Method for measuring calcination temperature of carbon material
By constructing the temperature and true density standard curves of petroleum coke samples and measuring the true density during the calcining of carbon materials, the problem of inaccurate temperature control of carbon calciner in the existing technology is solved, and the accurate determination of calcining temperature and product quality are achieved. Improved stability.
Patent Information
- Application Number
- CN202411398675.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, the temperature control of the carbon calciner furnace depends on operating experience, resulting in fluctuations in production processes and unstable product quality. Thermocouple measurement cost is high and the cycle is long, so it cannot accurately reflect the temperature distribution in the calciner furnace.
By pretreating petroleum coke, a standard curve of temperature and true density of petroleum coke samples was constructed, and calcined with carbon material under the same calcination conditions were measured to determine the true density of calcination coke to estimate the calcination temperature.
It improves the accuracy of measuring the calcining temperature of carbon materials, can quickly and accurately reflect the temperature distribution in the calcining furnace, improves stability and reduces costs, and is suitable for different types of carbon materials.
Smart Images

Figure CN119063868A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of carbon calcination, and in particular to a method for measuring the calcination temperature of a carbon material. Background Art
[0002] Raw material calcination is an important process in the carbon production process. The calcination operation is to preheat the carbon raw materials at high temperature under air-tight conditions. The purpose of calcining petroleum coke is to remove volatiles and moisture from the raw materials. During the calcination process, the structure and elemental composition of various carbon raw materials undergo a series of profound changes, thereby improving their physical and chemical properties. The quality of petroleum coke calcination has a great influence on the quality of carbon material finished products and the technical indicators of each process, so ensuring the quality of raw material calcination is an important prerequisite for ensuring the quality of the final product. The important factor affecting the quality of calcined petroleum coke is the control of calcination temperature. In industrial production, the calcination temperature of petroleum coke can usually reach 1100℃~1300℃. During the high-temperature calcination process, petroleum coke undergoes a violent thermal decomposition and polycondensation reaction, and its structure is constantly rearranged, gradually tending to be ordered and densified, accompanied by the removal of volatiles and the discharge of sulfur and hydrogen, which ultimately improves the physical and chemical properties of calcined petroleum coke.
[0003] At present, the temperature control of the calcining furnace of carbon enterprises mainly relies on the experience of operators to adjust, directly measured by thermocouples, and controlled by detecting the lattice size Lc value of reference coke. However, adjusting the temperature by manual experience is relatively rough, which can easily lead to large fluctuations in the production process and unstable product quality. Direct measurement by thermocouples is costly, has a long measurement cycle, and is complicated to operate, and cannot accurately reflect the temperature distribution in the calcining furnace. By detecting the lattice size Lc value of the reference coke to reversely infer, the test cost is high, the data fluctuates greatly, and it cannot accurately reflect the actual temperature situation in the furnace. Therefore, there is an urgent need for a method that can accurately test the temperature distribution in a carbon calcining furnace. Summary of the invention
[0004] The present application provides a method for determining the calcination temperature of a carbon material to solve the following technical problem: how to improve the accuracy of determining the calcination temperature of a carbon material.
[0005] The present application provides a method for determining the calcination temperature of a carbon material, the method comprising:
[0006] Pre-treating the petroleum coke to obtain a petroleum coke sample;
[0007] Under multiple temperature conditions, heat-treating multiple petroleum coke samples corresponding to the multiple temperature conditions, and measuring the true density of the multiple petroleum coke samples after the heat treatment, so as to construct a standard curve of temperature and true density of the petroleum coke samples;
[0008] Under the same calcination conditions, the carbon material to be calcined and the petroleum coke sample are calcined, and when the carbon material to be calcined reaches the calcination standard, a carbon calcined material and calcined coke are obtained;
[0009] determining the true density of the calcined coke; and
[0010] The calcination temperature of the carbon calcined material is obtained according to the standard curve and the true density of the calcined coke.
[0011] Optionally, the petroleum coke is pretreated, comprising:
[0012] The petroleum coke is crushed, dried and sized in sequence for pretreatment.
[0013] Optionally, the particle size of the crushing process is ≤5mm.
[0014] Optionally, the drying temperature is 105° C. to 150° C., and the drying time is 1 h to 2 h.
[0015] Optionally, the particle size of the petroleum coke sample is 1 mm to 3 mm.
[0016] Optionally, the sulfur content of the petroleum coke sample is ≤5%.
[0017] Optionally, the multiple temperature conditions include: 1100°C, 1150°C, 1200°C, 1250°C and 1300°C.
[0018] Optionally, the heat treatment adopts a rapid heating method, and the heat treatment insulation time is 1h to 2h.
[0019] Optionally, the true density is determined using a pycnometer method.
[0020] Optionally, the carbon material to be calcined satisfies at least one of the following properties when the calcination is qualified: true density is 2.0 g.cm -3 ~2.1g.cm -3 , the resistivity is 300Ω·m~500Ω·m.
[0021] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0022] The present application provides a method for determining the calcination temperature of a carbon material, comprising: pre-treating petroleum coke to obtain a petroleum coke sample; heat-treating a plurality of petroleum coke samples corresponding to the plurality of temperature conditions under a plurality of temperature conditions, and respectively measuring the true density of the plurality of petroleum coke samples after the heat treatment to construct a standard curve of the temperature and true density of the petroleum coke sample; calcining the carbon material to be calcined and the petroleum coke sample under the same calcination conditions, and obtaining a carbon calcined material and calcined coke when the carbon material to be calcined reaches a qualified calcination condition; measuring the true density of the calcined coke; and obtaining the calcination temperature of the carbon calcined material according to the standard curve and the true density of the calcined coke. By constructing a standard curve of the temperature and true density of the petroleum coke sample, the law of the true density of the petroleum coke changing with the heat treatment temperature can be accurately reflected. At the same time, since the carbon material and the petroleum coke sample are calcined under the same calcination conditions, the true density change of the petroleum coke sample can accurately reflect the calcination temperature of the carbon material, thereby improving the accuracy of the determination. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 A schematic flow chart of a method for determining the calcination temperature of a carbon material provided in an embodiment of the present application;
[0026] Figure 2 This is a standard curve diagram of temperature and true density of the petroleum coke sample provided in Example 1 of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0029] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0031] The creative ideas of the present invention are:
[0032] The density of the microstructure of calcined coke formed after calcining petroleum coke is closely related to its true density. Usually, the true density of petroleum coke at different calcination temperatures is different, and the true density of different types of calcined coke at the same calcination temperature is not much different. After high-temperature calcination, under the same treatment conditions and time, the true density of petroleum coke has a corresponding relationship with the calcination treatment temperature and has good reproducibility, which can be used to characterize the corresponding carbon calcination temperature. Using this principle, if a petroleum coke sample that has been selected in advance is placed in a predetermined position in the furnace, and the true density value is measured after calcination, the calcination temperature can be known with the help of the relationship curve between true density and calcination temperature.
[0033] Figure 1 A schematic flow chart of a method for determining the calcination temperature of a carbon material provided in an embodiment of the present application.
[0034] See also Figure 1 The present application provides a method for determining the calcination temperature of a carbon material, the method comprising:
[0035] S1. Pretreating petroleum coke to obtain a petroleum coke sample;
[0036] By pretreating petroleum coke, a certain number of petroleum coke samples are obtained. The petroleum coke samples are required to be uniform and consistent, and can quickly and accurately reflect the changes in calcination temperature, thereby having a positive effect on the stability of the quality of carbon calcined products.
[0037] In some embodiments, the pretreatment of petroleum coke comprises:
[0038] The petroleum coke is crushed, dried and sized in sequence for pretreatment.
[0039] In some embodiments, the particle size of the crushing process is ≤5 mm.
[0040] Through the crushing process, large pieces of petroleum coke are broken into smaller particles for subsequent processing and experiments. At the same time, the particle size of the crushing process is limited to ≤5mm, which helps to ensure that the petroleum coke is evenly heated during the heat treatment process and facilitates subsequent drying and screening operations. Exemplarily, the particle size of the crushing process can be 0.5mm, 1mm, 2mm, 3mm, 4mm, 5mm, etc.
[0041] In some embodiments, the drying temperature is 105° C. to 150° C., and the drying time is 1 h to 2 h.
[0042] The moisture in the petroleum coke is removed by drying to prevent the moisture from interfering with the subsequent experimental results. At the same time, the drying temperature is limited to 105°C to 150°C, and the drying time is 1h to 2h, so as to ensure that the moisture in the petroleum coke is fully removed and avoid increasing energy consumption and slight pyrolysis of the petroleum coke. Exemplarily, the drying temperature can be 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc., and the drying time can be 1h, 1.1h, 1.2h, 1.3h, 1.5h, 1.7h, 1.9h, 2h, etc.
[0043] In some embodiments, the particle size of the petroleum coke sample is 1 mm to 3 mm.
[0044] Through particle size screening, the particle size distribution of the petroleum coke sample is ensured to be consistent, so as to further eliminate the influence of raw material differences on the experimental results. At the same time, the particle size range is limited to 1mm to 3mm, which helps to improve the accuracy and repeatability of the measurement. For example, the particle size of the petroleum coke sample can be 1mm, 1.2mm, 1.5mm, 1.8mm, 2mm, 2.4mm, 2.8mm, 3mm, etc.
[0045] In some embodiments, the sulfur content of the petroleum coke sample is ≤ 5%.
[0046] Sulfur is one of the important factors affecting the performance of carbon materials. Therefore, controlling the sulfur content in petroleum coke to ≤5% is crucial to ensure the accuracy of experimental results. Petroleum coke with too high sulfur content may affect the performance of carbon materials and interfere with the accurate determination of calcination temperature. Exemplarily, the sulfur content of petroleum coke samples can be 0, 1%, 2%, 3%, 4%, 5%, etc.
[0047] S2. Under multiple temperature conditions, heat-treating multiple petroleum coke samples corresponding to the multiple temperature conditions, and measuring the true density of the multiple petroleum coke samples after the heat treatment, so as to construct a standard curve of temperature and true density of the petroleum coke samples;
[0048] By heat treating petroleum coke at different temperatures and measuring the true density of the heat treated petroleum coke, a standard curve between temperature and true density is established. This standard curve reflects the law of change of true density of petroleum coke with heat treatment temperature.
[0049] In some embodiments, the plurality of temperature conditions include: 1100°C, 1150°C, 1200°C, 1250°C, and 1300°C.
[0050] It is easy to understand that the multiple temperature conditions may include: 1100°C, 1150°C, 1200°C, 1250°C and 1300°C. These temperature points cover the common calcination temperature range of carbon materials and can fully reflect the structural changes and true density changes of petroleum coke at different temperatures.
[0051] In some embodiments, the heat treatment is performed by rapid heating, and the heat preservation time of the heat treatment is 1 hour to 2 hours.
[0052] Rapid heating can shorten the calcination time, improve efficiency, and help study the rapid response characteristics of petroleum coke at high temperatures. At the same time, the holding time of heat treatment has an important influence on the calcination effect of petroleum coke. Too short a holding time will result in insufficient calcination of petroleum coke and will not fully reflect the effect of temperature on true density; while too long a holding time will increase energy consumption and lead to a decrease in material properties. Therefore, it is necessary to select a suitable holding time to ensure that petroleum coke achieves the expected calcination effect. Exemplarily, the holding time of heat treatment can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc.
[0053] In some embodiments, the true density is measured using a pycnometer method.
[0054] It is easy to understand that the pycnometer method is based on the Archimedean principle and calculates the true density of a material by measuring the volume of liquid it displaces in a liquid.
[0055] S3, calcining the carbon material to be calcined and the petroleum coke sample under the same calcination conditions, and obtaining a carbon calcined material and calcined coke when the carbon material to be calcined reaches a qualified calcination condition;
[0056] The carbon material and the petroleum coke sample are made to experience the same temperature change under the same calcination conditions, so that the calcination temperature of the carbon material can be reflected by the change in the true density of the petroleum coke sample.
[0057] In some embodiments, the carbon material to be calcined meets at least one of the following properties when the calcination is qualified: true density is 2.0 g.cm -3 ~2.1g.cm -3 , the resistivity is 300Ω·m~500Ω·m.
[0058] S4, determining the true density of the calcined coke; and
[0059] S5. Obtaining the calcination temperature of the carbon calcined material according to the standard curve and the true density of the calcined coke.
[0060] By measuring the true density of the petroleum coke sample and combining it with the standard curve constructed previously, the calcination temperature of the carbon material can be calculated.
[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0062] Example 1
[0063] This embodiment provides a method for determining the calcination temperature of a carbon material, and the determination process includes the following steps:
[0064] S11, select 5000 kg of petroleum coke with a sulfur content of 0.5%, crush it into samples with a particle size of ≤5 mm, dry it at 105° C. for 2 h, stir it evenly, select samples with a particle size of 1 mm to 3 mm, and obtain petroleum coke samples;
[0065] S21. In the laboratory, the petroleum coke sample prepared in step S11 is heat treated at different temperatures of 1100°C, 1150°C, 1200°C, 1250°C, and 1300°C. Each heat treatment is to quickly heat the petroleum coke sample to a controlled temperature, keep it at this temperature for 1 hour, and then cool it naturally. The true density of the heat-treated petroleum coke sample is then determined by the pycnometer method, which is as follows: 1100°C: 2.01 g.cm -3 , 1150℃: 2.05g.cm -3 , 1200℃: 2.09g.cm -3 , 1250℃: 2.13g.cm -3 , 1300℃: 2.17g.cm -3 , draw a standard curve of the relationship between true density and temperature, the standard curve is as follows Figure 2 As shown;
[0066] S31, before the carbon material to be calcined is loaded into the calcining furnace, the graphite crucible containing the petroleum coke sample is sent into the calcining furnace together with the carbon material to be calcined, and after the calcination together with the carbon material is completed, when the carbon material to be calcined reaches the calcination qualified, the graphite crucible containing the petroleum coke sample is taken out to obtain the carbon calcined material and calcined coke;
[0067] S41, the true density of calcined coke was determined to be 2.08 g.cm -3 ;
[0068] S51. Based on the standard curve drawn in step S21 and the true density of the calcined coke, it can be inferred that the maximum temperature in the calcining furnace is 1187.5°C, which is 2.5°C different from the actual temperature of 1190°C measured by the thermocouple. Therefore, it can be determined that this method is reliable.
[0069] Example 2
[0070] This embodiment provides a method for determining the calcination temperature of a carbon material, and the determination process includes the following steps:
[0071] S12, selecting 2500 kg of petroleum coke with a sulfur content of 2%, crushing it into samples with a particle size of ≤5 mm, drying it at 120° C. for 1.5 h, stirring it evenly, and selecting a sample with a particle size of 1 mm to 3 mm to obtain a petroleum coke sample;
[0072] S22. The petroleum coke sample prepared in step S11 is heat treated in the laboratory at different temperatures of 1100°C, 1150°C, 1200°C, 1250°C, and 1300°C. Each heat treatment is to quickly heat the petroleum coke sample to a controlled temperature, keep it at this temperature for 1.5 hours, and then cool it naturally. The true density of the heat-treated petroleum coke sample is then measured by the pycnometer method, which is as follows: 1100°C: 1.98 g.cm -3 , 1150℃: 2.02g.cm -3 , 1200℃: 2.06g.cm -3 , 1250℃: 2.10g.cm -3 , 1300℃: 2.14g.cm -3 , draw a standard curve of the relationship between true density and temperature;
[0073] S32, before the carbon material to be calcined is loaded into the calcining furnace, the graphite crucible containing the petroleum coke sample is sent into the calcining furnace together with the carbon material to be calcined, and after calcining together with the carbon material, when the carbon material to be calcined reaches the calcination standard, the graphite crucible containing the petroleum coke sample is taken out to obtain the carbon calcined material and calcined coke;
[0074] S42, the true density of calcined coke was determined to be 2.12 g.cm -3 ;
[0075] S52. Based on the standard curve drawn in step S21 and the true density of the calcined coke, it can be inferred that the maximum temperature in the calcining furnace is 1175°C, which is 3°C different from the actual temperature of 1278°C measured by the thermocouple. Therefore, it can be determined that this method is reliable.
[0076] Example 3
[0077] This embodiment provides a method for determining the calcination temperature of a carbon material, and the determination process includes the following steps:
[0078] S13, select 50 kg of petroleum coke with a sulfur content of 5%, crush it into samples with a particle size of ≤5 mm, dry it at 150° C. for 1 h, stir it evenly, select samples with a particle size of 1 mm to 3 mm, and obtain petroleum coke samples;
[0079] S23, heat treatment is performed on the petroleum coke sample prepared in step S11 at different temperatures of 1100°C, 1150°C, 1200°C, 1250°C, and 1300°C in the laboratory. Each heat treatment is to quickly heat the petroleum coke sample to a controlled temperature, keep it at this temperature for 1.5 hours, and then cool it naturally. The true density of the heat-treated petroleum coke sample is then determined by the pycnometer method, which is as follows: 1100°C: 1.96 g.cm -3 , 1150℃: 2.00g.cm -3 , 1200℃: 2.04g.cm -3 , 1250℃: 2.08g.cm -3 , 1300℃: 2.12g.cm -3 , draw a standard curve of the relationship between true density and temperature;
[0080] S33, before the carbon material to be calcined is loaded into the calcining furnace, the graphite crucible containing the petroleum coke sample is sent into the calcining furnace together with the carbon material to be calcined, and after calcining together with the carbon material, the graphite crucible containing the petroleum coke sample is taken out, and when the carbon material to be calcined reaches the calcination standard, the graphite crucible containing the petroleum coke sample is taken out to obtain the carbon calcined material and calcined coke;
[0081] S42, the true density of calcined coke was determined to be 2.01 g.cm -3 ;
[0082] S53. Based on the standard curve drawn in step S21 and the true density of the calcined coke, it can be inferred that the maximum temperature in the calcining furnace is 1162.5°C, which is 3.5°C different from the actual temperature of 1266°C measured by the thermocouple. Therefore, it can be determined that this method is reliable.
[0083] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0084] (1) In the embodiments of the present invention, the method for determining the calcination temperature of the carbon material provided has a difference of ≤5°C from the temperature value actually measured by a thermocouple, and the method of the present invention is reliable.
[0085] (2) In the embodiments of the present invention, the method for determining the calcination temperature of carbon material provided can be used for daily monitoring of the quality of carbon calcined coke, and can effectively adjust the operation of the carbon calcining furnace in a timely manner. The calcination degree of different furnace chambers in the furnace can be studied, deficiencies can be found, the calcination effect can be improved, and the overall stability of the carbon calcination quality can be improved.
[0086] (3) In the embodiment of the present invention, the method for determining the calcination temperature of the carbon material provided uses the linear relationship between the true density of calcined petroleum coke and the calcination temperature to characterize the temperature distribution in the carbon calcination furnace. This method can quickly and accurately characterize the distribution of the calcination temperature of each furnace chamber of the carbon calcination furnace, and can make timely and effective adjustments to the calcination process, which has a positive effect on stabilizing the quality of carbon calcination products.
[0087] (4) In the embodiment of the present invention, the method for determining the calcination temperature of the carbon material provided indirectly estimates the calcination temperature of the carbon material by measuring the true density of the petroleum coke sample, without directly performing destructive testing on the carbon material itself. This means that the calcination temperature of the carbon material can be evaluated while maintaining its integrity and original performance, which is beneficial to subsequent use and processing.
[0088] (5) The method for determining the calcination temperature of carbon materials provided in the embodiments of the present invention is applicable to different types of carbon materials and heat treatment conditions. By simply adjusting the heat treatment temperature range and conditions of the petroleum coke sample, a temperature and true density standard curve applicable to different carbon materials can be constructed. In addition, by changing the parameters such as the heating method and the holding time of the heat treatment, the influence of these factors on the calcination temperature of the carbon material can be further studied.
[0089] (6) The method for determining the calcination temperature of carbon materials provided in the embodiments of the present invention provides a scientific basis and technical support for controlling the calcination temperature of carbon materials. By determining the calcination temperature of carbon materials, the calcination process parameters can be optimized, the performance and quality of carbon materials can be improved, and the demand for carbon materials in different fields can be met.
[0090] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for determining the calcination temperature of a carbon material, characterized in that: The method comprises: Pre-treating the petroleum coke to obtain a petroleum coke sample; Under multiple temperature conditions, heat-treating multiple petroleum coke samples corresponding to the multiple temperature conditions, and measuring the true density of the multiple petroleum coke samples after the heat treatment, so as to construct a standard curve of temperature and true density of the petroleum coke samples; Under the same calcination conditions, the carbon material to be calcined and the petroleum coke sample are calcined, and when the carbon material to be calcined reaches the calcination standard, a carbon calcined material and calcined coke are obtained; determining the true density of the calcined coke; and The calcination temperature of the carbon calcined material is obtained according to the standard curve and the true density of the calcined coke.
2. The method according to claim 1, characterized in that The petroleum coke is pretreated, comprising: The petroleum coke is crushed, dried and sized in sequence for pretreatment.
3. The method according to claim 2, characterized in that The particle size of the crushing process is ≤5mm.
4. The method according to claim 2, characterized in that: The drying temperature is 105° C. to 150° C., and the drying time is 1 h to 2 h.
5. The method according to claim 1, characterized in that The particle size of the petroleum coke sample is 1 mm to 3 mm.
6. The method according to claim 5, characterized in that The sulfur content of the petroleum coke sample is ≤5%.
7. The method according to claim 1, characterized in that The plurality of temperature conditions include: 1100°C, 1150°C, 1200°C, 1250°C and 1300°C.
8. The method according to claim 1, characterized in that The heat treatment adopts a rapid heating method, and the heat preservation time of the heat treatment is 1h to 2h.
9. The method according to claim 1, characterized in that: The true density is determined by a pycnometer method.
10. The method according to claim 1, characterized in that The carbon material to be calcined meets at least one of the following properties when the calcination is qualified: true density is 2.0g.cm -3 ~2.1g.cm -3 , the resistivity is 300Ω·m~500Ω·m.