Battery pole piece, battery as well as preparation method and application of battery pole piece
By designing specific active material layer areas and porosity distribution on the battery electrode, the problems of SOC unevenness and lithium evolution during the battery charging and discharging process are solved, and the fast charging performance and cycle stability of the battery are improved.
Patent Information
- Application Number
- CN202411369879.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the battery charging and discharging process, the temperature is high due to the enrichment of overcurrent on the positive and negative electrode ears, resulting in uneven current density and uneven SOC, which affects the fast charging performance and cyclic storage life of the battery, and the electrolyte in the middle of the electrode sheet is not wet. It fully leads to lithium extraction and affects the battery cycle life.
The active material layer of the battery electrode sheet is designed to be arranged in parallel along the length direction, and the first area, second area and third area are arranged in parallel, and the position and porosity are specially designed so that the liquid phase diffusion impedance in the intermediate area is lower than the two sides, offsetting the temperature difference. The low impedance problem caused by improving SOC uniformity and avoiding lithium evolution.
The SOC uniformity of the battery pole plate during charging and discharging is achieved, the lithium-ion phenomenon is avoided, the fast charging capacity and cycle stability of the battery are improved, and the battery life is extended.
Smart Images

Figure CN119069634A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of battery pole piece preparation, and in particular, to a battery pole piece, a battery, and a preparation method and application thereof. Background Art
[0002] During the battery charging and discharging process, overcurrent enrichment on the positive and negative pole ears causes the temperature on the positive and negative pole ears to be higher than the middle area away from the positive and negative pole ears. The temperature rise causes the impedance at the positive and negative pole ears to be lower. At the beginning of battery charging, the current density near the positive and negative pole ears is larger, resulting in uneven current density and SOC (State Of Charge) of the battery pole piece in the length direction, which in turn affects the normal performance of important electrochemical properties such as the fast charging performance and cycle storage life of the battery. In addition, the long pole piece length will also lead to insufficient electrolyte infiltration in the middle of the pole piece, resulting in lithium precipitation and other phenomena, which will affect the battery cycle life. Summary of the invention
[0003] In view of this, the present application provides a battery electrode, a battery, and a preparation method and application thereof, wherein the active material layer of the battery electrode comprises a first region, a second region, and a third region which are arranged in parallel in sequence along the length direction of the battery electrode, and the positions and porosities of the first region, the second region, and the third region are specially designed, so that the battery electrode has a high porosity in the middle and low porosity at both ends in the length direction, and the liquid phase diffusion impedance in the middle is lower than that on both sides, thereby offsetting the problem of inconsistent SOC in different regions of the electrode during the charging process due to low impedance caused by high temperature on both sides of the electrode ear caused by temperature difference, thereby improving the SOC uniformity of the battery during the charging and discharging process. In addition, the structure can also effectively avoid lithium plating during the cycle process caused by lack of electrolyte in the middle of the battery electrode due to poor wetting, thereby improving the cycle performance of the battery.
[0004] In a first aspect, the present application provides a battery electrode, which includes a current collector and an active material layer arranged on the surface of the current collector; the active material layer includes a first region, a second region and a third region arranged in parallel along the length direction of the battery electrode; the porosity of the second region is 25%-40%, the porosity of the second region is 2%-10% greater than the porosity of the first region, and the porosity of the second region is 2%-10% greater than the porosity of the third region.
[0005] In the embodiment of the present application, the porosity of the second region is 29%-35%.
[0006] In the embodiment of the present application, in the length direction of the battery electrode sheet, the distance between the center line of the second region and the center line of the active material layer is 0-100 mm.
[0007] In the embodiment of the present application, the porosity of the first region and the porosity of the third region are the same.
[0008] In the embodiment of the present application, the length of the second region in the length direction of the battery electrode sheet accounts for 25%-70% of the total length of the battery electrode sheet.
[0009] In an embodiment of the present application, the second region includes a pore structure, and the pore size of the pore structure is 0.01 μm-3 μm.
[0010] In the embodiment of the present application, the thickness of the active material layer is 110 μm-250 μm, and the thickness of the current collector is 4.5 μm-17 μm.
[0011] A second aspect of the present application provides a battery, which includes the battery electrode provided in the first aspect of the present application.
[0012] The third aspect of the present application provides a method for preparing the battery provided in the second aspect of the present application, comprising:
[0013] preparing a first active slurry, a second active slurry and a third active slurry, wherein the second active slurry includes an electrolyte additive;
[0014] The first active slurry, the second active slurry and the third active slurry are sequentially coated on the current collector along the length direction of the current collector to obtain the first region precursor, the second region precursor and the third region precursor respectively, thereby obtaining a battery pole sheet precursor;
[0015] After assembling the battery pole piece precursor and the diaphragm, injecting electrolyte, a battery is obtained; the battery pole piece precursor corresponds to the battery pole piece; the first region precursor corresponds to the first region, the second region precursor corresponds to the second region, and the third region precursor corresponds to the third region.
[0016] In an embodiment of the present application, the electrolyte additive includes one or more of 1,2-vinylidene carbonate, 1,3-propylene sultone, 1,3-propane sultone, methanedisulfonic acid methylene ester, 1,4-butane sultone, vinyl sulfate, succinonitrile, 2-fluorobiphenyl, succinic anhydride, phthalic anhydride, vinyl carbonate, vinyl ethylene carbonate and fluoroethylene carbonate.
[0017] In the embodiment of the present application, the mass percentage of the electrolyte additive in the second active slurry is 0.5%-10%.
[0018] In some embodiments of the present application, the mass percentage of the electrolyte additive in the second active slurry is 1%-5%.
[0019] In an embodiment of the present application, the coating surface density of the second region is lower than that of the first region, and the absolute value of the difference between the coating surface density of the second region and the first region is less than or equal to 15%; and / or the coating surface density of the second region is lower than that of the third region, and the absolute value of the difference between the coating surface density of the second region and the third region is less than or equal to 15%.
[0020] The fourth aspect of the present application provides an electrical device, which includes the battery provided in the second aspect of the present application or a battery prepared by the method for preparing the battery provided in the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the cross-sectional structure of a battery electrode provided in one embodiment of the present application;
[0022] Figure 2 A flow chart of a method for preparing a battery provided in one embodiment of the present application.
[0023] Description of Figure Numbers
[0024] 100 - battery pole piece; 11 - current collector; 12 - active material layer; 121 - first region; 122 - second region; 123 - third region. DETAILED DESCRIPTION
[0025] The present application is further described in detail below in conjunction with preferred embodiments, but the protection scope of the present application is not limited to the following specific embodiments.
[0026] In the present application, all professional terms have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present application.
[0027] Existing battery pole pieces are generally designed to be uniform in the length direction, that is, the active materials in the battery pole pieces are evenly distributed at the same thickness position. However, during the actual battery charging and discharging process, overcurrent enrichment on the positive and negative pole ears causes the temperature on the positive and negative pole ears to be higher than the middle area away from the positive and negative pole ears. The temperature rise causes the impedance at the positive and negative pole ears to be lower. At the initial stage of battery charging, the current density near the positive and negative pole ears is larger, resulting in uneven current density and SOC (State Of Charge) of the battery pole piece in the length direction, which in turn affects the normal performance of important electrochemical properties such as the fast charging performance and cycle storage life of the battery. In addition, the uneven current density will also cause different degrees of de-embedding / embedding of the battery pole piece at different positions, and it is more likely to cause adverse phenomena such as lithium precipitation, which further affects the electrochemical performance of the battery. In addition, the long length of the battery pole piece may also cause the electrolyte content in the middle area of the battery pole piece to be less than the area near the positive and negative ears due to insufficient electrolyte infiltration or slow electrolyte diffusion. The electrolyte consumption during the cycle process causes liquid shortage in the middle area and lithium precipitation, which leads to the battery cell experiencing a cycle dive.
[0028] In response to the above problems, the present application provides a battery electrode, the active material layer of which includes a first region, a second region and a third region arranged in sequence along the length direction of the battery electrode, and the positions and porosities of the first region, the second region and the third region are specially designed, so that the battery electrode has a high porosity in the middle and low porosity at both ends in the length direction, and the liquid phase diffusion impedance of the second region in the middle is lower than that of the first region and the third region on both sides, which offsets the problem of inconsistent SOC in different regions of the electrode during the charging process caused by low impedance caused by high temperature near the positive and negative electrode ears due to temperature difference, thereby improving the SOC uniformity of the battery during the charging and discharging process. In addition, the structure can also effectively avoid lithium plating during the cycle process caused by lack of electrolyte in the middle of the battery electrode due to poor wetting, thereby improving the cycle performance of the battery.
[0029] See also Figure 1The present application provides a battery electrode 100, which includes a current collector 11 and an active material layer 12 disposed on the surface of the current collector 11. In the embodiment of the present application, the active material layer 12 includes a first region 121, a second region 122, and a third region 123 which are sequentially arranged in parallel along the length direction of the battery electrode 100, that is, the second region 122 is located in the middle position in the length direction of the battery electrode 100, and the first region 121 and the third region 123 are located at both ends in the length direction of the battery electrode 100. In the embodiment of the present application, the electrode tabs are located at both ends in the length direction of the battery electrode 100, that is, in the length direction of the battery electrode 100, the first region 121 and the third region 123 are close to one side of the electrode tab, and the second region 122 is far away from one side of the electrode tab. In the embodiment of the present application, the porosity of the second region 122 is 25%-40%, the porosity of the second region 122 is 2%-10% greater than the porosity of the first region 121, and the porosity of the second region 122 is 2%-10% greater than the porosity of the third region 123. The present application controls the porosity of the second region 122 located in the middle of the battery pole piece 100 to be greater than the porosity of the first region 121 and the third region 123. On the one hand, the porosity of the second region 122 is larger, and the liquid phase diffusion impedance is lower, which makes up for the uneven current distribution problem caused by the lower impedance of the first region 121 and the third region 123 caused by the temperature difference, so that the reaction current of the active material layer 12 in the length direction of the battery pole piece 100 is more uniform, and the electrochemical reaction occurs at the same rate at the same time, so that the battery pole piece as a whole presents a uniform SOC in the length direction, effectively avoiding the uneven degree of lithium extraction / insertion of the battery pole piece 100 in the length direction, and largely avoiding the occurrence of lithium precipitation, thereby improving the fast charging capability, cycle stability, battery capacity and service life of the battery. In an embodiment of the present application, the porosity of the second region 122 is 25%-40%. In some specific embodiments, the porosity of the second region 122 may be, for example, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 40%. In some embodiments of the present application, the porosity of the second region 122 is 29%-35%. By controlling the porosity of the second region within an appropriate range, the present application can reduce resistance and improve the electrolyte retention capacity while ensuring that the active material in the second region provides sufficient battery capacity, thereby improving the SOC uniformity of the battery pole piece in the length direction and effectively avoiding the occurrence of lithium deposition on the battery pole piece. In an embodiment of the present application, the porosity of the second region 122 is 2%-10% greater than the porosity of the first region 121.In some specific embodiments, the porosity of the second region 122 may be, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% greater than the porosity of the first region 121. In the embodiment of the present application, the porosity of the second region 122 is 2%-10% greater than the porosity of the third region 123. In some specific embodiments, the porosity of the second region 122 may be, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% greater than the porosity of the third region 123. The present application controls the porosity of the second region to be greater than the porosity of the first region and the third region, and controls the porosity difference within an appropriate range, so that the impedance non-uniformity of the active material layer can match the current density distribution non-uniformity during actual battery application, thereby making the reaction current of the active material layer 12 in the length direction of the battery electrode 100 uniform, thereby improving the fast charging capability and cycle performance of the battery electrode.
[0030] In some embodiments of the present application, in the length direction of the battery electrode 100, the distance between the center line of the second region 122 and the center line of the active material layer 12 is 0-100 mm. In some specific embodiments, in the length direction of the battery electrode 100, the distance between the center line of the second region 122 and the center line of the active material layer 12 can be, for example, 0 mm, 10 mm, 20 mm, 30 mm, 50 mm, 100 mm. When the distance between the center line of the second region 122 and the center line of the active material layer 12 is 0 mm in the length direction of the battery electrode 100, that is, in the length direction of the battery electrode 100, the center line of the second region 122 coincides with the center line of the active material layer 12. In the length direction of the battery pole piece 100, the smaller the distance between the center line of the second region 122 and the center line of the active material layer 12, the better the uniformity of the current density and SOC of the battery pole piece 100 during the cycle use. However, there are certain errors in the actual production and preparation process, which makes it impossible for the center line of the second region 122 to completely coincide with the center line of the active material layer 12. The present application controls the distance between the second region and the center line of the active material layer in the length direction of the battery pole piece so that the second region is located in the middle of the battery pole piece as much as possible, and the distribution of the first region and the third region is more symmetrical, thereby further optimizing the impedance design of the pole piece, so that the current density and SOC of the battery pole piece during the cycle use are more uniform.
[0031] In some embodiments of the present application, the active material layer 12, the first region 121, the second region 122, and the third region 123 are all rectangular. That is, the present application arranges the second region 122 at a relatively middle position in the length direction of the active material layer 12, and the first region 121 and the third region 123 are located at both ends in the length direction of the active material layer 12, so that the second region with a larger porosity can be kept away from the positive and negative tabs at both ends of the battery pole piece 100, and the distribution of the first region and the third region in the length direction of the pole piece is relatively symmetrical, further optimizing the impedance design of the pole piece, so that the current density and SOC of the battery pole piece during the cycle use process are more uniform.
[0032] In some embodiments of the present application, the porosity of the first region 121 and the third region 123 are the same. The present application controls the porosity of the first region and the third region to be the same, thereby controlling the impedance of the first region and the third region and the electrolyte absorption and retention capacity to be roughly the same, further improving the current density and SOC uniformity of the electrode plate at both ends near the positive and negative tabs.
[0033] In the embodiment of the present application, the length of the second region 122 in the length direction of the battery electrode sheet 100 accounts for 25%-70% of the total length of the battery electrode sheet 100. In some specific embodiments, the length of the second region 122 in the length direction of the battery electrode sheet 100 may account for 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% of the total length of the battery electrode sheet 100. By controlling the length of the second region in the length direction of the battery electrode sheet within a suitable range, it is possible to further match the non-uniformity of the current density of the battery electrode sheet, thereby further improving the SOC uniformity of the battery electrode sheet in the length direction. In some embodiments of the present application, the length of the second region 122 in the length direction of the battery electrode sheet 100 may account for 40%-60% of the total length of the battery electrode sheet 100.
[0034] In the embodiment of the present application, the active material layer 12 may be distributed on one side surface of the current collector 11, or may be distributed on both side surfaces of the current collector 11. In some embodiments, the active material layer 12 is distributed on both side surfaces of the current collector 11. When the active material layer 12 is distributed on both side surfaces of the current collector 11, the length distribution of the first region 121, the second region 122, and the third region 123 of the active material layer 12 on both sides of the current collector in the length direction of the battery pole piece may be the same or different. In some specific embodiments, the length distribution of the first region 121, the second region 122, and the third region 123 of the active material layer 12 on both sides of the current collector in the length direction of the battery pole piece is the same, that is, the first region 121, the second region 122, and the third region 123 of the active material layer 12 on both sides of the current collector are symmetrically distributed in the thickness direction of the current collector.
[0035] In the embodiment of the present application, the second region 122 includes a pore structure, and the pore size of the pore structure is 0.01μm-3μm. In some specific embodiments, the pore size of the pore structure can be, for example, 0.01μm, 0.02μm, 0.05μm, 0.08μm, 0.1μm, 0.2μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm. In the present application, the pore size of the pore structure refers to the maximum cross-sectional lateral dimension of the pore structure. In some embodiments, when the pore structure is circular, the pore size is the diameter. The present application can further enhance the charge transfer in the second region by specially designing the pore structure of the second region. In addition, the special design of the pore structure can further enhance the absorption and storage capacity of the second region for the electrolyte, so as to ensure that the second region in the middle of the battery during the cycle has sufficient electrolyte to prevent lithium precipitation caused by the exhaustion of the electrolyte, thereby affecting the cycle performance of the battery.
[0036] In the embodiment of the present application, the thickness of the active material layer 12 is 110 μm-250 μm, and the thickness of the current collector 11 is 4.5 μm-17 μm. In some embodiments of the present application, the thickness of the active material layer 12 can be, for example, 110 μm, 120 μm, 130 μm, 150 μm, 170 μm, 180 μm, 200 μm, 220 μm, 240 μm, 250 μm, and the thickness of the current collector 11 can be, for example, 4.5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 13 μm, 15 μm, 17 μm. The active material layer of the battery pole piece provided in the present application is specially partitioned, and the porosity of each area is specially designed, so that the battery pole piece presents the characteristics of high porosity in the middle and low porosity on both sides in the length direction, and the liquid phase diffusion impedance of the second area in the middle is lower than that of the first area and the third area on both sides, which offsets the problem of inconsistent SOC in different areas of the pole piece during the charging process caused by low impedance caused by high temperature near the positive and negative pole ears due to temperature difference, thereby improving the SOC uniformity of the battery during the charging and discharging process. This structure can also effectively avoid lithium deposition during the cycle process due to lack of electrolyte in the middle of the pole piece due to poor wetting, thereby improving the cycle performance of the battery.
[0037] The present application also provides a battery, including a battery housing and a positive electrode sheet, a negative electrode sheet, a diaphragm and an electrolyte contained in the battery housing, wherein the diaphragm is disposed between the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet and / or the negative electrode sheet are the battery electrodes provided in the foregoing text of the present application. In an embodiment of the present application, when the positive electrode sheet and the negative electrode sheet are both the battery electrodes provided in the foregoing text of the present application, the porosity of the second region of the positive electrode sheet and the negative electrode sheet may be the same or different. In some embodiments, the porosity of the second region of the positive electrode sheet and the negative electrode sheet is different, and the porosity of the negative electrode sheet is greater than the porosity of the positive electrode sheet. Such a special design can further improve the fast charging performance of the battery.
[0038] like Figure 2 As shown, the present application also provides a method for preparing the battery provided above, comprising:
[0039] S101. Preparing a first active slurry, a second active slurry and a third active slurry, wherein the second active slurry comprises an electrolyte additive;
[0040] S102. sequentially coating the first active slurry, the second active slurry and the third active slurry on the current collector along the length direction of the current collector to obtain a first region precursor, a second region precursor and a third region precursor respectively, to obtain a battery pole sheet precursor;
[0041] S103. After assembling the battery electrode precursor and the separator, injecting electrolyte to obtain a battery.
[0042] In the embodiment of the present application, the battery electrode precursor in step S102 corresponds to the battery electrode in step S103; the first region precursor, the second region precursor, and the third region precursor in step S102 correspond to the first region, the second region, and the third region in step S103, respectively.
[0043] In step S101, the first active slurry, the second active slurry and the third active slurry include active materials. In some embodiments, when the battery pole piece is a positive pole piece, the active material can be any positive active material for a battery known in the art. In some embodiments, the positive active material can be, for example, one or more of a modified or unmodified phosphate-based positive active material and a transition metal oxide positive active material, wherein the phosphate-based positive active material includes but is not limited to one or more of materials such as lithium iron phosphate and lithium manganese iron phosphate, and the transition metal oxide positive active material includes but is not limited to one or more of materials such as ternary materials and lithium-rich layered oxides.
[0044] In some embodiments of the present application, when the battery pole piece is a negative pole piece, the active material can be any negative electrode active material for batteries known in the art. In some embodiments, the negative electrode active material can be, for example, one or more of a modified or unmodified carbon-based negative electrode active material, a silicon-based negative electrode active material, a tin-based negative electrode active material, and a lithium metal negative electrode active material. Among them, the carbon-based negative electrode includes but is not limited to natural graphite, artificial graphite, hard carbon, soft carbon, and graphene; the silicon-based negative electrode includes but is not limited to silicon, silicon carbon, and silicon oxygen; the tin-based negative electrode includes but is not limited to tin, tin carbon, tin oxygen, and tin metal compounds.
[0045] In the embodiment of the present application, the first active slurry, the second active slurry and the third active slurry also include a conductive agent and a binder, the conductive agent can be any conductive agent known in the art, and the binder can be any binder known in the art. In some embodiments of the present application, the conductive agent can be, for example, one or more of Super P-Li, Super P, acetylene black, graphene, and carbon nanotubes. In the embodiment of the present application, the binder can be any binder known in the art. In some embodiments of the present application, the binder can be, for example, one or more of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR).
[0046] In the embodiments of the present application, the first active slurry, the second active slurry and the third active slurry further include a solvent. In some embodiments, when the battery pole piece is a positive pole piece, the solvent includes but is not limited to N-methylpyrrolidone (NMP). In other embodiments, when the battery pole piece is a negative pole piece, the solvent includes but is not limited to N-methylpyrrolidone (NMP).
[0047] In the embodiment of the present application, the electrolyte additive includes one or more of 1,2-vinylidene carbonate, 1,3-propylene sultone, 1,3-propane sultone, methane disulfonic acid methylene ester, 1,4-butane sultone, vinyl sulfate, succinonitrile, 2-fluorobiphenyl, succinic anhydride, phthalic anhydride, vinyl carbonate, vinyl ethylene carbonate and fluoroethylene carbonate. The present application adds a suitable electrolyte additive to the second active slurry in the second region for forming the active material layer, so that when the prepared battery pole piece is applied to the battery, the electrolyte dissolves the electrolyte additive in the second region, thereby causing a pore structure to appear at the position of the electrolyte additive, thereby reducing the impedance of the second region, and the pore structure of the second region can also absorb and store more electrolyte, avoiding the lithium precipitation phenomenon caused by too little electrolyte content in the second region affecting the battery cycle performance. In addition, the dissolution of the electrolyte additive in the second region also increases the electrolyte concentration in the electrolyte near the second region located in the middle of the battery electrode, which can also effectively avoid lithium precipitation in the middle of the electrode due to too little electrolyte additive content, thereby improving the battery's cycle performance.
[0048] In the embodiment of the present application, the mass percentage of the electrolyte additive in the second active slurry is 0.5%-10%. In some specific embodiments, the mass percentage of the electrolyte additive in the second active slurry can be, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 8%, 10%. In some embodiments, the mass percentage of the electrolyte additive in the second active slurry can be 1%-5%. By controlling the content of the electrolyte additive in the second active slurry within a suitable range, the porosity of the second region of the active material layer of the battery pole piece finally obtained can be further controlled, thereby improving the SOC uniformity in the length direction of the battery pole piece and improving the electrochemical performance of the battery.
[0049] In step S102, in some embodiments, when the battery electrode is a positive electrode, the current collector may be, for example, aluminum foil. In other embodiments, when the battery electrode is a negative electrode, the current collector may be, for example, copper foil.
[0050] In some embodiments of the present application, in order to save preparation costs and shorten the process flow, the first active slurry and the third active slurry can be the same slurry, and the second active slurry is prepared by directly adding electrolyte additives to the first active slurry and the third active slurry. This method can further reduce preparation costs and shorten the process flow, which is conducive to large-scale production.
[0051] In some embodiments of the present application, after applying the first active slurry, the second active slurry and the third active slurry, drying and rolling are also included. In some embodiments of the present application, the drying temperature is 30°C-80°C, and the drying time is 3min-60min. In some specific embodiments, the drying temperature can be, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, and the drying time can be, for example, 3min, 5min, 10min, 20min, 30min, 40min, 50min, 60min.
[0052] In some embodiments of the present application, the coating surface density of the second region is lower than that of the first region, and the absolute value of the difference between the coating surface density of the second region and the first region is less than or equal to 15%; and / or the coating surface density of the second region is lower than that of the third region, and the absolute value of the difference between the coating surface density of the second region and the third region is less than or equal to 15%. The present application can further regulate the porosity of each region of the active material layer of the battery pole piece within a suitable range by reducing the coating surface density of the second region located in the middle region of the pole piece, thereby further improving the SOC uniformity in the length direction of the battery pole piece and improving the electrochemical performance of the battery.
[0053] The electrode preparation method provided in the present application increases the porosity of the active material layer by adding electrolyte additives to the active slurry, thereby improving the pore structure distribution of the electrode piece, thereby improving the cycle performance and service life of the battery electrode piece. The preparation method has a simple process, low cost, and is conducive to large-scale industrial production.
[0054] The present application also provides an electrical device, which includes the battery described above. The electrical device may be, for example, an electric car, a mobile phone, a tablet computer, a laptop computer, a wearable device (a watch, a bracelet), a digital camera, etc. The electrical device is powered by the battery described above and has good cycle performance.
[0055] The present application is further described below in multiple embodiments:
[0056] Example 1
[0057] The positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 95:2.5:2.5 to prepare a first positive electrode active slurry with a solid content of 63%; the first positive electrode active slurry is divided into two parts, one part is retained, and the electrolyte additives methanedisulfonic acid methylene ester and 1,2-vinylidene carbonate diester are continuously added to the other part to prepare a second positive electrode active slurry, the mass ratio of methanedisulfonic acid methylene ester and 1,2-vinylidene carbonate diester is 1:1, and the mass of the electrolyte additive in the second positive electrode active slurry accounts for 0.5% of the total mass of the second positive electrode active slurry; the prepared first positive electrode active slurry and the second positive electrode active slurry are mixed. , the first positive electrode active slurry is sequentially coated on both sides of the current collector aluminum foil along the length direction of the current collector, that is, the first positive electrode active slurry is coated on both ends of the current collector in the length direction, corresponding to the first region and the third region after drying, and the second positive electrode active slurry is coated on the middle position of the current collector in the length direction, corresponding to the second region after drying, wherein the coating surface density of the second region is 5% lower than that of the first region and the third region, and after drying, the first region, the second region and the third region on the positive electrode active layer are obtained, and the length of the second region in the length direction of the positive electrode sheet accounts for 50% of the total length of the positive electrode sheet; the positive electrode sheet is obtained after rolling and die-cutting;
[0058] The negative electrode active material artificial graphite, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 95:3:2 to prepare a first negative electrode active slurry with a solid content of 50%; the first negative electrode slurry is divided into two parts, one part is retained, and the electrolyte additives vinyl ethylene carbonate (VEC) and methylene disulfonate are continuously added to the other part to prepare a second negative electrode active slurry, wherein the mass ratio of vinyl ethylene carbonate (VEC) to methylene disulfonate is 1:1, and the mass of the electrolyte additive in the second negative electrode active slurry accounts for 1% of the total mass of the second negative electrode active slurry; the prepared first negative electrode active slurry, the second negative electrode active slurry, and the first The negative electrode active slurry is sequentially coated on both sides of the current collector copper foil along the length direction of the current collector, that is, the first negative electrode active slurry is coated on the two end positions of the current collector in the length direction, corresponding to the first region and the third region after drying, and the second negative electrode active slurry is coated on the middle position of the current collector in the length direction, corresponding to the second region after drying, wherein the coating surface density of the second region is 5% lower than that of the first region and the third region, and after drying, the first region, the second region and the third region on the negative electrode active layer are obtained, and the length of the second region in the length direction of the negative electrode sheet accounts for 50% of the total length of the negative electrode sheet; the negative electrode sheet is obtained after rolling and die cutting;
[0059] The prepared positive electrode sheet, the separator and the prepared negative electrode sheet are stacked in sequence, and after baking, an electrolyte is injected, and a battery is obtained after formation and capacity division.
[0060] Example 2
[0061] The difference from Example 1 is that the mass of the electrolyte additive in the second positive electrode active slurry accounts for 1% of the total mass of the second positive electrode active slurry; the mass of the electrolyte additive in the second negative electrode active slurry accounts for 1.5% of the total mass of the second negative electrode active slurry.
[0062] Example 3
[0063] The difference from Example 1 is that the mass of the electrolyte additive in the second positive electrode active slurry accounts for 1.5% of the total mass of the second positive electrode active slurry; the mass of the electrolyte additive in the second negative electrode active slurry accounts for 2.5% of the total mass of the second negative electrode active slurry.
[0064] Example 4
[0065] The positive electrode active material nickel-cobalt-manganese ternary positive electrode material, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 95:2:3 to prepare a first positive electrode active slurry with a solid content of 73%; the first positive electrode active slurry is divided into two parts, one part is retained, and the electrolyte additives fluoroethylene carbonate and 1,2-vinylidene carbonate diester are continuously added to the other part to prepare a second positive electrode active slurry, the sum of the masses of the electrolyte additives in the second positive electrode active slurry accounts for 1% of the total mass of the second positive electrode active slurry, and the mass ratio of fluoroethylene carbonate to 1,2-vinylidene carbonate diester is 6:1; the prepared first positive electrode active slurry, the second positive electrode active slurry, and the first The positive electrode active slurry is sequentially coated on both sides of the current collector aluminum foil along the length direction of the current collector, that is, the first positive electrode active slurry is coated on the two end positions of the current collector in the length direction, corresponding to the first region and the third region after drying, and the second positive electrode active slurry is coated on the middle position of the current collector in the length direction, corresponding to the second region after drying, wherein the coating surface density of the second region is 3% lower than that of the first region and the third region, and after drying, the first region, the second region and the third region on the positive electrode active layer are obtained, and the length of the second region in the length direction of the positive electrode sheet accounts for 40% of the total length of the positive electrode sheet; the positive electrode sheet is obtained after rolling and die-cutting;
[0066] The negative electrode active material artificial graphite, silicon-carbon negative electrode, binder polyvinylidene fluoride (PVDF), and conductive agent Super P were dissolved in N-methylpyrrolidone (NMP) in a mass ratio of 95:2:3 to prepare a first negative electrode active slurry with a solid content of 50%; the first negative electrode slurry was divided into two parts, one was retained, and electrolyte additives fluoroethylene carbonate and 1,2-vinylidene carbonate were continuously added to the other part to prepare a second negative electrode active slurry, the sum of the mass of the electrolyte additives in the second negative electrode active slurry accounted for 1.5% of the total mass of the second negative electrode active slurry, and the mass ratio of fluoroethylene carbonate to 1,2-vinylidene carbonate was 6:1; the prepared first negative electrode active slurry, the second negative electrode active slurry, and the first negative electrode active slurry were mixed. The active slurries are sequentially coated on both sides of the current collector copper foil along the length direction of the current collector, that is, the first negative active slurry is coated on the two end positions of the current collector in the length direction, corresponding to the first region and the third region after drying, and the second negative active slurry is coated on the middle position of the current collector in the length direction, corresponding to the second region after drying, wherein the coating surface density of the second region is 3% lower than that of the first region and the third region, and after drying, the first region, the second region and the third region on the negative active layer are obtained, and the length of the second region in the length direction of the negative electrode sheet accounts for 40% of the total length of the negative electrode sheet; the negative electrode sheet is obtained after rolling and die cutting;
[0067] The prepared positive electrode sheet, the separator and the prepared negative electrode sheet are stacked in sequence, and after baking, an electrolyte is injected, and a battery is obtained after formation and capacity division.
[0068] Example 5
[0069] The difference from Example 4 is that the length of the second region in the length direction of the positive electrode sheet accounts for 50% of the total length of the positive electrode sheet, and the length of the second region in the length direction of the negative electrode sheet accounts for 50% of the total length of the negative electrode sheet.
[0070] Example 6
[0071] The difference from Example 4 is that the length of the second region in the length direction of the positive electrode sheet accounts for 60% of the total length of the positive electrode sheet, and the length of the second region in the length direction of the negative electrode sheet accounts for 60% of the total length of the negative electrode sheet.
[0072] Example 7
[0073] The difference from Example 1 is that the coating surface density of the second region in the positive electrode sheet is the same as the coating surface density of the first and third regions; the coating surface density of the second region in the negative electrode sheet is the same as the coating surface density of the first and third regions.
[0074] Comparative Example 1
[0075] The positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 95:2.5:2.5 to prepare a positive electrode active slurry with a solid content of 63%, and the positive electrode active slurry is coated on both sides of the positive electrode current collector aluminum foil; after drying, rolling, and die-cutting, a positive electrode sheet is obtained;
[0076] The negative electrode active material artificial graphite, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 95:3:2 to prepare a first negative electrode active slurry with a solid content of 50%, and the negative electrode active slurry is coated on both sides of the negative electrode current collector copper foil; after drying, rolling, and die-cutting, a negative electrode sheet is obtained;
[0077] The prepared positive electrode sheet, the separator and the prepared negative electrode sheet are stacked in sequence, and after baking, an electrolyte is injected, and a battery is obtained after formation and capacity division.
[0078] Comparative Example 2
[0079] The difference from Example 4 is that: the positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 95:2.5:2.5 to prepare a positive electrode active slurry with a solid content of 63%, and the positive electrode active slurry is coated on both sides of the positive electrode current collector aluminum foil; after drying, rolling, and die-cutting, a positive electrode sheet is obtained;
[0080] The coating surface density of the second region in the negative electrode sheet is the same as that of the first region and the third region, and the total mass of the electrolyte additive in the second negative electrode active slurry accounts for 1% of the total mass of the second negative electrode active slurry.
[0081] Comparative Example 3
[0082] The difference from Example 1 is that: the positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 95:2.5:2.5 to prepare a positive electrode active slurry with a solid content of 63%, and the positive electrode active slurry is coated on both sides of the positive electrode current collector aluminum foil; after drying, rolling, and die-cutting, a positive electrode sheet is obtained;
[0083] No electrolyte additive is added to the second negative electrode active slurry.
[0084] Comparative Example 4
[0085] The difference from Example 4 is that: the positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride (PVDF), and the conductive agent Super P are dissolved in N-methylpyrrolidone (NMP) according to a mass ratio of 95:2.5:2.5 to prepare a positive electrode active slurry with a solid content of 63%, and the positive electrode active slurry is coated on both sides of the positive electrode current collector aluminum foil; after drying, rolling, and die-cutting, a positive electrode sheet is obtained;
[0086] The mass of the electrolyte additive in the second negative electrode active slurry accounts for 6% of the total mass of the second negative electrode active slurry.
[0087] The electrochemical performance of the battery positive electrodes prepared in Examples 1-7 and Comparative Examples 1-4 was tested, and the results are shown in Table 1.
[0088] SOC conformance test:
[0089] (1) Charge the battery cell to 100% SOC according to the 5C, 4.5C, 4C, 3.5C, 3C, 2.5C, 2C, 1.5C, 1C, and 0.33C fast charging steps. Charge 0.33C to the upper limit voltage (3.65V for lithium iron phosphate and 4.2V for nickel-cobalt-manganese ternary positive electrode material). For other rates, the copper wire three-electrode monitors the negative electrode potential to 0mV for jumping;
[0090] (2) The battery cell was disassembled, the negative electrode sheet was wiped into a single-sided sheet, and the sheets were cut from the left, middle and right sides to make button batteries for charging tests to compare the SOC states of the first area, the second area and the third area. The results are shown in Table 1.
[0091] Cycle performance test:
[0092] (1) Place in a 25°C thermostat for 6 h; (2) Charge to 3.65 V with 1C CC; (3) Leave for 0.5 h; (4) Discharge to 2.5 V with 1C CC; (5) Leave for 0.5 h; The capacity retention rate of steps (2) to (5) after 1000 cycles is shown in Table 1.
[0093] Porosity test: The porosity of the first, second and third regions of the electrode was measured by mercury intrusion method. The measured results are shown in Table 1.
[0094] Table 1
[0095]
[0096]
[0097] As can be seen from Table 1, the battery pole pieces provided in Examples 1 to 7 of the present application, by specially designing the positions and porosities of the first region, the second region, and the third region, make the battery pole pieces present the characteristics of high porosity in the middle and low porosity at both ends in the length direction, and control the difference in porosity between the second region and the first region and the third region within an appropriate range, so that the electrolyte content in the second region of the battery pole piece is increased, and the SOC consistency of the battery pole piece in the first region, the second region, and the third region is improved, thereby effectively improving the fast charging performance and cycle performance of the battery. And it can be seen from the data of Examples 1 and 7 that when the same mass of electrolyte additives are added to the active slurry, adjusting the coating density of the second region to be greater than the coating density of the first region and the third region can further optimize the porosity design of the battery pole piece in the length direction.
[0098] The preferred embodiments are described in detail above, but the present invention is not limited to the above-mentioned specific implementation modes. Under the guidance of the present application, technicians in this field can also make various specific changes without departing from the scope of protection of the present application, which all fall within the scope of protection of the present invention.
Claims
1. A battery pole piece, characterized in that: The battery electrode includes a current collector and an active material layer arranged on the surface of the current collector; the active material layer includes a first region, a second region and a third region arranged in sequence and in parallel along the length direction of the battery electrode; the porosity of the second region is 25%-40%, the porosity of the second region is 2%-10% greater than the porosity of the first region, and the porosity of the second region is 2%-10% greater than the porosity of the third region.
2. The battery pole piece according to claim 1, characterized in that: The porosity of the second region is 29%-35%.
3. The battery pole piece according to claim 1 or 2, characterized in that: In the length direction of the battery electrode sheet, the distance between the center line of the second region and the center line of the active material layer is 0-100 mm.
4. The battery pole piece according to any one of claims 1 to 3, characterized in that: The first region and the third region have the same porosity.
5. The battery pole piece according to any one of claims 1 to 4, characterized in that: The length of the second region in the length direction of the battery electrode sheet accounts for 25%-70% of the total length of the battery electrode sheet.
6. The battery pole piece according to any one of claims 1 to 5, characterized in that: The second region includes a pore structure, and the pore size of the pore structure is 0.01 μm-3 μm.
7. The battery pole piece according to any one of claims 1 to 6, characterized in that: The thickness of the active material layer is 110 μm-250 μm, and the thickness of the current collector is 4.5 μm-17 μm.
8. A battery, characterized in that: The battery comprises a battery pole piece as described in any one of claims 1-7.
9. A method for preparing a battery as claimed in claim 8, characterized in that: include: preparing a first active slurry, a second active slurry and a third active slurry, wherein the second active slurry includes an electrolyte additive; The first active slurry, the second active slurry and the third active slurry are sequentially coated on the current collector along the length direction of the current collector to obtain a first region precursor, a second region precursor and a third region precursor respectively, thereby obtaining a battery pole piece precursor; After assembling the battery pole piece precursor and the separator, injecting electrolyte to obtain a battery; The battery pole piece precursor corresponds to the battery pole piece; the first region precursor corresponds to the first region, the second region precursor corresponds to the second region, and the third region precursor corresponds to the third region.
10. The method for preparing a battery according to claim 9, characterized in that: The electrolyte additive includes one or more of 1,2-vinylidene carbonate, 1,3-propylene sultone, 1,3-propane sultone, methylene disulfonate, 1,4-butane sultone, vinyl sulfate, succinonitrile, 2-fluorobiphenyl, succinic anhydride, phthalic anhydride, vinyl carbonate, vinyl ethylene carbonate and fluoroethylene carbonate.
11. The method for preparing a battery according to claim 9 or 10, characterized in that: The mass percentage of the electrolyte additive in the second active slurry is 0.5%-10%.
12. The method for preparing a battery according to claim 11, characterized in that: The mass percentage of the electrolyte additive in the second active slurry is 1%-5%.
13. The method for preparing a battery according to claim 11, characterized in that: The coating surface density of the second region is lower than that of the first region, and the absolute value of the difference between the coating surface density of the second region and the first region is less than or equal to 15%; and / or the coating surface density of the second region is lower than that of the third region, and the absolute value of the difference between the coating surface density of the second region and the third region is less than or equal to 15%.
14. An electrical device, characterized in that: The electrical device comprises the battery as claimed in claim 8 or a battery prepared by the method for preparing a battery as claimed in claims 9-13.
Citation Information
Patent Citations
Positive plate, preparation method and battery
CN111952541A
Positive electrode sheet and battery
CN112018397A
Negative plate and lithium ion battery comprising same
CN113328098A
Pole piece and lithium ion battery
CN116093247A
Negative pole piece, battery monomer and electric device
CN117133861A