Electrode plate, preparation method thereof, secondary battery and electric device
By regulating the transmission speed of active ions in the electrode sheet of the secondary battery using the particle size layered structure, the problem of insufficient cycle life of the traditional secondary battery is solved, and the capacity of the electrode sheet is slowly released, which extends the battery life and improves the battery life. Energy density.
Patent Information
- Application Number
- CN202310637212.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The cycle life of traditional secondary batteries is due to the rapid capacity decay, which leads to insufficient service life in actual applications, and requires improved cycle life.
Design an electrode sheet, including a current collector, a first electrode film layer and a second electrode film layer, the first electrode film layer contains a first electrode active material, and its average particle size Dv50 is greater than that contained in the second electrode film layer The average particle size Dv50 of the second electrode active material regulates the transmission speed of active ions through a layered structure, so that the electrode sheet slowly releases its capacity in the early cycle period, and extends the battery life.
By regulating the particle size of the active material of the electrode sheet, the attenuation of the electrode sheet capacity is delayed, and the cycle life and energy density of the secondary battery are significantly improved.
Smart Images

Figure CN119069612A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to an electrode plate, a preparation method thereof, a secondary battery and an electrical device. Background Art
[0002] Secondary batteries have the advantages of high energy density, high operating voltage, no memory effect, and no pollution. They are widely used in electronic products, electric vehicles, power tools, etc. The secondary cycle life is one of the important indicators to measure its electrical performance. The cycle life of traditional secondary batteries needs to be further improved. Summary of the invention
[0003] Based on this, the present application provides an electrode plate, a preparation method thereof, a secondary battery and an electrical device to improve the cycle life of the secondary battery containing the electrode plate.
[0004] In a first aspect of the present application, an electrode plate is provided, comprising a current collector, a first electrode film layer and a second electrode film layer, wherein the first electrode film layer and the second electrode film layer are sequentially stacked on the same side surface of the current collector, the first electrode film layer comprises a first electrode active material, the second electrode film layer comprises a second electrode active material, and the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material.
[0005] In the above-mentioned electrode plate, the first electrode film layer is closer to the current collector, and the second electrode film layer is farther from the current collector. When the active ions are embedded in the electrode plate, they enter the second electrode film layer and the first electrode film layer in turn. Since the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material, the transmission speed of the active ions in the first electrode film layer is slower than the transmission speed in the second electrode film layer, so that the capacity of the electrode plate in the early stage of the cycle is slowly released and the capacity is in a climbing state (that is, the capacity released by the electrode plate in the early stage of the cycle gradually increases), until the capacity of the electrode plate reaches its maximum value and then gradually decays, thereby improving the problem of capacity decay of the electrode plate in the early stage of the cycle, thereby improving the cycle life of the secondary battery containing the electrode plate.
[0006] In some embodiments, the first electrode film layer further includes a third electrode active material, and the average particle size Dv50 of the third electrode active material is smaller than the average particle size Dv50 of the first electrode active material.
[0007] In some embodiments, the ratio of the average particle size Dv50 of the third electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9):1, optionally, (0.1-0.5):1.
[0008] In some embodiments, the mass ratio of the third electrode active material to the first electrode active material is (0.005-0.5):1.
[0009] In some embodiments, the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9):1, and can be optionally (0.1-0.5):1.
[0010] In some embodiments, the mass ratio of the second electrode active material to the first electrode active material is (0.25-1):1.
[0011] In some embodiments, based on the mass of the first electrode film layer, the mass fraction of the first electrode active material is 64%-99%; optionally, the first electrode film layer also includes a third electrode active material, and based on the mass of the first electrode film layer, the mass fraction of the third electrode active material is 4%-32%.
[0012] In some embodiments, based on the mass of the second electrode film layer, the mass fraction of the second electrode active material is 95%-99%.
[0013] In some embodiments, the average particle size Dv50 of the first electrode active material is 1 μm-50 μm.
[0014] In some embodiments, a single-side thickness H1 of the first electrode film layer and a single-side thickness H2 of the second electrode film layer satisfy the following condition: H2≤H1≤10H2.
[0015] In some embodiments, a conductive layer is further included between the first electrode film layer and the second electrode film layer, and the conductive layer includes a carbon material.
[0016] In some embodiments, the carbon material includes one or more of carbon nanotubes, graphene, and carbon nanofibers.
[0017] In some embodiments, based on the mass of the conductive layer, the mass fraction of the carbon material is 95%-99%.
[0018] In some embodiments, the single-side thickness H3 of the conductive layer and the single-side thickness H1 of the first electrode film layer satisfy the following condition: 28H3≤H1≤85H3.
[0019] In some embodiments, the electrode plate is a positive electrode plate or a negative electrode plate;
[0020] Optionally, the compaction density of the positive electrode sheet is 2.3 g / cm 3 -2.7g / cm3 ;
[0021] Optionally, the compaction density of the negative electrode plate is 0.8 g / cm 3 -2.4g / cm 3 .
[0022] The second aspect of the present application provides a method for preparing the electrode sheet according to the first aspect of the present application, comprising the following steps:
[0023] forming the first electrode film layer on at least one side of the current collector;
[0024] The second electrode film layer is formed on the surface of the first electrode film layer.
[0025] In some embodiments, after forming the first electrode film layer and before forming the second electrode film layer, the method further includes: coating a conductive slurry containing a carbon material on a surface of the first electrode film layer to form a conductive layer;
[0026] The second electrode film layer is formed on a surface of the conductive layer away from the first electrode film layer.
[0027] The third aspect of the present application provides a secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet is the electrode sheet described in the first aspect of the present application or the electrode sheet prepared by the preparation method described in the second aspect of the present application.
[0028] A fourth aspect of the present application provides an electrical device comprising the secondary battery described in the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a schematic diagram of a secondary battery according to one embodiment of the present application.
[0030] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.
[0031] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application.
[0032] Figure 4 It is a schematic diagram of a battery pack according to one embodiment of the present application.
[0033] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.
[0034] Figure 6 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.
[0035] Description of reference numerals:
[0036] 1-battery pack; 2-upper box; 3-lower box; 4-battery module; 5-secondary battery; 51-housing; 52-electrode assembly; 53-cover plate; 6-electrical device. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0038] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0039] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0041] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0042] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0043] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0044] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0046] Secondary batteries include lithium-ion batteries and sodium-ion batteries. Cycle life is an important indicator for evaluating the performance of secondary batteries. For practical applications, the longer the cycle life of secondary batteries, the better. However, due to the rapid capacity decay of traditional secondary batteries during the cycle process, the cycle life needs to be further improved. The present application provides an electrode plate, including a current collector, a first electrode film layer and a second electrode film layer, the first electrode film layer and the second electrode film layer are sequentially stacked on the same side surface of the current collector, the first electrode film layer includes a first electrode active material, the second electrode film layer includes a second electrode active material, and the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material; by layering the first electrode film layer and the second electrode film layer, the average particle size Dv50 of the first electrode active material and the average particle size Dv50 of the second electrode active material are simultaneously regulated, so that the capacity of the electrode plate is slowly released, thereby effectively slowing down the capacity decay of the electrode plate during the cycle, and thus improving the cycle life of the secondary battery containing the electrode plate.
[0047] Electrode
[0048] One embodiment of the present application provides an electrode plate, including a current collector, a first electrode film layer and a second electrode film layer, the first electrode film layer and the second electrode film layer are sequentially stacked on the same side surface of the current collector, the first electrode film layer includes a first electrode active material, the second electrode film layer includes a second electrode active material, and the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material.
[0049] In the above-mentioned electrode sheet, the first electrode film layer is closer to the current collector, and the second electrode film layer is farther from the current collector. When the active ions are embedded in the electrode sheet, they enter the second electrode film layer and the first electrode film layer in turn. Since the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material, the transmission speed of the active ions in the first electrode film layer is slower than that in the second electrode film layer, so that the capacity of the electrode sheet in the early stage of the cycle is slowly released and the capacity is in a climbing state (that is, the capacity released by the electrode sheet in the early stage of the cycle gradually increases), until the capacity of the electrode sheet reaches the maximum value and then gradually decays, which improves the problem of the capacity decay of the electrode sheet in the early stage of the cycle, and thus improves the cycle life of the secondary battery containing the electrode sheet. It can be understood that the first electrode film layer and the second electrode film layer can be located on one side surface of the current collector in the thickness direction, or on both side surfaces of the current collector in the thickness direction. Active ions include but are not limited to lithium ions and sodium ions.
[0050] Dv50 refers to the particle size corresponding to 50% in the volume distribution. As an example, Dv50 can refer to the particle size distribution laser diffraction method of GB / T19077-2016, peel the first electrode film layer and the second electrode film layer from the current collector, and conveniently measure it using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK.
[0051] In addition, Dv50 can also be determined using a scanning electron microscope (SEM) (e.g., ZEISS Sigma 300). By taking photos of the surface / cross-section of the electrode plate using SEM, the morphology of the surface / cross-section can be confirmed, and the Dv50 of each material in the electrode plate can be measured and counted.
[0052] In some embodiments, the first electrode film layer further includes a third electrode active material, and the average particle size Dv50 of the third electrode active material is smaller than the average particle size Dv50 of the first electrode active material. The third electrode active material added to the first electrode film layer increases the compaction density of the electrode sheet, thereby increasing the energy density of the secondary battery containing the electrode sheet, which refers to the volume energy density of the secondary battery.
[0053] In some embodiments, the ratio of the average particle size Dv50 of the third electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9):1. Controlling the ratio of the average particle size Dv50 of the above two materials to the above range is beneficial to improving the energy density of the secondary battery. It is understandable that the ratio of the average particle size Dv50 of the above two materials includes but is not limited to: 0.1:1, 0.2:1, 0.3:1, 0.5:1, 0.7:1, 0.9:1. Specifically, the ratio of the average particle size Dv50 of the third electrode active material to the average particle size Dv50 of the first electrode active material can be selected as (0.1-0.5):1.
[0054] In some embodiments, the mass ratio of the third electrode active material to the first electrode active material is (0.005-0.5):1. When the mass ratio of the third electrode active material to the first electrode active material is relatively large, the capacity of the electrode sheet in the early stage of the cycle is released faster; when the mass ratio of the third electrode active material to the first electrode active material is relatively small, the energy density of the secondary battery containing the above-mentioned electrode sheet is not significantly improved. Therefore, controlling the mass ratio of the third electrode active material to the first electrode active material is conducive to further improving the cycle life of the secondary battery containing the above-mentioned electrode sheet, while significantly improving the energy density of the secondary battery. It can be understood that the mass ratio of the third electrode active material to the first electrode active material includes but is not limited to: 0.005:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1.
[0055] In some embodiments, the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9): 1. By controlling the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material to be within the above range, the transmission speed of the active ions in the second electrode film layer and the first electrode film layer can be further controlled, so that the capacity of the electrode sheet in the early stage of the cycle is slowly released and the capacity is in a climbing state, thereby further improving the cycle life of the secondary battery containing the above electrode sheet. It should be noted that when the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material is large, the capacity of the electrode sheet in the early stage of the cycle will be released faster, and the cycle attenuation performance will not be significantly improved. It can be understood that the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material includes but is not limited to: 0.1: 1, 0.2: 1, 0.3: 1, 0.4: 1, 0.5: 1, 0.6: 1, 0.7: 1, 0.8: 1, 0.9: 1. Specifically, the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material can be selected as (0.1-0.5): 1.
[0056] In some embodiments, the mass ratio of the second electrode active material to the first electrode active material is (0.25-1):1. When the mass ratio of the second electrode active material to the first electrode active material is relatively large or small, the capacity of the electrode sheet in the early stage of the cycle is released faster or slower, and the cycle performance is not significantly improved. Therefore, controlling the mass ratio of the second electrode active material to the first electrode active material is beneficial to further significantly improve the cycle life of the secondary battery containing the above-mentioned electrode sheet. It can be understood that the mass ratio of the second electrode active material to the first electrode active material includes but is not limited to: 0.25:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1.
[0057] In some embodiments, based on the mass of the first electrode film layer, the mass fraction of the first electrode active material is 64%-99%. It is understood that based on the mass of the first electrode film layer, the mass fraction of the first electrode active material includes but is not limited to: 64%, 70%, 75%, 80%, 85%, 90%, 95%, 99%. Optionally, the first electrode film layer also includes a third electrode active material, and based on the mass of the first electrode film layer, the mass fraction of the third electrode active material is 4%-32%. As an example, the mass fraction of the third electrode active material can be 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 25%, 28%, 32%.
[0058] In some embodiments, based on the mass of the second electrode film layer, the mass fraction of the second electrode active material is 95%-99%. As an example, the mass fraction of the second electrode active material can be 95%, 96%, 97%, 98%, 99%.
[0059] Optionally, the average particle size Dv50 of the first electrode active material is 1 μm-50 μm. It is understood that the average particle size Dv50 of the first electrode active material includes but is not limited to: 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm.
[0060] In some embodiments, the single-side thickness H1 of the first electrode film layer and the single-side thickness H2 of the second electrode film layer satisfy the following condition: H2≤H1≤10H2.
[0061] The single-side thickness H1 of the first electrode film layer and the single-side thickness H2 of the second electrode film layer can be tested by methods known in the art, for example, by a step profiler test method. The stylus of the step profiler gently rubs across the sample surface with a very small force, and the micron or even nanometer level ups and downs of the sample surface are amplified millions of times by the sensor connected to the stylus, and then converted into electronic signals, input into computer software, and finally displayed in the form of digital and graphical data.
[0062] In some embodiments, a conductive layer is further provided between the first electrode film layer and the second electrode film layer, and the conductive layer includes a carbon material. The conductive layer containing the carbon material can improve the electronic conductivity, thereby improving the cycle performance of the secondary battery and its rate performance.
[0063] Optionally, the carbon material includes, but is not limited to, one or more of carbon nanotubes, graphene, and carbon nanofibers.
[0064] Optionally, based on the mass of the conductive layer, the mass fraction of the carbon material is 95%-99%. As an example, the mass fraction of the carbon material can be 95%, 96%, 97%, 98%, 99%.
[0065] Furthermore, the thickness H3 of the conductive layer on one side and the thickness H1 of the first electrode film layer on one side satisfy the following condition: 28H3≤H1≤85H3. In this way, the rate performance of the secondary battery can be further improved. As an example, the thickness H1 of the first electrode film layer on one side can be 28H3, 30H3, 40H3, 50H3, 60H3, 70H3, 80H3, 85H3.
[0066] In some embodiments, the electrode plate is a positive electrode plate or a negative electrode plate.
[0067] Positive electrode
[0068] The current collector used in the positive electrode sheet is a positive electrode current collector, and the first electrode active material, the second electrode active material and the third electrode active material are positive electrode active materials.
[0069] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0070] In some embodiments, the first electrode active material, the second electrode active material and the third electrode active material include one or more of lithium iron phosphate, ternary materials, lithium manganese phosphate and lithium cobalt oxide. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more. Among them, ternary materials such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 )、LiNi 0.85 Co 0.15 Al 0.05 At least one of O2 and its modified compounds, etc.
[0071] In some embodiments, the first electrode active material, the second electrode active material, and the third electrode active material include sodium ion active materials.
[0072] As an example, the sodium ion active material may include at least one of the following materials: at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.
[0073] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0074] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence state.
[0075] Polyanionic compounds can also be those with sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0076] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0077] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2 (P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0078] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0079] In some embodiments, the first electrode film layer and the second electrode film layer may further include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0080] In some embodiments, the first electrode film layer and the second electrode film layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0081] In some embodiments, the compaction density of the positive electrode sheet is 2.3 g / cm 3 -2.7g / cm 3 It is understood that the compaction density of the positive electrode includes but is not limited to: 2.3g / cm 3 , 2.4g / cm 3 , 2.5g / cm 3 , 2.6g / cm 3 , 2.7g / cm 3 Furthermore, the compaction density of the positive electrode sheet is 2.4g / cm 3 -2.5g / cm 3 .
[0082] Negative electrode
[0083] The current collector used in the negative electrode sheet is a negative electrode current collector, and the first electrode active material, the second electrode active material and the third electrode active material are negative electrode active materials.
[0084] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0085] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0086] In some embodiments, the first electrode film layer and the second electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0087] In some embodiments, the first electrode film layer and the second electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0088] In some embodiments, the first electrode film layer and the second electrode film layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0089] In some embodiments, the compaction density of the negative electrode sheet is 0.8 g / cm 3 -2.4g / cm 3 It is understood that the compaction density of the negative electrode sheet includes but is not limited to: 0.8g / cm3 , 1g / cm 3 , 1.2g / cm 3 , 1.4g / cm 3 , 1.6g / cm 3 , 1.8g / cm 3 , 2g / cm 3 , 2.2g / cm 3 , 2.4g / cm 3 Furthermore, the compaction density of the negative electrode sheet is 1g / cm 3 -2g / cm 3 .
[0090] Another embodiment of the present application provides a method for preparing the above-mentioned electrode sheet, comprising the following steps:
[0091] forming a first electrode film layer on at least one side of the current collector;
[0092] A second electrode film layer is formed on the surface of the first electrode film layer.
[0093] Therefore, the electrode plates can be easily prepared, which is convenient for large-scale production.
[0094] In some embodiments, the electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the electrode sheet, such as the first electrode active material, the second electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a first electrode slurry and a second electrode slurry; the first electrode slurry and the second electrode slurry are coated on the current collector, and after drying, cold pressing and other processes, the electrode sheet can be obtained.
[0095] In some embodiments, after forming the first electrode film layer and before forming the second electrode film layer, the method further includes: coating a conductive paste containing a carbon material on a surface of the first electrode film layer to form a conductive layer;
[0096] The second electrode film layer is formed on a surface of the conductive layer away from the first electrode film layer.
[0097] The conductive layer containing carbon material can improve the electronic conductivity, thereby improving the cycle performance of the secondary battery and improving its rate performance, and the preparation method of the conductive layer is relatively simple.
[0098] The above-mentioned conductive paste containing carbon material may also optionally include a binder, and the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin.
[0099] In addition, the secondary battery and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0100] An embodiment of the present application provides a secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet is the above-mentioned electrode sheet or the electrode sheet prepared by the above-mentioned preparation method.
[0101] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0102] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0103] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0104] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0105] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0106] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0107] Isolation film
[0108] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0109] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0110] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0111] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0112] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0113] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.
[0114] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0115] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0116] Figure 3 4 is an example of a battery module. Figure 3In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.
[0117] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0118] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0119] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0120] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.
[0121] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0122] Figure 6 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.
[0123] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0124] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0125] Example 1
[0126] The lithium-ion battery was prepared as follows:
[0127] (1) Preparation of slurry: LFP with a Dv50 of 0.5 μm, LFP (lithium iron phosphate) with a Dv50 of 1.2 μm and a carbon coating content of 1.2%, conductive carbon black, polyvinylidene fluoride and N-methylpyrrolidone are mixed in a mass ratio of 20:76:2:2 to obtain a first slurry, and the solid content of the first slurry is 40%; LFP with a Dv50 of 0.5 μm, conductive carbon black, polyvinylidene fluoride and N-methylpyrrolidone are mixed in a mass ratio of 96:2:2 to obtain a second slurry with a solid content of 40%; carbon nanotubes are mixed with sodium carboxymethyl cellulose, polyvinylidene fluoride and N-methylpyrrolidone in a mass ratio of 2:3:5:90 to form a conductive slurry;
[0128] (2) Preparation of positive electrode sheet: The first slurry was coated on both surfaces of the positive electrode current collector (aluminum foil), the conductive slurry was coated on the surface of the first slurry, and the second slurry was coated on the surface of the conductive slurry. The slurry was dried at 120°C for 3 hours and cold pressed to obtain a compaction density of 2.56 g / cm 3 A positive electrode sheet, wherein the single-side thickness of the first positive electrode film layer is 150 μm, the single-side thickness of the conductive layer is 3 μm, and the single-side thickness of the second positive electrode film layer is 30 μm;
[0129] (3) Preparation of negative electrode sheet: negative electrode active material (graphite), conductive agent (SP), binder (SBR), thickener (CMC) were mixed and dispersed with deionized water in a mass ratio of 97:0.7:0.8:1.5 to obtain negative electrode slurry; the negative electrode slurry was coated on both surfaces of copper foil, dried and cold pressed to obtain a compaction density of 1.5 g / cm 3 The negative electrode;
[0130] (4) Preparation of lithium-ion battery: The positive electrode sheet prepared in step (2), the negative electrode sheet prepared in step (3) and the isolation film are wound to obtain a bare battery cell, and then a square shell battery is obtained through packaging, liquid injection, formation, exhaust and other processes. The isolation film is a polyethylene isolation film, and the electrolyte is an electrolyte formed by dissolving lithium salt LiPF6 in an organic solvent, wherein the organic solvent is a mixed solution containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), the volume ratio of EC, EMC and DEC is 20:20:60, and the concentration of lithium salt is 1 mol / L.
[0131] Embodiment 2-20
[0132] It is basically the same as Example 1, except that the parameters described in Table 1 and Table 2 are different.
[0133] Embodiment 21
[0134] The lithium-ion battery was prepared as follows:
[0135] (1) Preparation of slurry: Graphite with a Dv50 of 0.5 μm, graphite with a Dv50 of 1.2 μm, conductive carbon black, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are mixed with deionized water in a mass ratio of 17:80:0.7:1.5:0.8 to obtain a first slurry, wherein the solid content of the first slurry is 60%; graphite with a Dv50 of 0.5 μm, conductive carbon black, sodium carboxymethyl cellulose and styrene-butadiene rubber are mixed with deionized water in a mass ratio of 97:0.7:1.5:0.8 to obtain a second slurry with a solid content of 60%; carbon nanotubes are mixed with sodium carboxymethyl cellulose, polyvinylidene fluoride and N-methylpyrrolidone in a mass ratio of 2:3:5:90 to form a conductive slurry;
[0136] (2) Preparation of negative electrode sheet: The first slurry was coated on both surfaces of the negative electrode current collector (copper foil), the conductive slurry was coated on the surface of the first slurry, and the second slurry was coated on the surface of the conductive slurry. The slurry was dried at 120°C for 3 hours and cold pressed to obtain a compaction density of 1.5 g / cm 3 A negative electrode sheet, wherein the single-side thickness of the first negative electrode film layer is 150 μm, the single-side thickness of the conductive layer is 3 μm, and the single-side thickness of the second negative electrode film layer is 30 μm;
[0137] (3) Preparation of positive electrode sheet: The positive electrode active material (lithium iron phosphate with a carbon coating content of 1.2%), the conductive agent (conductive carbon black), and the binder (polyvinylidene chloride) were mixed and dispersed with N-methylpyrrolidone in a mass ratio of 96:2:2 to obtain a positive electrode slurry; the positive electrode slurry was coated on both surfaces of the aluminum foil, dried, and cold pressed to obtain a compaction density of 2.56 g / cm 3 The positive electrode;
[0138] (4) Preparation of lithium-ion battery: The negative electrode sheet prepared in step (2), the positive electrode sheet prepared in step (3) and the isolation film are wound to obtain a bare battery cell, and then a square shell battery is obtained through packaging, liquid injection, formation, exhaust and other processes. The isolation film is a polyethylene isolation film, and the electrolyte is an electrolyte formed by dissolving lithium salt LiPF6 in an organic solvent, wherein the organic solvent is a mixed solution containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), the volume ratio of EC, EMC and DEC is 20:20:60, and the concentration of lithium salt is 1 mol / L.
[0139] Examples 22-23
[0140] It is basically the same as Example 21, except that the parameters described in Table 1 and Table 2 are different.
[0141] Comparative Examples 1-3
[0142] It is basically the same as Example 1, except that the parameters described in Table 1 and Table 2 are different.
[0143] Comparative Examples 4-6
[0144] It is basically the same as Example 21, except that the parameters described in Table 1 and Table 2 are different.
[0145] Performance Testing
[0146] 1. Compacted density test: According to the energy density design requirements, the pole piece coating surface density can be determined. After the pole piece is dried and cold pressed, use a micrometer to measure the total thickness of the pole piece, and the coating thickness can be calculated by deducting the current collector. Based on the two parameters of coating surface density and coating thickness, the compacted density of the pole piece can be calculated.
[0147] 2. Energy density test: Charge the battery to 3.65V at 1P constant power, and then discharge it to 2.5V at 1P constant power. Record the discharge energy and calculate the 1P energy density;
[0148] Energy density (Wh / L) = discharge capacity (Wh) / volume of lithium-ion battery (L).
[0149] 3. Cycle performance test: (1) stand for 5 min, (2) discharge at 0.5P to 2.5V, (3) stand for 30 min, (4) charge at 0.5P constant power to 3.65V, (5) stand for 1 min, (6) charge at 0.05P constant power to 3.65V, (7) stand for 30 min, (8) discharge at 0.5P constant power to 2.5V, (9) stand for 30 min; repeat steps (4)-(9) to make the battery perform 2000 charge and discharge cycles, and calculate the capacity retention rate of the battery after 2000 discharge cycles.
[0150] In Table 1-2, the ratio of the average particle size Dv50 of the third electrode active material to the average particle size Dv50 of the first electrode active material is A1, and the ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material is A2; the mass ratio of the third electrode active material to the first electrode active material is M1, and the mass ratio of the second electrode active material to the first electrode active material is M2.
[0151] Table 1
[0152]
[0153]
[0154]
[0155]
[0156] Table 2
[0157]
[0158]
[0159]
[0160] It can be seen from Table 1 and Table 2 that, compared with Comparative Examples 1-3, the capacity retention rate of the batteries prepared in Examples 1-20 after 2000 cycles is significantly improved; compared with Comparative Examples 4-6, the capacity retention rate of the batteries prepared in Examples 21-23 after 2000 cycles is significantly improved; This indicates that the present application effectively improves the cycle life of the battery by controlling the average particle size Dv50 of the first electrode active material in the first electrode film layer of the positive electrode sheet or the negative electrode sheet to be greater than the average particle size Dv50 of the second electrode active material in the second electrode film layer.
[0161] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0162] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the specification and drawings may be used to interpret the contents of the claims.
Claims
1. An electrode plate, characterized in that: It includes a current collector, a first electrode film layer and a second electrode film layer, the first electrode film layer and the second electrode film layer are stacked in sequence on the same side surface of the current collector, the first electrode film layer includes a first electrode active material, the second electrode film layer includes a second electrode active material, and the average particle size Dv50 of the first electrode active material is greater than the average particle size Dv50 of the second electrode active material.
2. The electrode plate according to claim 1, characterized in that: The first electrode film layer further includes a third electrode active material, wherein the average particle size Dv50 of the third electrode active material is smaller than the average particle size Dv50 of the first electrode active material; Optionally, the ratio of the average particle size Dv50 of the third electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9):1, more optionally, (0.1-0.5):1; Optionally, the mass ratio of the third electrode active material to the first electrode active material is (0.005-0.5):
1.
3. The electrode plate according to claim 1 or 2, characterized in that: The ratio of the average particle size Dv50 of the second electrode active material to the average particle size Dv50 of the first electrode active material is (0.1-0.9):1, and can be (0.1-0.5):1; Optionally, the mass ratio of the second electrode active material to the first electrode active material is (0.25-1):1; Optionally, based on the mass of the first electrode film layer, the mass fraction of the first electrode active material is 64%-99%; Optionally, the first electrode film layer further includes a third electrode active material, and based on the mass of the first electrode film layer, the mass fraction of the third electrode active material is 4%-32%; Optionally, based on the mass of the second electrode film layer, the mass fraction of the second electrode active material is 95%-99%; Optionally, the average particle size Dv50 of the first electrode active material is 1 μm-50 μm.
4. The electrode plate according to claim 1 or 2, characterized in that: The single-side thickness H1 of the first electrode film layer and the single-side thickness H2 of the second electrode film layer satisfy the following condition: H2≤H1≤10H2.
5. The electrode plate according to claim 1 or 2, characterized in that: A conductive layer is further included between the first electrode film layer and the second electrode film layer, and the conductive layer includes a carbon material; Optionally, the carbon material includes one or more of carbon nanotubes, graphene and carbon nanofibers; Optionally, based on the mass of the conductive layer, the mass fraction of the carbon material is 95%-99%; Optionally, a single-side thickness H3 of the conductive layer and a single-side thickness H1 of the first electrode film layer satisfy the following condition: 28H3≤H1≤85H3.
6. The electrode plate according to claim 1 or 2, characterized in that: The electrode plate is a positive electrode plate or a negative electrode plate; Optionally, the compaction density of the positive electrode sheet is 2.3 g / cm 3 -2.7g / cm 3 ; Optionally, the compaction density of the negative electrode plate is 0.8 g / cm 3 -2.4g / cm 3 .
7. The method for preparing an electrode sheet according to any one of claims 1 to 6, characterized in that: The steps include: forming the first electrode film layer on at least one side of the current collector; The second electrode film layer is formed on the surface of the first electrode film layer.
8. The preparation method according to claim 7, characterized in that: After forming the first electrode film layer and before forming the second electrode film layer, the method further includes: coating a conductive paste containing a carbon material on a surface of the first electrode film layer to form a conductive layer; The second electrode film layer is formed on a surface of the conductive layer away from the first electrode film layer.
9. A secondary battery, characterized in that: It comprises a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet is the electrode sheet according to any one of claims 1 to 6 or the electrode sheet prepared by the preparation method according to any one of claims 7 to 8.
10. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 9.
Citation Information
Patent Citations
Negative electrode of lithium ionic cell, preparing method and cell thereof
CN101453013A
High-power high-capacity lithium ion battery and preparation method thereof
CN106469825A
Lithium-ion battery separator and application thereof
CN106684298A
Negative pole piece, preparation method of negative pole piece, secondary battery and power utilization device
CN115084437A
Positive pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device
CN115832183A
Cited By
Sodium secondary battery and electric device
CN120767378A