is the XRD spectrum of Cs2NaScCl6:0.1Pb obtained in Example 3;

[0035] Fig.12 The afterglow emission spectrum of Cs2NaScCl6:0.1Pb obtained in Example 3, the charging light source is 254nm, and the charging time is 5min;

[0036] Fig.13 The afterglow decay spectrum of Cs2NaScCl6:0.1Pb obtained in Example 3, the charging light source is 254nm, the charging time is 5min, and the monitoring wavelength is 390nm;

[0037] Fig.14 This is a comparison diagram of the afterglow attenuation of Cs2NaScCl6:0.005Pb, Cs2NaScCl6:0.03Pb and Cs2NaScCl6:0.1Pb obtained in Examples 1-3;

[0038] Fig.15 This is a graph showing the dependence of the afterglow intensity of Cs2NaScCl6:xPb (x=0.005, 0.01, 0.03, 0.05, 0.07, 0.1) obtained in Example 4 on the Pb doping concentration 60 seconds after turning off the 254nm charging light source, and the charging time is 5 minutes. DETAILED DESCRIPTION

[0039] Example 1: Cs2NaScCl6:0.03Pb sample

[0040] The preparation method of the present invention is as follows: 2 mmol CsCl (0.3367 g) powder, 1 mmol NaCl (0.0584 g) powder, 1 mmol ScCl3 (0.1513 g) powder and 0.03 mmol PbCl2 (0.0083 g) powder are weighed into a reaction kettle lined with polytetrafluoroethylene, 4 mL of concentrated hydrochloric acid (30 wt%) is added, the reaction kettle is sealed after being loaded, and the mixture is kept warm at 200° C. for 12 hours, cooled naturally to room temperature, the obtained product is washed with ethanol for 3 times, dried at 40° C. for about 5 hours, taken out and crushed to obtain the final product.

[0041] Test conditions: The crystal structure of the sample was tested using a Rigaku X-ray diffractometer, with a Cu target as the radiation source, a tube voltage of 40 kV, a tube current of 40 mA, a scanning step of 0.02°, a scanning speed of 15° / min, and a scanning range of 10°-60°. The emission spectrum, excitation spectrum, afterglow emission spectrum, and afterglow decay spectrum of the sample were all obtained by testing with an FS-5 spectrometer.

[0042] Experimental results: Figure 1 The XRD spectrum of Cs2NaScCl6:0.03Pb is given, and it can be seen that a crystalline product has been obtained through this experimental scheme;

[0043] Figure 2 The fluorescence emission spectrum of Cs2NaScCl6:0.03Pb under 295nm excitation is given. The emission peak is at 385nm, corresponding to Pb 2+ The ultraviolet luminescence band;

[0044] Figure 3 The fluorescence excitation spectrum of Cs2NaScCl6:0.03Pb when monitoring the emission at 385nm is given, which shows two effective excitation peaks at 265 and 295nm, corresponding to the band gap transition and Pb 2+ absorption;

[0045] Figure 4 The fluorescence emission spectrum of Cs2NaScCl6:0.03Pb under 265nm excitation is given, which shows two effective emission peaks at 385 and 500nm, corresponding to Pb 2+ and self-trapped emission from the matrix;

[0046] Figure 5 Given is the fluorescence excitation spectrum of Cs2NaScCl6:0.03Pb when monitoring the emission at 500 nm, with the excitation peak at 265 nm, corresponding to the band gap transition;

[0047] Figure 6 The afterglow emission spectrum of Cs2NaScCl6:0.03Pb after 254nm irradiation and pre-charging for 5 minutes is shown, which only shows Pb 2+ The ultraviolet afterglow emission has a peak at 385nm, indicating that the sample has ultraviolet afterglow emission characteristics;

[0048] Figure 7 Given is the afterglow decay spectrum of Cs2NaScCl6:0.03Pb after 5 minutes of pre-charging under 254nm irradiation. The monitoring wavelength is 385nm. It can be seen that after 60 minutes of decay, the afterglow signal is still higher than the background noise, indicating that the ultraviolet afterglow decay time of the sample is greater than 1h.

[0049] Example 2: Cs2NaScCl6:0.005Pb sample

[0050] The preparation method of the present invention is as follows: 1 mmol Cs2CO3 (0.3258 g) powder, 0.5 mmol Na2CO3 (0.0530 g) powder, 0.5 mmol Sc2O3 (0.0690 g) powder and 0.005 mmol PbO (0.0011 g) powder are weighed into a polytetrafluoroethylene liner, 12 mL of concentrated hydrochloric acid (36 wt%) is added, the mixture is put into a reaction kettle, the mixture is kept at 180° C. for 6 hours, the mixture is naturally cooled to room temperature, the obtained product is washed with ethanol 3 times, and the mixture is dried at 60° C. for about 3 hours to obtain the final product.

[0051] Test conditions: the same as in Example 1.

[0052] Experimental results: Figure 8 The XRD spectrum of Cs2NaScCl6:0.005Pb is given. It can be seen that a crystalline powder product has been obtained through this experimental scheme;

[0053] Fig. 9 The afterglow emission spectrum of Cs2NaScCl6:0.005Pb is given, with the emission peak at 380nm;

[0054] Fig.10 Given is the afterglow decay spectrum of Cs2NaScCl6:0.005Pb after 5 minutes of pre-charging at 254nm, with the monitoring wavelength being 380nm.

[0055] Example 3: Cs2NaScCl6:0.1Pb sample

[0056] The preparation method of the present invention is as follows: 2 mmol CsCl (0.3367 g) powder, 1 mmol NaCl (0.0584 g) powder, 0.5 mmol Sc2O3 (0.0690 g) powder and 0.1 mmol PbCl2 (0.0278 g) powder are weighed into a polytetrafluoroethylene liner, 8 mL of concentrated hydrochloric acid (36 wt%) is added, the mixture is loaded into a reaction kettle, the mixture is kept at 150° C. for 3 hours, the mixture is naturally cooled to room temperature, the obtained product is washed with ethanol 3 times, and the mixture is dried at 80° C. for about 1 hour to obtain the final product.

[0057] Test conditions: the same as in Example 1.

[0058] Experimental results: Fig.11 The XRD spectrum of Cs2NaScCl6:0.1Pb is given, and it can be seen that a crystalline product has been obtained through this experimental scheme;

[0059] Fig.12 The afterglow emission spectrum of Cs2NaScCl6:0.1Pb is given, with the emission peak at 390nm;

[0060] Fig.13 Given is the afterglow decay spectrum of Cs2NaScCl6:0.1Pb after 5 minutes of pre-charging at 254nm, with the monitoring wavelength being 390nm.

[0061] Fig.14 This is a comparison chart of the afterglow decay of Cs2NaScCl6:0.005Pb, Cs2NaScCl6:0.03Pb and Cs2NaScCl6:0.1Pb obtained in Examples 1-3. The sample doped with 0.03Pb has stronger afterglow intensity and longer decay time.

[0062] Example 4: Cs2NaScCl6:xPb (x=0.005, 0.01, 0.03, 0.05, 0.07, 0.1) samples

[0063] The preparation method of the present invention is as follows: 2 mmol CsCl (0.3367 g) powder, 1 mmol NaCl (0.0584 g) powder, 1 mmol ScCl3 (0.1468 g) powder and x mmol PbCl2 (0.28711*x g) powder are weighed into a polytetrafluoroethylene liner, 12 mL of concentrated hydrochloric acid (38 wt%) is added, the mixture is loaded into a reaction kettle, the mixture is kept warm at 180° C. for 3 hours, the mixture is naturally cooled to room temperature, the obtained product is washed with ethanol 3 times, and the mixture is dried at 70° C. for about 3 hours to obtain the final product.

[0064] Test conditions: the same as in Example 1.

[0065] Experimental results: Fig.15 Given is a graph showing the dependence of the afterglow intensity of Cs2NaScCl6:xPb (x=0.005, 0.01, 0.03, 0.05, 0.07, 0.1) on the Pb doping concentration 60s after turning off the 254nm charging light source. It can be seen that the sample has better ultraviolet afterglow performance when doped with 0.03Pb.

[0066] Matters not covered by the present invention are known technologies.

Claims

1. A chloride ultraviolet afterglow material, characterized by The structural formula of the material is Cs2NaScCl6:xPb, 0.005≤x≤0.

1.

2. The chloride ultraviolet afterglow material as claimed in claim 1, characterized in that the material generates ultraviolet afterglow emission with a peak position near 385nm after being irradiated with 254nm deep ultraviolet light for 5 minutes.

3. The method for preparing the chloride ultraviolet afterglow material according to claim 1, characterized in that the method comprises the following steps: (1) weighing and mixing a Cs-containing compound, a Na-containing compound, a Sc-containing compound, and a Pb-containing compound in a reaction kettle lined with polytetrafluoroethylene; in, The Cs-containing compound is a chloride or carbonate of Cs; the Na-containing compound is a chloride or carbonate of Na; the Sc-containing compound is a chloride or oxide of Sc; the Pb-containing compound is a chloride or oxide of Pb; The ratio of the above salts is based on the corresponding amount of substance in Cs2NaScCl6:xPb, that is, Cs:Na:Sc:Pb=2:1:1:x; 0.005≤x≤0.1; (2) Add concentrated hydrochloric acid to the reaction kettle; add 4-12 mL of concentrated hydrochloric acid for every 2 mmol of CsCl; (3) Seal the reactor and heat it at 150-200 ℃ Keep warm for 3-12 hours, and then cool naturally to room temperature; (4) washing the crystal product with anhydrous ethanol; (5) Dry the product at 40-80°C for about 1-5 hours to obtain a powdery target product.

4. The method for preparing a chloride ultraviolet afterglow material as claimed in claim 4, wherein the concentration of the concentrated hydrochloric acid is 30-38wt%.

Citation Information

Patent Citations

  • Perovskite X-ray scintillator and preparation method thereof

    CN113060762A

  • Method for batch preparation of lead-free perovskite luminescent material at room temperature

    CN115873597A

  • White light long afterglow fluorescent powder and preparation method thereof

    CN118064138A

Cited By

  • Multi-emission double-perovskite fluorescent powder with multifunctional application and preparation method of multi-emission double-perovskite fluorescent powder

    CN120843099A

  • A multi-emission double perovskite phosphor for multi-functional applications and its preparation method

    CN120843099B