High-temperature-resistant ultrahigh-strength aviation fastener and production process thereof

By adding rare earth zirconium elements to nickel-cobalt-based high-temperature alloys and adopting specific heat treatment and cold drawing processes, the strength and high-temperature durability of high-temperature alloy fasteners are improved, and the performance of existing fasteners in high-temperature environments is solved. The problem of insufficient results enables efficient high temperature and ultra-high performance.

CN119061304APending Publication Date: 2024-12-03HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114163.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The strength and high-temperature durability of existing high-temperature alloy fasteners cannot meet the needs of aerospace and other fields, especially in high-temperature environments that cannot meet the requirements for long-term use.

Method used

Using nickel-cobalt-molybdenum-based high-temperature alloy and adding trace amounts of rare earth zirconium elements, the high-temperature strength and life of the alloy are improved through alloy strip heat treatment, cold drawing, round material heat treatment and hot upsetting processes. The specific steps include heating, insulation, cold drawing and localization. Induction heating, etc.

Benefits of technology

The tensile strength of the fastener reaches 1810~1820MPa, the HRC hardness is 44~46, the elongation after break is 7~8%, and the high temperature of 650℃ is 24~26 hours, meeting the high temperature in the aerospace field. Super high demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant ultrahigh-strength aviation fastener and a production process thereof. The fastener comprises the following chemical components in percentage by weight: 0.01%-0.04% of carbon, 18%-20% of chromium, 24%-27% of nickel, 6%-8% of molybdenum, 2.5%-3.2% of titanium, 0.1%-0.3% of aluminum, 0.3%-0.7% of niobium, 0.01%-0.03% of boron, 0.003%-0.008% of zirconium and the balance of cobalt and inevitable impurities. The production process comprises the steps of alloy wire rod heat treatment, cold drawing, round stock heat treatment and hot upsetting. The fastener provided by the process not only has strength and hardness which are not possessed by a common fastener, but also has good processing plasticity and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature alloy fasteners, and in particular relates to a high-temperature resistant ultra-high-strength aviation fastener and a production process thereof. Background Art

[0002] High-temperature alloy fasteners are mainly used in defense fields such as aerospace, nuclear power, etc. Among them, aviation fasteners, as key components for internal connections in aircraft engine combustion chambers, require not only a certain strength, but also a certain high-temperature durability.

[0003] With the continuous development and iteration of aviation engine technology, my country's demand for various types of high-temperature resistant and ultra-high-strength fasteners is increasing, and the performance, especially the strength, of existing fasteners can no longer meet the demand. Therefore, it is imperative to promote the high-end upgrading of domestic fastener products and adjust the industrial structure. Summary of the invention

[0004] The object of the present invention is to provide a high temperature resistant ultra-high strength aviation fastener and a production process thereof, wherein the fastener has a tensile strength of 1810-1820 MPa, an HRC hardness of 44-46, an elongation after fracture of 7-8%, and a high temperature durability of 650°C of 24-26 hours.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A high-temperature resistant ultra-high-strength aviation fastener, whose chemical composition and weight percentage are: carbon 0.01%-0.04%, chromium 18%-20%, nickel 24%-27%, molybdenum 6%-8%, titanium 2.5%-3.2%, aluminum 0.1%-0.3%, niobium 0.3%-0.7%, boron 0.01%-0.03%, zirconium 0.003%-0.008%, and the rest is cobalt and unavoidable impurities.

[0006] Furthermore, the size of the high temperature resistant and ultra-high strength aviation fastener of the present invention is φ8 to φ20 mm.

[0007] The production process of the high temperature resistant ultra-high strength aviation fasteners of the present invention includes heat treatment of alloy wire rods, cold drawing, heat treatment of round materials, and hot upsetting; the details are as follows: (1) heating an alloy wire rod to 1040-1060° C., keeping the temperature for 4-8 hours, and then air cooling to room temperature; the chemical composition and weight percentage of the alloy wire rod are: carbon 0.01%-0.04%, chromium 18%-20%, nickel 24%-27%, molybdenum 6%-8%, titanium 2.5%-3.2%, aluminum 0.1%-0.3%, niobium 0.3%-0.7%, boron 0.01%-0.03%, zirconium 0.003%-0.008%, and the remainder is cobalt and unavoidable impurities; (2) cold drawing the alloy wire rod heat treated in step (1) into a round material, then keeping the temperature at 540-600°C for 1-2 hours, raising the temperature to 650-670°C at a rate of 1-5°C / min, keeping the temperature for 4-5 hours, and then taking the material out of the furnace and air cooling it to room temperature; (3) The heat-treated round material is hot-forged into a semi-finished product, which is then ground and threaded in sequence to obtain the product.

[0008] Furthermore, in the production process of the present invention, the area reduction rate of the cold drawing in step (2) is 45-53%.

[0009] Furthermore, in the production process of the present invention, the heating method for hot upsetting the round material in step (3) is local induction heating, the heating temperature is 1130-1180° C., and the insulation time is 0.5-1.5 h.

[0010] The inventive principle of the technical solution of the present invention is that: on the basis of the nickel-cobalt-molybdenum-based high-temperature alloy composition, a trace amount of rare earth zirconium element is added to refine the grains, thereby improving the high-temperature strength of the alloy; the strength of the alloy is improved through a reasonable cold drawing hardening process; and through a subsequent two-stage heat treatment, the strength and life of the final fastener are further slowly improved.

[0011] The beneficial effect of adopting the above technical solution is that the fastener provided by the present invention not only has the strength and hardness that ordinary fasteners do not have, but also has good processing plasticity and service life; the tensile strength of the fastener is 1810~1820MPa, the HRC hardness is 44~46, the elongation after fracture is 7~8%, and the high temperature durability at 650℃ is 24~26h. DETAILED DESCRIPTION

[0012] The present invention will be further described below in conjunction with specific embodiments: Example 1

[0013] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.03%, chromium 19%, nickel 25%, molybdenum 7%, titanium 3%, aluminum 0.2%, niobium 0.3%, boron 0.03%, zirconium 0.004%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) heating the alloy wire rod to 1040°C, keeping the temperature for 8 hours, and then air cooling to room temperature; (2) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ10 mm after 50% surface shrinkage deformation; the round material at room temperature is kept at 580°C for 1 hour, then heated to 650°C at a rate of 3°C / min, kept for 4 hours, and then taken out of the furnace and air-cooled to room temperature; (3) The heat-treated round material is subjected to local induction heating at 1150°C for 1 hour, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ10 mm.

[0014] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 2

[0015] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.02%, chromium 18.5%, nickel 25.5%, molybdenum 6.5%, titanium 3.1%, aluminum 0.1%, niobium 0.4%, boron 0.02%, zirconium 0.005%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) heating the alloy wire rod to 1050°C, keeping the temperature for 6 hours, and then air cooling to room temperature; (2) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ15 mm after 52% surface shrinkage deformation; the round material at room temperature is kept at 540°C for 2 hours, then raised to 660°C at a rate of 2°C / min, kept for 4.5 hours, and then taken out of the furnace and air-cooled to room temperature; (3) The heat-treated round material is subjected to local induction heating at 1160°C for 1.5 hours, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ15 mm.

[0016] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 3

[0017] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.02%, chromium 18%, nickel 24%, molybdenum 8%, titanium 2.8%, aluminum 0.2%, niobium 0.5%, boron 0.02%, zirconium 0.005%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) heating the alloy wire rod to 1060°C, keeping the temperature for 5 hours, and then air cooling to room temperature; (2) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ18 mm after 48% surface shrinkage deformation; the round material at room temperature is kept at 590°C for 1.5 hours, then heated to 670°C at a rate of 2°C / min, kept for 4.5 hours, and then taken out of the furnace and air-cooled to room temperature; (4) The heat-treated round material is subjected to local induction heating at 1130°C for 0.5h, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ18mm.

[0018] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 4

[0019] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.04%, chromium 20%, nickel 27%, molybdenum 8%, titanium 3.2%, aluminum 0.3%, niobium 0.7%, boron 0.03%, zirconium 0.008%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) The alloy wire rod is heated to 1045°C, kept at this temperature for 4.5 hours, and then air-cooled to room temperature; (2) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ8 mm after 52% surface shrinkage deformation; the round material at room temperature is kept at 560°C for 1.5 hours, then heated to 655°C at a rate of 2°C / min, kept for 4.5 hours, and then taken out of the furnace and air-cooled to room temperature; (3) The heat-treated round material is subjected to local induction heating at 1170°C for 0.8h, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ8mm.

[0020] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 5

[0021] A high-temperature resistant ultra-high-strength aviation fastener, whose production process includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.01%, chromium 18.5%, nickel 26.5%, molybdenum 7.5%, titanium 2.8%, aluminum 0.25%, niobium 0.35%, boron 0.02%, zirconium 0.003%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) The alloy wire rod is heated to 1055°C, kept at this temperature for 7.5 hours, and then air-cooled to room temperature; (3) The heat-treated alloy wire rod is cold-drawn with a surface shrinkage deformation of 47% to form a cold-drawn round material with a diameter of φ13 mm; the round material at room temperature is kept at 575°C for 1 hour, then heated to 655°C at a rate of 5°C / min, kept for 4 hours, and then taken out of the furnace and air-cooled to room temperature; (4) The heat-treated round material is subjected to local induction heating at 1160°C for 1.5 hours, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ13 mm.

[0022] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 6

[0023] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.02%, chromium 18.5%, nickel 24.5%, molybdenum 6%, titanium 2.9%, aluminum 0.1%, niobium 0.45%, boron 0.03%, zirconium 0.008%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) heating the alloy wire rod to 1060°C, keeping the temperature for 4 hours, and then air cooling to room temperature; (2) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ9 mm after 53% surface shrinkage deformation, and then the round material at room temperature is kept at 580°C for 1 hour, and then raised to 670°C at a rate of 4°C / min, kept for 4 hours, and then taken out of the furnace and air-cooled to room temperature; (4) The heat-treated round material is subjected to local induction heating at 1180°C for 1 hour, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ9 mm.

[0024] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 7

[0025] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.04%, chromium 19%, nickel 25%, molybdenum 6.5%, titanium 2.5%, aluminum 0.15%, niobium 0.65%, boron 0.01%, zirconium 0.007%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) The alloy wire rod is heated to 1055°C, kept at this temperature for 7.5 hours, and then air-cooled to room temperature; (3) The heat-treated alloy wire rod is cold-drawn with a surface shrinkage deformation of 45% to form a cold-drawn round material with a diameter of φ20 mm; the round material at room temperature is kept at 600°C for 1.5 hours, then raised to 665°C at a rate of 2°C / min, kept for 5 hours, and then taken out of the furnace and air-cooled to room temperature; (4) The heat-treated round material is subjected to local induction heating at 1140°C for 1.5 hours, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ20 mm.

[0026] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1. Example 8

[0027] A high temperature resistant ultra-high strength aviation fastener, the production process of which includes: alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting, etc.; the chemical composition of the alloy wire rod is: carbon 0.02%, chromium 18.5%, nickel 25.5%, molybdenum 7.5%, titanium 2.6%, aluminum 0.25%, niobium 0.45%, boron 0.02%, zirconium 0.006%, and the rest is cobalt and unavoidable impurities; the specific production process is as follows: (1) heating the alloy wire rod to 1045°C, keeping the temperature for 5.5 hours, and then air cooling to room temperature; (3) The heat-treated alloy wire rod is cold-drawn into a cold-drawn round material with a diameter of φ16 mm through a 51% surface shrinkage deformation; the round material at room temperature is kept at 580°C for 1 hour, then heated to 655°C at a rate of 1°C / min, kept for 4.5 hours, and then taken out of the furnace and air-cooled to room temperature; (4) The heat-treated round material is subjected to local induction heating at 1170°C for 1.5 hours, hot-forged into a semi-finished product, and then surface ground to remove oxide scale, and threaded on a thread rolling machine to obtain a finished fastener with a specification of φ16 mm.

[0028] The mechanical properties of the high temperature resistant ultra-high strength aviation fastener of this embodiment are shown in Table 1.

[0029] Table 1 Mechanical properties of high temperature resistant ultra-high strength aviation fasteners of various embodiments

[0030] The fastener of the present invention has a tensile strength of 1810-1820 MPa, an HRC hardness of 44-46, an elongation after fracture of 7-8%, and a high-temperature durability of 650° C. of 24-26 hours, thus meeting the demand for improving the performance of existing fasteners.

Claims

1. A high temperature resistant ultra-high strength aviation fastener, characterized in that: The chemical composition of the fastener and its weight percentage are: carbon 0.01%-0.04%, chromium 18%-20%, nickel 24%-27%, molybdenum 6%-8%, titanium 2.5%-3.2%, aluminum 0.1%-0.3%, niobium 0.3%-0.7%, boron 0.01%-0.03%, zirconium 0.003%-0.008%, and the rest is cobalt and unavoidable impurities.

2. A high temperature resistant ultra-high strength aviation fastener according to claim 1, characterized in that: The fastener has a tensile strength of 1810-1820 MPa, an HRC hardness of 44-46, an elongation after fracture of 7-8%, and a high-temperature durability of 650° C. of 24-26 hours.

3. The high temperature resistant and ultra-high strength aviation fastener according to claim 1, characterized in that: The size of the fastener is φ8~φ20mm.

4. A production process for high temperature resistant ultra-high strength aviation fasteners, characterized in that: Including alloy wire rod heat treatment, cold drawing, round material heat treatment, hot upsetting; the details are as follows: (1) heating an alloy wire rod to 1040-1060° C., keeping the temperature for 4-8 hours, and then air cooling to room temperature; the chemical composition and weight percentage of the alloy wire rod are: carbon 0.01%-0.04%, chromium 18%-20%, nickel 24%-27%, molybdenum 6%-8%, titanium 2.5%-3.2%, aluminum 0.1%-0.3%, niobium 0.3%-0.7%, boron 0.01%-0.03%, zirconium 0.003%-0.008%, and the remainder is cobalt and unavoidable impurities; (2) Cold drawing the heat-treated alloy wire rod into a cold-drawn round material; keeping the round material at room temperature at 540-600°C for 1-2 hours, then raising the temperature to 650-670°C at a rate of 1-5°C / min, keeping the temperature for 4-5 hours, and then taking it out of the furnace and air cooling it to room temperature; (3) The heat-treated round material is hot-forged into a semi-finished product, and then ground and threaded in sequence to obtain the product.

5. The production process of a high temperature resistant ultra-high strength aviation fastener according to claim 4, characterized in that: The surface reduction rate of the cold drawing in step (2) is 45-53%.

6. The production process of a high temperature resistant ultra-high strength aviation fastener according to claim 1, characterized in that: The heating method for hot upsetting the round material in step (3) is local induction heating, the heating temperature is 1130-1180°C, and the insulation time is 0.5-1.5h.