Corrosion resistance test method, test device, test program, and recording medium

By forming a surface treatment film on a metal substrate and energizing the corrosion with an aqueous material and electrode, plus the posture correction step, the problems of the impact of test accuracy deviation of the coated metal material and gas egress in the prior art are solved, and the problems of the impact of the experimental accuracy of the coated metal material and the influence of gas escape are improved. The accuracy and reliability of corrosion resistance tests are provided.

CN119064248APending Publication Date: 2024-12-03MAZDA MOTOR CORP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410608014.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the corrosion resistance test method of coated metal materials has a large deviation in measurement accuracy under different postures and shapes, and the impact of gas emancipation on measurement accuracy is not effectively considered, resulting in insufficient measurement accuracy and reliability.

Method used

A corrosion resistance test method for coated metal materials is adopted. By forming a surface treatment film on a metal substrate, energizing corrosion by using aqueous materials and electrodes, and correcting the degree of corrosion aggravation according to the posture of the test object, the calculation and Evaluation steps improve test accuracy and reliability.

Benefits of technology

Through the correction step, the degree of corrosion aggravation error caused by different hydrogen egress is corrected, and the accuracy and reliability of corrosion resistance tests are improved. It is suitable for test objects in various postures and shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064248A_ABST
    Figure CN119064248A_ABST
Patent Text Reader

Abstract

The invention discloses a corrosion resistance test method, a test device, a test program, and a recording medium. A corrosion resistance test method in which a coated metal material (1) is obtained by forming an electrophoretic coating film (4) on a steel plate (2), the method comprising: arranging a container (11) that holds a water-containing material (6) such that the water-containing material comes into contact with the electrophoretic coating film (4) at a site (E) to be tested, and an electrode (12) that comes into contact with the water-containing material (6); a preparation step for electrically connecting the electrode and the steel plate by means of an external circuit (7); an energization step for energizing the electrode as an anode and the steel plate (2) as a cathode by means of an energization means (8), thereby aggravating the corrosion of the coated metal material; a calculation step of calculating the aggravation degree of corrosion; a correction step for correcting the degree of aggravation of corrosion in accordance with the posture of the test site; and an evaluation step for evaluating the corrosion resistance of the coated metal material on the basis of the correction value for the degree of aggravation of corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a corrosion resistance test method, a corrosion resistance test device, a corrosion resistance test program, and a recording medium for a coated metal material. Background Art

[0002] Conventionally, accelerated corrosion tests such as combined cycle tests and salt spray tests have been used as methods for evaluating coating performance.

[0003] However, in the above-mentioned accelerated corrosion test, it takes several months to perform the evaluation, so it is difficult to simply evaluate the constituent materials of the coated steel sheet or the state of the coating film under different baking conditions, and it is difficult to quickly optimize the coating conditions, etc. Therefore, in the fields of material development, process management of coating plants, and quality management related to vehicle rust prevention, it is desired to establish a quantitative evaluation method for quickly and simply evaluating the corrosion resistance of coated steel sheets.

[0004] In contrast, Patent Document 1 describes an evaluation method in which an electrode is arranged on the coating surface side of a coated metal material via an electrolyte material, a voltage is applied between the substrate of the coated metal material and the coating surface, and the corrosion resistance of the coated metal material is evaluated based on the voltage value when the insulation of the coating is destroyed.

[0005] Patent document 2 discloses a corrosion test device, which includes a test tank, a pressure head, and a slope measuring device. The test tank can be filled with an electrolyte solution and a metal sample is arranged inside, the pressure head can be inserted into the test tank, and the slope measuring device can measure the slope of the end surface of the metal sample and the pressure head. In addition, Patent document 2 also records that: using this device, a water film with uniform thickness can be formed on the surface of the metal sample, and electrochemical measurement can also be performed.

[0006] Patent document 3 describes a grounded electrochemical measurement component and an electrochemical measurement method using the component, wherein the component body is a magnetic sheet, the magnetic sheet includes an opening of a certain size for holding a paste electrolyte solution and a cover for preventing the electrolyte solution from drying, and a counter electrode component with a small polarization is provided at the opening, and the entire component is covered with a conductive shielding material, and the conductive shielding material is freely held on the coating film through a high insulating material, and the component body is grounded. In addition, Patent document 3 also records that: According to the component and method, regardless of the state of the coated surface, such as a curved surface, a severely uneven surface, a vertical surface, a downward surface, etc., it is possible to measure, and it is possible to avoid being affected by external noise and perform accurate measurements.

[0007] Patent Document 1: Japanese Patent Publication No. 2016-50915

[0008] Patent Document 2: Japanese Patent Publication No. 2021-085692

[0009] Patent Document 3: Japanese Patent Publication No. 2003-344332 Summary of the invention

[0010] -Technical problem to be solved by the invention-

[0011] As described in Patent Documents 1 to 3, various methods have been developed as quantitative evaluation methods for quickly and easily evaluating the corrosion resistance of coated metal materials. However, there is a problem that the measurement accuracy varies depending on the posture or shape of the test sample.

[0012] In this regard, the technology of Patent Document 3 utilizes the structure of the measurement component itself to ensure measurement accuracy regardless of the posture and shape of the test sample.

[0013] However, in the test, when gas is generated due to chemical reaction, the gas emission property varies depending on the posture and shape of the sample to be tested, which may affect the measurement accuracy. In the prior art, since such gas emission property is not taken into account, there is still room for improvement from the perspective of improving measurement accuracy.

[0014] Therefore, the purpose of the present disclosure is to provide a corrosion resistance test method, a corrosion resistance test device, a corrosion resistance test program and a recording medium for a coated metal material, which can improve the accuracy and reliability of the corrosion resistance test regardless of the posture of the test object part.

[0015] -Technical solutions for solving technical problems-

[0016] In order to solve the above technical problems, one aspect of the corrosion resistance test method of the coated metal material disclosed herein is:

[0017] A method for testing the corrosion resistance of a coated metal material, wherein the coated metal material is obtained by forming a surface treatment film on a metal substrate, characterized in that the method for testing the corrosion resistance of the coated metal material comprises a preparation step, a power-on step, a calculation step, a correction step, and an evaluation step.

[0018] In the preparation step, one or two containers are arranged to hold the aqueous material so that the aqueous material is in contact with the surface treatment film at the test object portion of the coated metal material, and one electrode in contact with the aqueous material stored in the one container or two electrodes in contact with the aqueous material stored in each of the two containers are arranged, and the electrode is electrically connected to the metal substrate or between the two electrodes by an external circuit.

[0019] In the energizing step, the electrode is used as an anode and the metal substrate is used as a cathode to energize the two electrodes by using an energizing unit provided on the external circuit, or one of the two electrodes is used as an anode and the other electrode is used as a cathode to energize the two electrodes, thereby aggravating the corrosion of the coated metal material.

[0020] In the calculation step, the degree of corrosion intensification in the energization step is calculated,

[0021] In the correction step, the degree of corrosion aggravation is corrected according to the posture of the test object part.

[0022] In the evaluation step, the corrosion resistance of the coated metal material is evaluated based on the correction value of the degree of corrosion aggravation.

[0023] It is known that metal corrosion is usually aggravated by the simultaneous occurrence of an anodic reaction (oxidation reaction) and a cathodic reaction (reduction reaction). In the anodic reaction, the metal in contact with water dissolves (ionizes) to generate free electrons, and in the cathodic reaction, the dissolved oxygen in the water generates hydroxide ions OH due to the free electrons. - wait.

[0024] In this configuration, the electrode is used as an anode and the metal substrate is used as a cathode to conduct electricity between the two electrodes, or one of the two electrodes is used as an anode and the other electrode is used as a cathode to conduct electricity between the two electrodes. In the case where the electrode is used as an anode and the metal substrate is used as a cathode and electricity is conducted, if the aqueous material that has penetrated into the surface treatment film reaches the metal substrate, a cathode reaction occurs at the contact portion between the aqueous material and the metal substrate. In addition, in the case where one of the two electrodes is used as an anode and the other electrode is used as a cathode, a cathode reaction occurs at the contact portion between the metal substrate located on the electrode side that becomes the anode and the aqueous material. Moreover, in any case, depending on the conditions for conducting electricity, that is, for example, when a voltage greater than the theoretical voltage for generating hydrogen by electrolysis of water (1.23 V when the system temperature is 25°C) is applied or when a current that requires such a voltage is applied, electrolysis of water also occurs to generate hydrogen.

[0025] If the cathode reaction is carried out, OH is generated. -, so the contact area between the water-containing material and the metal substrate becomes an alkaline environment. In this way, the base treatment layer (chemical conversion treatment layer) on the surface of the metal substrate will be damaged, and the adhesion of the surface treatment film will decrease (in the case of no base treatment, only the adhesion between the metal substrate and the surface treatment film will decrease), so that the surface treatment film will float at the contact area and the surface treatment film will swell. The surface treatment film with reduced adhesion to the metal substrate in an alkaline environment is electrolyzed by water or H + The hydrogen generated by the reduction of the surface treatment film is further pushed up, and the expansion of the surface treatment film will progress. The progress of this cathode reaction and the occurrence and progress of the expansion of the surface treatment film will accelerate the reproduction of the actual corrosion of the coated metal material. That is, in this specification, "intensify the corrosion of the coated metal material" means "cause the expansion of the surface treatment film to occur and progress". Therefore, for example, by observing the occurrence and progress of the expansion of the surface treatment film generated at the contact part, it is possible to measure the degree of aggravation of the corrosion of the coated metal material.

[0026] It should be noted that the test object part may be in various postures depending on the shape and layout of the coated metal material as the test object. In addition, the escape of hydrogen gas to the outside of the surface treatment film during the energization step varies depending on the posture of the test object part. If the escape of hydrogen gas changes, it will affect the degree of corrosion of the coated metal material.

[0027] Therefore, by providing a correction step to correct the corrosion severity according to the posture of the test object part, the error in the corrosion severity caused by the difference in hydrogen gas release properties can be corrected, thereby improving the accuracy and reliability of the corrosion resistance test.

[0028] It should be noted that, in the present specification, the "test target site of the coated metal material" refers to a portion of the coated metal material corresponding to the contact region between the water-containing material and the surface treatment film.

[0029] In this specification, the “posture of the test object site” refers to the posture of the surface of the metal substrate included in the test object site on which the surface treatment film is formed when the surface is assumed to be a flat surface.

[0030] Preferably, the posture of the test subject part is represented by an inclination angle relative to a reference posture of the test subject part.

[0031] The reference posture is a posture in which the test object site extends in a substantially horizontal direction in a state in which the coated metal material is arranged with the surface treatment film located on the upper side.

[0032] When the coated metal material is arranged with the surface treatment film on the upper side, the posture of the test object part extending in a substantially horizontal direction is the posture with the best hydrogen escape, so the degree of corrosion intensification in this posture is the most reliable when evaluating the corrosion resistance of the coated metal material. According to this configuration, since this posture is used as the reference posture, the reliability of the correction value for evaluating the corrosion resistance of the coated metal material is improved, and the test accuracy is improved.

[0033] It should be noted that, in the present specification, the “substantially horizontal direction” refers to a direction that includes the horizontal direction and has an angle with the horizontal direction within a range of ±5°.

[0034] Preferably, in the preparation step, the tilt angle is measured in advance.

[0035] In the correction step, the degree of corrosion is corrected based on a correlation between the tilt angle and the degree of corrosion that is experimentally determined in advance and the tilt angle measured in the preparation step.

[0036] According to this configuration, since the degree of corrosion progression is corrected based on the correlation obtained in advance, a corrosion resistance test with high reliability can be performed with a simple configuration.

[0037] In one embodiment, the correlation is a relationship in which the degree of corrosion decreases in proportion to the inclination angle.

[0038] In the correction step, the degree of corrosion aggravation is corrected according to the following formula (1).

[0039] A 0 =A+aθ……(1)

[0040] In formula (1), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, θ is the inclination angle, 0°≤θ≤90°.

[0041] According to this configuration, the degree of corrosion progression can be corrected with high accuracy using a simple formula.

[0042] In one embodiment, the correlation is a relationship in which the degree of corrosion decreases in proportion to the inclination angle.

[0043] In the correction step, the degree of corrosion aggravation is corrected according to the following formula (2).

[0044] A 0 =A / [1-(a / b)]×θ……(2)

[0045] Among them, in formula (2), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, b is the intercept of the correlation, θ is the tilt angle, 0°≤θ≤90°.

[0046] According to this configuration, since correction is performed while taking the intercept of the correlation into consideration, the degree of corrosion progression can be corrected with high accuracy.

[0047] Preferably, the coated metal material includes one or two scratches at the test object site that penetrate through the surface treatment film and reach the metal substrate.

[0048] The container is arranged so that the aqueous material is in contact with one of the wounds or both of the wounds.

[0049] Generally speaking, in a coated metal material including a surface treatment film, corrosion factors such as salt water penetrate the surface treatment film and reach the metal substrate, and corrosion begins. That is, the corrosion process of the coated metal material is divided into a process before corrosion occurs and a process of corrosion progression. The period before corrosion starts (corrosion inhibition period) and the speed of corrosion progression (corrosion progression speed) can be evaluated by respectively determining the period before corrosion starts (corrosion inhibition period) and the speed of corrosion progression (corrosion progression speed).

[0050] As in the present configuration, in the case where the coated metal material includes a scar that penetrates the surface treatment film and reaches the metal substrate, if the aqueous material as a corrosion factor is arranged to contact the scar, the aqueous material will penetrate into the inside of the scar and reach the exposed portion of the metal substrate. If the aqueous material contacts the exposed portion of the metal substrate, corrosion begins at the exposed portion. Then, by energizing, expansion of the surface treatment film will occur and progress around the exposed portion where the cathode reaction is performed. In other words, since the coated metal material includes scars, it is possible to simulate the state at the end of the corrosion suppression period during the corrosion process of the coated metal material. In this way, the time from the start of energization to the expansion of the surface treatment film can be shortened.

[0051] Preferably, in the energizing step, the aggravation of the corrosion of the coated metal material is manifested as the expansion of the surface treatment film generated around the scar.

[0052] In the calculation step, the degree of corrosion aggravation is calculated based on the size of the expansion of the surface treatment film, more preferably based on the size of the scratch before power-on and the size of the expansion of the surface treatment film after power-on.

[0053] In this configuration, the degree of corrosion aggravation of the coated metal material is calculated based on the size of the expansion of the surface treatment film, more preferably based on the size of the scar before power-on and the size of the expansion of the surface treatment film after power-on. This makes it possible to evaluate the corrosion resistance with high accuracy using a simple structure. This can improve the reliability and versatility of the corrosion resistance test.

[0054] It should be noted that, in this specification, "the size of the expansion of the surface treatment film" refers to the expansion diameter or expansion area, or the peeling diameter or peeling area. "Expansion diameter" and "expansion area" are respectively the diameter and area of ​​the expansion part of the surface treatment film. "Peeling diameter" and "peeling area" are respectively the diameter and area of ​​the exposed surface of the metal substrate, i.e., the peeling part, which is revealed after the expansion part of the surface treatment film is peeled off after the corrosion resistance test.

[0055] In this specification, "the size of the scar" refers to the size of the scar when viewed from above, and is the diameter, area, etc. of the scar. For example, if the shape of the scar is circular when viewed from above, the area of ​​the scar is the area of ​​the circle. The diameter of the scar is the maximum width of the scar. It should be noted that in this specification, it is assumed that the size of the scar is the same as the size of the exposed portion of the metal substrate at the scar.

[0056] Preferably, in the energizing step, a direct current constant current is applied between the electrode and the metal substrate, or between two electrodes.

[0057] By applying a constant direct current, corrosion is steadily accelerated, which can improve the reliability of the test.

[0058] Preferably, the surface treatment film is a resin coating film.

[0059] The coated metal material having a resin coating film formed as a surface treatment film on a metal substrate is suitable as a test object for this corrosion resistance test because corrosion easily progresses when electricity is applied.

[0060] One aspect of the corrosion resistance test device for the coated metal material disclosed herein is:

[0061] A corrosion resistance test device for a coated metal material, wherein the coated metal material is obtained by forming a surface treatment film on a metal substrate, and is characterized in that:

[0062] include:

[0063] One or two containers holding a water-containing material so that the water-containing material is in contact with the surface treatment film at the test object site of the coated metal material;

[0064] one electrode in contact with the aqueous material contained in one of the containers or two electrodes in contact with the aqueous material contained in each of the two containers;

[0065] An external circuit electrically connecting the electrode to the metal substrate or between two electrodes;

[0066] A current supply unit disposed on the external circuit and configured to conduct electricity between the electrode as an anode and the metal substrate as a cathode, or to conduct electricity between the two electrodes by configuring one of the two electrodes as an anode and the other electrode as a cathode;

[0067] a calculation unit for calculating a degree of aggravation of corrosion of the coating metal material aggravated by the energization;

[0068] a correction unit for correcting the degree of aggravation of the corrosion according to the posture of the test object part; and

[0069] An evaluation unit for evaluating the corrosion resistance of the coated metal material based on the correction value of the degree of corrosion aggravation.

[0070] By having the correction unit correct the corrosion severity according to the posture of the test object portion, it is possible to correct the error in the corrosion severity caused by the difference in hydrogen gas release properties, thereby improving the accuracy and reliability of the corrosion resistance test.

[0071] Preferably, the coated metal material includes one or two scratches at the test object site that penetrate through the surface treatment film and reach the metal substrate.

[0072] The container is arranged so that the water-containing material contacts one of the wounds or both of the wounds,

[0073] The intensification of the corrosion of the coated metal material is manifested as the expansion of the surface treatment film generated around the scar.

[0074] The calculation unit calculates the degree of corrosion progression of the coated metal material based on the size of the expansion of the surface treatment film, more preferably, based on the size of the scratch before energization and the size of the expansion of the surface treatment film after energization.

[0075] The coated metal material includes scars, so it is possible to simulate the state at the end of the corrosion inhibition period during the corrosion process of the coated metal material. In this way, the time from the start of power-on to the expansion of the surface treatment film can be shortened. In addition, the degree of corrosion aggravation of the coated metal material is calculated based on the size of the expansion of the surface treatment film, more preferably based on the size of the scar before power-on and the size of the expansion of the surface treatment film after power-on, so that the degree of corrosion aggravation of the coated metal material can be evaluated with high accuracy. In this way, the reliability and versatility of the corrosion resistance test can be improved.

[0076] Preferably, the posture of the test subject part is represented by an inclination angle relative to a reference posture of the test subject part.

[0077] The reference posture is a posture in which the test object site extends in a substantially horizontal direction in a state in which the coated metal material is arranged with the surface treatment film located on the upper side.

[0078] Preferably, the correction unit corrects the degree of corrosion based on a correlation between the inclination angle and the degree of corrosion that is experimentally determined in advance, and the inclination angle.

[0079] The correlation is a relationship in which the degree of corrosion is reduced in proportion to the inclination angle.

[0080] The correction unit corrects the aggravation of the corrosion according to the following formula (1) or the following formula (2):

[0081] A 0 =A+aθ……(1)

[0082] (Wherein, in formula (1), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, θ is the inclination angle, 0°≤θ≤90°. )

[0083] A 0 =A / [1-(a / b)]×θ……(2)

[0084] (Wherein, in formula (2), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, b is the intercept of the correlation, θ is the tilt angle, 0°≤θ≤90°. ).

[0085] The procedure for testing the corrosion resistance of coated metal materials disclosed herein is:

[0086] A procedure for testing the corrosion resistance of a coated metal material, the coated metal material being obtained by forming a surface treatment film on a metal substrate, characterized in that:

[0087] The corrosion resistance test includes a preparation step, a power-on step, a calculation step, a correction step, and an evaluation step.

[0088] In the preparation step, one or two containers are arranged to hold the aqueous material so that the aqueous material is in contact with the surface treatment film at the test object portion of the coated metal material, and one electrode in contact with the aqueous material stored in the one container or two electrodes in contact with the aqueous material stored in each of the two containers are arranged, and the electrode is electrically connected to the metal substrate or between the two electrodes by an external circuit.

[0089] In the energizing step, the electrode is used as an anode and the metal substrate is used as a cathode to energize the two electrodes by using an energizing unit provided on the external circuit, or one of the two electrodes is used as an anode and the other electrode is used as a cathode to energize the two electrodes, thereby aggravating the corrosion of the coated metal material.

[0090] In the calculation step, the degree of corrosion intensification in the energization step is calculated,

[0091] In the correction step, the degree of corrosion aggravation is corrected according to the posture of the test object part.

[0092] In the evaluation step, the corrosion resistance of the coated metal material is evaluated based on the correction value of the corrosion aggravation degree.

[0093] The program for testing the corrosion resistance of the coated metal material causes a computer to execute the processing of the correction step.

[0094] Since the processing of the correction step is executed by a computer, a corrosion resistance test with high reliability can be performed.

[0095] The recording medium disclosed herein records the above-mentioned corrosion resistance test program for the coated metal material, and the recording medium can be read by a computer.

[0096] - Effects of the Invention -

[0097] As described above, according to the present disclosure, by providing a correction step and correcting the corrosion severity according to the posture of the test object part, the error in the corrosion severity caused by the difference in hydrogen gas release properties can be corrected, thereby improving the accuracy and reliability of the corrosion resistance test. BRIEF DESCRIPTION OF THE DRAWINGS

[0098] Figure 1 is a diagram showing an example of a corrosion resistance test device according to the first embodiment;

[0099] Figure 2 is a flowchart for explaining the corrosion resistance test method involved in the first embodiment;

[0100] Figure 3 It is a diagram for explaining the relationship between the posture of the test subject part and the hydrogen release property;

[0101] Figure 4 is a graph showing the relationship between the inclination angle of the sample of the experimental example and the degree of corrosion;

[0102] Figure 5 is a diagram for explaining an example of a correction method;

[0103] Figure 6 is a diagram showing an example of a container of a corrosion resistance test device according to a second embodiment;

[0104] Figure 7 Yes Figure 6 A cross-sectional view of a container of a corrosion resistance test device cut along line AA is a view when the container is placed on a coated metal material with a test object portion in a reference posture;

[0105] Figure 8 Yes Figure 6 A cross-sectional view of a container of a corrosion resistance test device cut along line AA is a view when the container is placed on a coated metal material with a test object portion at an inclined angle of 90°;

[0106] Fig. 9 Viewed from the top end of the second tube Figure 6 Figure 1. A diagram of a container of a corrosion resistance test apparatus;

[0107] Fig.10 It is shown Figure 6 A diagram showing an example of a structure of a connection portion of a container;

[0108] Fig.11 This is a diagram showing an example of a corrosion resistance test device according to the third embodiment.

[0109] - Explanation of symbols -

[0110] 1-coated metal material; 2-steel plate (metal substrate); 3-chemical conversion film (metal substrate); 4-electrophoretic coating (surface treatment film); 6-water-containing material; 7-external circuit; 8-power supply unit (power supply unit, detection unit); 9-control device (calculation unit, correction unit, evaluation unit); 11-container; 12-electrode; 10-corrosion resistance test device; 100-container body; 110-first cylinder; 120-second cylinder; 130-connecting part; 150-angiometer (posture measurement unit); 127A-first incision; 127B-second incision; S1-preparation step; S3-power supply step; S4-calculation step; S5-correction step; S6-evaluation step. DETAILED DESCRIPTION

[0111] The following preferred embodiments are merely examples of the present invention and are not intended to limit the present invention, its application objects or its uses.

[0112] (First Embodiment)

[0113] Figure 1 The principle of the corrosion resistance test method according to the present embodiment and an example of a corrosion resistance test device are shown. In the figure, 1 is a coated metal material and 10 is a corrosion resistance test device.

[0114] <Coated Metal Materials>

[0115] like Figure 1 As shown, the coated metal material 1 used as a test object in the corrosion resistance test of the present embodiment is obtained by forming a surface treatment film on a metal substrate.

[0116] The metal substrate is, for example, a steel material constituting household electrical appliances, building materials, automobile parts, etc., such as a cold-rolled steel sheet (SPC), alloyed hot-dip galvanized steel sheet (GA), a high-tensile steel sheet or a hot stamping material, or may be a light alloy material. The metal substrate is preferably a steel sheet for automobile parts. The metal substrate may also be a material having a chemical conversion film (phosphate film (e.g., zinc phosphate film), chromate film, etc.) formed on the surface.

[0117] The resin coating is a resin coating formed using a resin coating, preferably an electrophoretic coating. A coated metal material having a resin coating as a surface treatment film formed on a metal substrate is suitable as a test object for this corrosion resistance test because corrosion is easy to progress when electricity is applied. Specifically, as the resin coating, for example, there are cationic electrophoretic coatings (primer coatings) such as epoxy resins and acrylic resins.

[0118] The coated metal material may also include a multilayer film of two or more layers as a surface treatment film. Specifically, for example, when the surface treatment film is a resin coating film, it may be a laminated coating film having a top coating film laminated on an electrophoretic coating film, a laminated coating film having a middle coating film and a top coating film laminated on the electrophoretic coating film, and the like.

[0119] The middle coating film has the function of ensuring the finishing and crack resistance of the coated metal material and improving the close contact between the electrophoretic coating film and the top coating film. The top coating film is a coating film used to ensure the color, finishing and weather resistance of the coated metal material. Specifically, these coating films can be formed by coatings made of base resins such as polyester resins, acrylic resins, alkyd resins and crosslinking agents such as melamine resins, urea resins, and polyisocyanate compounds (including blocks).

[0120] In the following description, the following coated metal material 1 is taken as an example. The coated metal material 1 is obtained by forming an electrophoretic coating 4 (resin coating) as a surface treatment film on a metal substrate, and the metal substrate is obtained by forming a chemical conversion film 3 on the surface of a steel plate 2.

[0121] Preferably, if Figure 1 As shown, a flaw 5 is formed at least at one location of the clad metal material 1, penetrating the electrophoretic coating 4 and the chemical conversion film 3 and reaching the steel plate 2. It should be noted that the flaw 5 can be artificially formed or naturally formed. The flaw 5 can also be formed at multiple locations separated from each other, in which case the one location means one of the multiple locations.

[0122] <Water-containing materials>

[0123] The water-containing material 6 contains water and a supporting electrolyte and has a function as a conductive material. The water-containing material 6 may also be a mud-like material containing clay minerals. When the water-containing material 6 contains clay minerals, in the holding step S2 and the energizing step S3 described later, ions and water in the water-containing material 6 easily penetrate into the electrophoretic coating film 4 around the scratch 5.

[0124] The supporting electrolyte is a salt, which is a substance used to give sufficient conductivity to the aqueous material 6. Specifically, for example, at least one salt selected from sodium chloride, sodium sulfate, calcium chloride, calcium phosphate, potassium chloride, potassium nitrate, potassium hydrogen tartrate and magnesium sulfate can be used as the supporting electrolyte. It is particularly preferred to use at least one salt selected from sodium chloride, sodium sulfate and calcium chloride as the supporting electrolyte. The content of the supporting electrolyte in the aqueous material 6 is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 15% by mass or less, and particularly preferably 5% by mass or more and 10% by mass or less.

[0125] Clay minerals are used to make the water-containing material 6 muddy and promote the movement of ions to the electrophoretic coating 4 and the penetration of water into the electrophoretic coating 4, thereby promoting the aggravation of corrosion in the energization step S3. For example, layered silicate minerals or zeolites can be used as clay minerals. For example, at least one selected from kaolinite, montmorillonite, sericite, illite, glauconite, chlorite and talc can be used as layered silicate minerals, and kaolinite is particularly preferred. The content of clay minerals in the water-containing material is preferably 1% by mass or more and 70% by mass or less, more preferably 10% by mass or more and 50% by mass or less, and particularly preferably 20% by mass or more and 30% by mass or less. It should be noted that by making the water-containing material 6 muddy, the water-containing material 6 can be arranged on the surface of the electrophoretic coating 4 even when the electrophoretic coating 4 is not in a horizontal state.

[0126] The aqueous material 6 may also contain additives other than water, supporting electrolytes and clay minerals. Specifically, for example, organic solvents such as acetone, ethanol, toluene, methanol, and substances that improve the wettability of the coating film can be cited as the above-mentioned additives. These organic solvents, substances, etc. can also have the function of promoting the penetration of water into the electrophoretic coating film 4. These organic solvents, substances, etc. can be added to the aqueous material 6 instead of clay minerals. In the case where the aqueous material 6 contains an organic solvent, the content of the organic solvent relative to water calculated by volume ratio is preferably 5% to 60%. The volume ratio is more preferably 10% to 40%, and further preferably 20% to 30%.

[0127] <Corrosion resistance test equipment for coated metal materials>

[0128] like Figure 1 As shown, the corrosion resistance tester 10 according to the present embodiment includes a container 11, an electrode 12, an external circuit 7, a power supply unit 8 (power supply unit, detection unit), and a control device 9 (calculation unit, correction unit, evaluation unit).

[0129] (container)

[0130] The container 11 is placed on the electrophoretic coating film 4 covering the metal material 1 via a seal (not shown) for preventing liquid leakage. The water-containing material 6 is placed in the container 11 and contacts the surface of the electrophoretic coating film 4 at the test site E.

[0131] The shape of the container 11 is not particularly limited, and may be, for example, a cylindrical shape, a polygonal cylindrical shape, or the like. The container 11 may be made of, for example, a resin material such as acrylic resin, epoxy resin, aromatic polyetheretherketone (PEEK), or ceramics, and is particularly preferably made of a resin material such as acrylic resin, epoxy resin, and aromatic polyetheretherketone (PEEK). In this way, the insulation between the container 11 and the outside can be ensured, and the corrosion resistance test device 10 can be made lightweight and low-cost.

[0132] The seal is, for example, a sheet seal made of silicone resin, which can improve the close contact between the container 11 and the electrophoretic coating film 4 and fill the gap between the container 11 and the electrophoretic coating film 4 when the container 11 is placed on the coated metal material 1. In this way, it is possible to effectively suppress the leakage of the aqueous material 6 from the gap between the container 11 and the electrophoretic coating film 4. A structure without a seal may be adopted, but from the viewpoint of sufficiently suppressing the leakage of the aqueous material 6, it is preferred to provide a seal.

[0133] (electrode)

[0134] The electrode 12 is used to apply a voltage between the steel plate 2 and the surface of the electrophoretic coating 4, and the electrode 12 is arranged on the electrophoretic coating 4 side of the coated metal material 1. Moreover, an aqueous material 6 is arranged between the electrophoretic coating 4 and the electrode 12, and the aqueous material 6 is in contact with the electrophoretic coating 4 and the electrode 12. Specifically, the electrode 12 is arranged in a state where at least one end thereof is buried in the aqueous material 6 and in contact with the aqueous material 6.

[0135] As the electrode 12 , an electrode generally used in electrochemical measurement can be used, and specifically, for example, a carbon electrode, a platinum electrode, or the like can be used.

[0136] The shape of the electrode 12 can be any shape commonly used in electrochemical measurement, such as a rod or plate. For example, a porous electrode having at least one hole at one end can be used as the electrode 12. For example, in the case of using a porous electrode with a ring-shaped front end, the porous electrode can be arranged so that the ring is roughly parallel to the electrophoretic coating film 4. Alternatively, a mesh electrode can be used as the porous electrode, and the mesh electrode can be arranged so that it is roughly parallel to the electrophoretic coating film 4 when it is buried in the water-containing material 6.

[0137] (External Circuit)

[0138] The external circuit 7 includes a wiring 71 and a current supply unit 8 disposed on the wiring 71. The wiring 71 electrically connects the electrode 12 and the steel plate 2. As the wiring 71, a known wiring can be used as appropriate.

[0139] (Power-on unit)

[0140] The power supply unit 8 is connected to the electrode 12 and the steel plate 2 through the wiring 71, and has the function of a power supply unit to energize between the electrode 12 and the steel plate 2, that is, to apply a voltage and / or current between the electrode 12 and the steel plate 2. At the same time, the power supply unit 8 also has the function of a current detection unit / voltage detection unit (detection unit), which detects the current and / or voltage flowing between the electrode 12 and the steel plate 2 accompanied by the application of voltage and / or current. Specifically, for example, a potentiostat / galvanostat that can control the application of voltage / current can be used as the power supply unit 8.

[0141] The energizing unit 8 is electrically or wirelessly connected to a control device 9 described later and is controlled by the control device 9. The energizing information such as the voltage value, current value, and energizing time applied to the external circuit 7 or detected by the energizing unit 8 is sent to the control device 9.

[0142] (Control device)

[0143] The control device 9 is, for example, a device based on a well-known microcomputer, and includes a control unit 91, a storage unit 92, and a computing unit 93. The control device 9 also includes an input unit 94 such as a keyboard and an output unit 95 such as a display. The storage unit 92 stores information such as various data and computing programs.

[0144] The calculation unit 93 performs various calculations based on the information stored in the storage unit 92, the information input through the input unit 94, and the like. That is, the calculation unit 93 functions as a calculation unit to calculate the degree of corrosion of the coated metal material 1 that is aggravated by the energization. The calculation unit 93 also functions as a correction unit to correct the degree of corrosion aggravation according to the posture of the test object part E. Furthermore, the calculation unit 93 also functions as an evaluation unit to evaluate the corrosion resistance of the coated metal material 1 based on the correction value of the degree of corrosion aggravation.

[0145] The calculation results including the information on the degree of corrosion of the coated metal material 1 and the correction value calculated by the calculation unit 93 are stored in the storage unit 92 .

[0146] The control unit 91 outputs a control signal to a control target based on the data stored in the storage unit 92 , the calculation result of the calculation unit 93 , and the like, and performs various controls.

[0147] (Other structures)

[0148] Although Figure 1Although not shown in the figure, in order to heat up and adjust the temperature of the water-containing material 6, especially the water-containing material 6 near the test object part, a heating and temperature adjustment unit such as a rubber heater or a film heater can be set in a state of covering the container 11 around the container 11, or the heating and temperature adjustment unit can be set on the electrophoretic coating 4 of the coated metal material 1 outside the container 11. In addition, for the same purpose, a heating plate, a Peltier element or other heating and temperature adjustment unit can also be set on the steel plate 2 side of the coated metal material 1. According to this configuration, since the water-containing material 6 and the coated metal material 1 can be properly heated and adjusted, the movement of ions to the electrophoretic coating 4 and the penetration of water to the electrophoretic coating 4 can be promoted, and the corrosion can be effectively aggravated. In this way, a corrosion resistance test with shorter time and higher reliability can be carried out. Since the temperature of the water-containing material 6 and the coated metal material 1 can be kept constant for a long time during the required test time, a corrosion resistance test with high reliability can be carried out under specified temperature conditions.

[0149] A temperature sensor (temperature detection unit) for detecting the temperature of the water-containing material 6 may also be provided. Specifically, the temperature sensor is, for example, a thermocouple, an optical fiber thermometer, an infrared thermometer, etc. In this corrosion resistance test, the temperature of the water-containing material 6, especially the temperature of the water-containing material 6 near the test object part, is very important. Therefore, when the temperature sensor is provided, it is preferred that the sensing part is arranged so as to be able to detect the temperature of the water-containing material 6 near the electrophoretic coating film 4.

[0150] The above-mentioned temperature increase and temperature control unit, temperature sensor, etc. are preferably electrically or wirelessly connected to the control device 9 and controlled by the control device 9.

[0151] A camera may also be provided as a device for taking photos of the surface of the coated metal material 1. The camera is composed of, for example, a CCD camera. The camera is electrically or wirelessly connected to the control device 9. The photos taken by the camera, i.e., image data, are sent to the control device 9. The camera takes photos of the scar 5 before power is applied and photos of the expansion of the electrophoretic coating 4 after power is applied.

[0152] (feature)

[0153] In the present corrosion resistance test device 10, the calculation unit 93 corrects the corrosion severity according to the posture of the test object part E, as described in detail later. In this way, the error in the corrosion severity caused by the difference in hydrogen gas release can be corrected, thereby improving the accuracy and reliability of the corrosion resistance test.

[0154] It should be noted that, when the test object part E has a scar 5, the aggravation of the corrosion of the coated metal material 1 is manifested as the expansion of the electrophoretic coating film 4 generated around the scar. In this case, the calculation unit 93 calculates the aggravation of the corrosion of the coated metal material 1 according to the size of the expansion of the electrophoretic coating film 4. By calculating the aggravation of the corrosion of the coated metal material according to the size of the expansion of the surface treatment film, the corrosion resistance can be evaluated with high accuracy with a simple structure. In this way, the reliability and versatility of the corrosion resistance test can be improved.

[0155] <Corrosion resistance test method of coated metal materials>

[0156] Figure 2 It is a flowchart showing the process of the corrosion resistance testing method concerning this embodiment. Figure 3 This is a diagram for explaining the relationship between the posture of the test subject's part and the hydrogen release property. Figure 4 It is a graph showing the relationship between the inclination angle of the sample of the experimental example and the degree of corrosion advancement.

[0157] Figure 5 is a diagram for explaining an example of a correction method. Figure 2 to Figure 5 The corrosion resistance test method according to the present embodiment will be described.

[0158] like Figure 2 As shown, the present corrosion resistance test method includes a preparation step S1, an optional holding step S2, an energization step S3, a calculation step S4, a correction step S5, and an evaluation step S6. Each step will be described below.

[0159] (Preparation Steps)

[0160] In the preparation step S1 , a coated metal material 1 is prepared, and preferably a coated metal material 1 having one flaw 5 penetrating through the electrophoretic coating film 4 and the chemical conversion film 3 and reaching the steel sheet 2 is prepared.

[0161] The scar 5 of the coated metal material 1 may not be formed, but it is preferably formed for the following reasons. That is, if there is a scar 5 that penetrates the electrophoretic coating film 4 and the chemical conversion film 3 and reaches the steel plate 2, when the scar 5 is brought into contact with the water-containing material 6, the water-containing material 6 will penetrate into the scar 5 and contact the steel plate 2 exposed at the scar 5. Therefore, by applying the scar 5, it is possible to simulate the state in which the process before corrosion occurs in the above-mentioned corrosion process of the coated metal material 1 has ended, that is, the state in which the corrosion suppression period has ended. In this way, information related to the corrosion progress rate can be effectively obtained in the corrosion resistance test.

[0162] As described above, the scar 5 may be a natural scar or an artificial scar formed artificially, but preferably an artificial scar. By artificially forming the scar 5, the shape and size of the scar 5 can be made to a certain extent into the desired shape and size. In this way, the expansion of the electrophoretic coating film 4 occurring in the energizing step S3 is easily advanced.

[0163] The scar 5 may be a dot-shaped scar or a linear scar such as a cut scar, but a dot-shaped scar is preferred. "Dot-shaped" refers to a shape that is circular, polygonal, etc. when viewed from above, and the ratio of the maximum width to the minimum width is less than 2. By making the scar 5 dot-shaped, the electrophoretic coating film 4 can be effectively expanded into a dome shape with corrosion, thereby improving the promotion of corrosion.

[0164] When the flaw 5 is an artificial flaw, the type of tool for applying the flaw 5 is not particularly limited. When forming a dot-shaped flaw 5, in order to prevent the size and depth of the flaw 5 from being varied, that is, from the viewpoint of quantitatively forming the flaw, it is preferred to use, for example, a method using a punch for automatically forming the flaw, a method using a Vickers hardness tester and forming the flaw with a predetermined load using its indenter, etc. When forming a shape other than a dot-shaped flaw, such as forming the linear flaw 5 described above, a cutter or the like may be used.

[0165] It is preferred to measure the size of the scar 5 in advance. The method for measuring the size of the scar 5 is not particularly limited, and it can be measured using a known method. Specifically, for example, a camera is used to photograph the area around the scar 5 on the surface of the electrophoretic coating film 4. The size of the scar 5 is measured in the obtained image data using the computing unit 93, that is, the diameter, area, etc. of the scar 5 are measured.

[0166] When the shape of the scar 5 is a dot, the diameter of the scar 5 is preferably 0.1 mm to 7 mm, more preferably 0.2 mm to 5 mm, and particularly preferably 0.3 mm to 1.5 mm. Regardless of the shape of the scar 5, the area of ​​the scar 5 is preferably 0.01 mm 2 Above 40mm 2 Below, more preferably 0.02mm 2 Above 20mm 2 Below, particularly preferably 0.05 mm 2 2mm above 2 the following.

[0167] In the above preferred range, the smaller the diameter or area, the more accelerated the corrosion in the energizing step S3. However, if the diameter is reduced to less than 0.1 mm (and / or the area is reduced to less than 0.01 mm 2), the conductivity is reduced and the cathode reaction is difficult to proceed. On the other hand, if the diameter is increased to more than 7 mm (and / or the area is more than 40 mm 2 ), the cathode reaction becomes unstable, and the expansion of the electrophoretic coating film 4 described later slows down. By making the size of the scar 5 within the above range, the cathode reaction and the expansion of the electrophoretic coating film 4 are promoted.

[0168] Next, the posture of the test object part E is adjusted by an inclination angle θ (refer to Figure 3 In the case of (c)), it is preferable to measure the inclination angle θ in the preparation step S1.

[0169] It should be noted that if Figure 3 As shown in (a), the reference posture is preferably a posture in which the test object part E is extended in a substantially horizontal direction when the coated metal material 1 is arranged so that the electrophoretic coating film 4 is located on the upper side, but there is no intention to limit the reference posture. Since this posture is a posture with good hydrogen escape, the reliability of the degree of corrosion aggravation in this posture is the highest from the perspective of evaluating the corrosion resistance of the coated metal material 1. By using this posture as the reference posture, the reliability of the correction value for evaluating the corrosion resistance of the coated metal material is improved, and the test accuracy is improved.

[0170] The inclination angle θ may be measured using any instrument without particular limitation, and may be measured using a known instrument such as a commercially available goniometer or protractor.

[0171] Next, the container 11, the water-containing material 6, and the electrode 12 are arranged on the electrophoretic coating film 4 side of the coated metal material 1. The water-containing material 6 is stored and held in the container 11, and is arranged in a state of contact with the electrophoretic coating film 4 at the test object site E of the coated metal material 1, preferably in a state of contact with the scar 5. The electrode 12 is arranged in contact with the water-containing material 6.

[0172] Specifically, for example, first, a container 11 is set on the surface of the electrophoretic coating 4 of the sample coated with the metal material 1 through a sealing material in a state preferably surrounding the flaw 5, and the water-containing material 6 is filled into the container 11. Then, the water-containing material 6 is brought into contact with the surface of the electrophoretic coating 4, preferably the flaw 5. Next, the electrode 12 connected to one end of the wiring 71 is immersed in the water-containing material 6. The other end of the wiring 71 is connected to the steel plate 2. Therefore, the electrode 12 and the steel plate 2 are in a state of being electrically connected via the external circuit 7.

[0173] The container 11 is preferably disposed concentrically with the artificial flaw 5. When a holed electrode is used as the electrode 12, the electrode 12 is preferably disposed so that the end 12a having the hole is parallel to the surface of the electrophoretic coating 4 and concentrically with the flaw 5.

[0174] (Keep Steps)

[0175] Before the next power-on step S3 is performed, a holding step S2 may be provided, in which the state in which the water-containing material 6 is arranged on the surface of the electrophoretic coating film 4 of the test object portion E is maintained for a predetermined time. The predetermined time, i.e., the holding time, is preferably from 1 minute to 1 day, more preferably from 10 minutes to 120 minutes, and particularly preferably from 15 minutes to 60 minutes.

[0176] By maintaining the water-containing material 6 in a state arranged on the surface of the electrophoretic coating 4, the penetration of the water-containing material 6 into the electrophoretic coating 4 can be promoted in advance, and in particular, the movement of ions into the electrophoretic coating 4 and the penetration of water into the electrophoretic coating 4 can be promoted. This means that in the test object portion E, the state at the end of the so-called corrosion inhibition period is simulated and reproduced in a form closer to the actual corrosion process. In this way, the corrosion of the coated metal material 1 in the next energization step S3 can be more smoothly intensified, thereby promoting the progress of the expansion of the electrophoretic coating 4, which is used to evaluate the corrosion progress rate representing the process of corrosion progress. This can shorten the test time and improve the reliability of the corrosion resistance test.

[0177] It should be noted that in the holding step S2 and the power-on step S3, the coated metal material 1 and / or the water-containing material 6 are preferably heated and the temperature is adjusted. The temperature of the coated metal material 1 and / or the water-containing material 6 is preferably 30°C to 100°C, more preferably 50°C to 100°C, and particularly preferably 50°C to 80°C. In this way, the movement of ions to the electrophoretic coating 4 and the penetration of water into the electrophoretic coating 4 can be promoted. Therefore, a corrosion resistance test with high reliability can be performed under specified temperature conditions.

[0178] (Power-on steps)

[0179] The power-on step S3 is as follows: Figure 1 As shown, the electrode 12 is used as an anode and the steel plate 2 is used as a cathode by the current supply unit 8 to conduct electricity between the two, thereby accelerating the corrosion of the steel plate 2, preferably accelerating the corrosion of the steel plate 2 around the flaw 5.

[0180] When the electrode 12 is used as an anode and the steel plate 2 is used as a cathode and electricity is applied, a cathode reaction is performed at the contact portion between the water-containing material 6 and the steel plate 2, preferably at the exposed portion 5A of the flaw 5 exposed to the steel plate 2. In addition, depending on the conditions of electricity application, the electrolysis of water is also accelerated to generate hydrogen, that is, when, for example, a voltage higher than the theoretical voltage (1.23 V when the system temperature is 25° C.) for generating hydrogen by the electrolysis of water is applied or a current requiring such a voltage is applied, the electrolysis of water is also accelerated to generate hydrogen.

[0181] As described above, when the cathode reaction proceeds, the electrophoretic coating film 4 expands. In addition, the hydrogen gas promotes the expansion of the electrophoretic coating film 4.

[0182] The progress of such a cathode reaction and the expansion of the electrophoretic coating 4, preferably the progress of the cathode reaction generated around the scar 5 and the progress of the expansion of the electrophoretic coating 4, accelerate the reproduction of the actual corrosion of the coated metal material 1. That is, the progress of the expansion of the electrophoretic coating 4 is equivalent to the simulated reproduction of the intensification of the corrosion of the coated metal material 1. Therefore, by evaluating the size of the expansion of the electrophoretic coating 4 at the moment when a specified time has passed since the start of the power-on, the degree of intensification of the corrosion of the coated metal material 1 can be evaluated. In particular, the rate of increase in the size of the expansion of the electrophoretic coating 4 is equivalent to the rate of corrosion progression in the corrosion process of the above-mentioned metal. Therefore, by obtaining the rate of increase in the size of the expansion of the electrophoretic coating 4 as the intensification of the corrosion of the coated metal material 1, the corrosion resistance related to the rate of corrosion progression of the coated metal material 1 can be evaluated with high accuracy.

[0183] It should be noted that in the energizing step S3, by applying voltage to the water-containing material 6, the anions (Cl - etc.) and cations (Na + etc.) respectively move to the steel plate 2 through the electrophoretic coating film 4. Moreover, water is attracted by the anions and the cations and permeates into the electrophoretic coating film 4.

[0184] When the flaw 5 is formed, the electrode 12 is arranged to surround the flaw 5 , so that voltage is stably applied to the electrophoretic coating film 4 around the flaw 5 , and ions can be efficiently moved to the electrophoretic coating film 4 and water can be permeated into the electrophoretic coating film 4 when current is applied.

[0185] In this way, the permeation of ions and water into the electrophoretic coating film 4 is promoted by the energization, so that the flow of electricity quickly reaches a stable state. The progress of the expansion of the electrophoretic coating film 4 is thereby stabilized.

[0186] As described above, in the present embodiment, the progress of the cathode reaction and the expansion of the electrodeposition coating film 4 can be stably promoted, so that the corrosion resistance test of the coated metal material 1 can be performed in a very short time with high accuracy.

[0187] It should be noted that, ideally, in the energizing step S3, a DC constant current or a constant voltage is applied between the electrode 12 and the steel plate 2, preferably a constant current is applied. By applying a DC constant current, corrosion is stably intensified. In this way, the reliability of the test can be improved.

[0188] The current value in the power-on step S3 is preferably 10 μA to 10 mA, more preferably 100 μA to 5 mA, and particularly preferably 500 μA to 2 mA. When the current value is lower than 10 μA, the accelerated reproducibility of corrosion is reduced, and the time required for the test becomes longer. On the other hand, if the current value exceeds 10 mA, the corrosion reaction rate becomes unstable, and the correlation with the actual corrosion aggravation becomes poor. By making the current value within the above range, the test time can be shortened and the reliability of the test can be improved.

[0189] From the viewpoint of being able to fully expand the coating film and shorten the test time, the energizing time in the energizing step S3 can be, for example, 0.05 hours to 24 hours, preferably 0.1 hours to 10 hours, more preferably 0.1 hours to 5 hours. It should be noted that, when the holding step S2 is provided, it is preferably 0.1 hours to 1 hour.

[0190] (Calculation steps)

[0191] In the calculation step S4, the degree of corrosion of the clad metal material 1 in the energization step S3 is calculated.

[0192] As described above, by observing the extent to which the expansion of the electrophoretic coating film 4 progresses when a predetermined time has passed since the start of energization in the energization step S3 , the extent to which the corrosion of the coated metal material 1 has progressed can be obtained.

[0193] As an index indicating the degree of corrosion aggravation, the expansion size of the electrophoretic coating film 4 (when the scar 5 is not formed or the size of the scar 5 is extremely small), the difference between the size of the scar 5 before power-on and the expansion size of the electrophoretic coating film 4 after power-on, the expansion progress rate of the electrophoretic coating film 4 obtained by dividing the difference by the power-on time, etc. are listed, and the expansion progress rate of the electrophoretic coating film 4 is preferably used. This is because the expansion progress rate of the electrophoretic coating film 4 is equivalent to the above-mentioned corrosion progress rate.

[0194] The size of the expansion of the electrophoretic coating film 4 can be measured in the same manner as the size of the scratch 5 .

[0195] In the above-mentioned preparation step S1, when the diameter of the scar 5 is measured as the size, the size of the expansion of the electrophoretic coating 4 can be obtained by, for example, measuring the diameter of the circle around the scar 5 that appears due to the expansion of the electrophoretic coating 4 ("expansion diameter"). Preferably, the size of the expansion of the electrophoretic coating 4 can also be obtained by sticking an adhesive tape on the electrophoretic coating 4 after the corrosion resistance test, peeling off the expanded part of the electrophoretic coating 4, and measuring the diameter of the exposed surface of the steel plate 2 ("peeling diameter").

[0196] Specifically, for example, a camera is used to capture images of the periphery of the scar 5 after the peeling. The calculation unit 93 can measure the expansion diameter or the peeling diameter from the obtained image data.

[0197] It should be noted that, in the above-mentioned preparation step S1 , when the surface area of ​​the flaw 5 is used as the size of the flaw 5 , the surface area may also be used as the size of the expansion of the electrophoretic coating film 4 .

[0198] When calculating the expansion progress rate of the electrophoretic coating film 4 as the degree of corrosion aggravation, the following procedure is performed, for example. Based on the area or diameter of the scar 5, and the expansion area or peeling area or the expansion diameter or peeling diameter, the area or distance of the region where the expansion of the electrophoretic coating film 4 has progressed during the energization process is calculated. Based on the area or distance of the region where the expansion has progressed and the energization time in the energization step S3, the expansion progress rate of the electrophoretic coating film 4 is calculated.

[0199] This makes it possible to evaluate the degree of corrosion of the coated metal material with high accuracy, thereby improving the reliability and versatility of the corrosion resistance test.

[0200] (Correction steps)

[0201] Next, in the correction step S5 , the degree of corrosion progression obtained in the calculation step S4 is corrected according to the posture of the test object portion E.

[0202] It can be predicted that the degree of corrosion in the energization step S3 varies according to the posture of the test object part E as described above. Specifically, it can be expected that: Figure 3 As shown, for example, when the tilt angle θ is 0° ( Figure 3 (a)) and when the inclination angle θ is 90° ( Figure 3 (b)), the release properties of hydrogen in the energization step S3 are different.

[0203] - Experimental example -

[0204] Experiments were conducted to verify the above hypothesis.

[0205] First, a test sample (also referred to as “TP”) to be used in a corrosion resistance test of an experimental example was prepared.

[0206] The specifications of the coated metal material 1 are as follows. That is, as the metal substrate, a substrate having a zinc phosphate film as a chemical conversion film 3 formed on the surface of the SPC as a flat steel plate 2 is used. It should be noted that the chemical conversion treatment time required to form the zinc phosphate film is 120 seconds. As a surface treatment film, an electrophoretic coating film 4 formed of an epoxy resin is formed. The electrophoretic baking conditions are 140°×15 minutes, and the thickness of the electrophoretic coating film 4 is about 10μm.

[0207] Using a Vickers hardness tester, a scratch 5 was artificially formed on the surface of the TP on which the electrophoretic coating film 4 was formed, using a load of 30 kg. The size of the scratch 5 before energization was 0.8 mm to 0.9 mm.

[0208] Then, the inclination angle θ of TP is set to three types: 0°, 45°, and 90°. Figure 1 The device shown in the figure was subjected to a corrosion resistance test. Specifically, the water-containing material 6 was left to stand for 30 minutes at a temperature of 65°C, and then a constant current of 1 mA was applied for 30 minutes at the same temperature. It should be noted that as the water-containing material 6, simulated mud (composition: 1.2 L of water, 1 kg of kaolinite, 50 g of sodium sulfate, 50 g of sodium chloride, and 50 g of calcium chloride) was used.

[0209] Then, the simulated mud was removed, the surface of the TP was cleaned, and then the swollen portion of the electrophoretic coating film 4 was removed with an adhesive tape, and then the peeling diameter was measured.

[0210] Figure 4 A digital microscope photograph of the TP surface after peeling and a graph showing the peeling diameter plotted against the tilt angle θ are shown.

[0211] like Figure 4 As shown, it can be seen that the peeling diameter decreases proportionally as the inclination angle θ increases from 0° to 45° and 90°. Thus, the results of this experiment show that the degree of corrosion progression varies depending on the posture of the test object portion E.

[0212] It should be noted that when Figure 4 When we look for the formula of the approximate straight line L on the graph of Figure 4 The equation y=ax+b (where a=-0.0567, b=10.25) is shown. This equation represents the correlation between the inclination angle θ and the degree of corrosion. It is conceivable that the degree of corrosion obtained in the energization step S3 is corrected using this equation.

[0213] - Example of correction method -

[0214] That is, the following example can be given: Based on the correlation between the tilt angle θ and the degree of corrosion obtained experimentally in advance (such as Figure 4 The degree of corrosion aggravation is corrected by using the formula shown in FIG. 1 and the inclination angle θ of the test object portion E of the coated metal material 1 measured in the preparation step S1.

[0215] According to this configuration, since the degree of corrosion progression is corrected based on the correlation obtained in advance, a corrosion resistance test with high reliability can be performed with a simple configuration.

[0216] Specifically, by Figure 4 From the curve graph, it can be seen that there is a correlation between the tilt angle θ and the degree of corrosion, in which the degree of corrosion decreases in proportion to the tilt angle. This correlation is represented by y=ax+b (where a<0, b>0).

[0217] An example of a correction method is: Figure 5 As shown in (a), the method of correcting the degree of corrosion aggravation is carried out according to the following formula (1).

[0218] A 0 =A+aθ……(1)

[0219] In formula (1), A 0 is the correction value, A is the measured value of the corrosion severity, a is the slope of the correlation, and θ is the inclination angle (0°≤θ≤90°).

[0220] In this configuration, the slope a of the correlation relationship obtained experimentally in advance is used to correct the measured value A of the degree of corrosion at various tilt angles θ to the value A at the reference posture (θ = 0°). 0 .like Figure 5 As shown in (a), the slope a is used directly as the correction coefficient. According to this configuration, the degree of corrosion progression can be corrected with high accuracy using a simple formula.

[0221] Another example of a correction method is: Figure 5 (b) shows a method for correcting the degree of corrosion according to the following formula (2).

[0222] A 0 =A / [1-(a / b)]×θ……(2)

[0223] Among them, in formula (2), A 0 is the correction value, A is the degree of corrosion aggravation, a is the slope of the correlation, b is the intercept of the correlation, and θ is the tilt angle (0°≤θ≤90°).

[0224] In this configuration, the slope a and intercept b of the correlation relationship obtained experimentally in advance are used to correct the measured value A of the degree of corrosion at various tilt angles θ to the value A at the reference posture (θ = 0°). 0 .

[0225] According to this configuration, since the correction is performed while taking into account the intercept of the correlation, the degree of corrosion can be corrected with high accuracy. In addition, in formula (1), when the measured value A is extremely small, the correction value may become a negative value depending on the setting of the reference posture. In formula (2), even in this case, an appropriate correction value can be obtained.

[0226] Thus, by providing the correction step S5 and correcting the corrosion severity according to the posture of the test object portion E, the error in the corrosion severity caused by the difference in hydrogen gas release properties can be corrected, thereby improving the accuracy and reliability of the corrosion resistance test.

[0227] It should be noted that the correlation, especially the values ​​of a and b, may vary depending on the specification of the clad metal material 1 , the conditions of the corrosion resistance test, etc. The correlation may be experimentally obtained in advance for various conditions and stored in the storage unit 92 .

[0228] (Evaluation Steps)

[0229] The evaluation step S6 is a step of evaluating the corrosion resistance of the coated metal material 1 based on the correction value of the degree of corrosion progression obtained in the correction step S5.

[0230] This correction value can be used, for example, to correlate with an actual corrosion test and evaluate the corrosion resistance of the coated metal material 1. Specifically, for example, the relationship between the correction value of the degree of corrosion aggravation obtained by the corrosion resistance test and the corrosion progression rate obtained by the actual corrosion test is obtained in advance, and based on the corrosion resistance test result, it can be determined what degree of corrosion resistance it corresponds to in the actual corrosion test.

[0231] <Corrosion resistance test procedure and recording medium>

[0232] At least a part of the processes in the above-mentioned corrosion resistance test method is programmed as a corrosion resistance test program. Specifically, the corrosion resistance test program involved in the present embodiment is a program that enables a computer to at least perform the processing of the correction step S5 in the above-mentioned processes, preferably the processing of the power-on step S3, the processing of the calculation step S4, the processing of the correction step S5, and the processing of the evaluation step S6. The corrosion resistance test program can be executed by the control unit 91 and the operation unit 93 in a state stored in the storage unit 92. The corrosion resistance test program is not limited to the state stored in the storage unit 92, and can also be recorded in various known recording media that can be read by a computer, such as an optical disk medium or a magnetic tape medium. Moreover, the program can be executed by installing such a recording medium on a readout device (not shown) of the control device 9 and reading the corrosion resistance test program.

[0233] According to this configuration, since the processing of the correction step S5 is executed by a computer, a corrosion resistance test with high reliability can be performed.

[0234] (Second Embodiment)

[0235] Hereinafter, other embodiments of the present disclosure will be described in detail. It should be noted that in the description of these embodiments, the same reference numerals are given to the same parts as those of the first embodiment, and detailed description thereof will be omitted.

[0236] The container 11 used in the corrosion resistance test device 10 is not limited to the structure in the first embodiment. Figure 6 to Figure 10 The container 11 shown is suitable for use in the present corrosion resistance test.

[0237] like Figure 6 to Figure 8 As shown, the container 11 includes a cylindrical container body 100 and a goniometer 150 (posture measurement unit).

[0238] (Container body)

[0239] The container body 100 is placed on the electrophoretic coating film 4 side of the metal material 1, thereby being able to hold the water-containing material 6 inside. Figure 6 to Figure 10 The container 11 shown has a container body 100 in a square tube shape, but is not limited to this shape as long as it is a tube shape, and may be a cylindrical shape as in the first embodiment, or may be another shape such as a polygonal tube shape.

[0240] The container body 100 includes a first cylindrical portion 110 in contact with the electrophoretic coating film 4 at the base end portion 111 side, and a second cylindrical portion 120 connected to the tip end portion 112 side of the first cylindrical portion 110 via a connecting portion 130 .

[0241] The second barrel 120 has a base end portion 121 and a top end portion 122. The base end portion 121 is arranged on the top end portion 112 side of the first barrel 110, and the top end portion 122 extends on the side of the base end portion 121 opposite to the first barrel 110 and is inclined at a specified angle relative to the base end portion 121.

[0242] The inner circumferential portion 123 of the second cylindrical portion 120 communicates with the inner circumferential portion 113 of the first cylindrical portion 110 .

[0243] A through hole 124 is formed on the side wall of the top end 122 of the second cylinder 120. The through hole 124 is provided for the following purposes: to suppress the internal pressure in the container body 100 from excessively rising due to hydrogen gas or volatile components of the water-containing material generated during the test, to release the internal pressure; to inject the water-containing material 6; and to lead out the electrode 12 or the wiring 71 of the external circuit 7. It should be noted that, as Figure 7 , Figure 8 As shown, the interior of the container body 100 may be filled with the water-containing material 6, and the through hole 124 may be plugged with a plug or the like when the top end surface 122A of the second cylindrical portion 120 is not covered with a lid.

[0244] like Figure 6 As shown by the hollow arrow in , the second barrel portion 120 is connected to the first barrel portion 110 via the connecting portion 130 and can rotate relative to the first barrel portion 110 along the circumferential direction of the first barrel portion 110 .

[0245] By rotating the second tube 120 relative to the first tube 110 according to the posture of the test subject, the tip 122 of the second tube 120 can be arranged to always face upward in the vertical direction. This can prevent the water-containing material contained in the container body from leaking out of the container body.

[0246] It should be noted that in Figure 6 to Figure 8 In the example of the container 11, the first cylinder 110 and at least the base end 121 of the second cylinder 120 are arranged on the same axis. Therefore, when the second cylinder 120 is rotated along the circumferential direction of the first cylinder 110, at least the base end 121 of the second cylinder 120 rotates along the circumferential direction of the base end 121.

[0247] exist Figure 6 to Figure 8 In the example of the container 11, from the perspective of sealing, the second cylinder 120 can only be in a state where it does not rotate along the circumferential direction of the first cylinder 110 ( Figure 7 ) and the state rotated 180° ( Figure 6 and Figure 8 ) in any state.

[0248] Figure 7The case where the container 11 of the present embodiment is placed on a sample of the coated metal material 1 with the posture of the test target portion being the reference posture, that is, the horizontal direction.

[0249] like Figure 7 As shown, the container 11 is placed on the sample in a state where the base end surface 111A of the first cylinder 110 contacts the electrophoretic coating film 4. In addition, the top end 122 of the second cylinder 120 is arranged to extend upward in the vertical direction. This can prevent the water-containing material 6 in the container body 100 from leaking.

[0250] It should be noted that in Figure 7 The sample shown has a welded portion 1A. Even if the welded portion 1A or the like makes it difficult to arrange a cylindrical container extending in one direction like the container 11 of the first embodiment, the container 11 and the water-containing material 6 can be easily and stably arranged by using the container 11 of this embodiment.

[0251] Figure 8 The case where the container 11 of the embodiment is placed on a sample of the coated metal material 1 whose posture of the test target portion, that is, the tilt angle θ with respect to the horizontal direction is 90° is shown.

[0252] like Figure 8 As shown in FIG. 1 , when the inclination angle θ of the test object part is 90°, the second cylinder 120 can be moved from Figure 7 The state of the second cylindrical portion 120 is rotated 180° along the circumferential direction of the first cylindrical portion 110 so that the top end surface 122A of the second cylindrical portion 120 faces upward in the vertical direction. In this way, even when the inclination angle θ of the test object portion is 90°, the top end surface 122A faces upward, which can effectively suppress leakage of the water-containing material 6.

[0253] The connection portion 130 may have any structure as long as the second tube portion 120 is rotatable relative to the first tube portion 110 in the circumferential direction of the first tube portion 110 and leakage of the water-containing material 6 inside to the outside can be suppressed.

[0254] Fig. 9 A specific example of the structure of the connection portion 130 is shown.

[0255] The connection portion 130 may be configured to include, for example, an annular sealing member. Fig. 9 (a) is an example in which the connection portion 130 is formed of an annular sealing member.

[0256] like Fig. 9 As shown in (a), for example, the outer diameter of the base end portion 121 of the second cylindrical portion 120 may be smaller than the inner diameter of the distal end portion 112 of the first cylindrical portion 110 .

[0257] Furthermore, the connection portion 130 may be configured to include an annular sealing member disposed between the outer peripheral surface 121A of the base end portion 121 of the second cylindrical portion 120 and the inner peripheral surface 112A of the top end portion 112 of the first cylindrical portion 110 and in contact with the outer peripheral surface 121A and the inner peripheral surface 112A.

[0258] As the annular sealing member, specifically, for example, a lip seal having a flexible lip structure can be cited. As the lip seal, for example, a U-shaped seal, a V-shaped seal, a Y-shaped seal, etc. can be cited, and a U-shaped seal is preferred.

[0259] By configuring the connection portion 130 to include the annular sealing member, the second cylindrical portion 120 can smoothly rotate in the circumferential direction of the first cylindrical portion 110 , and leakage of the water-containing material 6 inside to the outside can be effectively suppressed.

[0260] like Fig. 9 As shown in (b), the connection portion 130 may also be configured to include a magnet. Fig. 9 In (b), the top end surface 112B of the top end portion 112 of the first barrel 110 and the base end surface 121B of the base end portion 121 of the second barrel 120 are configured to be removable via a magnet. In this case, specifically, for example, the magnet is fixed to one of the top end surface 112B and the base end surface 121B by an adhesive, a resin mold, etc., and a metal plate or the like is fixed to the other by an adhesive, a resin mold, etc., so that the two can be removably connected to each other.

[0261] According to this configuration, since the two are detachably connected to each other via magnets, the second tube portion 120 can be fixed at a position rotated by a desired angle in the circumferential direction of the first tube portion 110. This improves the versatility of the device.

[0262] Furthermore, if Fig. 9 As shown in (c), the connecting portion 130 may also have a corrugated structure. Thus, the second barrel 120 can be oriented in various directions relative to the first barrel 110. In this way, since the degree of freedom of the sample of the test object is improved, the versatility of the device is improved. In addition, since the first barrel 110 and the second barrel 120 can be formed into one, the leakage of the water-containing material 6 can be effectively suppressed.

[0263] like Figure 6 to Figure 8 and Fig.10 As shown, the tip portion 122 of the second cylindrical portion 120 has a first notch 127A provided for observing the test object site. The first notch 127A is provided from the tip surface 122A of the tip portion 122 to the inner peripheral surface 122B.

[0264] A second notch 127B for observing the test object site is provided on the inner circumferential surface of the connection portion between the base end portion 121 and the distal end portion 122 of the second cylindrical portion 120. The second notch 127B is provided to extend in the axial direction of the base end portion 121 and the axial direction of the distal end portion 122.

[0265] Especially if Fig.10 As shown, the radial cross-sections of the first cutout 127A and the second cutout 127B are triangular, but are not limited to this shape and may also be circular, other polygonal shapes, etc.

[0266] like Figure 7 , Figure 8 , Fig.10 As shown, when the interior of the container body 100 is observed from the top surface 122A side of the top end portion 122, an observation window is formed by the first cutout 127A and the second cutout 127B, preferably a rectangular observation window. Figure 7 and Figure 8 As shown by the two-dot chain line in the middle, when observing the inside of the container body from the outside of the container body (the top end surface side of the top end), the test object part E, especially the part with the scar 5, can be observed through the observation window. Fig.10 In the embodiment, the shape of the observation window is a rectangle, but is not limited to this shape, and may be other shapes such as a circle, an ellipse, a polygon, etc.

[0267] (Anglometer)

[0268] The goniometer 150 is attached to the container body 100 to measure the posture of the coated metal material 1, preferably to measure the inclination angle θ with respect to the reference posture. The goniometer 150 is attached to the top end portion 112 side of the first barrel 110. Thus, when the container body 100 is placed on the electrophoretic coating 4 of the coated metal material 1, the goniometer 150 is arranged on the electrophoretic coating 4 near the test object part. In this way, the inclination angle θ of the test object part and the reference posture can be measured by the goniometer 150 (to be precise, the inclination angle near the test object part is measured, but since it is sufficiently close, it can be approximated to the inclination angle θ of the measurement object part).

[0269] According to this configuration, the tilt angle can be automatically measured simply by placing the container 11 on the sample, so the process of the corrosion resistance test can be simplified.

[0270] (feature)

[0271] As described above, the container 11 used in the corrosion resistance tester 10 according to the second embodiment has the following features.

[0272] The container includes a cylindrical container body and a posture measuring unit (goniometer). The container body is capable of retaining the water-containing material inside by being placed on the surface treatment film side of the coated metal material. The posture measuring unit (goniometer) is attached to the container body to measure the posture of the coated metal material, preferably measuring the inclination angle relative to a reference posture.

[0273] The container body includes a first cylindrical portion and a second cylindrical portion. The first cylindrical portion is in contact with the surface treatment film at a base end side, and the second cylindrical portion is provided to extend at a tip end side of the first cylindrical portion.

[0274] The inner circumference of the second cylindrical portion is communicated with the inner circumference of the first cylindrical portion.

[0275] The second tube portion has a base end portion and a tip end portion. The base end portion is arranged on the tip end side of the first tube portion. The tip end portion extends on the side of the base end portion opposite to the first tube portion and is inclined at a predetermined angle relative to the base end portion.

[0276] The second barrel is connected to the first barrel and can rotate relative to the first barrel along the circumferential direction of the first barrel. By rotating the second barrel relative to the first barrel according to the posture of the test object part, the top end of the second barrel can be arranged to always face upward in the vertical direction. In this way, the water-containing material contained in the container body can be prevented from leaking from the container body.

[0277] At least base ends of the first cylindrical portion and the second cylindrical portion are coaxially arranged.

[0278] By rotating the second cylindrical portion in the circumferential direction of the first cylindrical portion, at least the base end portion of the second cylindrical portion rotates in the circumferential direction of the base end portion.

[0279] The second barrel portion is connected to the first barrel portion via a connecting portion.

[0280] The outer diameter of the base end portion of the second cylindrical portion may be smaller than the inner diameter of the distal end portion of the first cylindrical portion.

[0281] The connecting portion may include an annular sealing component, preferably a lip-shaped sealing gasket with a flexible lip structure, and more preferably a U-shaped sealing gasket, wherein the sealing component is arranged between the outer peripheral surface of the base end portion of the second barrel portion and the inner peripheral surface of the top end portion of the first barrel portion and is in contact with the outer peripheral surface and the inner peripheral surface.

[0282] The connecting portion may include a magnet.

[0283] The connecting portion may also have a corrugated structure.

[0284] The distal end of the second tube has a first notch provided for observing the test object site. The first notch is provided from the distal end surface of the distal end of the second tube to the inner peripheral surface.

[0285] A second notch for observing the test object site is provided on the inner peripheral surface of the connection portion between the base end portion and the distal end portion of the second cylindrical portion. The second notch is provided to extend in the axial direction of the base end portion and the distal end portion of the second cylindrical portion.

[0286] When the interior of the container body is observed from the top end surface side of the top end portion of the second barrel portion, an observation window is formed by the first cutout and the second cutout, preferably a rectangular observation window. Thus, when the interior of the container body is observed from the outside of the container body (the top end surface side of the top end portion), the test object part, especially the part with the scar 5, can be observed through the observation window.

[0287] (Third Embodiment)

[0288] In the first and second embodiments, the test method in which electricity is passed between the electrode 12 and the steel sheet 2 is described as an example, but the present invention is not limited to this structure.

[0289] like Fig.11 As shown, the following test method may also be adopted: the container 11 is set at two locations, the water-containing material 6 and the electrode 12 are arranged at each of the two locations, and electricity is passed between the two electrodes 12 .

[0290] In this case, in the preparation step S1 , two containers 11 and two electrodes 12 are arranged, the two electrodes 12 being in contact with the water-containing material 6 accommodated in each of the two containers, respectively, and the two electrodes 12 are electrically connected by an external circuit.

[0291] It should be noted that if Fig.11 As shown, the coated metal material 1 may include two flaws penetrating the electrophoretic coating film 4 and reaching the steel plate 2 at two test target locations E. In this case, the two containers 11 are arranged so that the water-containing material 6 in each container 11 contacts a corresponding flaw of the two flaws.

[0292] In the present embodiment, the corrosion resistance test device 10 includes two containers 11 , two electrodes that are in contact with the water-containing material 6 contained in the two containers, respectively, and an external circuit that electrically connects the two electrodes.

[0293] Then, in the energizing step S3, the energizing means 8 makes one of the two electrodes serve as an anode and the other electrode serve as a cathode to energize between the two electrodes. This will intensify the corrosion of the coated metal material 1.

[0294] For example, Fig.11In the embodiment, the electrode 12 on the left is a cathode and the electrode 12 on the right is an anode. In this case, the test object site E on the left is an anode site, preferably, the scar 5 is an anode site, and the test object site E on the right is a cathode site, preferably, the scar 5 is a cathode site.

[0295] In the anode portion, the anode reaction proceeds and the cathode reaction is suppressed, so that the electrodeposition coating film 4 hardly expands.

[0296] On the other hand, the expansion of the electrophoretic coating film 4 progresses at the cathode portion. Therefore, by evaluating the expansion of the electrophoretic coating film 4 at the cathode portion at a time when a predetermined time has passed since the start of energization, the degree of corrosion of the coated metal material 1 can be evaluated.

[0297] It should be noted that, depending on the size and shape of the scar 5 and the current value when the power supply unit 8 is energized, a cathode reaction sometimes also occurs at the anode portion. That is, in the present embodiment, it is preferred that the scar 5 that undergoes an anode reaction and the scar 5 that undergoes a cathode reaction are clearly separated in the two scars 5, but sometimes the separation is unclear. In this case, the expansion of the electrophoretic coating 4 may also progress at the anode portion. In this case, since the expansion of the electrophoretic coating 4 may be aggravated in both scars 5, in the calculation step S4, the degree of aggravation of the corrosion of the coated metal material 1 is calculated based on the scar 5 where the electrophoretic coating 4 expands more.

[0298] As described above, in this embodiment, by energizing, the anode portion where the anodic reaction occurs and the cathode portion where the cathodic reaction occurs are separated, and the progress of the two reactions and the expansion of the electrophoretic coating 4 can be stably promoted, thereby enabling the corrosion resistance test of the coated metal material 1 to be performed with high precision in an extremely short time.

[0299] It should be noted that, similar to the first embodiment, it is preferable to apply a constant current or a constant voltage between the two electrodes 12 , and it is preferable to apply a constant voltage.

[0300] It is also preferable that the value of the current flowing between the two electrodes 12 is the same as that in the first embodiment.

[0301] It should be noted that, when forming the scar 5, it is preferred that at least one of the two scars 5 is formed in a dot shape. In addition, the scar 5 with a larger expansion size of the electrophoretic coating film 4 is preferably formed in a dot shape in the preparation step S1. Furthermore, the scar 5 that undergoes a cathode reaction in the energization step S3, that is, the scar 5 that becomes the cathode part, is preferably formed in a dot shape. In this case, the shape of the scar 5 that becomes the anode part is not particularly limited, and can be a dot shape or a linear shape such as a cutting scar.

[0302] From the viewpoint of easily confirming the expansion of the electrophoretic coating film 4 , the distance between the two scratches 5 is preferably 2 cm or more, and more preferably 3 cm or more.

[0303] For passing Fig.11 As for the corrosion aggravation degree obtained by the test method, the corrosion aggravation degree can be corrected according to the posture of the test object part E, and the corrosion resistance can be evaluated according to the obtained correction value. By correcting the corrosion aggravation degree according to the posture of the test object part, the error of the corrosion aggravation degree caused by the difference in hydrogen gas evolution can be corrected, thereby improving the accuracy and reliability of the corrosion resistance test.

[0304] - Industrial Applicability -

[0305] The present disclosure can provide a corrosion resistance test method, a corrosion resistance test device, a corrosion resistance test program and a recording medium for a coated metal material, which can improve the accuracy and reliability of the corrosion resistance test regardless of the posture of the test object part, and is therefore extremely useful.

Claims

1. A method for testing the corrosion resistance of a coated metal material, wherein the coated metal material is obtained by forming a surface treatment film on a metal substrate, Features: The corrosion resistance test method of the coated metal material comprises a preparation step, an energization step, a calculation step, a correction step and an evaluation step. In the preparation step, one or two containers are arranged to hold the aqueous material so that the aqueous material is in contact with the surface treatment film at the test object portion of the coated metal material, and one electrode in contact with the aqueous material stored in the one container or two electrodes in contact with the aqueous material stored in each of the two containers are arranged, and the electrode is electrically connected to the metal substrate or between the two electrodes by an external circuit. In the energizing step, the electrode is used as an anode and the metal substrate is used as a cathode to energize the two electrodes by using an energizing unit provided on the external circuit, or one of the two electrodes is used as an anode and the other electrode is used as a cathode to energize the two electrodes, thereby aggravating the corrosion of the coated metal material. In the calculation step, the degree of corrosion intensification in the energization step is calculated, In the correction step, the degree of corrosion aggravation is corrected according to the posture of the test object part. In the evaluation step, the corrosion resistance of the coated metal material is evaluated based on the correction value of the degree of corrosion aggravation.

2. The corrosion resistance test method of the coated metal material according to claim 1, Features: The posture of the test object part is represented by an inclination angle relative to a reference posture of the test object part. The reference posture is a posture in which the test object site extends in a substantially horizontal direction in a state in which the coated metal material is arranged with the surface treatment film located on the upper side.

3. The corrosion resistance test method of the coated metal material according to claim 2, Features: In the preparation step, the tilt angle is measured in advance, In the correction step, the degree of corrosion is corrected based on a correlation between the tilt angle and the degree of corrosion that is experimentally determined in advance and the tilt angle measured in the preparation step.

4. The corrosion resistance test method of the coated metal material according to claim 3, Features: The correlation is a relationship in which the degree of corrosion decreases in proportion to the inclination angle. In the correction step, the degree of corrosion is corrected according to the following formula (1): A 0 =A+aθ……(1) In formula (1), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, θ is the inclination angle, 0°≤θ≤90°.

5. The corrosion resistance test method of the coated metal material according to claim 3, Features: The correlation is a relationship in which the degree of corrosion decreases in proportion to the inclination angle. In the correction step, the degree of corrosion is corrected according to the following formula (2): A 0 =A / [1-(a / b)]×θ……(2) Among them, in formula (2), A 0 is the correction value, A is the degree of corrosion, a is the slope of the correlation, b is the intercept of the correlation, θ is the tilt angle, 0°≤θ≤90°.

6. The corrosion resistance test method of the coated metal material according to claim 1 or 2, Features: The coated metal material includes one or two scratches at the test object site that penetrate through the surface treatment film and reach the metal substrate, The container is arranged so that the aqueous material is in contact with one of the wounds or both of the wounds.

7. The corrosion resistance test method of the coated metal material according to claim 6, Features: In the energizing step, the corrosion of the coated metal material is aggravated by the expansion of the surface treatment film generated around the scratch. In the calculation step, the degree of aggravation of the corrosion is calculated according to the expansion of the surface treatment film.

8. The corrosion resistance test method of the coated metal material according to claim 1 or 2, Features: In the energizing step, a direct current constant current is applied between the electrode and the metal substrate, or between two electrodes.

9. The corrosion resistance testing method of the coated metal material according to claim 1 or 2, Features: The surface treatment film is a resin coating film.

10. A corrosion resistance test device for a coated metal material, the coated metal material being obtained by forming a surface treatment film on a metal substrate, Features: include: One or two containers holding a water-containing material so that the water-containing material is in contact with the surface treatment film at the test object site of the coated metal material; one electrode in contact with the aqueous material contained in one of the containers or two electrodes in contact with the aqueous material contained in each of the two containers; An external circuit electrically connecting the electrode to the metal substrate or between two electrodes; A current supply unit disposed on the external circuit and configured to conduct electricity between the electrode as an anode and the metal substrate as a cathode, or to conduct electricity between the two electrodes by configuring one of the two electrodes as an anode and the other electrode as a cathode; a calculation unit for calculating a degree of aggravation of corrosion of the coating metal material aggravated by the energization; a correction unit for correcting the degree of aggravation of the corrosion according to the posture of the test object part; as well as An evaluation unit for evaluating the corrosion resistance of the coated metal material based on the correction value of the degree of corrosion aggravation.

11. The corrosion resistance testing device for coated metal materials according to claim 10, Features: The coated metal material includes one or two scratches at the test object site that penetrate through the surface treatment film and reach the metal substrate, The container is arranged so that the water-containing material contacts one of the wounds or both of the wounds, The intensification of the corrosion of the coated metal material is manifested as the expansion of the surface treatment film generated around the scar. The calculation unit calculates a degree of aggravation of corrosion of the coated metal material based on a size of expansion of the surface treatment film.

12. A procedure for testing the corrosion resistance of a coated metal material, the coated metal material being obtained by forming a surface treatment film on a metal substrate, Features: The corrosion resistance test includes a preparation step, a power-on step, a calculation step, a correction step, and an evaluation step. In the preparation step, one or two containers are arranged to hold the aqueous material so that the aqueous material is in contact with the surface treatment film at the test object portion of the coated metal material, and one electrode in contact with the aqueous material stored in the one container or two electrodes in contact with the aqueous material stored in each of the two containers are arranged, and the electrode is electrically connected to the metal substrate or between the two electrodes by an external circuit. In the energizing step, the electrode is used as an anode and the metal substrate is used as a cathode to energize the two electrodes by using an energizing unit provided on the external circuit, or one of the two electrodes is used as an anode and the other electrode is used as a cathode to energize the two electrodes, thereby aggravating the corrosion of the coated metal material. In the calculation step, the degree of corrosion intensification in the energization step is calculated, In the correction step, the degree of corrosion aggravation is corrected according to the posture of the test object part. In the evaluation step, the corrosion resistance of the coated metal material is evaluated based on the correction value of the corrosion aggravation degree. The program for testing the corrosion resistance of the coated metal material causes a computer to execute the processing of the correction step. 13 . A recording medium having the corrosion resistance test program of the coated metal material according to claim 12 recorded thereon, the recording medium being readable by a computer.

Citation Information

Cited By

  • Test method for rapidly evaluating corrosion resistance of automobile steel

    CN120927559A

  • Method and system for testing reliability of solid state disk

    CN121237182A