High-strength silk knife scraping cloth and processing method thereof
By introducing MOFs materials into polyurethane resin to form supramolecular crosslinking points, the problems of unenvironmental protection and poor aging resistance of traditional PVC knife scrapers are solved, and the tensile, wear and corrosion resistance of the knife scrapers are improved, and the tensile, wear and corrosion resistance of the knife scrapers are extended. It has a service life and is suitable for a variety of printer models and ink types, achieving high-strength, long-life knife scraping cloth.
Patent Information
- Application Number
- CN202411561979.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional PVC knife scraping cloth is not environmentally friendly, has poor aging resistance, poor printing effect, heavy weight, and low temperature resistance. It cannot adapt to a variety of printer models and ink types, and has a short service life.
MOFs materials are introduced into polyurethane resin, and supramolecular crosslinking points are formed through covalent bonds and multiple hydrogen bonds to form supramolecular polymer networks, improving the tensile, wear and corrosion resistance of the knife scraper, and using modified coating Combination structure of layer and surface layer.
It significantly improves the quality of the knife scraper, extends the service life, enhances tensile, wear and corrosion resistance, and is suitable for a variety of printer models and ink types, with excellent flame retardant performance.
Smart Images

Figure CN119061709A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of silk weaving technology, and in particular relates to a high-strength silk knife scraper cloth and a processing method thereof. Background Art
[0002] Traditional PVC scraper cloth is made of polyester filament. The specifications of the cloth are 500D×500D, 28s×28s and 1000D×1000D, 20s×20s. A layer of PVC resin paste with a thickness of about 0.08mm is applied on the front and back of the cloth by scraping. Then, it is put into an oven at 130-150℃. After the PVC resin paste melts, it is cooled and solidified into a film after it comes out of the oven, and then rolled.
[0003] PVC scraper cloth is used to make outdoor advertisements. Its advantages are: (1) Simple production process and low price. (2) PVC coating can be dissolved or swelled by solvents, so it can be used directly to print pictures and texts. However, it also has many disadvantages: (1) Not environmentally friendly. PVC will release hydrogen chloride above 60°C. (2) PVC has poor aging resistance. The nominal shelf life of outdoor advertisements made with PVC scraper cloth is two years, but the actual outdoor shelf life is only about one year. (3) Poor printing effect. The general resolution can only reach about 370dpi, and it can only be used for strong solvent models and strong solvent inks. It cannot be used for weak solvent, UV and other models and inks. The compatibility is poor. (4) Heavy weight. Since the specific gravity of PVC is 1.45, the scraper cloth produced is 510-560g per square meter, and each outdoor advertisement is about 50m² and weighs more than 25kg, resulting in poor performance in resisting bad weather. (5) Not resistant to low temperatures. Although PVC is added with anti-low temperature additives, it still becomes hard and brittle under climatic conditions of ≤-20℃, so it cannot be used in high-latitude areas.
[0004] Therefore, providing a new formula of scraper cloth and a processing method thereof to solve the above-mentioned defects is an urgent problem to be solved. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a high-strength wire scraper cloth and a processing method thereof. The present application introduces MOFs material into a polyurethane polymer, and utilizes the covalent bond between the two to connect the MOFs nanocrystals in series. At the same time, the introduced MOFs material synergizes with the multiple hydrogen bonds and polyrotaxanes present in the composite modified liquid to form supramolecular cross-linking points, thereby forming a supramolecular polymer network in the polyurethane system. Introducing the supramolecular polymer network structure into the preparation process of the scraper cloth can greatly improve the tensile resistance, wear resistance, corrosion resistance and other properties of the prepared scraper cloth, so that the prepared scraper cloth has excellent quality and long service life.
[0006] To achieve the above object, the present invention provides the following technical solutions: A high-strength wire scraper cloth, which comprises a base cloth layer, a modified coating layer and a surface layer from the inside to the outside; The modified coating comprises the following components in parts by mass: 200-250 parts of modified polyurethane resin, 5-10 parts of foaming agent, 8-15 parts of foam stabilizer, 0.2-3 parts of curing agent, and 0.1-0.5 parts of thickener.
[0007] Preferably, in the modified coating, the modified polyurethane resin is prepared by the following steps: S11. Mix 100-150 parts of polyurethane resin and 30-80 parts of dioxane by mass, stir, dissolve, add 10-50 parts of MOFs material, mix, heat to 50-100 ° C and stir for 1-2h, stop heating, cool, and obtain a preliminary modified polyurethane resin; S12. Mix 100-150 parts of the preliminarily modified polyurethane resin with 50-60 parts of dimethyl sulfoxide by mass, stir, add 20-30 parts of the modifying liquid, heat to 60-80°C and stir for 20-30h, stop heating, cool, add 10-15 parts of adamantane amine, mix and stir for 20-30min, and obtain the modified polyurethane resin.
[0008] Preferably, the MOFs material is ZIF-8.
[0009] Preferably, the modified liquid comprises the following components in parts by mass: 30-40 parts of cyclodextrin, 20-30 parts of dimer fatty acid, 10-15 parts of ethylenediamine, 15-20 parts of p-tolylsulfonyl isocyanate, 3-5 parts of ethylene glycol, 4-8 parts of glycerol, and 5-10 parts of trimethylolpropane.
[0010] Preferably, the curing agent is a water-based isocyanate curing agent; and the thickener is an alkali-swellable acrylic thickener.
[0011] Preferably, the foaming agent is one or more of azobisisobutyronitrile and azodicarbonamide; the foam stabilizing agent is one or more of dodecyldimethylamine oxide and sodium dodecyl sulfate.
[0012] Preferably, the base fabric layer is a biaxial warp knitted base fabric.
[0013] Preferably, the surface layer comprises the following components in parts by mass: 3-4 parts of butanone, 1-5 parts of toluene, and 10-15 parts of polyethylene; and the thickness of the surface layer is 0.15-0.25 mm.
[0014] A method for processing a high-strength wire scraper cloth, used for preparing the high-strength wire scraper cloth, comprises the following steps: S1. Ingredients: weigh the components in proportion and prepare the slurry of the modified coating and surface layer; S2. Scraping the modified coating: unwind the biaxial warp knitted base fabric, heat the slurry of the modified coating to 160-170°C, apply sizing to both sides of the biaxial warp knitted base fabric with a scraper, cool it so that both sides of the base fabric layer are bonded with the modified coating, and keep it at 180°C-200°C. The thickness of the modified coating is 0.5-0.8mm; S3. Surface coating: prepare the surface layer slurry in proportion, apply the surface layer slurry on the surface of the double-sided modified coating to obtain the high-strength wire knife scraping cloth.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present application introduces MOFs material into polyurethane polymer, utilizes the covalent bond action of the two to connect MOFs nanocrystals in series, and at the same time, the introduced MOFs material synergizes with the multiple hydrogen bonds and polyrotaxanes present in the composite modified liquid to form supramolecular cross-linking points, thereby forming a supramolecular polymer network in the polyurethane system. Introducing the supramolecular polymer network structure into the preparation process of the scraper cloth can greatly improve the tensile resistance, wear resistance, corrosion resistance and other properties of the prepared scraper cloth, so that the prepared scraper cloth has excellent quality and long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a process flow chart for preparing the high-strength wire scraper cloth of the present invention; Figure 2 This is a process flow chart for preparing the modified polyurethane resin of the present invention; Figure 3 This is a product rendering of the high-strength wire knife scraper cloth described in the present invention. DETAILED DESCRIPTION
[0017] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] See also Figure 1-Figure 3 , the present invention provides a technical solution: Embodiment 1: A method for processing a high-strength wire knife scraper cloth: S1. Ingredients: weigh the components in proportion and prepare the slurry of the modified coating and surface layer; S2. Scraping of modified coating: unwind the biaxial warp knitted base fabric, heat the slurry of the modified coating to 160°C, apply sizing to both sides of the biaxial warp knitted base fabric with a scraper, cool, so that both sides of the base fabric layer are bonded with the modified coating, keep warm at 180°C, the thickness of the modified coating is 0.5mm; S3. Surface coating: prepare the surface layer slurry in proportion, apply the surface layer slurry on the surface of the double-sided modified coating with a thickness of 0.15 mm, and obtain the high-strength wire knife scraper cloth.
[0019] In the above process, the modified coating comprises the following components: Components <![CDATA[Dosage (kg / m 3 ).]]> Modified polyurethane resin 20 Foaming agent 0.5 Foam stabilizer 0.8 Curing agent 0.02 Thickener 0.01 The modified polyurethane resin is prepared by the following preparation method: S11. 10 kg of polyurethane resin was mixed with 3 kg of dioxane, stirred, dissolved, and then 1 kg of ZIF-8 material was added and mixed, heated to 50 ° C and stirred for 2 h, the heating was stopped, and the polyurethane resin was initially modified; S12. 10 kg of the initially modified polyurethane resin was mixed with 5 kg of dimethyl sulfoxide, stirred, and then 2 kg of the modified solution was added, the temperature was raised to 60 ° C and stirred for 30 h, the heating was stopped, cooled, 1 kg of adamantane amine was added, and the mixture was mixed and stirred for 30 min to obtain the modified polyurethane resin; The polyurethane resin is of grade UW-2001D and was purchased from UBE Co., Ltd. The modified liquid comprises the following components: Components <![CDATA[Dosage (kg / m 3 ).]]> Cyclodextrin 3 Dimerized fatty acid 2 Ethylenediamine 1 p-Toluenesulfonyl isocyanate 1.5 Ethylene glycol 0.3 glycerin 0.4 Trimethylolpropane 0.5 The thickener is an alkali-swellable acrylic thickener, specifically RHEOTECH 3800; The curing agent is a water-based isocyanate curing agent, specifically Bayhydur XP 2655; The foaming agent is azodicarbonamide; The foam stabilizer is sodium lauryl sulfate; The surface layer slurry comprises the following components: Components <![CDATA[Dosage (kg / m 3 ).]]> Butanone 0.3 Toluene 0.1 Polyethylene 1 Example 2: Example 2 is different from Example 1 in that, in Example 2, the modified coating comprises the following components: Components <![CDATA[Dosage (kg / m 3 ).]]> Modified polyurethane resin 25 Foaming agent 1 Foam stabilizer 1.5 Curing agent 0.3 Thickener 0.05 The remaining steps are exactly the same in Example 2 and Example 1.
[0020] Embodiment 3: Embodiment 3 is different from Embodiment 1 in that, in Embodiment 3, the modified liquid comprises the following components: Components <![CDATA[Dosage (kg / m 3 )]]> Cyclodextrin 4 Dimerized fatty acid 3 Ethylenediamine 1.5 p-Toluenesulfonyl isocyanate 2 Ethylene glycol 0.5 glycerin 0.8 Trimethylolpropane 1 The remaining steps are exactly the same in Example 3 and Example 1.
[0021] Example 4: Example 4 is different from Example 1 in that, in Example 4, the modified polyurethane resin is prepared by the following preparation method: S11. 15 kg of polyurethane resin was mixed with 8 kg of dioxane, stirred, dissolved, and then 5 kg of ZIF-8 material was added and mixed, heated to 100 ° C and stirred for 1 h, the heating was stopped, and the polyurethane resin was initially modified; S12. 15 kg of the initially modified polyurethane resin was mixed with 6 kg of dimethyl sulfoxide, stirred, and then 3 kg of the modified solution was added, the temperature was raised to 80 ° C and stirred for 25 h, the heating was stopped, cooled, 1.5 kg of adamantane amine was added, and the mixture was mixed and stirred for 30 min to obtain the modified polyurethane resin; The remaining steps are exactly the same in Example 4 and Example 1.
[0022] Example 5: Example 5 is different from Example 1 in that, in Example 5, the modified polyurethane resin is prepared by the following preparation method: S11. 13 kg of polyurethane resin was mixed with 5 kg of dioxane, stirred, dissolved, and then 3 kg of ZIF-8 material was added and mixed, heated to 100 ° C and stirred for 1 h, the heating was stopped, and the polyurethane resin was initially modified; S12. 13kg of the initially modified polyurethane resin was mixed with 6kg of dimethyl sulfoxide, stirred, and then 2.5kg of the modified solution was added, the temperature was raised to 80 ° C and stirred for 25h, the heating was stopped, cooled, 1.25kg of adamantane amine was added, and the mixture was mixed and stirred for 30min to obtain the modified polyurethane resin; The remaining steps are exactly the same in Example 5 and Example 1.
[0023] Comparative Example Comparative Example 1: Comparative Example 1 is different from Example 1 in that the preparation method of the modified polyurethane resin in Example 1 is omitted in Comparative Example 1, thereby omitting the step of "mixing 10 kg of the initially modified polyurethane resin with 5 kg of dimethyl sulfoxide, stirring, adding 2 kg of the modifying liquid, heating to 60° C. and stirring for 30 h, stopping heating, cooling, adding 1 kg of adamantane amine, mixing and stirring for 30 min, and obtaining the modified polyurethane resin". The remaining steps are exactly the same in Comparative Example 1 and Example 1.
[0024] Comparative Example 2: Comparative Example 2 is different from Example 1 in that the preparation method of the modified polyurethane resin in Example 1 is omitted in Comparative Example 2, thereby omitting the addition of dioxane and ZIF-8, and the remaining steps are exactly the same in Comparative Example 2 and Example 1.
[0025] Comparative Example 3: Comparative Example 3 is different from Example 1 in that the preparation method of the modified polyurethane resin originally existing in Example 1 is omitted in Comparative Example 3, so that in Comparative Example 3, only the unmodified polyurethane resin is added, and the remaining steps are exactly the same in Comparative Example 3 and Example 1.
[0026] The high-strength wire scraper cloths prepared in Examples 1-5 and Comparative Examples 1-3 were tested for their warp and weft tensile load according to GB / T1040.3-2006, their warp and weft tearing load according to HG / T2581.1-2009, and their peeling load according to GB / T8808-1988. The test results are as follows:
[0027] The flame retardant properties of the high-strength wire scraper cloths prepared in Examples 1-5 were tested according to GB / T 5455-2014, and the test results are as follows:
[0028] Referring to the test data of Examples 1-5, it can be seen that the tensile load of the high-strength wire knife scraper provided by the present invention is higher than 2300N / 5cm (radial) and 2100N / 5cm (weft); the tearing load is higher than 500N (radial) and 460N (weft); the peeling load is higher than 55N / 5cm (radial) and 53N / 5cm (weft), and the mechanical properties are excellent; and compared with the test data of Comparative Example 1, the mechanical properties of Examples 1-5 are significantly better than those of Comparative Example 1-3, which strongly proves that the present application introduces MOFs materials into polyurethane polymers and utilizes the covalent bond between the two. The MOFs nanocrystals are connected in series, and the introduced MOFs materials act synergistically with the multiple hydrogen bonds and polyrotaxanes present in the composite modified liquid to form supramolecular cross-linking points, thereby forming a supramolecular polymer network in the polyurethane system. The supramolecular polymer network structure is introduced into the preparation process of the scraper cloth, which can greatly improve the tensile resistance, wear resistance, corrosion resistance and other properties of the prepared scraper cloth. The flame retardant performance test data of Examples 1-5 described in this application show that the high-strength wire scraper cloth prepared in this application also has excellent flame retardant properties, which further proves that the scraper cloth described in this application has the characteristics of excellent quality and long service life.
[0029] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-strength wire scraper cloth, It is characterized in that From inside to outside, there are base fabric layer, modified coating layer and surface layer; The modified coating comprises the following components in parts by mass: 200-250 parts of modified polyurethane resin, 5-10 parts of foaming agent, 8-15 parts of foam stabilizer, 0.2-3 parts of curing agent, and 0.1-0.5 parts of thickener.
2. A high-strength wire knife scraper cloth according to claim 1, It is characterized in that In the modified coating, the modified polyurethane resin is specifically prepared by the following steps: S11. Mix 100-150 parts of polyurethane resin and 30-80 parts of dioxane by mass, stir, dissolve, add 10-50 parts of MOFs material, mix, heat to 50-100 ° C and stir for 1-2h, stop heating, cool, and obtain a preliminary modified polyurethane resin; S12. Mix 100-150 parts of the preliminarily modified polyurethane resin with 50-60 parts of dimethyl sulfoxide by mass, stir, add 20-30 parts of the modifying liquid, heat to 60-80°C and stir for 20-30h, stop heating, cool, add 10-15 parts of adamantane amine, mix and stir for 20-30min, and obtain the modified polyurethane resin.
3. A high-strength wire knife scraper cloth according to claim 2, It is characterized in that The MOFs material is ZIF-8.
4. A high-strength wire knife scraper cloth according to claim 2, It is characterized in that The modified liquid comprises the following components by mass: 30-40 parts of cyclodextrin, 20-30 parts of dimer fatty acid, 10-15 parts of ethylenediamine, 15-20 parts of p-tolylsulfonyl isocyanate, 3-5 parts of ethylene glycol, 4-8 parts of glycerol, and 5-10 parts of trimethylolpropane.
5. A high-strength wire knife scraper cloth according to claim 1, It is characterized in that The curing agent is a water-based isocyanate curing agent; the thickener is an alkali-swellable acrylic thickener.
6. A high-strength wire knife scraper cloth according to claim 1, It is characterized in that The foaming agent is one or more of azobisisobutyronitrile and azodicarbonamide; the foam stabilizing agent is one or more of dodecyldimethylamine oxide and sodium dodecyl sulfate.
7. A high-strength wire knife scraper cloth according to claim 1, It is characterized in that The base fabric layer is a biaxial warp knitted base fabric.
8. A high-strength wire knife scraper cloth according to claim 1, It is characterized in that The surface layer comprises the following components by mass: 3-4 parts of butanone, 1-5 parts of toluene, and 10-15 parts of polyethylene; the thickness of the surface layer is 0.15-0.25 mm.
9. A method for processing a high-strength wire scraper cloth, used for preparing the high-strength wire scraper cloth according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1. Ingredients: weigh the components in proportion and prepare the slurry of the modified coating and surface layer; S2. Scraping the modified coating: unwind the biaxial warp knitted base fabric, heat the slurry of the modified coating to 160-170°C, apply sizing to both sides of the biaxial warp knitted base fabric with a scraper, cool it so that both sides of the base fabric layer are bonded with the modified coating, and keep it at 180°C-200°C. The thickness of the modified coating is 0.5-0.8mm; S3. Surface coating: prepare the surface layer slurry in proportion, apply the surface layer slurry on the surface of the double-sided modified coating to obtain the high-strength wire knife scraping cloth.