Polyamine modified lignin / kapok fiber and preparation method thereof
Through the preparation method of polyamine-modified lignin/kapop fiber, polyamine modifiers are prepared by reacting amine compounds with methyl acrylate, which solves the problem of low dyeing rate of kapok fibers and achieves dye adhesion rate of more than 80% , suitable for the development of the clothing field.
Patent Information
- Application Number
- CN202310644365.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
The development and utilization of kapok fibers in the field of clothing are limited by the problem of low dyeing rate.
Polyamine modifiers are used to prepare polyamine modifiers by reacting amine compounds with methyl acrylate, and combined with lignin/kapop fibers, adjust the pH value and temperature to react to improve their adhesion rate with dyes.
The dyeing rate of kapok fiber is significantly improved, making its dye adhesion rate higher than 80%, and is suitable for the development and utilization of the clothing field.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer composite materials, and in particular relates to a polyamine-modified lignin / kapok fiber and a preparation method thereof. Background Art
[0002] Kapok is a natural plant fiber, mainly composed of cellulose, lignin, hemicellulose, etc. Its fiber length is about 5-35 mm, its diameter distribution is about 20-45 μm, its appearance is rod-shaped, the surface is covered with a layer of wax, the surface is smooth, and it has a unique thin-walled large hollow structure, with a hollow rate of more than 80%. Kapok fiber has the characteristics of light weight, warmth retention, antibacterial, strong moisture absorption but poor water absorption. After processing, it can be used as bedding filling, life jacket filling, blended fiber, etc. Although kapok fiber has outstanding performance, it has a low dyeing rate. This defect seriously limits the development and utilization of kapok fiber in the field of clothing. Summary of the invention
[0003] In order to overcome the defects of the prior art, the present invention provides a polyamine-modified lignin / kapok fiber and a preparation method thereof, which can significantly improve the dyeing rate of kapok fiber in the printing and dyeing process.
[0004] The purpose of the present invention can be achieved through the following technical solutions.
[0005] A polyamine modified lignin / kapok fiber and a preparation method thereof, characterized in that the raw materials of the polyamine modifier are amine compounds and methyl acrylate, and the molar ratio of the amine compounds to methyl acrylate is 1: (0.1-0.3).
[0006] The amine compound is one or more of ethylenediamine, diethylenetriamine and tetraethylenepentamine.
[0007] A polyamine-modified lignin / kapok fiber and a preparation method thereof, characterized in that the preparation of the polyamine modifier comprises the following steps: dissolving an amine compound in methanol, adjusting the pH value of the system to 7, heating the system to 60-80°C, then dripping methyl acrylate therein, keeping the temperature in a water bath for 2-4 hours, and drying to obtain the polyamine modifier.
[0008] The dropping time of the methyl acrylate is 30 to 45 minutes.
[0009] A polyamine-modified lignin / kapok fiber and a preparation method thereof, characterized in that the preparation method of lignin / kapok fiber comprises the following steps: dispersing kapok fiber and sodium sulfide in distilled water, wherein the mass ratio of kapok fiber to sodium sulfide is 1:(0.01-0.05), adjusting the pH value to 10-12, and reacting in a water bath at 85-95°C for 0.5-2 h. Subsequently, the kapok fiber is filtered and washed with clean water to obtain lignin / kapok fiber.
[0010] A polyamine-modified lignin / kapok fiber and a preparation method thereof, characterized in that a polyamine modifier and lignin / kapok fiber are dispersed in deionized water in a mass ratio of 1:(5-8), epichlorohydrin is added, and the polyamine-modified lignin / kapok fiber is obtained by filtering and drying after reacting in a water bath at 70°C for 1 hour. The polyamine-modified lignin / kapok fiber is dyed.
[0011] The concentration of epichlorohydrin added is 1-5 wt%.
[0012] Compared with the prior art, the present invention can improve the dyeing rate of reactive dyes on kapok fibers. The dyeing rate of the modified kapok fibers prepared by the present invention can be higher than 80%, making the kapok fibers more suitable for development and utilization in the field of clothing. Implementation
[0013] The present invention is described in detail below with reference to specific embodiments. Example 1
[0014] Diethylenetriamine and methyl acrylate were added to methanol in a molar ratio of 1:0.1, the pH value of the system was adjusted to 7, the temperature was raised to 60°C, the reaction was kept in a water bath for 2 hours, and the polyamine modifier was obtained by drying. The methyl acrylate was added dropwise gradually for 30 minutes.
[0015] Kapok fiber and sodium sulfide were dispersed in distilled water, the mass ratio of kapok fiber to sodium sulfide was 1:0.01, the pH value was adjusted to 10, and the reaction was carried out in a water bath at 85 °C for 0.5 h. The kapok fiber was filtered and washed with clean water to obtain lignin / kapok fiber.
[0016] The polyamine modifier and lignin / kapok fiber were dispersed in deionized water at a mass ratio of 1:5, and epichlorohydrin was added. After reacting in a water bath at 70°C for 1 h, the polyamine modified lignin / kapok fiber was filtered and dried. The concentration of the added epichlorohydrin was 1 wt%.
[0017] The polyamine modified lignin / kapok fiber was immersed in 1% (owf) Cibacloren FN-R blue, and the immersion time was controlled to be 15 min. Then sodium chloride was added, and its concentration was controlled to be 40 g / L. The immersion continued for 15 min. Then soda ash was added, and the concentration of soda ash was 10 g / L. The immersion continued for 20 min. The kapok fiber was taken out, and the dye uptake was determined to be 80% by the residual liquid concentration method. Example 2
[0018] Tetraethylenepentamine and methyl acrylate were added to methanol in a molar ratio of 1:0.3, the pH value of the system was adjusted to 7, the temperature was raised to 80°C, the reaction was carried out in a water bath for 4 hours, and the polyamine modifier was obtained by drying. The methyl acrylate was added dropwise gradually for 45 minutes.
[0019] Kapok fiber and sodium sulfide were dispersed in distilled water, the mass ratio of kapok fiber to sodium sulfide was 1:0.05, the pH value was adjusted to 12, and the reaction was carried out in a water bath at 90 °C for 2 h. The kapok fiber was filtered and washed with clean water to obtain lignin / kapok fiber.
[0020] The polyamine modifier and lignin / kapok fiber were dispersed in deionized water at a mass ratio of 1:8, and epichlorohydrin was added. After reacting in a water bath at 70°C for 1 h, the polyamine modified lignin / kapok fiber was filtered and dried. The concentration of the added epichlorohydrin was 5 wt%.
[0021] The polyamine modified lignin / kapok fiber was immersed in 1% (owf) of Cibacloren FN-R blue, and the immersion time was controlled to be 15 min. Then sodium chloride was added, and its concentration was controlled to be 40 g / L. The immersion continued for 15 min. Then soda ash was added, and the concentration of soda ash was 10 g / L. The immersion continued for 20 min. The kapok fiber was taken out, and the dye uptake was determined to be 87% by the residual liquid concentration method. Example 3
[0022] Tetraethylenepentamine and methyl acrylate were added to methanol in a molar ratio of 1:0.2, the pH value of the system was adjusted to 7, the temperature was raised to 70°C, the reaction was carried out in a water bath for 4 hours, and the polyamine modifier was obtained by drying. The methyl acrylate was added dropwise gradually for 40 minutes.
[0023] Kapok fiber and sodium sulfide were dispersed in distilled water, the mass ratio of kapok fiber to sodium sulfide was 1:0.03, the pH value was adjusted to 11, and the reaction was carried out in a water bath at 90 °C for 1 h. The kapok fiber was filtered and washed with clean water to obtain lignin / kapok fiber.
[0024] The polyamine modifier and lignin / kapok fiber were dispersed in deionized water at a mass ratio of 1:6, and epichlorohydrin was added. After reacting in a water bath at 70°C for 1 hour, the polyamine modified lignin / kapok fiber was filtered and dried. The concentration of the added epichlorohydrin was 3 wt%.
[0025] The polyamine modified lignin / kapok fiber was immersed in 1% (owf) Cibacloren FN-R blue, and the immersion time was controlled to be 15 min. Then sodium chloride was added, and its concentration was controlled to be 40 g / L. The immersion continued for 15 min. Then soda ash was added, and the concentration of soda ash was 10 g / L. The immersion continued for 20 min. The kapok fiber was taken out, and the dye uptake was determined by the residual liquid concentration method to be 86%.
Claims
1. A polyamine-modified lignin / kapok fiber and a preparation method thereof, It is characterized in that The preparation of the polyamine modifier includes the following steps: dissolving an amine compound in methanol, adjusting the pH value of the system to 7, heating the system to 60-80°C, then dropping methyl acrylate therein, keeping the temperature in a water bath for 2-4 hours, and drying to obtain the polyamine modifier.
2. A polyamine-modified lignin / kapok fiber and a preparation method thereof according to claim 1, It is characterized in that The raw materials of the polyamine modifier are amine compounds and methyl acrylate, and the molar ratio of amine compounds to methyl acrylate is 1: (0.1-0.3). The amine compound is one or more of ethylenediamine, diethylenetriamine, and tetraethylenepentamine. The dripping time of the methyl acrylate is 30-45 min.
3. A polyamine-modified lignin / kapok fiber and a preparation method thereof, It is characterized in that The preparation method of lignin / kapok fiber comprises the following steps: dispersing kapok fiber and sodium sulfide in distilled water, adjusting the pH value to 10-12, reacting in a water bath for 0.5-2 h, filtering the kapok fiber and washing it with clean water to obtain lignin / kapok fiber.
4. A polyamine-modified lignin / kapok fiber and a preparation method thereof according to claim 3, It is characterized in that The mass ratio of kapok fiber to sodium sulfide is 1:(0.01~0.05), and the water bath reaction temperature is 85~95 ℃.
5. A polyamine-modified lignin / kapok fiber and a preparation method thereof, It is characterized in that The polyamine modifier and lignin / kapok fiber were dispersed in deionized water in a mass ratio of 1:(5-8), epichlorohydrin was added, and the mixture was reacted in a water bath at 70 °C for 1 h. The polyamine-modified lignin / kapok fiber was obtained by filtration and drying.
6. A polyamine-modified lignin / kapok fiber prepared by the preparation method according to any one of claims 1 to 5.