Lithium ion secondary battery, lithium supplementing negative plate, lithium supplementing negative plate assembly, lithium supplementing method and power utilization device

By setting up a multi-layer structure and a lithium supplement layer in the negative electrode sheet of the lithium-ion secondary battery, the first negative electrode active layer with high conductivity accelerates the embedding of lithium ions, and the problem of insufficient cycle life of the lithium ion secondary battery is solved. Achieve longer battery life.

CN119069643APending Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411566347.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing lithium-ion secondary batteries are deactivated and lithium-ionized during the circulation process, resulting in insufficient cycle life and difficult to meet the needs of high cycle life.

Method used

By providing a first negative electrode active layer and a second negative electrode active layer with a multi-layer structure in the negative electrode sheet, and a lithium supplement layer is provided on the surface thereof, the active lithium is accelerated by using the first negative electrode active layer with high conductivity and low powder resistivity. The embedded and lithium supplement efficiency reduces the generation of inactivated lithium and extends battery life.

Benefits of technology

The cycle life performance of lithium-ion secondary batteries is significantly improved, and the lithium-ion production is reduced by rapidly embedding active lithium ions and extending the battery service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069643A_ABST
    Figure CN119069643A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion secondary battery, a lithium supplement negative plate, a lithium supplement assembly, a lithium supplement method and a power utilization device. The lithium ion secondary battery comprises a negative pole piece; the negative electrode plate comprises a negative electrode current collector, and a second negative electrode active layer and a first negative electrode active layer which are sequentially arranged on at least one side of the negative electrode current collector; the negative electrode plate meets one or two of the following characteristics (i) and (ii): (i) the conductivity of the first negative electrode active layer is higher than that of the second negative electrode active layer; and (ii) the powder resistivity of the first negative electrode active layer is lower than that of the second negative electrode active layer, and the negative electrode plate is subjected to negative electrode lithium supplement treatment. The lithium ion secondary battery has improved long cycle life performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion secondary batteries, and further relates to a lithium-ion secondary battery, a lithium-supplemented negative electrode sheet, a component, a method and an electrical device, and further relates to a lithium-ion secondary battery and a preparation method thereof, a lithium-supplemented negative electrode sheet, a component for preparing a lithium-ion secondary battery and an electrical device. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] With the development of lithium-ion secondary battery technology, lithium-ion secondary batteries are widely used in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. They are also widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations. Currently, the demand for long cycle life of lithium-ion secondary batteries is increasing. Summary of the Invention

[0004] According to various embodiments and examples of the present application, a lithium-ion secondary battery, a lithium-supplemented negative electrode sheet, an assembly, a method, and an electrical device are provided. Furthermore, a lithium-ion secondary battery and a method for preparing the same, a lithium-supplemented negative electrode sheet, an assembly for preparing the lithium-ion secondary battery, and an electrical device are provided. The lithium-ion secondary battery has improved long cycle life performance.

[0005] In a first aspect of the present application, a lithium-ion secondary battery is provided, comprising a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0006] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0007] The negative electrode plate is treated with negative electrode lithium supplementation.

[0008] In this application, unless otherwise specified, in a lithium-ion secondary battery, "the negative electrode plate has been subjected to a negative electrode lithium replenishment treatment" means that "the negative electrode plate includes lithium pre-embedded by the negative electrode lithium replenishment", which means that the negative electrode plate of the lithium-ion secondary battery has been subjected to a negative electrode lithium replenishment treatment, so that the negative electrode plate includes, in addition to the lithium embedded in the negative electrode during the formation process, the lithium additionally introduced by the negative electrode lithium replenishment treatment. During the negative electrode lithium replenishment process, the lithium replenishment material carried by the negative electrode plate releases active lithium ions, and the released active lithium ions are embedded in the negative electrode active material, thereby obtaining a negative electrode plate subjected to a negative electrode lithium replenishment treatment. The lithium embedded in the negative electrode during the negative electrode lithium replenishment process can be referred to as "pre-embedded lithium"; after the negative electrode plate subjected to the negative electrode lithium replenishment treatment is introduced into the lithium-ion secondary battery, the negative electrode plate can release the pre-embedded lithium during the charge and discharge process of the lithium-ion secondary battery, thereby replenishing the lithium continuously consumed by the battery system. Compared with the case where the negative electrode plate has not been subjected to a lithium replenishment treatment, the lithium-ion secondary battery provided in the first aspect of this application has a significantly extended cycle life.

[0009] In the present application, unless otherwise specified, the negative electrode lithium replenishment material used in the negative electrode lithium replenishment treatment undergone by the negative electrode plate is provided by the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer, that is, "the negative electrode plate undergoes negative electrode lithium replenishment treatment" means that the negative electrode plate undergoes lithium replenishment treatment with the lithium replenishment layer located on the surface of the first negative electrode active layer away from the second negative electrode active layer; accordingly, "the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment" means that the negative electrode plate includes lithium pre-embedded by the lithium replenishment treatment of the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0010] In the present application, "lithium replenishment efficiency" may reflect the ratio of the amount of lithium effectively embedded in the negative electrode active material to the total amount of lithium supplied by the lithium replenishment material.

[0011] By arranging a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer of the negative electrode active material layer of the negative electrode plate (with the direction away from the surface of the negative electrode current collector being the upper layer and the direction toward the surface of the negative electrode current collector being the lower layer), the negative electrode plate is further made to meet one or both of the characteristics (i) and (ii): (i) the first negative electrode active layer located on the upper layer has a higher electrical conductivity, and (ii) the first negative electrode active layer located on the upper layer has a lower powder resistivity, so that the negative electrode plate can achieve efficient lithium replenishment by adopting a process of arranging a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer, thereby making the negative electrode plate include lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishment layer. During lithium replenishment using this process, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Because the first negative electrode active layer has a higher electrical conductivity and / or a lower powder resistivity, this facilitates faster embedding of active lithium into the first negative electrode active layer, thereby inhibiting the deactivation of active lithium before it is embedded in the negative electrode active material. This can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving lithium replenishment efficiency. Thus, a negative electrode plate treated with high-efficiency negative electrode lithium replenishment can be obtained. Furthermore, by introducing a negative electrode plate treated with high-efficiency negative electrode lithium replenishment into a lithium-ion secondary battery, active lithium can be replenished continuously during the charge and discharge cycles, thereby continuously replenishing capacity. Furthermore, during the charging process, the faster embedding of active lithium ions helps reduce the accumulation of lithium ions on the surface of the negative electrode active material, thereby reducing the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0012] The enhanced effects described in any part of this application are not intended to be limited by any theory.

[0013] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0014] The powder resistivity of the first negative electrode active layer is 1 mΩ·cm to 100 mΩ·cm, and can be optionally 1 mΩ·cm to 20 mΩ·cm;

[0015] The powder resistivity of the second negative electrode active layer is 1 mΩ·cm to 100 mΩ·cm, and can be optionally 1 mΩ·cm to 20 mΩ·cm.

[0016] By controlling the powder resistivity of the first negative electrode active layer or the second negative electrode active layer within the aforementioned range, the lithium ion secondary battery can have better dynamic performance.

[0017] In some embodiments, in the negative electrode sheet, a lithium-supplemented residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer, and the lithium-supplemented residual layer contains inactive lithium;

[0018] The negative electrode plate meets one or more of the following characteristics:

[0019] Measured on one side of the negative electrode current collector, the thickness of the lithium supplement residual layer is less than 0.1 μm, optionally, less than 0.08 μm, further optionally, less than 0.05 μm;

[0020] Based on one side of the negative electrode current collector, the coverage area percentage of the lithium replenishing residual layer relative to the first negative electrode active layer is less than or equal to 98%, and can be optionally 50%-98% or 30%-70%, and further optionally 50%-70%.

[0021] During the process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer for negative electrode lithium replenishment treatment, if the active lithium provided by the negative electrode lithium replenishment material does not have time to be embedded in the negative electrode active material and becomes inactivated, a lithium replenishment residual layer including inactive lithium may be formed at the position of the lithium replenishment layer.

[0022] By controlling one or both of the thickness of the lithium-replenishing residual layer and the percentage of coverage of the lithium-replenishing residual layer relative to the first negative electrode active layer within the aforementioned ranges, efficient lithium replenishment of the negative electrode is achieved while also ensuring that the lithium-replenishing residual layer has a more appropriate thickness, thereby achieving good electrolyte wetting and charge transfer performance, thereby facilitating good battery kinetics. Furthermore, a higher electrical conductivity and / or lower powder resistivity of the first negative electrode active layer facilitates increased charging rate, further improving battery kinetics.

[0023] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0024] The first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder, wherein the mass fraction of the first binder in the first negative electrode active layer is lower than the mass fraction of the second binder in the second negative electrode active layer;

[0025] The first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent. The mass fraction of the first conductive agent in the first negative electrode active layer is higher than the mass fraction of the second conductive agent in the second negative electrode active layer.

[0026] In some embodiments, the first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder; the mass fraction of the first binder in the first negative electrode active layer is lower than the mass fraction of the second binder in the second negative electrode active layer.

[0027] In some embodiments, the first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent; the mass fraction of the first conductive agent in the first negative electrode active layer is higher than the mass fraction of the second conductive agent in the second negative electrode active layer.

[0028] By setting a lower content of binder in the first negative electrode active layer, the content of organic components with relatively poor conductivity can be reduced, which is beneficial to improving the conductivity of the negative electrode plate, facilitating the rapid embedding of lithium ions, and further improving the lithium replenishment efficiency.

[0029] By providing a higher content of conductive agent in the first negative electrode active layer, it is beneficial to improve the electron transmission rate of the first negative electrode active layer, thereby improving the electron conduction performance, and is more conducive to improving the lithium replenishment efficiency.

[0030] By synergistically controlling the contents of the binder and the conductive agent in the first negative electrode active layer, it is beneficial to better control the conductivity of the first negative electrode active layer and to better improve the lithium replenishment efficiency.

[0031] In addition, the improvement of the conductivity of the negative electrode sheet is also beneficial to optimizing battery dynamics.

[0032] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0033] The mass fraction of the first binder in the first negative electrode active layer is 1% to 15%;

[0034] The mass fraction of the second binder in the second negative electrode active layer is 1% to 15%;

[0035] The mass fraction of the first conductive agent in the first negative electrode active layer is 0.1% to 10%;

[0036] The mass fraction of the second conductive agent in the second negative electrode active layer is 0.1% to 10%.

[0037] By controlling one or more parameters including the mass fraction of the first binder in the first negative electrode active layer, the mass fraction of the second binder in the second negative electrode active layer, the mass fraction of the first conductive agent in the first negative electrode active layer, and the mass fraction of the second conductive agent in the second negative electrode active layer within the aforementioned range, it is beneficial to make the negative electrode sheet have higher conductivity and to make the lithium-ion secondary battery have better kinetic performance.

[0038] In some embodiments, in a thermogravimetric test performed under a nitrogen atmosphere, the mass loss of the first negative electrode active layer at 350° C. to 450° C. is lower than that of the second negative electrode active layer.

[0039] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0040] The mass fraction of the styrene-butadiene rubber in the first negative electrode active layer is lower than the mass fraction of the styrene-butadiene rubber in the second negative electrode active layer;

[0041] The mass fraction of styrene-butadiene rubber in the first negative electrode active layer is 0.1% to 10%;

[0042] The mass fraction of styrene-butadiene rubber in the second negative electrode active layer is 0.1% to 10%.

[0043] At 350°C ~ 450°C, binders such as but not limited to styrene-butadiene rubber will generally degrade. Taking styrene-butadiene rubber (SBR) as an example, its glass transition temperature is usually lower than -20°C, and its molecules may migrate during the drying process of the electrode. By controlling the binder content distribution in the negative electrode to meet the above-mentioned thermal gravimetric test, it is beneficial to control the content distribution of such binders in the negative electrode, and further help to improve the distribution stability of such binders during the preparation of the negative electrode, reduce the precipitation and aggregation of such binders on the surface of the negative electrode, and help to improve the dynamic performance of the battery.

[0044] In some embodiments, the first binder includes a lithium-containing binder.

[0045] Providing a lithium-containing binder in the first negative electrode active layer is beneficial for improving the lithium ion conductivity of the first negative electrode active layer and further accelerating the lithium replenishment efficiency.

[0046] In some embodiments, by providing a lithium-containing binder in the first negative electrode active layer, the lithium ion diffusion rate of the first negative electrode active layer can be increased, which is beneficial to improving the initial coulombic efficiency.

[0047] In addition, the lithium provided by the lithium-containing binder can also occupy some active sites, which is beneficial to reduce the lithium consumption in film formation.

[0048] In some embodiments, the first negative electrode active layer comprises a first graphite material, and the second negative electrode active layer comprises a second graphite material; the OI value of the first graphite material is lower than the OI value of the second graphite material;

[0049] The OI value refers to the intensity ratio of the (004) crystal plane to the (110) crystal plane in the powder X-ray diffraction pattern.

[0050] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0051] The OI value of the first graphite material is 3 to 7;

[0052] The OI value of the second graphite material is 3-7.

[0053] By setting the first graphite material to have a lower OI value, the isotropy of the material is enhanced, the lithium ion insertion channels are increased, and the lithium ion diffusion kinetics in the first negative electrode active layer are improved, which helps further improve the lithium replenishment efficiency. In addition, it also helps improve battery dynamics.

[0054] In some embodiments, the first negative electrode active layer includes a first negative electrode active material, the second negative electrode active layer includes a second negative electrode active material, and the D of the first negative electrode active material is v 50 is lower than the D of the second negative electrode active material v 50;

[0055] Among them, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the multi-particle mixture reaches 50%.

[0056] By arranging the negative electrode active material with a smaller particle size in the first negative electrode active layer, it is beneficial to reduce the solid phase diffusion path and improve the battery kinetics.

[0057] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0058] The D of the first negative electrode active material v 50 satisfies 5μm≤D v 50≤15μm;

[0059] The D of the second negative electrode active material v 50Satisfies 10μm≤D v 50≤18μm.

[0060] In some embodiments, the D of the first negative electrode active material is v 50 satisfies 7μm≤D v 50≤13μm.

[0061] By adding the D v 50 is set within the aforementioned range, which is more conducive to reducing the solid-phase diffusion path and further improving battery kinetics.

[0062] In some embodiments, the ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f. H , satisfying 20%≤f H ≤70%.

[0063] In some embodiments, 30%≤f H≤50%.

[0064] The ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer (f H , calculated on one side of the negative electrode current collector) within the aforementioned range, it is beneficial to better balance the higher lithium replenishment efficiency provided by the first negative electrode active layer, better battery kinetics and the overall energy density of the negative electrode sheet. In addition, by controlling f H The aforementioned range is more conducive to processing.

[0065] Furthermore, by regulating the compaction density of the second negative electrode active layer and / or the powder compaction density of the second negative electrode material, the comprehensive advantages of high lithium replenishment efficiency and high energy density can be better balanced.

[0066] In some embodiments, the constituent material of the first negative electrode active layer is recorded as a first negative electrode material, and the constituent material of the second negative electrode active layer is recorded as a second negative electrode material;

[0067] The negative electrode plate meets one or both of the following characteristics:

[0068] The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer;

[0069] Under the same test conditions, the powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0070] By regulating the compaction density of the second negative electrode active layer to be higher than that of the first negative electrode active layer, the energy density of the lithium-ion secondary battery is improved, thereby facilitating both high energy density and high lithium replenishment efficiency.

[0071] By controlling the powder compaction density of the second negative electrode material to be higher than the powder compaction density of the first negative electrode active material, it is beneficial to give the second negative electrode active layer a higher compaction density during the cold pressing process of the electrode.

[0072] By controlling the second negative electrode active layer located in the lower layer to have a higher compaction density and / or the second negative electrode material to have a higher powder compaction density, it is beneficial to improve the energy density of the lower layer, so that the negative electrode plate can have both higher energy density and higher lithium replenishment efficiency.

[0073] In some embodiments, the negative electrode plate satisfies one or both of the following characteristics:

[0074] When the battery is fully discharged, the compaction density of the negative electrode is 1.08 g / cm 3 ~ 1.71 g / cm 3 ;

[0075] When the battery is fully discharged, the surface density of the negative electrode is 10 mg / cm 2 ~ 26 mg / cm 2 .

[0076] In some embodiments, the negative electrode plate satisfies one or both of the following characteristics:

[0077] When the battery is fully discharged, the compaction density of the negative electrode is 1.17 g / cm 3 ~ 1.52 g / cm 3 ;

[0078] When the battery is fully discharged, the surface density of the negative electrode is 15 mg / cm 2 ~ 20 mg / cm 2 .

[0079] By controlling the compaction density and / or surface density of the negative electrode sheet within the aforementioned range, it is also beneficial for the battery to have a higher energy density.

[0080] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is advantageous to achieve both high energy density and high lithium replenishment efficiency.

[0081] In some embodiments, the lithium-ion secondary battery further includes a positive electrode plate, and the NP ratio of the lithium-ion secondary battery is 1.05-1.3, which is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

[0082] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.1 to 1.3.

[0083] By controlling the NP ratio of the lithium-ion secondary battery within the aforementioned range, it is beneficial for the negative electrode to store more lithium ions, facilitates the continuous release of supplementary capacity in the later stages of cycling or storage, and can better extend the battery cycle life.

[0084] In some embodiments, the lithium-ion secondary battery further comprises an electrolyte;

[0085] The electrolyte includes additives, wherein the additives include one or more of vinylene carbonate (VC) and sulfur-containing additives; the sulfur-containing additives include one or more of diethyl sulfate (DTD), ethylene sulfite (ES) and propylene sulfite (PS).

[0086] By adding vinylene carbonate (VC) to the electrolyte, a dense solid electrolyte interface (SEI) film can be formed at the negative electrode, which can reduce the side reactions caused by the contact between the negative electrode active material and the electrolyte, which is beneficial to inhibit capacity attenuation and further extend the battery cycle life.

[0087] Introducing the aforementioned sulfur-containing additives into the electrolyte forms a sulfur-containing solid electrolyte interface (SEI) film, which exhibits excellent thermal stability and acid corrosion resistance, thereby improving battery cycling performance. Furthermore, the sulfur-containing polymers formed by the decomposition of the aforementioned sulfur-containing additives facilitate good lithium-ion interfacial transport, thus optimizing battery dynamics.

[0088] In some embodiments, the lithium-ion secondary battery includes the negative electrode plate and the positive electrode plate, the positive electrode plate includes a positive electrode active material, and the positive electrode active material includes one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate; the modified form includes one or more of doping modification and coating modification.

[0089] In some embodiments, the positive electrode active material includes carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body, and the carbon coating layer includes one or more of soft carbon, hard carbon and amorphous carbon.

[0090] The lithium-ion secondary battery provided above can flexibly select a variety of positive electrode active materials.

[0091] When the positive electrode active material includes carbon-coated lithium iron phosphate, the conductivity of the surface of the lithium iron phosphate body can be improved, and the conductive network inside the positive electrode sheet can be optimized, thereby improving the battery cycle performance.

[0092] In another aspect of the present application, a negative electrode sheet is provided, comprising a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0093] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0094] The negative electrode plate is treated with negative electrode lithium supplementation.

[0095] The negative electrode plate is a negative electrode plate that has been treated with negative electrode lithium replenishment, and its negative electrode active material layer is provided with a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer (the upper layer is the direction away from the surface of the negative electrode current collector, and the lower layer is the direction toward the surface of the negative electrode current collector). Furthermore, the negative electrode plate satisfies one or both of the characteristics (i) and (ii): (i) the first negative electrode active layer located on the upper layer has a higher electrical conductivity, and (ii) the first negative electrode active layer located on the upper layer has a lower powder resistivity, so that the negative electrode plate can achieve efficient lithium replenishment by using a process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer. As a result, the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishment layer. During negative electrode lithium replenishment using this process, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Because the first negative electrode active layer has higher conductivity and / or lower powder resistivity, this facilitates faster embedding of active lithium into the first negative electrode active layer, thereby inhibiting the deactivation of active lithium before it is embedded in the negative electrode active material. This can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving lithium replenishment efficiency. Thus, a negative electrode plate treated with efficient negative electrode lithium replenishment can be obtained. By introducing a negative electrode plate treated with efficient negative electrode lithium replenishment into a lithium-ion secondary battery, active lithium can be replenished continuously during the charge and discharge cycles, thereby continuously replenishing capacity. Furthermore, during the charging process, the faster embedding of active lithium ions helps reduce the accumulation of lithium ions on the surface of the negative electrode active material, thereby reducing the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0096] In some embodiments, the negative electrode plate is the negative electrode plate in the lithium-ion secondary battery described in the first aspect of this application.

[0097] In a second aspect of the present application, a lithium-supplementing negative electrode sheet is provided, comprising a negative electrode current collector and a second negative electrode active layer, a first negative electrode active layer and a lithium-supplementing layer sequentially disposed on at least one side of the negative electrode current collector;

[0098] The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer.

[0099] A lithium-supplemented negative electrode sheet having a lithium-supplementing layer disposed on the surface of a negative electrode active material layer is provided. By disposing a first negative electrode active layer and a second negative electrode active layer on the negative electrode active material layer, and ensuring that the first negative electrode active layer on the side closest to the lithium-supplementing layer has a higher electrical conductivity and / or a lower powder resistivity, the lithium-supplementing treatment of the lithium-supplemented negative electrode sheet facilitates rapid intercalation of active lithium ions into the first negative electrode active layer. During the process of assembling a lithium-ion secondary battery using the lithium-supplemented negative electrode sheet, after injecting the electrolyte, the active lithium provided by the lithium-supplementing layer is facilitated to be more rapidly intercalated into the first negative electrode active layer. This helps inhibit the deactivation of the active lithium before intercalation into the negative electrode active material, reduces the generation of deactivated lithium during lithium-supplementation, and significantly improves the lithium-supplementing efficiency. This results in a negative electrode sheet with efficient lithium-supplementing treatment. The resulting lithium-ion secondary battery can sustainably replenish active lithium and capacity during charge and discharge cycles, and can also reduce lithium ion accumulation on the surface of the negative electrode active material, thereby reducing lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0100] In some embodiments, the lithium replenishing layer includes elemental lithium.

[0101] When elemental lithium is introduced into the lithium replenishment layer to provide active lithium, the cost is more controllable.

[0102] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics, measured on a single side of the negative electrode current collector:

[0103] The thickness of the lithium supplement layer is less than the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer;

[0104] Calculated on one side of the negative electrode current collector, the coverage area percentage of the lithium replenishing layer relative to the first negative electrode active layer is less than or equal to 98%.

[0105] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics:

[0106] The thickness of the lithium supplement layer is less than 8.5 μm on a single side of the negative electrode current collector;

[0107] Based on a single side of the negative electrode current collector, the coverage area percentage of the lithium replenishing layer relative to the first negative electrode active layer is 30% to 70%.

[0108] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics:

[0109] The thickness of the lithium replenishing layer is less than or equal to 4.8 μm, measured on a single side of the negative electrode current collector;

[0110] Based on a single side of the negative electrode current collector, the coverage area percentage of the lithium replenishing layer relative to the first negative electrode active layer is 50% to 70%.

[0111] The thickness of the lithium replenishment layer can be adjusted based on the amount of lithium replenishment required for the negative electrode. Furthermore, controlling the thickness of the lithium replenishment layer within the aforementioned range facilitates controlling the thickness of the lithium replenishment residual layer within a more appropriate range, thereby achieving better electrolyte wetting and charge transfer performance, and contributing to good battery kinetics.

[0112] During the production process, residual water often remains within the negative electrode, making it difficult to completely remove. This water may react with the lithium-replenishing material in the lithium-replenishing layer, generating heat. The thicker the lithium-replenishing layer, the higher the heat generation. While not being bound by theory, controlling the lithium-replenishing layer thickness within the aforementioned range helps better control heat generation caused by the water-lithium reaction, thereby improving production safety.

[0113] By controlling the coverage area percentage of the lithium-replenishing layer relative to the first negative electrode active layer in the lithium-replenishing negative electrode sheet within the aforementioned range, it is beneficial to control the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer in the lithium-ion secondary battery within a more appropriate range, which is beneficial to better achieve good electrolyte infiltration performance and charge transfer performance, and is beneficial to making the battery have good battery dynamics.

[0114] In some embodiments, the lithium-supplemented negative electrode sheet satisfies one or more of the following characteristics:

[0115] The first negative electrode active layer and the second negative electrode active layer in the lithium-supplemented negative electrode sheet meet the characteristics described in the lithium-ion secondary battery of the first aspect of the present application;

[0116] The compaction density of the lithium-supplemented negative electrode sheet is 1.3 g / cm 3 ~ 1.8 g / cm 3 , optional 1.4 g / cm 3 ~ 1.6g / cm 3 ;

[0117] The surface density of the lithium-supplemented negative electrode sheet is 10 mg / cm 2 ~ 26 mg / cm 2 , optional 15 mg / cm 2 ~ 20 mg / cm 2 .

[0118] By adjusting the compaction density and / or areal density of the lithium-supplemented negative electrode sheet, the compaction density and / or areal density of the negative electrode sheet in the lithium-ion secondary battery can be correspondingly controlled. By controlling the compaction density and / or areal density of the lithium-supplemented negative electrode sheet within the aforementioned range, the battery can also achieve a higher energy density.

[0119] In a third aspect of the present application, there is provided an assembly for preparing a lithium-ion secondary battery, comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises a positive electrode sheet, a lithium-supplemented negative electrode sheet, and a separator, wherein the separator is disposed between the positive electrode sheet and the lithium-supplemented negative electrode sheet;

[0120] The lithium-supplemented negative electrode sheet is the lithium-supplemented negative electrode sheet described in the second aspect of this application.

[0121] By introducing the aforementioned lithium-replenishing negative electrode sheet into the components used for lithium-ion secondary batteries, it is beneficial to enable the active lithium provided by the lithium-replenishing layer to be embedded in the first negative electrode active layer more quickly, which is beneficial to inhibiting the deactivation of the active lithium before being embedded in the negative electrode active material, and can reduce the generation of deactivated lithium during lithium replenishment, which is beneficial to significantly improve the lithium replenishment efficiency, and obtain a negative electrode sheet treated with high-efficiency lithium replenishment. The obtained lithium-ion secondary battery can persistently replenish active lithium during the charge and discharge cycle, continuously replenish capacity, and can also reduce the enrichment of lithium ions on the surface of the negative electrode active material and reduce the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0122] In a fourth aspect of the present application, a method for preparing a lithium-ion secondary battery is provided, comprising the following steps:

[0123] Assembling a positive electrode sheet, a separator, and a lithium-supplemented negative electrode sheet into an electrode assembly, wherein the separator is disposed between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector, and a second negative electrode active layer, a first negative electrode active layer, and a lithium-supplemented layer disposed in sequence on at least one side of the negative electrode current collector; and wherein the lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; and (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer.

[0124] The electrode assembly is placed in the housing cavity of the shell, and an electrolyte is injected to allow the electrolyte to soak the positive electrode sheet and the lithium-supplemented negative electrode sheet, and then the electrolyte is formed to obtain the lithium-ion secondary battery.

[0125] By contacting an electrode assembly including the aforementioned lithium-replenishing negative electrode sheet with an electrolyte, impregnating the sheet, and chemically converting the sheet, a negative electrode sheet that has undergone negative electrode lithium replenishment treatment can be prepared. The negative electrode active material layer of the negative electrode sheet is provided with a first negative electrode active layer located in an upper layer and a second negative electrode active layer located in a lower layer (the direction away from the negative electrode current collector surface is considered to be the upper layer, and the direction toward the negative electrode current collector surface is considered to be the lower layer). Furthermore, the first negative electrode active layer located in the upper layer has a higher electrical conductivity and / or a lower powder resistivity. During the process of performing negative electrode lithium replenishment using the aforementioned method, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Based on the higher electrical conductivity and / or lower powder resistivity of the first negative electrode active layer, it is beneficial for faster embedding of active lithium. Into the first negative electrode active layer, which is beneficial to inhibit the deactivation of active lithium before being embedded in the negative electrode active material, and can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving the lithium replenishment efficiency. Therefore, the introduction of negative electrode plates that have undergone high-efficiency negative electrode lithium replenishment treatment into lithium-ion secondary batteries can durably replenish active lithium and continuously replenish capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is beneficial to reducing the enrichment of lithium ions on the surface of the negative electrode active material, and thus is beneficial to reducing the generation of lithium plating, so that the lithium-ion secondary battery can have improved long cycle life performance.

[0126] In some embodiments, the lithium-supplementing layer in the lithium-supplementing negative electrode sheet satisfies the following formula:

[0127] 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3;

[0128] Among them, C N_A is the preset surface capacity of the negative electrode, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

[0129] The negative electrode preset surface capacity can be calculated based on the theoretical gram capacity of the negative electrode active material and the surface density of the negative electrode active material in the negative electrode sheet. N_A =Theoretical gram capacity of negative electrode active material × surface density of negative electrode active material in the negative electrode sheet.

[0130] The positive electrode preset surface capacity can be calculated based on the theoretical gram capacity of the positive electrode active material and the surface density of the positive electrode active material in the positive electrode sheet. P_A =Theoretical gram capacity of positive electrode active material × surface density of positive electrode active material in the positive electrode sheet.

[0131] Without being bound by theory, controlling the surface density of the lithium replenishment layer to satisfy the aforementioned formula can extend the battery's cycle life while also helping to maintain a more appropriate thickness of the residual lithium replenishment layer. Furthermore, this helps to better control heat generation caused by the reaction between water and lithium, thereby improving production safety.

[0132] In some embodiments, the lithium-supplemented negative electrode sheet is prepared by a method comprising the following steps:

[0133] The second negative electrode active layer is formed on at least one side surface of the negative electrode substrate, the first negative electrode active layer is formed on the surface of the second negative electrode active layer away from the negative electrode substrate, and the lithium replenishing layer is added on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0134] In some embodiments, the prepared lithium ion secondary battery is the lithium ion secondary battery described in the first aspect of this application.

[0135] In the fifth aspect of the present application, an electrical device is provided, which includes at least one of the lithium-ion secondary battery described in the first aspect of the present application and the lithium-ion secondary battery prepared by the preparation method of the lithium-ion secondary battery described in the fourth aspect of the present application.

[0136] The details of one or more embodiments or examples of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0137] In order to better describe and illustrate the embodiments, examples or examples provided in this application, reference may be made to one or more drawings. The additional details or examples used to describe the drawings should not be considered as limiting the scope of the disclosed application, the currently described embodiments, examples or examples, and any of the currently understood best modes of these applications. Moreover, the same figure numbers are used to represent the same components in all the drawings. It should also be noted that the drawings are drawn in a simplified form and are only used to assist in the explanation of this application for convenience and clarity. The various dimensions of each component shown in the drawings are arbitrarily shown and may be accurate or not drawn to scale. For example, in order to make the illustration clearer, the dimensions of the components are appropriately exaggerated in some places in the drawings. Unless otherwise specified, the components in the drawings are not drawn to scale. This application does not limit every dimension of every component.

[0138] In the attached figure:

[0139] Figure 1Schematic diagram of the structure of the lithium-supplemented negative electrode sheet in one embodiment of the present application, corresponding to the side view, showing the cross section of the lithium-supplemented negative electrode sheet.

[0140] Figure 2 yes Figure 1 Schematic diagram of the structure of the lithium-replenishing negative electrode sheet, corresponding to the top view, showing the surface of one side of the lithium-replenishing negative electrode sheet where the lithium-replenishing layer is provided.

[0141] Figure 3 It is a structural schematic diagram of a lithium-supplementing negative electrode sheet in another embodiment of the present application, corresponding to a top view, showing a surface of one side of the lithium-supplementing negative electrode sheet on which a lithium-supplementing layer is provided.

[0142] Figure 4 It is a structural schematic diagram of a lithium-supplementing negative electrode sheet in another embodiment of the present application, corresponding to a top view, showing a surface of one side of the lithium-supplementing negative electrode sheet on which a lithium-supplementing layer is provided.

[0143] Figure 5 This is a schematic diagram of a battery cell according to one embodiment of the present application.

[0144] Figure 6 for Figure 5 FIG. 1 is an exploded view of a battery cell according to an embodiment of the present application.

[0145] Figure 7 FIG. 1 is a schematic diagram of a battery device according to an embodiment of the present application.

[0146] Figure 8 Schematic diagram of a battery pack according to one embodiment of the present application.

[0147] Figure 9 for Figure 8 An exploded view of a battery pack according to an embodiment of the present application is shown.

[0148] Figure 10 Schematic diagram of an electrical device using a lithium-ion secondary battery as a power source according to one embodiment of the present application.

[0149] Description of reference numerals:

[0150] X is the X direction; Y is the Y direction; Z is the Z direction; 12, lithium-replenishing negative electrode sheet; 102, negative electrode current collector; 104, second negative electrode active layer; 106, first negative electrode active layer; 108, lithium-replenishing layer; 1, battery pack; 2, upper case; 3, lower case; 4, battery assembly; 5, battery cell; 51, casing; 52, electrode assembly; 53, cover plate; 6, electrical device.

[0151] Among them, the X direction corresponds to the width direction of the electrode (which can be consistent with the height direction of the wound battery cell), the Y direction corresponds to the length direction of the electrode, and the Z direction corresponds to the thickness direction of the electrode. DETAILED DESCRIPTION

[0152] Below, some embodiments and examples of the lithium-ion secondary battery, lithium-supplemented negative electrode sheet, assembly, method and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0153] " scope " disclosed in the present application can be limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and any end value can be included or not included independently, and can be arbitrarily combined, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if minimum range values ​​1 and 2 are listed, and if maximum range values ​​3,4 and 5 are also listed, then the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is merely an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to listing the parameter as, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and so on. For example, when a parameter is expressed as an integer selected from "2-10", this is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0154] In this application, references to "plurality," "multiple," "multiple," "several," and the like, unless otherwise specified, refer to a quantity greater than or equal to two. For example, "one or more" means one or ≥ (greater than or equal to) two. It is understood that references to "any number" of items refer to any suitable combination of multiple items, i.e., any combination of "any number" of items that is consistent with the present application and that allows for the implementation of the present application.

[0155] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0156] References to "embodiments" herein mean that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of such phrases in various locations in the specification does not necessarily refer to the same embodiment, nor does it necessarily refer to independent or alternative embodiments that are mutually exclusive with other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments. References to "implementations" herein have a similar understanding.

[0157] In this application, open technical features or technical solutions described with words such as "contain," "include," and "include" do not exclude additional members besides the listed members unless otherwise specified, and can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions including additional members besides the listed members. For example, "a" includes a1, a2, and a3. Unless otherwise specified, it may also include other members or not. This can be regarded as providing both the feature or solution of "a consists of a1, a2, and a3" or "a is selected from a1, a2, and a3," and the feature or solution of "a includes not only a1, a2, and a3, but also other members."

[0158] In this application, unless otherwise specified, M (such as m1) means that m1 is a non-limiting example of M. It can be understood that M is not limited to m1.

[0159] In this application, "optionally" and "optional" mean optional, that is, they refer to either option selected from the two parallel options of "with" or "without". If a technical solution contains multiple "optional" items, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" item is independent. Unless otherwise specified, the description "optionally includes" in this application, such as "optionally includes", means "may include or not include".

[0160] In this application, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more relevant listed items, and also include any and all combinations of the relevant listed items, wherein any and all combinations include any two relevant listed items, any more relevant listed items, or a combination of all relevant listed items. For example, "M and / or N" means a group consisting of M, N, and "a combination of M and N." Among them, "including M and / or N" can mean "including M, including N, and including M and N", and can also mean "including M, including N, or including M and N", which can be appropriately understood according to the sentence in which it is located.

[0161] Herein, the word “suitable” in “suitable combination”, “suitable method”, etc., shall be based on the technical solution that can implement the present application.

[0162] Herein, the terms "better," "more preferred," and "excellent" are used solely to describe preferred implementations or examples and should not be construed as limiting the scope of protection of this application. If multiple "preferred" terms appear in a technical solution, each "preferred" term is considered independent unless otherwise specified and there are no contradictions or mutual constraints.

[0163] In this application, "further", "further", "particularly", "for example", "such as", "example", etc. are used for descriptive purposes to indicate differences in content, but should not be understood as limiting the scope of protection of this application.

[0164] In this application, the terms "first", "second", "third", "fourth", "fifth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", "the fifth aspect", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", "fifth", etc. only serve the purpose of non-exhaustive enumeration and description, and should be understood not to constitute a closed limitation on quantity.

[0165] In the description of this application, it should be understood that the terms "length", "width", "thickness", "height", "up", "down", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application.

[0166] In this application, unless otherwise specified or limited, the term "connection" and other terms should be understood in a broad sense. For example, it can refer to a fixed connection, a detachable connection, or an integral connection. For those skilled in the art, the appropriate meaning of the above terms in this application can be understood according to the circumstances.

[0167] In this application, unless otherwise expressly specified or limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediary. In this application, unless otherwise expressly specified or limited, a first feature being "above" or "below" a second feature may refer to a relative horizontal positional relationship, or may simply refer to an attachment relationship without limiting the relative horizontal positional relationship.

[0168] In this application, the term "room temperature" generally refers to 4°C to 35°C, and may refer to 20°C ± 5°C. In some embodiments or examples of this application, room temperature refers to 20°C to 30°C.

[0169] In this application, when referring to a range of units, if only the right endpoint is followed by the unit, it means that the units of the left and right endpoints are the same. For example, 3~5 μm or 3-5 μm both indicate that the units of the left endpoint "3" and the right endpoint "5" are both μm (micrometers), and both have the same meaning as 3 μm ~ 5 μm. Similarly, descriptions of other parameters such as temperature and size are understood in the same manner.

[0170] In this application, "greater than or equal to" and "≥" have the same meaning and can be used interchangeably; "less than or equal to" and "≤" have the same meaning and can be used interchangeably; "greater than" can be equivalently expressed as ">", and "less than" can be equivalently expressed as "<". In this application, unless otherwise specified, "greater than or equal to" and "≥" can be regarded as providing two solutions of "greater than" and "equal to". In this application, unless otherwise specified, "less than or equal to" and "≤" can be regarded as providing two solutions of "less than" and "equal to".

[0171] In this application, exemplary descriptions such as "in some embodiments (or examples)" and "in one embodiment (or example)" may include but are not limited to the following meanings: these solutions can be combined with other solutions in a suitable manner to form new technical solutions.

[0172] The improvements described in this application are not intended to be limited by any theory unless otherwise stated.

[0173] At present, the demand for long cycle life of lithium-ion secondary batteries is getting higher and higher. The battery cycle life can be extended by lithium replenishment technology. As a non-limiting example, in the process of preparing the negative electrode sheet, a lithium replenishment layer containing a lithium replenishment material can be provided on the surface of the negative electrode active material layer. After being infiltrated with an electrolyte, the active lithium ions released by the lithium replenishment material are embedded in the negative electrode active material, playing the role of negative electrode lithium replenishment. These lithium stored in the negative electrode can play the role of replenishing capacity, thereby extending the battery cycle life. However, if the active lithium ions released by the lithium replenishment material cannot be embedded in the negative electrode active material in time, it is easy to cause the active lithium to be deactivated and unable to play the role of replenishing capacity, affecting the efficiency of lithium replenishment, and even the lithium ion negative electrode may produce lithium precipitation on the surface of the negative electrode active material.

[0174] According to various embodiments and examples of the present application, a lithium-ion secondary battery, a lithium-supplemented negative electrode sheet, an assembly, a method, and an electrical device are provided. Furthermore, a lithium-ion secondary battery and a method for preparing the same, a lithium-supplemented negative electrode sheet, an assembly for preparing the lithium-ion secondary battery, and an electrical device are provided. The lithium-ion secondary battery has improved long cycle life performance.

[0175] In this application, unless otherwise specified, the term "lithium-ion secondary battery" refers to a secondary battery whose active ions include lithium ions, and "lithium-ion battery cell" refers to a battery cell whose active ions include lithium ions. Typically, a lithium-ion secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. In some embodiments, the active ions are lithium ions.

[0176] In this application, unless otherwise specified, the "electrode active material layer" includes at least one of the positive electrode active material layer of the positive electrode sheet and the negative electrode active material layer of the negative electrode sheet. Depending on the detailed situation, the electrode active material layer may refer to the positive electrode active material layer or the negative electrode active material layer.

[0177] In this application, the term "negative electrode sheet" includes a negative electrode active material layer, which includes a negative electrode active material. The term "negative electrode active material" refers to a material used in a negative electrode sheet that is capable of reversibly inserting and extracting active ions.

[0178] In this application, unless otherwise specified, the term "negative electrode sheet" includes the negative electrode current collector. The term "negative electrode current collector" refers to the structure responsible for collecting and conducting electrons at the negative electrode. In a negative electrode sheet, the negative electrode active material layer is located on at least one side of the negative electrode current collector, which can be on one or both sides.

[0179] In this application, the term "positive electrode sheet" includes a positive electrode active material layer, which includes a positive electrode active material. The term "positive electrode active material" refers to a material used in a positive electrode sheet that is capable of reversibly extracting and inserting active ions.

[0180] In this application, unless otherwise specified, the term "positive electrode sheet" includes the positive electrode current collector. The term "positive electrode current collector" refers to the structure at the positive electrode responsible for collecting and conducting electrons. In a positive electrode sheet, the positive electrode active material layer is located on at least one side of the positive electrode current collector, which can be on one or both sides.

[0181] In this application, unless otherwise specified, “separator” and “diaphragm” have the same meaning and can be used interchangeably.

[0182] In a first aspect of the present application, a lithium-ion secondary battery is provided.

[0183] In some embodiments, a lithium-ion secondary battery is provided, comprising a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0184] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0185] The negative electrode plate undergoes negative electrode lithium replenishment treatment.

[0186] In this application, unless otherwise specified, in a lithium-ion secondary battery, "the negative electrode plate has been subjected to a negative electrode lithium replenishment treatment" means that "the negative electrode plate includes lithium pre-embedded by the negative electrode lithium replenishment", which means that the negative electrode plate of the lithium-ion secondary battery has been subjected to a negative electrode lithium replenishment treatment, so that the negative electrode plate includes, in addition to the lithium embedded in the negative electrode during the formation process, the lithium additionally introduced by the negative electrode lithium replenishment treatment. During the negative electrode lithium replenishment process, the lithium replenishment material carried by the negative electrode plate releases active lithium ions, and the released active lithium ions are embedded in the negative electrode active material, thereby obtaining a negative electrode plate subjected to a negative electrode lithium replenishment treatment. The lithium embedded in the negative electrode during the negative electrode lithium replenishment process can be referred to as "pre-embedded lithium"; after the negative electrode plate subjected to the negative electrode lithium replenishment treatment is introduced into the lithium-ion secondary battery, the negative electrode plate can release the pre-embedded lithium during the charge and discharge process of the lithium-ion secondary battery, thereby replenishing the lithium continuously consumed by the battery system. Compared with the case where the negative electrode plate has not been subjected to a lithium replenishment treatment, the lithium-ion secondary battery provided in the first aspect of this application has a significantly extended cycle life.

[0187] In the present application, unless otherwise specified, the negative electrode lithium replenishment material used in the negative electrode lithium replenishment treatment undergone by the negative electrode plate is provided by the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer, that is, "the negative electrode plate undergoes negative electrode lithium replenishment treatment" means that the negative electrode plate undergoes lithium replenishment treatment with the lithium replenishment layer located on the surface of the first negative electrode active layer away from the second negative electrode active layer; accordingly, "the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment" means that the negative electrode plate includes lithium pre-embedded by the lithium replenishment treatment of the lithium replenishment layer, and the lithium replenishment layer is located on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0188] In the present application, "lithium replenishment efficiency" may reflect the ratio of the amount of lithium effectively embedded in the negative electrode active material to the total amount of lithium supplied by the lithium replenishment material.

[0189] In some embodiments, a lithium-ion secondary battery is provided, comprising a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode active material layer on at least one side comprises a second negative electrode active layer and a first negative electrode active layer disposed sequentially in a direction away from the negative electrode current collector;

[0190] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0191] The negative electrode plate undergoes negative electrode lithium replenishment treatment.

[0192] In the present application, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector. The negative electrode active material layer has a multilayer structure, including multiple negative electrode active layer structures. Furthermore, the negative electrode active material layer includes a first negative electrode active layer and a second negative electrode active layer, with the second negative electrode active layer located between the negative electrode current collector and the first negative electrode active layer.

[0193] In this application, unless otherwise specified, the terms “first” and “second” in “first negative electrode active layer” and “second negative electrode active layer” are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.

[0194] In this application, unless otherwise specified, "conductivity" has a well-known meaning in the art and can be used to characterize the strength of a substance's ability to conduct electric current. The higher the conductivity, the stronger the current conducting ability.

[0195] Unless otherwise specified, the "electrical conductivity" of the first negative electrode active layer and the second negative electrode active layer includes ionic conductivity and electronic conductivity.

[0196] In this application, the conductivity of the first negative electrode active layer and the second negative electrode active layer can be tested and compared using conventional methods in the art. For example, the conductivity of the membrane can be tested using a conductivity meter, such as a four-probe tester. For powder materials, a powder resistance meter can be used. The higher the conductivity, the better the electrical conductivity.

[0197] In this application, unless otherwise specified, "resistivity" has a well-known meaning in the art and can be used to characterize the magnitude of a substance's resistance to electric current. The greater the resistance, the greater the resistance to electric current.

[0198] For a membrane structure of a selected size, conductivity σ and resistivity ρ are reciprocals of each other. The greater the conductivity, the smaller the resistivity, and conversely, the smaller the conductivity, the greater the resistivity. Similarly, the greater the resistivity, the smaller the conductivity, and the smaller the resistivity, the greater the conductivity.

[0199] Those skilled in the art know that the resistance formula is R = ρ·L / S, where R is the resistance, ρ is the resistivity, L is the length along the current conduction direction, and S is the cross-sectional area perpendicular to the current conduction direction. Conductivity σ = L / (R×S).

[0200] Without limitation, a powder resistance test can be used to compare the conductivity of the first and second negative electrode active layers. The following test method can be used: disassemble the battery cell, remove the negative electrode sheets, and based on the thickness analysis results of the different negative electrode active layers, scrape and dry to obtain dry powders of the first and second negative electrode active layers, respectively. The extract from the first negative electrode active layer corresponds to the first negative electrode material and can also be recorded as the "upper layer powder." The extract from the second negative electrode active layer corresponds to the second negative electrode material and can also be recorded as the "lower layer powder." Equal masses of the upper and lower layer powders are weighed and pressed under the same pressure for the same length of time. Resistance values ​​are obtained using a powder resistance meter, and resistivity test values ​​can also be obtained. For example, a pressure of several tons (e.g., 3T to 5T, further e.g., 3T, 4T, 5T, etc., where 1 ton of pressure is recorded as 1T) can be used. The pressing time can be several seconds or longer, for example, the pressure can be maintained for 30 seconds. The mass of the upper and lower layer powders is 20 grams (g). If the resistivity of the upper layer powder obtained from the test is lower than that of the lower layer powder (in this case, the resistivity of the powder of the first negative electrode active layer is lower than that of the powder of the second negative electrode active layer), or if the resistance value of the upper layer powder obtained from the test is lower than that of the lower layer powder, it is considered that "the conductivity of the first negative electrode active layer is higher than that of the second negative electrode active layer." The corresponding conductivity can also be calculated by combining the formula conductivity σ = L / (R×S) and the resistance test results.

[0201] In this application, the characteristics of negative electrode lithium replenishment technology can be incorporated. For example, the determination of whether a negative electrode plate has undergone negative electrode lithium replenishment can be made by detecting areas covered by and uncovered by lithium replenishment residues. Taking the use of metallic lithium foil for negative electrode lithium replenishment as a non-limiting example, lithium replenishment can be achieved by reacting the lithium foil with the negative electrode active material under the action of an electrolyte, allowing lithium ions released by the lithium foil to be intercalated into the negative electrode active material. After lithium replenishment using this method, a residual region, similar in shape to the area covered by the lithium foil, is typically formed at the location where the lithium foil was initially placed. This residual region may contain inactive substances such as lithium oxide (Li2O) and other byproducts. Furthermore, unreacted metallic lithium may also be present in the residual region. SEM and EDS can be combined to identify the residual region and the area uncovered by the lithium foil. For example, differences in the distribution of carbon and / or silicon can be used to distinguish the residual region from the area uncovered by the lithium foil. The aforementioned testing and analysis can be performed on the battery under test after full discharge, or on a battery that has undergone a relatively low number of cycles (for non-limiting examples, no more than five cycles).

[0202] By arranging a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer of the negative electrode active material layer of the negative electrode plate (with the direction away from the surface of the negative electrode current collector being the upper layer and the direction toward the surface of the negative electrode current collector being the lower layer), the negative electrode plate is further made to meet one or both of the characteristics (i) and (ii): (i) the first negative electrode active layer located on the upper layer has a higher electrical conductivity, and (ii) the first negative electrode active layer located on the upper layer has a lower powder resistivity, so that the negative electrode plate can achieve efficient lithium replenishment by adopting a process of arranging a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer, thereby making the negative electrode plate include lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishment layer. During lithium replenishment using this process, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Because the first negative electrode active layer has a higher electrical conductivity and / or a lower powder resistivity, this facilitates faster embedding of active lithium into the first negative electrode active layer, thereby inhibiting the deactivation of active lithium before it is embedded in the negative electrode active material. This can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving lithium replenishment efficiency. Thus, a negative electrode plate treated with high-efficiency negative electrode lithium replenishment can be obtained. Furthermore, by introducing a negative electrode plate treated with high-efficiency negative electrode lithium replenishment into a lithium-ion secondary battery, active lithium can be replenished continuously during the charge and discharge cycles, thereby continuously replenishing capacity. Furthermore, during the charging process, the faster embedding of active lithium ions helps reduce the accumulation of lithium ions on the surface of the negative electrode active material, thereby reducing the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0203] In the present application, microscopic morphology observations can be performed on the cross-section of the negative electrode sheet to observe the microscopic morphology of each negative electrode active layer in the negative electrode active material layer of the negative electrode sheet and the boundaries between different negative electrode active layers, thereby determining the thickness of different negative electrode active layers. "Cross-section of the negative electrode sheet" refers to a cross-section perpendicular to the thickness direction of the negative electrode sheet. Furthermore, microscopic morphology observations can be performed on the cross-section of the negative electrode sheet and combined with composition analysis (such as energy dispersive spectroscopy (EDS) and X-ray diffraction (XRD) analysis) to identify the element types to confirm the composition of different negative electrode active layers in the negative electrode active material layer. Non-limitingly, instruments or equipment including, but not limited to, focused electron beam (FIB) electron microscopes (non-limiting examples include FEIScios 2HiVac equipment), ion cross-section polishers (non-limiting examples include JEOL's IB-09010 CP argon ion cross-section polisher and IB-19500CP ion cross-section polisher), etc., can be used to obtain the cross-section of the negative electrode piece. A plasma quenching method can also be used to obtain the cross-section of the negative electrode piece. Microscopic morphology observation methods can use instruments or equipment including, but not limited to, scanning electron microscopy (SEM) technology. Non-limitingly, a high-resolution field emission scanning electron microscope can be used. Non-limiting examples of SEM instruments include the Sigma 300 scanning electron microscope and the Apreo 2 SEM field emission scanning electron microscope from ZEISS, Germany.

[0204] In the SEM microscopic morphology image of the cross section of the negative electrode sheet, the boundaries between different negative electrode active layers and the thickness of each negative electrode active layer can be confirmed based on the obvious discontinuous changes in the microscopic morphology.

[0205] In this application, unless otherwise specified, the “cross section of the negative electrode sheet” refers to the cross section of the negative electrode sheet.

[0206] Those skilled in the art can identify the components in the negative electrode active material layer, the first negative electrode active layer, and the second negative electrode active layer by one or more of the following detection methods, including but not limited to: Fourier transform infrared (FT-IR) spectroscopy, ultraviolet spectroscopy, nuclear magnetic resonance spectroscopy (NMR), and the like. 1 H NMR), gel permeation chromatography (GPC), high performance liquid chromatography (HPLC), mass spectrometry, X-ray diffraction (XRD), Raman spectroscopy, single crystal X-ray diffraction (SCXRD), inductively coupled plasma spectroscopy (ICP), energy dispersive spectroscopy (EDS) analysis, etc. The sample preparation methods and testing methods of these testing methods are known to those skilled in the art, and the testing parameters can be appropriately adjusted according to the structure of the material or substance and the characteristics of the sample.

[0207] As a non-limiting example, Si and C can be distinguished using EDS.

[0208] Taking the distinction between natural graphite and artificial graphite in the negative electrode active material as a non-limiting example, natural graphite and artificial graphite can be distinguished by the appearance of the particles; X-ray diffraction (XRD) analysis can be further performed. In the XRD spectrum, if the characteristic peak near 2θ 26.5° is very sharp and has a high intensity, it is natural graphite; if the characteristic peak near 2θ 26.5° is relatively broad and has a weak intensity, it is artificial graphite.

[0209] Taking the distinction between graphite and amorphous carbon as an example, Raman spectroscopy can be used for testing and analysis. The characteristic peak information of the carbon component in the spectrum (such as the intensity ratio of D peak / G peak, I D / G ) to analyze amorphous carbon. Both D peak and G peak are Raman characteristic peaks of carbon atom crystals. D peak represents the defects of carbon atom crystals. The more defects there are, the greater the D peak intensity is. The D peak intensity can reflect the content of amorphous (turbostratified stacking) regions. G peak represents the in-plane stretching vibration of carbon atom sp2 hybridization. The G peak intensity can reflect the content of graphitized (layered structure) regions. As the degree of disorder of carbon atoms increases, the intensity ratio of D peak to G peak also increases. You can also compare Raman spectra I D / G Standard Raman spectrum of graphite I D / G Similarly, the intensity difference between the D and G peaks in the Raman spectrum can be used to distinguish natural graphite from artificial graphite.

[0210] As non-limiting examples, FT-IR, UV spectroscopy, 1 The type and content of the binder can be detected by one or more methods such as H NMR, but is not limited thereto. For another example, EDS can be used to detect the type and content of the conductive agent, but is not limited thereto. Furthermore, scanning electron microscopy (SEM) and transmission electron microscopy (TEM) test images can also be combined to identify or differentiate the conductive agent.

[0211] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0212] The powder resistivity of the first negative electrode active layer is 1 mΩ·cm to 100 mΩ·cm, and can be optionally 1 mΩ·cm to 20 mΩ·cm;

[0213] The powder resistivity of the second negative electrode active layer is 1 mΩ·cm~100 mΩ·cm, and can be optionally 1 mΩ·cm~20 mΩ·cm.

[0214] In some embodiments, the powder resistivity of the first negative electrode active layer is 1 mΩ·cm~100 mΩ·cm, which can be optionally 1 mΩ·cm~20 mΩ·cm, or can be any of the following values ​​or a range consisting of any two of the following values: 1 mΩ, 2 mΩ, 3 mΩ, 4 mΩ, 5 mΩ, 6 mΩ, 7 mΩ, 8 mΩ, 9 mΩ, 10 mΩ, 11 mΩ, 12 mΩ, 13 mΩ, 14 mΩ, 15 mΩ, 16 mΩ, 18 mΩ, 20 mΩ, 25 mΩ, 30 mΩ, 35 mΩ, 40 mΩ, 45 mΩ, 50 mΩ, 60 mΩ, 70 mΩ, 80 mΩ, 90 mΩ, 100 mΩ, etc. Without limitation, the powder resistivity of the first negative electrode active layer can also be selected from any of the following ranges: 1 mΩ·cm~20 mΩ·cm, 1 mΩ·cm~15 mΩ·cm, 1 mΩ·cm~10 mΩ·cm, 2 mΩ·cm~20 mΩ·cm, 2 mΩ·cm~15 mΩ·cm, 2 mΩ·cm~10 mΩ·cm, 5 mΩ·cm~20 mΩ·cm, 5 mΩ·cm~15 mΩ·cm, 5 mΩ·cm~10 mΩ·cm, etc.

[0215] In some embodiments, the powder resistivity of the second negative electrode active layer is 1 mΩ·cm~100 mΩ·cm, which can be optionally 1 mΩ·cm~20 mΩ·cm, or can be any of the following values ​​or a range consisting of any two of the following values: 1 mΩ, 2 mΩ, 3 mΩ, 4 mΩ, 5 mΩ, 6 mΩ, 7 mΩ, 8 mΩ, 9 mΩ, 10 mΩ, 11 mΩ, 12 mΩ, 13 mΩ, 14 mΩ, 15 mΩ, 16 mΩ, 18 mΩ, 20 mΩ, 25 mΩ, 30 mΩ, 35 mΩ, 40 mΩ, 45 mΩ, 50 mΩ, 60 mΩ, 70 mΩ, 80 mΩ, 90 mΩ, 100 mΩ, etc. Without limitation, the powder resistivity of the second negative electrode active layer can also be selected from any of the following ranges: 1 mΩ·cm~20 mΩ·cm, 1 mΩ·cm~15 mΩ·cm, 1 mΩ·cm~10 mΩ·cm, 2 mΩ·cm~20 mΩ·cm, 2 mΩ·cm~15 mΩ·cm, 2 mΩ·cm~10 mΩ·cm, 5 mΩ·cm~20 mΩ·cm, 5 mΩ·cm~15 mΩ·cm, 5 mΩ·cm~10 mΩ·cm, etc.

[0216] In some embodiments, exemplary values ​​of the electrical conductivity of the first negative electrode active layer can be calculated according to the aforementioned formula and the powder resistivity of the first negative electrode active layer.

[0217] In some embodiments, the exemplary range of the electrical conductivity of the first negative electrode active layer can be calculated based on the aforementioned formula and two boundary values ​​of the exemplary range of the powder resistivity of the first negative electrode active layer.

[0218] In some embodiments, exemplary values ​​of the electrical conductivity of the second negative electrode active layer can be calculated based on the aforementioned formula and the powder resistivity of the second negative electrode active layer.

[0219] In some embodiments, the exemplary range of the electrical conductivity of the second negative electrode active layer can be calculated based on the aforementioned formula and two boundary values ​​of the exemplary range of the powder resistivity of the second negative electrode active layer.

[0220] By controlling the powder resistivity of the first negative electrode active layer or the second negative electrode active layer within the aforementioned range, the lithium ion secondary battery can have better dynamic performance.

[0221] In some embodiments, in a negative electrode sheet of a lithium-ion secondary battery, a lithium-supplemented residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer.

[0222] In some embodiments, a lithium-ion secondary battery is provided, comprising a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0223] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0224] In the negative electrode sheet, a lithium supplement residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer.

[0225] In some embodiments, a lithium-ion secondary battery is provided, comprising a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode active material layer on at least one side comprises a second negative electrode active layer and a first negative electrode active layer disposed sequentially in a direction away from the negative electrode current collector;

[0226] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0227] In the negative electrode sheet, a lithium supplement residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer.

[0228] In some embodiments, in a negative electrode sheet of a lithium-ion secondary battery, a lithium-replenishing residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer. Furthermore, the lithium-replenishing residual layer contains inactive lithium.

[0229] A non-limiting example of inactive lithium is lithium oxide.

[0230] In this application, unless otherwise specified, in a lithium-ion secondary battery, a "lithium-replenishing residual layer" in a negative electrode sheet refers to a structural layer containing at least a portion of the same components as the residue remaining after lithium replenishment using the lithium-replenishing layer. Unless otherwise specified, a "lithium-replenishing layer" refers to a structural layer containing a lithium-replenishing material. As a non-limiting example, the lithium-replenishing layer may be a lithium sheet. The lithium-replenishing material contained in the lithium-replenishing layer disposed in the corresponding lithium-replenishing negative electrode sheet may also be referred to as the negative electrode lithium-replenishing material.

[0231] In some embodiments, in a negative electrode sheet of a lithium-ion secondary battery, a lithium-replenishing residual layer is present on a surface of the first negative electrode active layer distal from the second negative electrode active layer. The lithium-replenishing residual layer comprises inactive lithium, and the thickness of the lithium-replenishing residual layer (measured on a single side of the negative electrode current collector) is less than 0.1 μm, optionally less than 0.08 μm, and further optionally less than 0.05 μm. Without limitation, the thickness of the lithium-replenishing residual layer (measured on a single side of the negative electrode current collector) can also be any of the following values, less than any of the following values, or a range consisting of any two of the following values: 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, etc.

[0232] In some embodiments, in the negative electrode sheet, the percentage of the area covered by the lithium-replenishing residual layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is less than or equal to 98%, and optionally less than or equal to 70%. In some embodiments, in the negative electrode sheet, the percentage of the area covered by the lithium-replenishing residual layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is greater than 0 and less than or equal to 90%. In some embodiments, in the negative electrode sheet, the percentage of the area covered by the lithium-replenishing residual layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is greater than 0 and less than or equal to 70%. Without limitation, in the negative electrode sheet, the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, may also be any of the following percentages, or any two percentages selected from the following: 0.1%, 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 98%, etc. Without limitation, the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, may be selected from any appropriate range: greater than 0 and less than or equal to 50%, 30%-98%, 30%-70%, 30%-50%, 50%-98%, 50%-70%, etc.

[0233] In some embodiments, in the negative electrode sheet of a lithium-ion secondary battery, the lithium-supplemented residual layer satisfies one or more of the following characteristics:

[0234] Measured on a single side of the negative electrode current collector, the thickness of the lithium supplement residual layer is less than 0.1 μm, optionally, less than 0.08 μm, further optionally, less than 0.05 μm (can also be selected from any appropriate value or range in the context);

[0235] Measured on a single side of the negative electrode current collector, the coverage area percentage of the lithium-supplemented residual layer relative to the first negative electrode active layer is less than or equal to 98%, and can be optionally 30% to 98%, further optionally 50% to 98% or 30% to 70%, and further optionally 50% to 70% (can also be selected from any appropriate value or range in the context).

[0236] In this application, unless otherwise specified, the “thickness of the lithium supplement residual layer” refers to the thickness on one side of the negative electrode current collector.

[0237] As an example, a cross-section of the negative electrode sheet can be microscopically observed to confirm the thickness of the lithium-replenishing residual layer, for example, to determine whether the thickness of the lithium-replenishing residual layer is less than 0.1 μm. The definition of "cross-section of the negative electrode sheet" is consistent with that described above. Microscopic observation of the surface of the negative electrode sheet can also be performed in conjunction with elemental analysis (e.g., EDS, XRD, etc.) to determine the percentage of coverage of the lithium-replenishing residual layer relative to the first negative electrode active layer.

[0238] Taking lithium foil replenishment as an example, when the lithium foil fully contacts and reacts with the electrolyte, the thickness of the lithium replenishment residual layer formed may be much lower than 0.1 μm, such as less than 0.05 μm, or even less than 0.02 μm.

[0239] During the process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer for negative electrode lithium replenishment treatment, if the active lithium provided by the negative electrode lithium replenishment material does not have time to be embedded in the negative electrode active material and becomes inactivated, a lithium replenishment residual layer including inactive lithium may be formed at the position of the lithium replenishment layer.

[0240] By controlling one or both of the thickness of the lithium-replenishing residual layer and the percentage of coverage of the lithium-replenishing residual layer relative to the first negative electrode active layer within the aforementioned ranges, efficient lithium replenishment of the negative electrode is achieved while also ensuring that the lithium-replenishing residual layer has a more appropriate thickness, thereby achieving good electrolyte wetting and charge transfer performance, thereby facilitating good battery kinetics. Furthermore, a higher electrical conductivity and / or lower powder resistivity of the first negative electrode active layer facilitates increased charging rate, further improving battery kinetics.

[0241] In this application, unless otherwise specified, in the first negative electrode active layer, the negative electrode active material is referred to as the "first negative electrode active material," the binder is referred to as the "first binder," and the conductive agent is referred to as the "first conductive agent." In the second negative electrode active layer, the negative electrode active material is referred to as the "second negative electrode active material," the binder is referred to as the "second binder," and the conductive agent is referred to as the "second conductive agent." In the context of this application, unless otherwise specified, the terms "first" and "second" in "first negative electrode active material," "second negative electrode active material," "first binder," "second binder," "first conductive agent," and "second conductive agent" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the technical features indicated.

[0242] For the negative electrode plate, the negative electrode plate includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material. It can be understood that the first negative electrode active material and the second negative electrode active material are both contained in the negative electrode active material.

[0243] In some embodiments, the first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder; the mass fraction of the first binder in the first negative electrode active layer is lower than the mass fraction of the second binder in the second negative electrode active layer.

[0244] By setting a lower content of binder in the first negative electrode active layer, the content of organic components with relatively poor conductivity can be reduced, which is beneficial to improving the conductivity of the negative electrode plate, facilitating the rapid embedding of lithium ions, and further improving the lithium replenishment efficiency.

[0245] In some embodiments, the first negative active layer includes a first conductive agent, and the second negative active layer includes a second conductive agent; the mass fraction of the first conductive agent in the first negative active layer is higher than the mass fraction of the second conductive agent in the second negative active layer.

[0246] By providing a higher content of conductive agent in the first negative electrode active layer, it is beneficial to improve the electron transmission rate of the first negative electrode active layer, thereby improving the electron conduction performance, and is more conducive to improving the lithium replenishment efficiency.

[0247] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:

[0248] The first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder, wherein the mass fraction of the first binder in the first negative electrode active layer is lower than the mass fraction of the second binder in the second negative electrode active layer;

[0249] The first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent. The mass fraction of the first conductive agent in the first negative electrode active layer is higher than the mass fraction of the second conductive agent in the second negative electrode active layer.

[0250] By synergistically controlling the contents of the binder and the conductive agent in the first negative electrode active layer, it is beneficial to better control the conductivity of the first negative electrode active layer and to better improve the lithium replenishment efficiency.

[0251] In addition, the improvement of the conductivity of the negative electrode sheet is also beneficial to optimizing battery dynamics.

[0252] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0253] The mass fraction of the first binder in the first negative electrode active layer is 1% to 15%;

[0254] The mass fraction of the second binder in the second negative electrode active layer is 1% to 15%;

[0255] The mass fraction of the first conductive agent in the first negative electrode active layer is 0.1% to 10%;

[0256] The mass fraction of the second conductive agent in the second negative electrode active layer is 0.1% to 10%.

[0257] By controlling one or more parameters including the mass fraction of the first binder in the first negative electrode active layer, the mass fraction of the second binder in the second negative electrode active layer, the mass fraction of the first conductive agent in the first negative electrode active layer, and the mass fraction of the second conductive agent in the second negative electrode active layer within the aforementioned range, it is beneficial to make the negative electrode sheet have higher conductivity and to make the lithium-ion secondary battery have better kinetic performance.

[0258] Without limitation, the mass fraction of the first binder in the first negative electrode active layer may be 0%-15%, further 0%-10%, further 0-5%, further 1%-5%, further optionally 1%-3%. Without limitation, the mass fraction of the first binder in the first negative electrode active layer can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.05%, 0.1%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.6%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc. For example, the mass fraction of the first binder in the first negative electrode active layer can be selected from any of the following ranges: 0.1%-15%, 0.5%-15%, 1%-15%, 2%-15%, 3%-15%, 4%-15%, 5%-15%, 0.1%-10%, 0.5%-10%, 1%-10%, 2%-10%, 3%-10%, 4%-10%, 5%-10%, etc.

[0259] Without limitation, the mass fraction of the second binder in the second negative electrode active layer may be 0% to 15%, further 0% to 10%, further 0% to 5%, further 1% to 5%, and further optionally 1% to 3%. Without limitation, the mass fraction of the second binder in the second negative electrode active layer may also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.05%, 0.1%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.6%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc. For example, the mass fraction of the second binder in the second negative electrode active layer may be selected from any of the following ranges: 0.1%-15%, 0.5%-15%, 1%-15%, 2%-15%, 3%-15%, 4%-15%, 5%-15%, 0.1%-10%, 0.5%-10%, 1%-10%, 2%-10%, 3%-10%, 4%-10%, 5%-10%, etc.

[0260] Without limitation, the mass fraction of the first conductive agent in the first negative electrode active layer may be 0% to 10%, and may further be 0% to 5%. Without limitation, the mass fraction of the first conductive agent in the first negative electrode active layer may be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, etc. For example, the mass fraction of the first conductive agent in the first negative electrode active layer may be selected from any of the following ranges: 0.1% to 10%, 0.2% to 10%, 0.3% to 10%, 0.4% to 10%, 0.5% to 10%, 1% to 10%, 2% to 10%, 3% to 10%, 4% to 10%, 5% to 10%, etc.

[0261] Without limitation, the mass fraction of the second conductive agent in the second negative electrode active layer may be 0% to 10%, and may further be 0% to 5%. Without limitation, the mass fraction of the second conductive agent in the second negative electrode active layer may also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, etc. For example, the mass fraction of the second conductive agent in the second negative electrode active layer may be selected from any of the following ranges: 0.1% to 10%, 0.2% to 10%, 0.3% to 10%, 0.4% to 10%, 0.5% to 10%, 1% to 10%, 2% to 10%, 3% to 10%, 4% to 10%, 5% to 10%, etc.

[0262] In some embodiments, in a thermogravimetric test performed under a nitrogen atmosphere, the mass loss of the first negative electrode active layer at 350° C. to 450° C. is lower than that of the second negative electrode active layer.

[0263] At 350°C ~ 450°C, binders such as but not limited to styrene-butadiene rubber will generally degrade. Taking styrene-butadiene rubber (SBR) as an example, its glass transition temperature is usually lower than -20°C, and its molecules may migrate during the drying process of the electrode. By controlling the binder content distribution in the negative electrode to meet the above-mentioned thermal gravimetric test, it is beneficial to control the content distribution of such binders in the negative electrode, and further help to improve the distribution stability of such binders during the preparation of the negative electrode, reduce the precipitation and aggregation of such binders on the surface of the negative electrode, and help to improve the dynamic performance of the battery.

[0264] In this application, unless otherwise specified, thermogravimetric (TG) analysis can be used to obtain the "mass loss at 350°C to 450°C" of each negative electrode active layer. Without limitation, the following method can be used for thermogravimetric analysis: disassemble the battery cell, remove the negative electrode sheet, and separately extract the first negative electrode material (also referred to as the "upper layer powder") and the second negative electrode material (also referred to as the "lower layer powder"). Weigh equal masses of the upper and lower layer powders, for example, 10 mg each. Test using a thermogravimetric analyzer in a nitrogen atmosphere at a heating rate of 5°C / min over the temperature range of 25°C to 600°C to obtain the mass loss at different temperatures. The mass loss in the temperature range of 350°C to 450°C can then be calculated.

[0265] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0266] The mass fraction of the styrene-butadiene rubber in the first negative electrode active layer is lower than the mass fraction of the styrene-butadiene rubber in the second negative electrode active layer;

[0267] The mass fraction of styrene-butadiene rubber in the first negative electrode active layer is 0.1% to 10%;

[0268] The mass fraction of styrene-butadiene rubber in the second negative electrode active layer is 0.1% to 10%.

[0269] In some embodiments, the mass fraction of the styrene-butadiene rubber in the first negative electrode active layer is lower than the mass fraction of the styrene-butadiene rubber in the second negative electrode active layer.

[0270] In some embodiments, the mass fraction of styrene-butadiene rubber in the first negative electrode active layer can be 0.1%~10%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, etc. For example, the mass fraction of the second conductive agent in the second negative electrode active layer can be selected from any of the following ranges: 0.1%~10%, 0.2%~10%, 0.3%~10%, 0.4%~10%, 0.5%~10%, 1%~10%, 2%~10%, 3%~10%, 4%~10%, 5%~10%, etc.

[0271] In some embodiments, the mass fraction of styrene-butadiene rubber in the second negative electrode active layer can be 0.1%~10%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, etc. For example, the mass fraction of the second conductive agent in the second negative electrode active layer can be selected from any of the following ranges: 0.1%~10%, 0.2%~10%, 0.3%~10%, 0.4%~10%, 0.5%~10%, 1%~10%, 2%~10%, 3%~10%, 4%~10%, 5%~10%, etc.

[0272] In some embodiments, the first binder includes a lithium-containing binder.

[0273] In this application, unless otherwise specified, "lithium-containing binder" refers to a binder containing lithium ions. Non-limiting examples of lithium-containing binders include binders in the form of lithium salts, and further non-limiting examples include lithium salts of polyacrylate binders and lithium carboxymethyl cellulose (CMC-Li). Lithium-containing binders can be commercially available or obtained by modifying corresponding binders to form lithium salts.

[0274] Providing a lithium-containing binder in the first negative electrode active layer is beneficial for improving the lithium ion conductivity of the first negative electrode active layer and further accelerating the lithium replenishment efficiency.

[0275] In some embodiments, by providing a lithium-containing binder in the first negative electrode active layer, the lithium ion diffusion rate of the first negative electrode active layer can be increased, which is beneficial to improving the initial coulombic efficiency.

[0276] In addition, the lithium provided by the lithium-containing binder can also occupy some active sites, which is beneficial to reduce the lithium consumption in film formation.

[0277] In some embodiments, the first negative electrode active layer includes a first graphite material, and the second negative electrode active layer includes a second graphite material; the OI value of the first graphite material is lower than the OI value of the second graphite material; wherein the OI value refers to the intensity ratio of the (004) crystal plane to the (110) crystal plane in the powder X-ray diffraction pattern.

[0278] In this application, unless otherwise specified, "graphite material" refers to a negative electrode active material having a graphitized layered crystal structure. The terms "first" and "second" in "first graphite material" and "second graphite material" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor as implicitly designating the importance or quantity of the technical features indicated.

[0279] In this application, unless otherwise specified, the "OI value" of a graphite material refers to the intensity ratio of the (004) crystal plane to the (110) crystal plane in the X-ray diffraction pattern of the rolled graphite sheet. The OI value can be used to characterize the orientation of the graphite particle packing and reflect the degree of isotropy of the graphite particle packing.

[0280] By setting the first graphite material to have a lower OI value, the isotropy of the material is enhanced, the lithium ion insertion channels are increased, and the lithium ion diffusion kinetics in the first negative electrode active layer are improved, which helps further improve the lithium replenishment efficiency. In addition, it also helps improve battery dynamics.

[0281] The OI value (GOI) of the first graphite material and the second graphite material can be tested by X-ray diffraction (XRD) with reference to the contents of Appendix F of the national standard GB / T 24533-2019 "Graphite Anode Materials for Lithium-ion Batteries". The powder sample to be tested can be rolled into a sheet, and then the sheet sample can be subjected to XRD testing to obtain an X-ray diffraction spectrum. After the sample is rolled, the arrangement orientation (OI value) of the artificial or natural hexagonal graphite on the electrode sheet is analyzed by X-ray polycrystalline diffraction. The peak area C of the (004) crystal plane diffraction peak is obtained after analysis and calculation by XRD spectrum analysis software such as Highscore Plus or Jade. 004 and the peak area C of the (110) crystal plane diffraction peak 110 OI value = C 004 / C 110 . It can be tested using an X-ray diffractometer (such as Bruker-D8advance, etc.).

[0282] Without limitation, samples for OI value testing can be obtained by the following method: a solvent (such as dimethyl carbonate) can be used to fully soak the powder material extracted from the corresponding negative electrode active layer, so that the organic components therein, such as the binder and thickener, are dissolved in the solvent (ultrasonic dispersion can also be used to promote dissolution). After washing and filtering, the collected solid phase is used as the powder of the negative electrode active material to be tested. After the powder sample to be tested is rolled into a sheet, the sheet sample is subjected to XRD testing. It should be noted that the small amount of conductive agent that may be contained in the test sample does not affect the comparison of the OI values ​​of the negative electrode active materials in the first negative electrode active layer and the second negative electrode active layer.

[0283] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0284] The OI value of the first graphite material is 3~7;

[0285] The OI value of the second graphite material is 3-7.

[0286] In some embodiments, the OI value of the first graphite material can be 3-7, or any of the following values ​​or a range consisting of any two of the following values: 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, etc.

[0287] In some embodiments, the OI value of the second graphite material can be 3-7, or any of the following values ​​or a range consisting of any two of the following values: 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, etc.

[0288] Without limitation, in some embodiments, the OI value of the first graphite material and the second graphite material can be independently 3 to 7, and can also be independently any of the following values ​​or a range consisting of any two of the following values: 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, etc.

[0289] In some embodiments, the OI value of the first graphite material is greater than or equal to 3 and less than 7, and the OI value of the second graphite material is greater than 3 and less than or equal to 7.

[0290] In some embodiments, the first negative electrode active layer includes a first negative electrode active material, the second negative electrode active layer includes a second negative electrode active material, and the D of the first negative electrode active material is v 50 is lower than the D of the second negative electrode active material v 50;

[0291] Among them, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the multi-particle mixture reaches 50%.

[0292] In this application, unless otherwise stated, D v 50 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%. This parameter indicates that the particle size of 50% of the material volume is less than or equal to D v 50, and the particle size of 50% of the material volume is larger than D v 50. D v 50 can be obtained from the volume cumulative distribution curve of the material particle size. If there is no other explanation, the volume cumulative distribution curve starts from zero from the small particle size side. Those skilled in the art will understand that D v 50, and can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E Laser Particle Size Analyzer from Malvern Instruments Ltd., UK, or the LS-909 Laser Particle Size Analyzer (Omega). Testing can be performed according to the standard procedure GB / T 19077-2016 / ISO 13320:2009.

[0293] By arranging the negative electrode active material with a smaller particle size in the first negative electrode active layer, it is beneficial to reduce the solid phase diffusion path and improve the battery kinetics.

[0294] In this application, the "negative electrode active material" sample to be tested in the negative electrode sheet of a lithium-ion secondary battery can be obtained by disassembling the battery to obtain a powder sample to be tested. The particle components in different negative electrode active layers can be identified and tested and analyzed using methods such as energy dispersive spectrometer (EDS), inductively coupled plasma (ICP), and XRD testing and analysis. Without limitation, methods such as EDS, XRD, and ICP can be used to identify different types of particles and conduct quantitative testing and analysis of their component content. Samples of different negative electrode active layers can be extracted from different locations on the negative electrode sheet. Different types of solid particles can be collected using methods including but not limited to solvent washing, ultrasonic dispersion, and graded sedimentation. The types of different solid particles can then be identified using component analysis methods. For example, the negative electrode active material layer can be digested using reagents (such as aqua regia, reverse aqua regia, or a combination of aqua regia and hydrogen fluoride), and the composition of the negative electrode active material can be tested and analyzed using methods such as inductively coupled plasma emission spectrometry. For another example, a solvent (such as dimethyl carbonate) can be used to fully soak the powder material extracted from the corresponding negative electrode active layer, so that the organic components such as binders and thickeners are dissolved in the solvent (ultrasonic dispersion can also be used to promote dissolution). After washing and filtering, the collected solid phase is used as the powder of the negative electrode active material to be tested. It should be noted that the small amount of conductive agent that may be contained in the test sample does not affect the D v 50 comparative analysis.

[0295] In some embodiments, the D of the first negative electrode active material v 50 satisfies 5μm≤D v 50≤15μm, optionally, 7μm≤D v 50≤13μm. In a non-limiting manner, the D v 50 can also be any of the following values ​​or a range consisting of any two of the following values: 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc.

[0296] In this application, the solid-phase diffusion rate can also be compared by comparing the lithium ion solid-phase diffusion coefficient. A higher ion solid-phase diffusion coefficient is more favorable for battery kinetic performance. The lithium ion solid-phase diffusion coefficient can be measured using methods known in the art, such as the GITT method.

[0297] By adding the D v 50 is set within the aforementioned range, which is more conducive to reducing the solid-phase diffusion path and further improving battery kinetics.

[0298] In some embodiments, the D of the second negative electrode active material v 50Satisfies 10μm≤D v 50≤18μm. In a non-limiting manner, the D of the second negative electrode active material v 50 can also be any of the following values ​​or a range consisting of any two of the following values: 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, etc.

[0299] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0300] D of the first negative electrode active material v 50 satisfies 5μm≤D v 50≤15μm, optionally, 7μm≤D v 50≤13μm;

[0301] D of the second negative electrode active material v 50Satisfies 10μm≤D v 50≤18μm.

[0302] The following method can be used to test the D of the first negative electrode active material and the second negative electrode active material: v 50. Take a clean beaker, add an appropriate amount of the sample to be tested, and ultrasonicate at 120W / 5min to ensure complete dispersion of the sample. The test instrument is a Malvern 2000 from the United States. After the sample is poured into the injection tower, it circulates with the solution to the test optical system. Under the irradiation of the laser beam, the particles receive and measure the energy distribution of the scattered light to obtain the particle size distribution characteristics (shading degree: 8-12%). Based on the test data, a particle size volume distribution graph is drawn. From the distribution graph, it is found that: if 50% of the total volume of particles has a diameter greater than a certain Dv50 value, and another 50% of the total volume of particles has a diameter less than this Dv50 value, then this Dv50 value is the volume average particle size of the particles.

[0303] In some embodiments, the ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f. H , satisfying 20%≤f H ≤70%, optionally, 30%≤f H ≤60%, further optionally, 30%≤f H ≤50%. Without limitation, f HIt can also be any of the following percentages or a range consisting of any two of the following percentages: 20%, 30%, 40%, 50%, 60%, 70%, etc. In some embodiments, 40%≤f H ≤60%.

[0304] The ratio of the thickness of the first negative electrode active layer to the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer (f H , calculated on one side of the negative electrode current collector) within the aforementioned range, it is beneficial to better balance the higher lithium replenishment efficiency provided by the first negative electrode active layer, better battery kinetics and the overall energy density of the negative electrode sheet. In addition, by controlling f H The aforementioned range is more conducive to processing.

[0305] Furthermore, by regulating the compaction density of the second negative electrode active layer and / or the powder compaction density of the second negative electrode material, the comprehensive advantages of high lithium replenishment efficiency and high energy density can be better balanced.

[0306] In some embodiments, in the negative electrode sheet of a lithium-ion secondary battery, the compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer.

[0307] In this application, unless otherwise specified, in a lithium-ion secondary battery, the "compacted density of the second negative electrode active layer" in the negative electrode sheet refers to the ratio of the mass to the volume of the second negative electrode active layer, and the "compacted density of the first negative electrode active layer" in the negative electrode sheet refers to the ratio of the mass to the volume of the first negative electrode active layer.

[0308] In a non-limiting manner, the compaction density of the second negative electrode active layer may be increased by adjusting the particle size of the second negative electrode active material, but is not limited thereto.

[0309] To test the compacted density of the first and second negative electrode active layers in the negative electrode sheet of a lithium-ion secondary battery, the battery can be disassembled to obtain the negative electrode sheet, dried, and punched into small discs of a certain area A0. First negative electrode material powder of a certain thickness d1 of the first negative electrode active layer is scraped from the corresponding thickness position, and the powder mass M1 is weighed. The compacted density of the first negative electrode active layer can be calculated as PD1 = M1 / (A0 × d1). Multiple discs are tested and the average value is taken. Second negative electrode material powder of a certain thickness d2 of the second negative electrode active layer is scraped from the corresponding thickness position, and the powder mass M2 is weighed. The compacted density of the second negative electrode active layer can be calculated as PD2 = M2(A0 × d2). Multiple discs are tested and the average value is taken.

[0310] By regulating the compaction density of the second negative electrode active layer to be higher than that of the first negative electrode active layer, the energy density of the lithium-ion secondary battery is improved, thereby facilitating both high energy density and high lithium replenishment efficiency.

[0311] In this application, unless otherwise specified, the "compacted density" of an electrode sheet has a meaning well known in the art and is one of the reference indicators of material energy density. The compacted density of an electrode sheet refers to the ratio of the mass of the electrode active material layer to its volume. The compacted density of a positive electrode sheet refers to the ratio of the mass of the positive electrode active material layer to its volume, and the compacted density of a negative electrode sheet refers to the ratio of the mass of the negative electrode active material layer to its volume. The compacted density of any active layer structure in the "electrode active material layer" refers to the ratio of the mass of the active layer structure to its volume, which is applicable to both the negative electrode active layers in the lithium-supplemented negative electrode sheet and the negative electrode active layers in the negative electrode sheet of a lithium-ion secondary battery.

[0312] In some embodiments, in the lithium-supplemented negative electrode sheet, the compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer.

[0313] Without limitation, the following method can be used to test the compaction density of the negative electrode sheet in the lithium-ion secondary battery: disassemble the battery cell, remove the negative electrode sheet, and punch it into 1540.25mm 2 Take a small disc and measure the mass M and thickness L of the disc. Take the negative electrode sheet from another area, wipe off the negative electrode active material layer on the surface and remove the remaining negative electrode current collector foil (which can be recorded as empty negative electrode current collector foil). Also punch it into 1540.25mm 2 The mass of the empty negative electrode current collector foil is weighed as M0 and the thickness is L0. The compaction density of the negative electrode sheet is PD = (M-M0) / [1.54025 × (L-L0)]. The compaction density of the negative electrode sheet measured by disassembling the battery after fully discharging the battery corresponds to the compaction density of the negative electrode sheet when the battery is fully discharged; the compaction density of the negative electrode sheet measured by disassembling the battery after fully charging the battery corresponds to the compaction density of the negative electrode sheet when the battery is fully charged.

[0314] It is understandable that the negative electrode sheets in lithium-ion secondary batteries, compared to the “lithium-supplemented negative electrode sheets with additional lithium-supplemented layers after rolling”, usually have a certain rebound after being infiltrated by the electrolyte, resulting in the compaction density of the negative electrode sheets in the battery usually being lower than the compaction density of the lithium-supplemented negative electrode sheets. Furthermore, after the formation process, the negative electrode active material reacts with the electrolyte at the interface to form a solid electrolyte interface (SEI) film on the surface of the negative electrode active material. The SEI film will also have a certain effect on the compaction density of the negative electrode active material, but the effect is relatively small. In addition, in lithium-ion secondary batteries, the compaction density of the negative electrode sheet and the negative electrode active layers it contains is also related to the charge and discharge state. The negative electrode sheet expands in the charged state, and the negative electrode sheet shrinks in the discharged state. Without limitation, based on the volume of the lithium-supplemented negative electrode sheet or the negative electrode active layer thereof after rolling to add the lithium-supplemented layer, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer thereof when the lithium-ion secondary battery is fully charged can be 1.2-1.4, and the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer thereof when the lithium-ion secondary battery is fully discharged can be 1.05-1.2. Without limitation, based on the volume of the lithium-supplemented negative electrode sheet or the negative electrode active layer thereof after rolling to add the lithium-supplemented layer, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer thereof when the lithium-ion secondary battery is fully charged can also be any of the following values ​​or a range consisting of any two of the following values: 1.20, 1.2, 1.25, 1.26, 1.28, 1.30, 1.3, 1.32, 1.34, 1.35, 1.36, 1.38, 1.4, 1.40, etc. Without limitation, based on the volume of the lithium-supplemented negative electrode sheet or the negative electrode active layer thereof after rolling and adding the lithium-supplemented layer as a reference, the volume expansion coefficient of the negative electrode sheet or the negative electrode active layer thereof in the fully discharged state of the lithium-ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, 1.2, etc. It will be understood that the compacted density of the negative electrode sheet or the negative electrode active layer thereof in the lithium-ion secondary battery can be calculated by dividing the compacted density of the lithium-supplemented negative electrode sheet or the negative electrode active layer thereof after rolling and adding the lithium-supplemented layer by the corresponding volume expansion coefficient.

[0315] In this application, unless otherwise specified, a "lithium-supplemented negative electrode sheet with a lithium-supplemented layer added after rolling" refers to a lithium-supplemented negative electrode sheet with a lithium-supplemented layer added after rolling, but not yet assembled into an electrode assembly. It is understood that a "lithium-supplemented negative electrode sheet with a lithium-supplemented layer added after rolling" has not yet come into contact with, or been soaked by, the electrolyte.

[0316] In some embodiments, the compaction density of the lithium-supplemented negative electrode sheet with the additional lithium-supplemented layer after roller pressing is 1.3 g / cm3 ~1.8g / cm 3 , optional 1.4g / cm 3 ~1.6 g / cm 3 , can also be any of the following values ​​or a range consisting of any two of the following values: 1.3 g / cm 3 , 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45 g / cm 3 , 1.50 g / cm 3 , 1.55g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 、1.71 g / cm 3 , 1.75 g / cm 3 , 1.8 g / cm 3 , 1.80 g / cm 3 wait.

[0317] In addition, regarding the compaction density of the first negative electrode active layer and the second negative electrode active layer in the negative electrode sheet obtained by cold pressing (without the addition of the lithium supplement layer), the compaction density of different negative electrode active layers can be calculated based on the coating surface density of different negative electrode active layers and the thickness of different negative electrode active layers after drying.

[0318] In this application, unless otherwise specified, the term “cold-pressed negative electrode sheet (without additional lithium supplement layer)” refers to a state where the first negative electrode active layer located on the upper layer has been cold-pressed but a lithium supplement layer has not yet been added to the first negative electrode active layer.

[0319] In some embodiments, under the same test conditions, the powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0320] In this application, unless otherwise specified, the constituent materials of the negative electrode active material layer are referred to as negative electrode materials, the constituent materials of the first negative electrode active layer are referred to as first negative electrode materials, and the constituent materials of the second negative electrode active layer are referred to as second negative electrode materials. The terms "first" and "second" in "first negative electrode material" and "second negative electrode material" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor as implicitly indicating the importance or quantity of the indicated technical features.

[0321] In this application, unless otherwise specified, "powder compaction density" has the well-known meaning in the art, which refers to the ratio of mass to volume of the powder material after compaction under a certain pressure. The "powder compaction density" of the negative electrode material can be measured using instruments and methods known in the art. For example, it can be measured by an electronic pressure testing machine (such as UTM7305) with reference to the standard GB / T24533-2009. The exemplary test method is as follows: weigh a negative electrode material with a mass of M (such as 1g), add a bottom area of ​​A (such as 1.327cm 2 ) in a mold, pressurize to a certain pressure P (such as 3T), maintain the pressure for a certain time (such as 3T for 30 seconds), then release the pressure and maintain it for a period of time (such as 10 seconds). Then, record and calculate the powder compaction density of the negative electrode material under pressure P. The following method can be used to obtain the first negative electrode material in the first negative electrode active layer and the second negative electrode material in the second negative electrode active layer: disassemble the battery cell and remove the electrode sheets, scrape the powder at the thickness of the first negative electrode active layer and the second negative electrode active layer in the negative electrode sheets, and dry them to obtain the first negative electrode material (taken from the first negative electrode active layer) and the second negative electrode material (taken from the second negative electrode active layer).

[0322] By controlling the powder compaction density of the second negative electrode material to be higher than the powder compaction density of the first negative electrode active material, it is beneficial to give the second negative electrode active layer a higher compaction density during the cold pressing process of the pole piece.

[0323] It is understood that for lithium-ion secondary batteries, the relative compaction density of the negative electrode material powders in different negative electrode active layers can be determined based on the relative compaction density test values ​​obtained under the same sample parameters and test conditions. Generally, comparison can be made based on the relative compaction density test values ​​under the same test pressure. Similarly, for lithium-supplemented negative electrode sheets, the relative compaction density of the negative electrode material powders in different negative electrode active layers can also be determined based on the relative compaction density test values ​​obtained under the same sample parameters and test conditions.

[0324] The powder compaction density of the negative electrode active material can be denoted as the first state in the negative electrode sheet of a lithium-ion secondary battery; the second state in the cold-pressed negative electrode sheet (before the lithium-supplementing layer is added) or the second state in the lithium-supplemented negative electrode sheet after roller pressing. The third state is the state of the negative electrode active material used to prepare the negative electrode sheet before cold pressing. The third state can include the raw powder state, the state suspended in the negative electrode slurry, or the state coated on the surface of the negative electrode current collector. The powder compaction density of the negative electrode active material in the third state is numerically equal to or similar to the powder compaction density in the raw powder state. In the second state, after cold pressing (before the lithium-supplementing layer is added) or roller pressing to form the negative electrode lithium-supplementing layer, the negative electrode active material particles may deform or even break. Therefore, re-extracting the negative electrode active material powder sample and re-measuring the powder compaction density may result in a different value from the powder compaction density in the raw powder state. In the first state, the negative electrode active material is in contact with and soaked in the electrolyte. After formation, the negative electrode active material undergoes its initial charge, resulting in the presence of embedded lithium ions and the formation of an SEI film on its surface. As the battery undergoes charge and discharge cycles, the negative electrode active material undergoes reversible lithium ion insertion and extraction. During the charge state, the negative electrode active material is embedded with lithium ions, and during the discharge state, the embedded lithium ions are extracted. Therefore, it is understandable that the powder compaction density of the negative electrode active material may differ to some extent between the first and third states. The terms "first," "second," and "third" in the aforementioned "first state," "second state," and "third state" are for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor as implicitly designating the importance or quantity of the technical features indicated.

[0325] Although the compaction density of the negative electrode active material powder may vary in value under different conditions, it does not affect the determination of the relative compaction density of the negative electrode material powder in different negative electrode active layers.

[0326] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or both of the following characteristics:

[0327] The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer;

[0328] Under the same test conditions, the powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

[0329] By controlling the second negative electrode active layer located in the lower layer to have a higher compaction density and / or the second negative electrode material to have a higher powder compaction density, it is beneficial to improve the energy density of the lower layer, so that the negative electrode plate can have both higher energy density and higher lithium replenishment efficiency.

[0330] In some embodiments, when the battery is fully discharged, the compaction density of the negative electrode sheet is 1.08 g / cm 3 ~1.71g / cm 3 , optional 1.17g / cm 3 ~1.52 g / cm 3 Without limitation, when the battery is fully discharged, the compaction density of the negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 1.08 g / cm 3 , 1.10 g / cm 3 , 1.15g / cm 3 , 1.20 g / cm 3 , 1.25 g / cm 3 , 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45 g / cm 3 , 1.50 g / cm 3 , 1.55 g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 、1.71 g / cm 3 wait.

[0331] In some embodiments, the surface density of the negative electrode sheet in the lithium-ion secondary battery is 10 mg / cm 2 ~26mg / cm 2 , optional 15mg / cm 2 ~20mg / cm 2 Without limitation, when the battery is fully discharged, the surface density of the negative electrode sheet in the lithium-ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 10 mg / cm 2 , 12 mg / cm 2 、15 mg / cm 2 , 16 mg / cm 2 、18 mg / cm 2 , 20 mg / cm 2 , 22 mg / cm 2 , 24 mg / cm2 , 25mg / cm 2 , 26 mg / cm 2 wait.

[0332] In this application, unless otherwise specified, the "areal density" of an electrode sheet has the commonly known meaning in the art, and refers to the ratio of the mass to the area of ​​the electrode active material layer in the electrode sheet. When the electrode active material layer is disposed on both sides of the current collector, the areal density of the electrode sheet is equal to the ratio of the total mass of the electrode active material layers on both sides to the area of ​​the electrode active material layers.

[0333] For the electrode sheet obtained by cold pressing (corresponding to the negative electrode, it refers to the state without the addition of the lithium supplement layer), the compaction density can be calculated using the following formula:

[0334] Compacted density = coating area density / thickness of the electrode active material layer, coating area density = coating dry weight of the electrode slurry / area of ​​the electrode active material layer.

[0335] The thickness of the electrode active material layer on both sides corresponds to the sum of the coating area density on both sides, while the thickness on one side corresponds to the coating area density on one side. When the electrode active material layers on both sides of the current collector are essentially the same, the compacted density can be calculated using the following formula: compacted density = coating area density on one side / thickness of the electrode active material layer on one side. The "one side" and "two sides" of the electrode active material layer refer to the distribution of the electrode active material layer relative to the current collector.

[0336] For the compaction density of the lithium-supplemented negative electrode sheet (not yet assembled into an electrode assembly) that has been roller-pressed and has an additional lithium-supplemented layer, the corresponding compaction density can be calculated using the following formula: compaction density = mass of the negative electrode active material layer (excluding the lithium-supplemented layer) / volume of the negative electrode active material layer, where both mass and volume are calculated based on the total amount on both sides.

[0337] For the compaction density of the negative electrode plate (after impregnation and formation) in a lithium-ion secondary battery, the corresponding compaction density can be calculated using the following formula: compaction density = mass of the negative electrode active material layer / volume of the negative electrode active material layer, where both mass and volume are calculated based on the total amount on both sides; after the battery is fully discharged, the battery cell can be disassembled and the electrode plate can be taken out for testing.

[0338] It's understandable that the rebound of the negative electrode sheet has little or no effect on its areal density. The negative electrode SEI film formed during chemical formation will have some impact on the areal density of the electrode sheet, but the effect is small. The battery's charge and discharge state may also have some impact on the areal density of the electrode sheet, but at full discharge, the impact on the areal density of the negative electrode sheet is relatively small. Therefore, it's generally assumed that the areal density of the negative electrode sheet in a lithium-ion secondary battery at full discharge is similar to the areal density of the lithium-supplemented negative electrode sheet (not yet assembled into an electrode assembly).

[0339] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or two of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0340] When the battery is fully discharged, the compaction density of the negative electrode is 1.08g / cm 3 ~1.71 g / cm 3 , optional 1.17g / cm 3 ~1.52 g / cm 3 ;

[0341] When the battery is fully discharged, the surface density of the negative electrode is 10 mg / cm 2 ~26mg / cm 2 , optional 15 mg / cm 2 ~20mg / cm 2 .

[0342] In some embodiments, the negative electrode plate in the lithium-ion secondary battery satisfies one or two of the following characteristics (any numerical parameter in the following characteristics can also be selected from any appropriate value or range in the context):

[0343] When the battery is fully discharged, the compaction density of the negative electrode is 1.17g / cm 3 ~1.52 g / cm 3 ;

[0344] When the battery is fully discharged, the surface density of the negative electrode is 15 mg / cm 2 ~20mg / cm 2 .

[0345] By controlling the compaction density and / or surface density of the negative electrode sheet within the aforementioned range, it is also beneficial for the battery to have a higher energy density.

[0346] In some exemplary embodiments, by adjusting one or both of the compaction density and the surface density of the negative electrode sheet within the aforementioned range, it is advantageous to achieve both high energy density and high lithium replenishment efficiency.

[0347] In some embodiments, the lithium-ion secondary battery further includes a positive electrode plate, and the NP ratio of the lithium-ion secondary battery is 1.05-1.3, which is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

[0348] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.1 to 1.3.

[0349] In some embodiments, the NP ratio of the lithium ion secondary battery is 1.1 to 1.2.

[0350] Without limitation, the NP ratio of the lithium ion secondary battery can also be any of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.08, 1.10, 1.12, 1.14, 1.15, 1.16, 1.18, 1.20, 1.22, 1.24, 1.25, 1.26, 1.28, 1.30, etc.

[0351] In this application, unless otherwise specified, the "NP ratio" of a lithium-ion secondary battery refers to the ratio of the negative electrode capacity to the positive electrode capacity, which can be expressed in English as Negative / Positive Ratio. The "NP ratio" of a lithium-ion secondary battery can be measured and obtained using conventional methods in the art.

[0352] In some embodiments, the following methods can be used to test the negative electrode capacity and the positive electrode capacity respectively:

[0353] Negative electrode capacity test: fully charge the battery, disassemble the cell, take the negative electrode sheet, and punch it into small discs with a diameter of 14 mm (corresponding to area A N ), separate the small disc and the lithium sheet with an isolation film, add electrolyte and package it into 4 button half-cells; use a 0.1C rate to charge and discharge within the voltage range of 0.005V~2V for 1 cycle, and take the average of the discharge capacity of the 4 batteries to get the negative electrode capacity C N , negative electrode surface capacity = negative electrode capacity ÷ area A N .

[0354] Positive electrode capacity test: disassemble the battery cell, take the positive electrode and punch it into small discs with a diameter of 14mm (corresponding to area A P ), separate the small disc and the lithium sheet with an isolation film, add electrolyte and package it into 4 button half-cells; use a 0.1C rate to charge and discharge for 1 cycle in the voltage range of 2.5V~3.65V, and take the average of the discharge capacity of the 4 batteries to get the positive electrode capacity C P , positive electrode surface capacity = positive electrode capacity ÷ area A P .

[0355] NP ratio of lithium-ion secondary battery = negative electrode surface capacity / positive electrode surface capacity; N Equal to A P In the case of , the following formula can also be used: NP ratio = C N / C P .

[0356] By controlling the NP ratio of the lithium-ion secondary battery within the aforementioned range, it is beneficial for the negative electrode to store more lithium ions, facilitates the continuous release of supplementary capacity in the later stages of cycling or storage, and can better extend the battery cycle life.

[0357] In some embodiments, the lithium-ion secondary battery further includes an electrolyte, and the electrolyte includes an additive; without limitation, in the electrolyte of the lithium-ion secondary battery, the additive may include one or more of vinylene carbonate (VC) and a sulfur-containing additive; without limitation, the sulfur-containing additive may include one or more of vinyl sulfate (DTD), vinyl sulfite (ES) and propylene sulfite (PS).

[0358] By adding vinylene carbonate (VC) to the electrolyte, a dense solid electrolyte interface (SEI) film can be formed at the negative electrode, which can reduce the side reactions caused by the contact between the negative electrode active material and the electrolyte, which is beneficial to inhibit capacity attenuation and further extend the battery cycle life.

[0359] Introducing the aforementioned sulfur-containing additives into the electrolyte forms a sulfur-containing solid electrolyte interface (SEI) film, which exhibits excellent thermal stability and acid corrosion resistance, thereby improving battery cycling performance. Furthermore, the sulfur-containing polymers formed by the decomposition of the aforementioned sulfur-containing additives facilitate good lithium-ion interfacial transport, thus optimizing battery dynamics.

[0360] Those skilled in the art will appreciate that, after the formation treatment, the content of some additive components in the electrolyte may change. As a non-limiting example, for example, some film-forming additive components are reduced in content due to their participation in the formation of the solid electrolyte interface film of the positive and / or negative electrodes. As a non-limiting example, relative to the electrolyte before the formation treatment, the content of additives such as vinylene carbonate (VC), diethylene sulfate (DTD), vinyl sulfite (ES) and propylene sulfite (PS) in the electrolyte is generally reduced after the formation treatment.

[0361] It can be understood that the lithium-ion secondary battery further includes a positive electrode plate, and the positive electrode plate includes a positive electrode active material.

[0362] It will be appreciated that the positive electrode active material includes a lithium ion active material.

[0363] In some embodiments, the positive electrode active material includes one or more of lithium composite metal oxides, lithium-containing phosphates, and modified forms of any of the foregoing positive electrode active materials; the modified forms include one or more of doping modification and coating modification.

[0364] In some embodiments, a lithium-ion secondary battery includes a negative electrode plate and a positive electrode plate, the positive electrode plate includes a positive electrode active material, and further, the positive electrode active material may include one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate, and the modified form may include one or more of a doping modification and a coating modification.

[0365] In some embodiments, a lithium-ion secondary battery includes a negative electrode sheet and a positive electrode sheet, the positive electrode sheet includes a positive electrode active material, and further, the positive electrode active material may include a ternary positive electrode material, lithium iron phosphate, lithium manganese iron phosphate, and one or more modified forms of any of the foregoing positive electrode active materials; the modified form includes one or more of doping modification and coating modification.

[0366] In this application, unless otherwise specified, "lithium composite metal oxide" refers to a lithium ion active material comprising lithium, a non-lithium metal element, and oxygen, used as a positive electrode active material. Typically, the non-lithium metal element in the lithium composite metal oxide includes a transition metal element; therefore, the lithium composite metal oxide may also be referred to as a "lithium transition metal oxide."

[0367] In this application, unless otherwise specified, "lithium-containing phosphate" refers to a lithium ion active material comprising lithium, a transition metal element, and a phosphate radical, used as a positive electrode active material. Typically, the lithium-containing phosphate used as a positive electrode active material may have an olivine structure. Non-limiting examples of lithium-containing phosphates having an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0368] In this application, unless otherwise specified, "a modified form of a certain positive electrode active material" includes the positive electrode active material itself and the modifying element. Furthermore, the modifying element may exist as a doping element, a coating element, or a combination of a doping element and a coating element. Unless otherwise specified, "a modified form of a certain positive electrode active material" still falls within the scope of positive electrode active materials.

[0369] In this application, unless otherwise specified, a "doping element" in a positive electrode active material refers to a modifying element doped into the positive electrode active material. Unless otherwise specified, a "coating element" in a positive electrode active material refers to a positive electrode active material comprising a main body of positive electrode active particles and a coating layer located on at least a portion of the surface of the main body of the positive electrode active particles, wherein the coating element is a modifying element located within the coating layer. As a non-limiting example, in a positive electrode active material, "the modifying element is present as a combination of a doping element and a coating element" means that the positive electrode active material comprises a main body of positive electrode active particles and a coating layer located on at least a portion of the surface of the main body of the positive electrode active particles, at least a portion of the modifying element is doped into the main body of the positive electrode active material, and at least a portion of the modifying element is also contained within the coating layer. The main body of the positive electrode active particles can be the positive electrode active material itself or a doped and modified form thereof. In some embodiments, the doping element can include one or more of Na, K, Ca, Ba, Sb, Ti, Zr, W, Sr, Nb, Mo, Si, Mg, B, Cr, Ta, and the like. In some embodiments, the coating element may include one or more of Ti, Mg, Nb, C, and the like.

[0370] In this application, unless otherwise specified, "ternary cathode material" refers to one or more of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. The chemical formula of the ternary cathode material can be: The ternary cathode material is a lithium ion active material.

[0371] In this application, unless otherwise specified, "lithium ion active material" refers to a positive electrode active material that can provide active lithium ions at the positive electrode.

[0372] In this application, unless otherwise specified, "lithium ion active material" refers to a positive electrode active material that can provide active lithium ions in the positive electrode.

[0373] In some embodiments, the positive electrode active material includes a lithium iron phosphate-based positive electrode active material. The "lithium iron phosphate-based positive electrode active material" includes at least a lithium iron phosphate body and may further include a carbon coating layer located on at least a portion of a surface of the lithium iron phosphate body. Optionally, the carbon coating layer may include one or more of soft carbon, hard carbon, and amorphous carbon.

[0374] Without limitation, the lithium iron phosphate-based positive electrode active material may include carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body. Optionally, the carbon coating layer may include one or more of soft carbon, hard carbon and amorphous carbon.

[0375] Those skilled in the art can use conventional techniques to select and control the mass percentage of the carbon coating layer in a lithium iron phosphate-based positive electrode active material (an example of a lithium iron phosphate-based positive electrode active material is carbon-coated lithium iron phosphate) and the thickness or average thickness of the carbon coating layer. Without limitation, the mass percentage of the carbon coating layer in the lithium iron phosphate-based positive electrode active material can be 0.5% to 2%, but is not limited thereto. Without limitation, the average thickness of the carbon coating layer in the lithium iron phosphate-based positive electrode active material can be 10 nm to 20 nm, but is not limited thereto. Without limitation, the mass percentage of the carbon coating layer in the carbon-coated lithium iron phosphate can be 0.5% to 2%, but is not limited thereto. Without limitation, the average thickness of the carbon coating layer in the carbon-coated lithium iron phosphate can be 10 nm to 20 nm, but is not limited thereto.

[0376] The lithium-ion secondary battery provided above can flexibly select a variety of positive electrode active materials.

[0377] When the lithium iron phosphate-based positive electrode active material includes a carbon coating layer, for example, when the positive electrode active material includes carbon-coated lithium iron phosphate, the conductivity of the surface of the lithium iron phosphate body can be improved, and the conductive network inside the positive electrode sheet can be optimized, thereby improving the battery cycle performance.

[0378] In some embodiments, a lithium-ion secondary battery includes battery cells.

[0379] In this application, unless otherwise specified, a "battery cell" refers to a basic unit that can achieve the mutual conversion of chemical energy and electrical energy. Further, generally speaking, it includes at least a positive electrode plate, a negative electrode plate, and an electrolyte. During the battery's charge and discharge process, active ions are embedded in and out of the positive and negative electrode plates. The electrolyte plays the role of conducting active ions between the positive and negative electrode plates.

[0380] The following is some description about the positive electrode.

[0381] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.

[0382] Without limitation, the mass fraction of the positive electrode active material in the positive electrode active material layer can be greater than or equal to 80%, further can be greater than or equal to 90%, and can also be any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, etc.

[0383] As a non-limiting example, the positive electrode current collector has two surfaces facing away from each other in its thickness direction, and the positive electrode active material layer is disposed on either or both of the two facing surfaces of the positive electrode current collector.

[0384] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. In the positive electrode current collector, the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. In the positive electrode current collector, the composite current collector may be obtained by forming a metal material on a polymer material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include at least one of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. In the positive electrode current collector, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), and the like.

[0385] The types of positive electrode active materials can be found in the above text. The positive electrode active materials may also include other types of positive electrode active materials known in the art for lithium-ion secondary batteries. The positive electrode active materials may be used alone or in combination of two or more.

[0386] As non-limiting examples, the positive electrode active material may include, but is not limited to, one or more of the following materials: olivine-structured lithium-containing phosphates, lithium transition metal oxides, and modified compounds thereof.

[0387] In some embodiments, the positive electrode active material includes one or more of a lithium-containing phosphate-based active material and a lithium composite metal oxide-based active material.

[0388] In some embodiments, the positive electrode active material includes a lithium-containing phosphate-based active material.

[0389] In this application, unless otherwise specified, the lithium-containing phosphate active material may include at least one of lithium-containing phosphate and its modified form. The lithium-containing phosphate active material may have an olivine structure. Unless otherwise specified, "lithium-containing phosphate" refers to a material comprising lithium, a transition metal element, and phosphate ions (PO4 3- ) positive electrode active material. Non-limiting examples of olivine-structured lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0390] In some embodiments, the positive electrode active material includes an olivine-structured lithium-containing phosphate. Non-limiting examples of olivine-structured lithium-containing phosphates include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. An example of lithium iron phosphate is LiFePO4 (also referred to as LFP). An example of lithium manganese phosphate is LiMnPO4.

[0391] In some embodiments, the positive electrode active material includes a lithium composite metal oxide-based active material.

[0392] In the present application, unless otherwise specified, lithium composite metal oxide active materials include at least one of lithium composite metal oxides and modified forms thereof. Unless otherwise specified, "lithium composite metal oxide" refers to a positive electrode active material including lithium elements, non-lithium metal elements and oxygen elements. Generally, the non-lithium metal elements of lithium composite metal oxides include transition metal elements, and therefore, lithium composite metal oxides can also be referred to as "lithium transition metal oxides". Lithium composite metal oxide active materials can have crystal structures such as layered structures and spinel structures suitable for positive electrode active materials. In some embodiments, the lithium composite metal oxide active material comprises a layered structure. In some embodiments, the lithium composite metal oxide active material is a layered structure.

[0393] In some embodiments, the positive electrode active material includes a lithium transition metal oxide. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and modified compounds thereof. Non-limiting examples of lithium cobalt oxide may include LiCoO2; non-limiting examples of lithium nickel oxide may include LiNiO2; non-limiting examples of lithium manganese oxide may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxide may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxide may include LiNi 0.80 Co 0.15 Al 0.05 O2.

[0394] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charge and discharge process, and the content of Li in the positive electrode sheet is different when the battery is discharged to different states. In the exemplary description of the positive electrode active material in this application, unless otherwise specified, the Li content can be the initial state of the material or the non-initial state after the charge and discharge cycle. The positive electrode active material is applied to the positive electrode in the battery system, and after the charge and discharge cycle, the Li content in the positive electrode active material at the positive electrode will usually change. Among them, the Li content can be measured by atomic molar content, but is not limited to this. Regarding "the Li content is the initial state of the material", the initial state of the material refers to the state before it is made into a positive electrode active material layer. It is understandable that new materials or new substances obtained by appropriate modification of the listed positive electrode active materials are also within the scope of positive electrode active materials. The aforementioned appropriate modification refers to acceptable modification methods for positive electrode active materials, and non-limiting examples include one or more of coating modification and doping modification.

[0395] In the exemplary descriptions of the positive electrode active materials in this application, the oxygen (O) content is only a theoretical value. Oxygen release from the lattice will cause the atomic molar content of oxygen to change, and the actual O content will fluctuate. The O content can be measured in atomic molar content, but is not limited to this.

[0396] In some embodiments, the positive electrode active material layer optionally includes a binder. The binder in the positive electrode active material layer may be referred to as a positive electrode binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. Typically, the mass fraction of the binder in the positive electrode active material layer may be 0 to 10%, further 0 to 8%, and further 1% to 5%, based on the total mass of the positive electrode active material layer.

[0397] In some embodiments, the positive electrode active material layer optionally includes a conductive agent. The conductive agent in the positive electrode active material layer may be referred to as a positive electrode conductive agent. As non-limiting examples, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Typically, the mass fraction of the conductive agent in the positive electrode active material layer may be 0-10%, further 0-8%, and even further 0-5%, based on the total mass of the positive electrode active material layer.

[0398] In some embodiments, a positive electrode sheet can be prepared by dispersing the components for preparing the positive electrode sheet described above, such as the positive electrode active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry. The positive electrode slurry is then coated on at least one surface of a positive electrode current collector. After drying and cold pressing, the positive electrode sheet is obtained. Cold pressing can be performed using a cold rolling mill. The solvent in the positive electrode slurry can include, but is not limited to, any of the aforementioned embodiments, such as N-methylpyrrolidone (NMP), or further NMP. The positive electrode slurry can be coated on a single surface of the positive electrode current collector or on both surfaces of the positive electrode current collector. The solids content of the positive electrode slurry can range from 40 wt% to 80 wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to between 5,000 mPa·s and 25,000 mPa·s.

[0399] In this application, "wt%" means weight percentage or mass percentage.

[0400] In some embodiments, the positive electrode active material includes a lithium-containing phosphate active material. Furthermore, the mass proportion of the lithium-containing phosphate active material in the positive electrode active material can be greater than or equal to 50%, but is not limited thereto. When applying the positive electrode slurry, the coating area density (based on the coating area density on both sides) on a dry weight basis (excluding the solvent) can also be (0.2~1.0) g / 1540.25mm 2 , optional (0.4 ~ 0.8) g / 1540.25mm 2 , but not limited to this. The compaction density of the positive electrode sheet can be 2.0g / cm 3 ~2.8 g / cm 3 , optional 2.3g / cm 3 ~2.6 g / cm 3 .

[0401] In some embodiments, the positive electrode active material includes a lithium composite metal oxide active material. Further, the mass proportion of the lithium composite metal oxide active material in the positive electrode active material can be greater than or equal to 50%, but is not limited thereto. When applying the positive electrode slurry, the coating area density (based on the coating area density on both sides) on a dry weight basis (excluding the solvent) can be (0.1 to 1.2) g / 1540.25 mm 2 , optional (0.2~ 0.6) g / 1540.25mm 2 The compaction density of the positive electrode can be 3.0 g / cm 3 ~ 4.2 g / cm 3 , optional 3.3 g / cm 3 ~ 3.8 g / cm 3 .

[0402] The following are some additional descriptions about the negative electrode.

[0403] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on at least one surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material. It is understood that the at least one negative electrode active layer includes a first negative electrode active layer and a second negative electrode active layer, with the second negative electrode active layer located between the negative electrode current collector and the first negative electrode active layer. The first negative electrode active layer includes a first negative electrode active material, and the second negative electrode active layer includes a second negative electrode active material. The definitions of the first negative electrode active material and the second negative electrode active material can be found above.

[0404] As a non-limiting example, the negative electrode sheet includes a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector.

[0405] Without limitation, the mass fraction of the first negative electrode active material in the first negative electrode active layer may be greater than or equal to 80%, further may be greater than or equal to 90%, and may be any of the following percentages or a range consisting of any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, etc.

[0406] Without limitation, the mass fraction of the second negative electrode active material in the second negative electrode active layer may be greater than or equal to 80%, further may be greater than or equal to 90%, and may be any of the following percentages or a range selected from any two of the following percentages: 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 98.1%, etc.

[0407] As a non-limiting example, the negative electrode current collector has two surfaces facing away from each other in its thickness direction, and the negative electrode active layer is disposed on either or both of the two facing surfaces of the negative electrode current collector.

[0408] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. In the negative electrode current collector, the composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. In the negative electrode current collector, the composite current collector may be formed by forming a metal material on a polymer base layer. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. In the negative electrode current collector, the polymer base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), and the like.

[0409] In some embodiments, the types of the first negative electrode active material and the second negative electrode active material can refer to the above. The first negative electrode active material and the second negative electrode active material can also each independently include other types of negative electrode active materials for lithium-ion secondary batteries that are well known in the art. As a non-limiting example, the first negative electrode active material and the second negative electrode active material can each independently include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. Silicon-based materials can include one or more of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. Tin-based materials can include one or more of elemental tin, tin oxides and tin alloys. However, the present application is not limited to these materials or substances, and other traditional materials that can be used as battery negative electrode active materials can also be used. These negative electrode active materials can be used alone or in combination of two or more.

[0410] In some embodiments, the first negative electrode active material and the second negative electrode active material may each independently include a carbon-based material. Without limitation, the mass fraction of the carbon-based material in the first negative electrode active material or the second negative electrode active material may each independently be ≥80%, optionally ≥90%, further optionally ≥95%, further optionally ≥96%, and further optionally 100%. The mass fraction ratio of the carbon-based material in the first negative electrode active material or the second negative electrode active material may also be any of the following percentages, or greater than or equal to any of the following percentages and less than or equal to 100%, or selected from an interval consisting of any two of the following percentages: 80%, 82%, 83%, 84%, 85%, 86%, 88%, 90%, 92%, 94%, 95%, 96%, 98%, and the like. The carbon-based material may include, but is not limited to, one or more of graphite materials, soft carbon, hard carbon, and the like. The graphite material may include one or more of artificial graphite and natural graphite. In some embodiments, the carbon-based material may be a graphite material.

[0411] In some embodiments, the first negative electrode active layer and the second negative electrode active layer each independently optionally include a binder. In some embodiments, the first negative electrode active layer includes a first binder, and the second negative electrode active layer includes a second binder.

[0412] Without limitation, in the negative electrode sheet, the first binder and the second binder may each independently include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0413] The type of the first binder and its mass fraction in the first negative electrode active layer can be found in the above text.

[0414] The mass fraction of the second binder in the second negative electrode active layer can be found in the above text.

[0415] In some embodiments, the first negative electrode active layer and the second negative electrode active layer each independently optionally include a conductive agent. In some embodiments, the first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent.

[0416] Without limitation, in the negative electrode sheet, the first conductive agent and the second conductive agent may each independently include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0417] The mass fraction of the first conductive agent in the first negative electrode active layer can be found in the above text.

[0418] The mass fraction of the second conductive agent in the second negative electrode active layer can be found in the above text.

[0419] In some embodiments, the first negative electrode active layer and the second negative electrode active layer may each independently include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)). Without limitation, the mass fraction of the other additives in the first negative electrode active layer or the second negative electrode active layer may independently be 0% to 15%, further optionally 0% to 10%, further optionally 0% to 5%, further optionally 0% to 3%, and further optionally 0% to 2%.

[0420] In some embodiments, the preparation method of the lithium-supplemented negative electrode sheet can refer to the fourth aspect of the present application, and can also refer to the third aspect of the present application.

[0421] In some embodiments, the preparation method of the lithium-ion secondary battery can refer to the fourth aspect of the present application, and can also refer to the third aspect of the present application.

[0422] The electrolyte is exemplarily described below.

[0423] The electrolyte conducts ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0424] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0425] In some embodiments, the electrolyte is a non-aqueous electrolyte. The non-aqueous electrolyte may include an electrolyte salt and a solvent.

[0426] The concentration of the electrolyte salt in the electrolyte solution may generally be 0.5 mol / L to 5 mol / L, and may be optionally 0.8 mol / L to 1.2 mol / L.

[0427] In some embodiments, the electrolyte salt includes an electrolyte lithium salt. Without limitation, the electrolyte lithium salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorobis(oxalatophosphate) (LiDFOP), and lithium tetrafluorooxalatophosphate (LiTFOP).

[0428] In some embodiments, the solvent in the non-aqueous electrolyte may include ethylene carbonate (EC, ), propylene carbonate (PC, ), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate ( ), one or more of fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0429] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0430] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), and the like.

[0431] The separator is exemplarily described below.

[0432] In some embodiments, the lithium-ion secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0433] In some embodiments, the material of the separator can include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0434] In some embodiments, the thickness of the isolation film is 6 μm to 40 μm, and optionally 6 μm to 20 μm.

[0435] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0436] In some embodiments, the lithium-ion secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0437] In some embodiments, the outer packaging of the lithium-ion secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium-ion secondary battery can also be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic. Further, non-limiting examples of plastic can include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0438] A lithium-ion secondary battery includes at least one battery cell. A lithium-ion secondary battery may include one or more battery cells.

[0439] The present application has no particular restrictions on the shape of the battery cell, which can be cylindrical, square or any other shape. For example, Figure 5 The battery cell 5 is a square structure as an example.

[0440] In some embodiments, reference Figure 6 The outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to actual needs.

[0441] The lithium-ion secondary battery may be the battery device 4 or the battery pack 1 .

[0442] The battery device includes at least one battery cell. The number of battery cells contained in the battery device can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery device.

[0443] Figure 7 4 is an example of a battery device. Figure 7 In the battery device 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery device 4. Of course, they may also be arranged in any other manner. The plurality of battery cells 5 may further be fixed by fasteners.

[0444] Optionally, the battery device 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.

[0445] In some embodiments, the battery devices may be assembled into a battery pack. The battery pack may contain one or more battery devices. Those skilled in the art may select an appropriate number based on the application and capacity of the battery pack.

[0446] Figure 8 and Figure 9 The battery pack 1 is used as an example. Figure 8 and Figure 9 The battery pack 1 may include a battery box and multiple battery devices 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form an enclosed space for accommodating the battery devices 4. The multiple battery devices 4 can be arranged in any manner in the battery box.

[0447] In another aspect of the present application, a negative electrode sheet is provided, comprising a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0448] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0449] The negative electrode plate undergoes negative electrode lithium replenishment treatment.

[0450] In some embodiments, a negative electrode sheet is provided, comprising a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially disposed on at least one side of the negative electrode current collector;

[0451] The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0452] In the negative electrode sheet, a lithium supplement residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer.

[0453] The negative electrode plate is a negative electrode plate that has been treated with negative electrode lithium replenishment, and its negative electrode active material layer is provided with a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer (the upper layer is the direction away from the surface of the negative electrode current collector, and the lower layer is the direction toward the surface of the negative electrode current collector). Furthermore, the negative electrode plate satisfies one or both of the characteristics (i) and (ii): (i) the first negative electrode active layer located on the upper layer has a higher electrical conductivity, and (ii) the first negative electrode active layer located on the upper layer has a lower powder resistivity, so that the negative electrode plate can achieve efficient lithium replenishment by using a process of providing a lithium replenishment layer on the surface of the first negative electrode active layer away from the second negative electrode active layer. As a result, the negative electrode plate includes lithium pre-embedded by negative electrode lithium replenishment through the lithium replenishment layer. During negative electrode lithium replenishment using this process, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Because the first negative electrode active layer has higher conductivity and / or lower powder resistivity, this facilitates faster embedding of active lithium into the first negative electrode active layer, thereby inhibiting the deactivation of active lithium before it is embedded in the negative electrode active material. This can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving lithium replenishment efficiency. Thus, a negative electrode plate treated with efficient negative electrode lithium replenishment can be obtained. By introducing a negative electrode plate treated with efficient negative electrode lithium replenishment into a lithium-ion secondary battery, active lithium can be replenished continuously during the charge and discharge cycles, thereby continuously replenishing capacity. Furthermore, during the charging process, the faster embedding of active lithium ions helps reduce the accumulation of lithium ions on the surface of the negative electrode active material, thereby reducing the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0454] In some embodiments, the negative electrode plate is the negative electrode plate of the lithium-ion secondary battery described in the first aspect of this application.

[0455] In a second aspect of the present application, a lithium-supplementing negative electrode sheet is provided, comprising a negative electrode current collector and a second negative electrode active layer, a first negative electrode active layer and a lithium-supplementing layer sequentially disposed on at least one side of the negative electrode current collector;

[0456] The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer.

[0457] A lithium-supplemented negative electrode sheet having a lithium-supplementing layer disposed on the surface of a negative electrode active material layer is provided. By disposing a first negative electrode active layer and a second negative electrode active layer on the negative electrode active material layer, and ensuring that the first negative electrode active layer on the side closest to the lithium-supplementing layer has a higher electrical conductivity and / or a lower powder resistivity, the lithium-supplementing treatment of the lithium-supplemented negative electrode sheet facilitates rapid intercalation of active lithium ions into the first negative electrode active layer. During the process of assembling a lithium-ion secondary battery using the lithium-supplemented negative electrode sheet, after injecting the electrolyte, the active lithium provided by the lithium-supplementing layer is facilitated to be more rapidly intercalated into the first negative electrode active layer. This helps inhibit the deactivation of the active lithium before intercalation into the negative electrode active material, reduces the generation of deactivated lithium during lithium-supplementation, and significantly improves the lithium-supplementing efficiency. This results in a negative electrode sheet with efficient lithium-supplementing treatment. The resulting lithium-ion secondary battery can sustainably replenish active lithium and capacity during charge and discharge cycles, and can also reduce lithium ion accumulation on the surface of the negative electrode active material, thereby reducing lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0458] In the present application, the lithium replenishing layer in the lithium replenishing negative electrode sheet includes a negative electrode lithium replenishing material.

[0459] Without limitation, the lithium replenishing layer may include one or more of elemental lithium and a lithium alloy. A non-limiting example of a lithium alloy is a lithium-tin alloy. In some embodiments, the lithium replenishing layer includes elemental lithium, and in this case, the negative electrode lithium replenishing material includes elemental lithium.

[0460] In some embodiments, the lithium supplement layer is provided by lithium foil, and the lithium foil is rolled onto the first negative electrode active layer to form a lithium film corresponding to the lithium supplement layer.

[0461] When elemental lithium (such as lithium foil) is introduced into the lithium replenishment layer to provide active lithium, the cost is more controllable.

[0462] In some embodiments, the thickness of the lithium replenishing layer on a single side of the negative electrode current collector is less than the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer.

[0463] In some embodiments, the thickness of the lithium supplement layer on one side of the negative electrode current collector is less than 8.5 μm, and may be 0.5 μm to 8.5 μm, or further may be 1 μm to 8.5 μm.

[0464] In some embodiments, the thickness of the lithium replenishing layer on one side of the negative electrode current collector is less than or equal to 4.8 μm, and may be 1 μm to 4.8 μm, or further may be 2 μm to 4.8 μm.

[0465] Without limitation, the thickness of the lithium replenishing layer on a single side of the negative electrode current collector can also be any of the following values ​​or a range selected from any two of the following values: 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.8μm, 5μm, 6μm, 7μm, 8μm, 8.5μm, etc.

[0466] In this application, unless otherwise specified, the “thickness of the lithium supplement layer” refers to the thickness on one side of the negative electrode current collector, which may also be referred to as the “single-side thickness of the lithium supplement layer”.

[0467] The thickness of the lithium replenishment layer can be measured and analyzed based on the cross-sectional SEM image of the lithium replenishment negative electrode sheet, or by using a laser thickness gauge. The method for obtaining the cross-sectional SEM image of the lithium replenishment negative electrode sheet can refer to the cross-sectional SEM image of the negative electrode sheet.

[0468] In this application, unless otherwise specified, the “cross section of the lithium-supplemented negative electrode sheet” refers to the cross section of the lithium-supplemented negative electrode sheet.

[0469] The thickness of the lithium replenishment layer can be adjusted based on the amount of lithium replenishment required for the negative electrode. Furthermore, controlling the thickness of the lithium replenishment layer within the aforementioned range facilitates controlling the thickness of the lithium replenishment residual layer within a more appropriate range, thereby achieving better electrolyte wetting and charge transfer performance, and contributing to good battery kinetics.

[0470] During the production process, residual water often remains within the negative electrode, making it difficult to completely remove. This water may react with the lithium-replenishing material in the lithium-replenishing layer, generating heat. The thicker the lithium-replenishing layer, the higher the heat generation. While not being bound by theory, controlling the lithium-replenishing layer thickness within the aforementioned range helps better control heat generation caused by the water-lithium reaction, thereby improving production safety.

[0471] In some embodiments, in the lithium-supplemented negative electrode sheet, the coverage area percentage of the lithium-supplemented layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is less than or equal to 98%, and optionally less than or equal to 70%. In some embodiments, the coverage area percentage of the lithium-supplemented layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is greater than 0 and less than or equal to 90%. In some embodiments, in the negative electrode sheet, the coverage area percentage of the lithium-supplemented layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, is greater than 0 and less than or equal to 70%. Without limitation, in the negative electrode sheet, the coverage area percentage of the lithium-replenishing layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, may also be any of the following percentages, or any two of the following percentages: 0.1%, 1%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 98%, etc. Without limitation, the coverage area percentage of the lithium-replenishing layer relative to the first negative electrode active layer, measured on a single side of the negative electrode current collector, may be selected from any appropriate range: greater than 0 and less than or equal to 50%, 30%-98%, 30%-70%, 30%-50%, 50%-98%, 50%-70%, etc.

[0472] By controlling the coverage area percentage of the lithium-replenishing layer relative to the first negative electrode active layer in the lithium-replenishing negative electrode sheet within the aforementioned range, it is beneficial to control the coverage area percentage of the lithium-replenishing residual layer relative to the first negative electrode active layer in the lithium-ion secondary battery within a more appropriate range, which is beneficial to better achieve good electrolyte infiltration performance and charge transfer performance, and is beneficial to making the battery have good battery dynamics.

[0473] The shape of the area covered by the lithium-replenishing layer on the first negative electrode active layer is not particularly limited and may be any suitable shape, such as a strip or a grid, but is not limited thereto. A shape that is more easily handled in the process can be selected. By adjusting the shape of the area covered by the lithium-replenishing layer on the first negative electrode active layer, the percentage of the area covered by the residual lithium-replenishing layer relative to the first negative electrode active layer can be adjusted.

[0474] Without limitation, the shape and size of the lithium replenishing layer (such as stripe spacing, grid spacing, etc.) can be measured using a ruler or a CCD (inductively coupled device).

[0475] Figure 1 This is a schematic structural diagram of a lithium-supplemented negative electrode sheet in one embodiment of the present application, corresponding to a side view. Figure 2 yes Figure 1 Schematic diagram of the structure of the lithium-supplemented negative electrode sheet, corresponding to the top view. Figure 1The lithium-supplementing negative electrode sheet 12 in the illustrated embodiment includes a negative electrode current collector 102 and a second negative electrode active layer 104 , a first negative electrode active layer 106 and a lithium-supplementing layer 108 sequentially disposed on one side of the negative electrode current collector 102 . Figure 1 In the embodiment, the second negative electrode active layer 104, the first negative electrode active layer 106 and the lithium replenishing layer 108 are sequentially stacked along the thickness direction Z of the negative electrode sheet, and the lithium replenishing layer covers the first negative electrode active layer in a strip shape.

[0476] In this application, unless otherwise specified, the X direction corresponds to the width direction of the electrode (which may be consistent with the height direction of the wound battery cell), the Y direction corresponds to the length direction of the electrode, and the Z direction corresponds to the thickness direction of the electrode.

[0477] Taking an electrode assembly assembled in a winding manner as an example, the Y direction may correspond to the winding direction of the electrode sheet, and the X direction may correspond to the direction in which the tab extends, that is, the X direction may correspond to the height direction of the electrode assembly or the bare cell.

[0478] Figure 3 This is a schematic diagram of the structure of the lithium-supplemented negative electrode sheet in another embodiment of the present application, corresponding to the top view, Figure 3 In the embodiment, the lithium replenishing layer covers the first negative electrode active layer in a strip-like shape.

[0479] Figure 4 This is a schematic diagram of the structure of the lithium-supplemented negative electrode sheet in another embodiment of the present application, corresponding to the top view, Figure 4 In the embodiment, the shape of the covering area of ​​the lithium replenishing layer on the first negative electrode active layer is a grid.

[0480] In some embodiments, the compaction density of the lithium-supplemented negative electrode sheet is 1.3 g / cm 3 ~1.8g / cm 3 , optional 1.4g / cm 3 ~1.6g / cm 3 Without limitation, the compaction density of the lithium supplemented negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 1.3 g / cm 3 , 1.30 g / cm 3 , 1.35 g / cm 3 , 1.40 g / cm 3 , 1.45 g / cm 3 , 1.50g / cm 3 , 1.55 g / cm 3 , 1.60 g / cm 3 , 1.65 g / cm 3 , 1.70 g / cm 3 、1.71 g / cm 3 , 1.75 g / cm3 , 1.8 g / cm 3 , 1.80 g / cm 3 wait.

[0481] In some embodiments, the surface density of the lithium-supplemented negative electrode sheet is 10 mg / cm 2 ~26mg / cm 2 , optional 15mg / cm 2 ~20mg / cm 2 Without limitation, the surface density of the lithium-supplemented negative electrode sheet can also be any of the following values ​​or a range consisting of any two of the following values: 10 mg / cm 2 , 12 mg / cm 2 、15 mg / cm 2 , 16 mg / cm 2 、18 mg / cm 2 , 20 mg / cm 2 , 22mg / cm 2 , 24 mg / cm 2 , 25 mg / cm 2 , 26 mg / cm 2 wait.

[0482] By adjusting the compaction density and / or areal density of the lithium-supplemented negative electrode sheet, the compaction density and / or areal density of the negative electrode sheet in the lithium-ion secondary battery can be correspondingly controlled. By controlling the compaction density and / or areal density of the lithium-supplemented negative electrode sheet within the aforementioned range, the battery can also achieve a higher energy density.

[0483] In this application, unless otherwise specified, the compaction density of a lithium-supplemented negative electrode sheet refers to the ratio of the mass to volume of the negative electrode active material layer (excluding the lithium-supplemented layer) in the lithium-supplemented negative electrode sheet.

[0484] In this application, unless otherwise specified, the areal density of the lithium-supplemented negative electrode sheet refers to the areal density calculated on the total amount on both sides, which is equal to the compaction density of the lithium-supplemented negative electrode sheet multiplied by the total thickness on both sides of the negative electrode active material layer.

[0485] Without limitation, the following method can be used to obtain the compaction density and the surface density of the lithium-supplemented negative electrode sheet based on the total amount on both sides:

[0486] (1) Punch the lithium-supplemented negative electrode sheet into a piece with an area of ​​A (e.g. 1540.25 mm 2 ) and measure the weight m and thickness L of the small disc;

[0487] (2) Take another lithium-supplemented negative electrode sheet, wipe off the surface film layer and the remaining empty current collector foil, and also punch out the area A (such as 1540.25mm 2) small disc, weigh the empty foil mass M0, thickness L0;

[0488] (3) The sum of the double-sided density of the lithium-replenishing layer on the first negative electrode active layer in the lithium-replenishing negative electrode sheet of the tested embodiment is recorded as ρ A The total thickness of the lithium supplement layer on both sides is recorded as d D ;

[0489] (4) Calculation:

[0490] Compaction density PD of lithium-supplemented negative electrode sheet A =(M-M0-ρ A ×d D ) / [A×(L-L0-d D )].

[0491] Surface density of lithium-supplemented negative electrode sheet (based on the total amount on both sides) = (M-M0-ρ A ×d D ) / A.

[0492] In some embodiments, the preparation method of the lithium-supplemented negative electrode sheet can refer to the fourth aspect of this application.

[0493] In the third aspect of the present application, a component for preparing a lithium-ion secondary battery is also provided, which includes an electrode assembly and an electrolyte, the electrode assembly includes a positive electrode sheet, a lithium-supplemented negative electrode sheet and an isolation membrane, and an isolation membrane is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; the lithium-supplemented negative electrode sheet can be the lithium-supplemented negative electrode sheet described in the second aspect of the present application.

[0494] In this application, unless otherwise specified, "assembly for preparing a lithium-ion secondary battery" includes at least an assembled electrode assembly and an electrolyte. The assembly may be in a state before the electrolyte is injected, in which case the electrode assembly and the electrolyte are placed separately. The assembly may also be in a state after the electrolyte is injected but before it is fully soaked. In the assembly for preparing a lithium-ion secondary battery, the negative electrode lithium-replenishing material in the lithium-replenishing layer has not been consumed or has only been partially consumed.

[0495] By introducing the aforementioned lithium-replenishing negative electrode sheet into the components used for lithium-ion secondary batteries, it is beneficial to enable the active lithium provided by the lithium-replenishing layer to be embedded in the first negative electrode active layer more quickly, which is beneficial to inhibiting the deactivation of the active lithium before being embedded in the negative electrode active material, and can reduce the generation of deactivated lithium during lithium replenishment, which is beneficial to significantly improve the lithium replenishment efficiency, and obtain a negative electrode sheet treated with high-efficiency lithium replenishment. The obtained lithium-ion secondary battery can persistently replenish active lithium during the charge and discharge cycle, continuously replenish capacity, and can also reduce the enrichment of lithium ions on the surface of the negative electrode active material and reduce the generation of lithium plating, thereby enabling the lithium-ion secondary battery to have improved long cycle life performance.

[0496] In some embodiments, in a component for preparing a lithium-ion secondary battery, the electrolyte includes an additive; without limitation, in a component for preparing a lithium-ion secondary battery, the additive in the electrolyte may include one or more of vinylene carbonate (VC) and a sulfur-containing additive; without limitation, the sulfur-containing additive may include one or more of vinyl sulfate (DTD), vinyl sulfite (ES) and propylene sulfite (PS).

[0497] In some embodiments, in a component for preparing a lithium-ion secondary battery, the additive in the electrolyte includes vinylene carbonate (VC), fluoroethylene carbonate (FEC) and diethylene sulfate (DTD), and may further be a combination of vinylene carbonate (VC), fluoroethylene carbonate (FEC) and diethylene sulfate (DTD). Without limitation, in a component for preparing a lithium ion secondary battery, the mass fraction of vinylene carbonate (VC) in the electrolyte can be 0-3%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, etc.

[0498] Without limitation, in the components for preparing lithium-ion secondary batteries, the mass fraction of fluoroethylene carbonate (FEC) in the electrolyte can be 0-6%, and can also be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc.

[0499] Without limitation, in the components for preparing lithium-ion secondary batteries, the mass fraction of vinyl sulfate (DTD) in the electrolyte can be 0~4%, or can be any of the following percentages or a range consisting of any two of the following percentages: 0%, 0.01%, 0.05%, 0.06%, 0.08%, 0.1%, 0.12%, 0.15%, 0.16%, 0.18%, 0.2%, 0.25%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, 3.5%, 4%, etc.

[0500] In a fourth aspect of the present application, a method for preparing a lithium-ion secondary battery is provided, which can be used to prepare the lithium-ion secondary battery of the first aspect of the present application.

[0501] In some embodiments, a method for preparing a lithium-ion secondary battery is provided, comprising the following steps:

[0502] S100: Assembling a positive electrode sheet, a separator, and a lithium-supplemented negative electrode sheet into an electrode assembly, wherein a separator is provided between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active layer, a first negative electrode active layer, and a lithium-supplemented layer provided in sequence on at least one side of the negative electrode current collector; the lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer;

[0503] S200: placing the electrode assembly in the housing cavity of the shell, injecting electrolyte (to obtain components for preparing lithium-ion secondary batteries), allowing the electrolyte to infiltrate the positive electrode sheet and the lithium-supplemented negative electrode sheet, and forming them to obtain a lithium-ion secondary battery.

[0504] As defined above, a "lithium replenishing layer" refers to a structural layer containing a lithium replenishing material. As a non-limiting example, the lithium replenishing layer can be a lithium sheet. The lithium replenishing material contained in the lithium replenishing layer disposed on a lithium replenishing negative electrode sheet can also be referred to as the negative electrode lithium replenishing material.

[0505] In step S200, after impregnation and formation, the negative electrode lithium replenishment material in the lithium replenishment layer reacts with the electrolyte and is consumed, releasing active lithium. The released active lithium is then embedded in the negative electrode active material layer, achieving lithiation. The lithium replenishment negative electrode sheet is converted into a negative electrode sheet, and the first and second negative electrode active layers in the lithium replenishment negative electrode sheet are respectively converted into the first and second negative electrode active layers of the negative electrode sheet of the lithium-ion secondary battery. It is understood that the second and first negative electrode active layers each independently include pre-intercalated lithium. The locations of the consumed lithium replenishment layers typically produce residues generated during the lithium replenishment process. Non-limiting examples of such residues include lithium that has been deactivated due to not having enough time to embed into the negative electrode active material. Consequently, a lithium replenishment residual layer comprising inactive lithium is formed at the locations of the lithium replenishment layers. Accordingly, the lithium replenishment residual layer formed at the location of the first lithium replenishment layer is referred to as the first lithium replenishment residual layer, and the lithium replenishment residual layer formed at the location of the second lithium replenishment layer is referred to as the second lithium replenishment residual layer.

[0506] In step S200, after infiltration and formation, the lithium ions released from the lithium replenishing layer are embedded in the negative electrode active material, at least in the first negative electrode active layer, so that the first negative electrode active layer is pre-intercalated with lithium. Similarly, the second negative electrode active layer is also pre-intercalated with lithium.

[0507] By contacting the electrode assembly including the aforementioned lithium-supplemented negative electrode sheet with an electrolyte, impregnating it, and chemically forming it, a negative electrode sheet including a negative electrode lithium-supplemented negative electrode sheet can be prepared. The negative electrode sheet is provided with a first negative electrode active layer located on the upper layer and a second negative electrode active layer located on the lower layer (the direction away from the negative electrode current collector surface is considered the upper layer, and the direction toward the negative electrode current collector surface is considered the lower layer). Furthermore, the first negative electrode active layer located on the upper layer has a higher electrical conductivity and / or a lower powder resistivity. In the process of performing negative electrode lithium replenishment using the aforementioned method, the negative electrode lithium replenishment material in the lithium replenishment layer provides active lithium. Based on the higher electrical conductivity and / or lower powder resistivity of the first negative electrode active layer, it is beneficial for the active lithium to be embedded into the first negative electrode faster. The active layer is conducive to inhibiting the deactivation of active lithium before it is embedded in the negative electrode active material, which can reduce the generation of deactivated lithium during lithium replenishment, thereby significantly improving the lithium replenishment efficiency. Therefore, the introduction of negative electrode plates that have undergone high-efficiency negative electrode lithium replenishment treatment into lithium-ion secondary batteries can persistently replenish active lithium and continuously replenish capacity during the charge and discharge cycle; in addition, during the charging process, the faster embedding of active lithium ions is conducive to reducing the enrichment of lithium ions on the surface of the negative electrode active material, which is conducive to reducing the generation of lithium plating, thereby making the lithium-ion secondary battery have improved long cycle life performance.

[0508] Without limitation, in step S200, the soaking temperature can be 20°C~60°C, or any of the following temperatures or a range consisting of any two of the following temperatures: 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C, etc.

[0509] Without limitation, in step S200, the immersion time can be 10 h to 50 h, or any of the following durations or a range consisting of any two of the following durations: 10 h, 12 h, 15 h, 16 h, 18 h, 20 h, 24 h, 25 h, 26 h, 28 h, 30 h, 35 h, 36 h, 40 h, 42 h, 45 h, 48 h, 50 h, etc.

[0510] By controlling the wetting parameters within the aforementioned range, it is beneficial for the electrolyte to more fully infiltrate the negative electrode plate.

[0511] In step 200, the negative electrode lithium supplement material may release active lithium while generating gas. For example, when the negative electrode lithium supplement material is elemental lithium, the elemental lithium reacts with the electrolyte to form lithium ions, and the electrolyte decomposes to generate gas.

[0512] In some embodiments, the lithium-supplementing layer in the lithium-supplementing negative electrode sheet satisfies the following formula:

[0513] 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3;

[0514] Among them, C N_A is the preset surface capacity of the negative electrode, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

[0515] The negative electrode preset surface capacity can be calculated based on the theoretical gram capacity of the negative electrode active material and the surface density of the negative electrode active material in the negative electrode sheet. N_A =Theoretical gram capacity of negative electrode active material × surface density of negative electrode active material in the negative electrode sheet.

[0516] The positive electrode preset surface capacity can be calculated based on the theoretical gram capacity of the positive electrode active material and the surface density of the positive electrode active material in the positive electrode sheet. P_A =Theoretical gram capacity of positive electrode active material × surface density of positive electrode active material in the positive electrode sheet.

[0517] ρ A It can be calculated based on the ratio between the total mass of both sides of the lithium replenishing layer (i.e., the mass of the lithium foil on both sides) and the average spreading area of ​​the lithium replenishing layer on its surface (on the surface of the first negative electrode active layer). The spreading area of ​​the lithium replenishing layer on its surface includes the covered area and the uncovered area.

[0518] In this application, "the average spreading area of ​​the lithium-replenishing layer on the first negative electrode active layer" refers to the average value of the spreading area on both sides of the negative electrode current collector. When the lithium-replenishing layer is only provided on one side of the negative electrode current collector, the average spreading area is the same as the spreading area on the single side, and the total mass of the lithium-replenishing layer on both sides is the same as the mass of the lithium-replenishing layer on the single side.

[0519] In this application, unless otherwise specified, the theoretical gram capacity of lithium, C Li / g It can be calculated as 3860mAh / g. In addition, the volume density of lithium can be calculated as 0.534g / cm 3 count.

[0520] In some embodiments, the lithium-supplementing layer in the lithium-supplementing negative electrode sheet satisfies the following formula:

[0521] 1.1≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3.

[0522] Without limitation, C N_A / (C Li / g ×ρ A +C P_A The value can be any one of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.08, 1.10, 1.12, 1.14, 1.15, 1.16, 1.18, 1.20, 1.22, 1.24, 1.25, 1.26, 1.28, 1.30, etc.

[0523] Without being limited by theory, controlling the thickness of the lithium replenishment layer to satisfy the aforementioned formula can not only extend the battery cycle life through lithium replenishment, but also help control the thickness of the lithium replenishment layer residue to a more appropriate level. Furthermore, it can better control the heat generated by the reaction between water and lithium, thereby improving production safety.

[0524] In some embodiments, the lithium-supplemented negative electrode sheet is prepared by a method comprising the following steps:

[0525] A second negative electrode active layer is formed on at least one side surface of the negative electrode substrate, a first negative electrode active layer is formed on the surface of the second negative electrode active layer away from the negative electrode substrate, and a lithium supplement layer is added on the surface of the first negative electrode active layer away from the second negative electrode active layer.

[0526] In some embodiments, the negative electrode substrate includes a negative electrode current collector. In some embodiments, the negative electrode substrate is a negative electrode current collector, and further can be copper foil.

[0527] In some embodiments, the lithium-supplemented negative electrode sheet is prepared by a method comprising the following steps S110, S120, and S130:

[0528] S110: Prepare a first negative electrode slurry and a second negative electrode slurry. The components used to prepare the first negative electrode active layer, such as the first negative electrode active material, the first conductive agent, the first binder, and any other components, are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form the first negative electrode slurry. The components used to prepare the second negative electrode active layer, such as the second negative electrode active material, the second conductive agent, the second binder, and any other components, are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form the second negative electrode slurry.

[0529] S120: Preparing a non-lithium-supplemented negative electrode sheet. A double-layer coating machine is used to coat the second negative electrode slurry and the first negative electrode slurry onto at least one side of the negative electrode current collector. The second negative electrode slurry is applied first, followed by the first negative electrode slurry. After drying and cold pressing, a non-lithium-supplemented negative electrode sheet comprising a second negative electrode active layer and a first negative electrode active layer is obtained. The second negative electrode active layer is located between the first negative electrode active layer and the negative electrode current collector. The composition of the non-solvent of the first negative electrode slurry forms the first negative electrode active layer, and the composition of the non-solvent of the second negative electrode slurry forms the second negative electrode active layer. Cold pressing can be performed using a cold rolling mill. The negative electrode slurry can be applied to a single surface of the negative electrode current collector or to both surfaces of the negative electrode current collector. The solids content of the first negative electrode slurry and the second negative electrode slurry can each independently be 30 wt% to 70 wt%, and can each independently be 40 wt% to 60 wt%. The viscosity of the first negative electrode slurry and the second negative electrode slurry at room temperature can be independently adjusted to 2000 mPa·s to 10000 mPa·s, and can be independently adjusted to 3000 mPa·s to 10000 mPa·s. The coating density of the negative electrode sheet and the compaction density of the negative electrode sheet can be referred to the second aspect of this application.

[0530] S130: Covering the first negative electrode active layer with a lithium foil, and laminating the lithium foil to the first negative electrode active layer by roller pressing.

[0531] The “un-lithium-supplemented negative electrode sheet” in step S120 corresponds to the aforementioned cold-pressed negative electrode sheet (without the lithium-supplemented layer).

[0532] In step S130, the amount of lithium foil can be calculated according to formula C N_A / (C Li / g ×ρ A +C P_A ) or C N_A / (C Li / g ×m Li / A Li +CP_A ) value to control. C N_A 、C P_A 、C Li / g and ρ A The definition of can be found in the above text, for example, can be found in the fourth aspect of this application. Li represents the mass of lithium foil, A Li It represents the average spreading area of ​​the lithium supplement layer on the first negative electrode active layer after roller pressing, and the spreading area includes the areas of the covered area and the uncovered area.

[0533] In some embodiments, the amount of lithium foil can be calculated according to the formula 1.1≤C N_A / (C Li / g ×m Li / A Li +C P_A )≤1.3 for control.

[0534] Without limitation, C N_A / (C Li / g ×ρ A +C P_A ) or C N_A / (C Li / g ×m Li / A Li +C P_A ) can be any one of the following values ​​or a range consisting of any two of the following values: 1.05, 1.06, 1.08, 1.10, 1.12, 1.14, 1.15, 1.16, 1.18, 1.20, 1.22, 1.24, 1.25, 1.26, 1.28, 1.30, etc.

[0535] By adjusting the mass of the lithium foil, rolling parameters and other parameters, one or more parameters such as the thickness of the lithium replenishing layer in the lithium replenishing negative electrode sheet and the coverage area percentage on the first negative electrode active layer can be adjusted.

[0536] The NP ratio of the prepared lithium-ion secondary battery can be tested and the measured value can be compared with the preset NP ratio. When there is a deviation, the NP ratio of the lithium-ion secondary battery can be more suitable by adjusting the quality of the lithium foil, rolling parameters and other parameters, but is not limited to this.

[0537] The NP ratio test method of lithium ion secondary battery can be found in the context of this application, including the first aspect of this application. NP ratio of lithium ion secondary battery = negative electrode surface capacity / positive electrode surface capacity; N Equal to A P In the case of , the following formula can also be used: NP ratio = C N / C P Negative electrode surface capacity = negative electrode capacity ÷ area A NPositive electrode surface capacity = positive electrode capacity ÷ area A P .

[0538] In some embodiments, the composition of the first negative electrode slurry may refer to the composition of the first negative electrode active layer.

[0539] In some embodiments, the composition of the second negative electrode slurry may refer to the composition of the second negative electrode active layer.

[0540] In some embodiments, the first negative electrode slurry can be prepared by dispersing the components for preparing the first negative electrode active layer, such as the first negative electrode active material, the conductive agent, the binder, and any other components (such as a thickener) in a solvent (a non-limiting example of the solvent is deionized water) to form a first negative electrode slurry.

[0541] In some embodiments, the second negative electrode slurry may be prepared by dispersing the components for preparing the second negative electrode active layer, such as the second negative electrode active material, the conductive agent, the binder, and any other components (such as a thickener) in a solvent (a non-limiting example of the solvent is deionized water) to form a second negative electrode slurry.

[0542] Without limitation, the solid content of the first negative electrode slurry and the second slurry can each independently be 30 wt% to 70 wt%, and optionally 40 wt% to 70 wt%. The viscosity of the first negative electrode slurry and the second slurry at room temperature can each independently be adjusted to 2000 mPa·s to 10000 mPa·s, and optionally 3000 mPa·s to 10000 mPa·s.

[0543] In some embodiments, the prepared lithium ion secondary battery is the lithium ion secondary battery described in the first aspect of this application.

[0544] In yet another aspect of the present application, a method for preparing a lithium-supplemented negative electrode sheet is provided, and reference may be made to the fourth aspect of the present application.

[0545] In the fifth aspect of the present application, an electrical device is provided, which includes at least one of the lithium-ion secondary battery described in the first aspect of the present application and the lithium-ion secondary battery prepared by the preparation method of the lithium-ion secondary battery described in the fourth aspect of the present application.

[0546] In some embodiments, an electric device includes the lithium-ion secondary battery according to any embodiment provided herein.

[0547] Lithium-ion secondary batteries can be used as power sources for electrical devices or as energy storage units for these devices. Electrical devices may include, but are not limited to, mobile devices, electric vehicles, electric trains, ships, satellites, and energy storage systems. Examples of mobile devices include, but are not limited to, mobile phones and laptop computers; examples of electric vehicles include, but are not limited to, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, electric motorcycles, and power tools. These electrical devices may also be used in fields such as military equipment and aerospace, and in energy storage power systems such as hydropower, thermal power, wind power, and solar power stations.

[0548] As an electrical device, a lithium-ion secondary battery can be selected according to its usage requirements.

[0549] Figure 10 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the power consumption device's requirements for high power and high energy density of lithium-ion secondary batteries, a battery device or battery pack can be used.

[0550] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a lithium-ion secondary battery as a power source.

[0551] The following describes some embodiments of the present application. The embodiments described are only a portion of the embodiments of the present application, rather than all of the embodiments. The embodiments described below are exemplary and are only used to explain the present application, and should not be understood as limiting the present application and its applications. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0552] If the techniques or conditions are not specified in the examples, the methods were carried out according to the description above, or according to the techniques or conditions described in the literature in the field, or according to the product instructions. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially or can be synthesized from commercial products according to conventional methods.

[0553] In the following examples, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument testing accuracy or operating accuracy are allowed.

[0554] In the following examples, room temperature refers to 20°C to 30°C.

[0555] 1. Implementation

[0556] (1) Preparation of lithium-supplemented negative electrode sheets and lithium-ion secondary batteries

[0557] Example 1.

[0558] (1) Positive electrode sheet: The positive electrode active material lithium iron phosphate (LFP, surface coated with soft carbon, the mass proportion of soft carbon in the positive electrode active material is about 1.5%), the conductive agent carbon black (Super P) and the binder polyvinylidene fluoride (PVDF) are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) at a mass ratio of 96.8:1.0:2.2 to obtain a positive electrode slurry with a solid content of about 60wt%; the positive electrode slurry is coated on both sides of the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through drying, cold pressing, slitting, cutting and other processes.

[0559] The coating density of the positive electrode slurry on both sides of the positive electrode current collector is 37.2 mg / cm based on the dry weight of the coating on both sides (excluding the weight of the solvent). 2 The total mass of the positive electrode active material layer on both sides is 572 mg, and the total density of the double-sided coating surface is 572 mg / 1540.25 mm 2 The compaction density of the positive electrode is 2.4g / cm 3 .

[0560] (2) Lithium supplementation negative electrode sheet: The second negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) were mixed in a solvent deionized water at a mass ratio of 96.3:0.4:2.2:1.1, with a solid content of about 53wt% to obtain the lower negative electrode slurry (corresponding to the second negative electrode active layer); the first negative electrode active material artificial graphite, conductive agent carbon black (Super P) were mixed in a solvent deionized water at a mass ratio of 96.3:0.4:2.2:1.1 to obtain the lower negative electrode slurry (corresponding to the second negative electrode active layer); P), binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed evenly in a solvent deionized water according to a mass ratio of 98.1:0.6:0.4:0.9, with a solid content of about 53wt% to obtain an upper negative electrode slurry (corresponding to the first negative electrode active layer). The two negative electrode slurries are coated on the double-sided surface of the negative electrode collector copper foil using a double-layer coating machine. The lower negative electrode slurry is coated first and then the upper negative electrode slurry is coated. Drying, cold pressing, slitting, and cutting are carried out to form the second negative electrode active layer and the first negative electrode active layer on the surface of the negative electrode collector copper foil in sequence to obtain an unreplenished lithium negative electrode sheet. The lithium foil is placed on the first negative electrode active layer and rolled to adhere the lithium foil to the first negative electrode active layer to obtain a single-sided unit area mass of about 0.1mg / cm 2 The lithium film (corresponding to the lithium replenishing layer) is obtained to obtain a lithium replenishing negative electrode sheet, which includes a negative electrode collector and a second negative electrode active layer, a first negative electrode active layer and a lithium replenishing layer sequentially arranged on both sides of the negative electrode collector.

[0561] The first negative electrode active layer is an upper layer, and the second negative electrode active layer is a lower layer.

[0562] In this example,

[0563] The upper and lower layers are made of artificial graphite from the same source. v 50 is 13.4μm and the OI value is about 3.6.

[0564] Lower layer (second negative electrode active layer): The solid content of the lower layer negative electrode slurry is about 53wt%, and the total coating density of the lower layer on both sides of the negative electrode current collector is 8.7mg / cm 2 , with a thickness of about 60μm.

[0565] Upper layer (first negative electrode active layer): The solid content of the upper negative electrode slurry is about 53wt%;

[0566] The total coating density of the upper layer on both sides of the negative electrode current collector is 8.7 mg / cm 2 , with a thickness of about 60μm.

[0567] The overall compaction density of the lithium-supplemented negative electrode sheet is 1.45g / cm 3 The total coating density on both sides is 17.4 mg / cm 2 .

[0568] In the lithium-supplemented negative electrode sheet, the thickness of a single side of the lithium-supplemented layer satisfies ≤8.5 μm, further satisfies ≤4.8 μm, and further falls within the range of 1 μm to 4.8 μm.

[0569] (3) Separator: Use a polypropylene separator with a thickness of 12 μm.

[0570] (4) Electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were mixed at a mass ratio of 30:30:40 to obtain an organic solvent. Fully dried lithium hexafluorophosphate (LiPF6) was dissolved in the above organic solvent. Vinylene carbonate (VC), fluoroethylene carbonate (FEC) and vinyl sulfate (DTD) were added to prepare an electrolyte containing 2.5 wt% VC, 1 wt% FEC, 0.5 wt% DTD and 1 mol / L LiPF6.

[0571] (5) Preparation of lithium-ion secondary batteries: The positive electrode sheet, separator, and lithium-supplemented negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing at 45°C for 24 hours, formation, shaping, and other processes, a lithium-ion secondary battery is obtained.

[0572] Example 2-4: The method is basically the same as that of Example 1, except that at least one of the type and amount of the binder and the amount of the conductive agent is adjusted. See Table 1.

[0573] Example 2 A lithium ion secondary battery was prepared using a method substantially the same as that of Example 1, except that the content of the first binder in the first negative electrode active layer and the content of the second binder in the second negative electrode active layer were adjusted.

[0574] Example 3 A lithium ion secondary battery is prepared using a method substantially the same as Example 1, except that the contents of the first binder and the first conductive agent in the first negative electrode active layer and the contents of the second binder and the second conductive agent in the second negative electrode active layer are adjusted.

[0575] In Example 4, a lithium-ion secondary battery was prepared using a method substantially similar to that of Example 1, except that the CMC-Na in both the first and second negative electrode active layers was replaced with lithium carboxymethyl cellulose (CMC-Li). The mass fractions of CMC-Li in the upper and lower layers were the same as those of CMC-Na in Example 1. CMC-Li served as a lithium-containing binder.

[0576] Comparative Example 1-3. A method substantially the same as that of Example 1 was used, with the main difference being that the electrical conductivities of the first negative electrode active layer and the second negative electrode active layer were substantially the same.

[0577] Each negative electrode active layer in Comparative Example 1 is the same as the upper layer (first negative electrode active layer) in Example 1.

[0578] Each negative electrode active layer in Comparative Example 2 is the same as the lower layer (second negative electrode active layer) in Example 1.

[0579] The material composition of the upper and lower layers of Comparative Example 3 is the same, and the mass ratio of negative electrode active material: SBR: conductive agent: CMC-Na is 97.2:1.3:1:0.5. Compared with Example 1, the total coating surface density is basically the same, and the overall compaction density of the negative electrode sheet is basically the same.

[0580] Comparative Example 4: The method is basically the same as that in Example 1, except that the coating positions of the first negative electrode slurry and the second negative electrode slurry are replaced, that is, the positions of the first negative electrode active layer and the second negative electrode active layer are changed, and the coating amounts of the upper layer and the lower layer are basically the same as those in Example 1.

[0581] The composition of the upper layer in this example corresponds to the composition of the second negative electrode active layer in Example 1, and the composition of the lower layer in this example corresponds to the composition of the first negative electrode active layer in Example 1.

[0582] Comparative Example 5. A method substantially the same as that of Example 1 was used, except that the negative electrode lithium replenishment treatment step was omitted during the preparation of the negative electrode sheet.

[0583] Negative electrode sheet: The second negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed in a solvent deionized water at a mass ratio of 96.3:0.4:2.2:1.1, with a solid content of about 53wt% to obtain the lower negative electrode slurry (corresponding to the second negative electrode active layer); the first negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed uniformly in a solvent deionized water in a mass ratio of 98.1:0.6:0.4:0.9 with a solid content of about 53wt% to obtain an upper negative electrode slurry (corresponding to the first negative electrode active layer). The two negative electrode slurries are coated on the double-sided surfaces of the negative electrode collector copper foil using a double-layer coater, first coating the lower negative electrode slurry and then coating the upper negative electrode slurry. The process is dried, cold pressed, slit, and cut to form the second negative electrode active layer and the first negative electrode active layer in sequence on the surface of the negative electrode collector copper foil to obtain a negative electrode sheet. The negative electrode sheet is a negative electrode sheet that has not been treated with lithium supplementation, and includes a negative electrode collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on the double-sided surfaces of the negative electrode collector.

[0584] Please refer to Table 1.

[0585] (2) Adjusting the OI values ​​of the first and second negative electrode active materials.

[0586] Examples 5-8. The same method as Example 1 was used, with the main difference being that negative electrode active materials with different OI values ​​were selected and the OI values ​​of the first negative electrode active material and / or the second negative electrode active material were changed. See Table 3.

[0587] Comparative Example 6 employed a method essentially identical to Comparative Example 3, with the primary difference being that the first and second negative electrode active materials had different OI values. See Table 3 for details. In Comparative Example 6, the upper and lower layers had the same material composition. See Table 3 for details.

[0588] Comparative Example 7 uses a method substantially the same as Comparative Example 6, with the main difference being that the first negative electrode active material is selected to have a different OI value, so that the OI value of the upper layer is higher than that of the lower layer. See Table 3.

[0589] (3) Adjust D v 50.

[0590] Example 9-13. Using the same method as in Example 1, the main difference is that the D of the first negative electrode active material and / or the second negative electrode active material is changed. v 50 value; relative to Example 1, the upper and lower layer densities and compaction densities are substantially the same, and the upper and lower layer thicknesses and overall compaction densities are adaptively adjusted.

[0591] Comparative Example 8 uses a method substantially the same as that of Comparative Example 3, the main difference being that the first negative electrode active material and the second negative electrode active material have different D v 50% of the negative electrode active material. In Comparative Example 8, the material compositions of the upper and lower layers are the same. Please refer to Table 4.

[0592] 2. Test and analysis methods:

[0593] The instruments involved in the following test and analysis methods are non-limiting examples, and those skilled in the art may also use other types of equipment or similar methods to perform test and analysis.

[0594] (1) Material testing

[0595] 1. D of negative electrode active material v 50

[0596] Sample: raw materials of the first negative electrode active material and the second negative electrode active material.

[0597] The test instrument is Malvern 2000 from the United States.

[0598] Test method: Take a clean beaker, add an appropriate amount of the sample to be tested (control the sample concentration to make the shading degree 8%-12%), and use ultrasound at 120W / 5min to ensure that the sample is completely dispersed. After the sample is poured into the injection tower, it circulates with the solution to the test optical system. When the particles are irradiated by the laser beam, the particle size distribution characteristics of the particles can be obtained by receiving and measuring the energy distribution of the scattered light. A particle size volume distribution diagram is drawn based on the test data. From the particle size volume distribution diagram, it can be obtained that: 50% of the particles in the total volume have a diameter greater than a certain particle size value, and another 50% of the particles in the total volume have a diameter less than this particle size value. This particle size value is the volume average particle size D of the particles. v 50.

[0599] 2. OI values ​​of the first negative electrode active material and the second negative electrode active material.

[0600] Sample: raw materials of the first negative electrode active material and the second negative electrode active material.

[0601] Testing instrument: X-ray diffractometer (XRD) Bruker-D8 advance.

[0602] Test parameters: Cu target Kα1 radiation, wavelength λ of 0.15406 nm, 2θ(°) scanning range of 10°~80°, 2θ(°) scanning speed of 0.02° / s.

[0603] The battery was disassembled, and the first negative electrode active material and the second negative electrode active material were extracted respectively. The samples were dried and rolled into sheets to obtain sheet samples to be tested. XRD test and OI value calculation were performed, and the results were basically the same as those of directly testing the OI values ​​of the first negative electrode active material and the second negative electrode active material.

[0604] Without limitation, samples for OI value testing can be obtained by the following method: using a solvent (dimethyl carbonate) to fully soak the powder materials extracted from the first and second negative electrode active layers, respectively, so that the organic components (including binders and thickeners) therein are dissolved in the solvent, and ultrasonic dispersion is used to promote dissolution. After washing and filtering, the collected solid phase is dried to obtain the test powder of the first and second negative electrode active materials. After rolling the powder sample to be tested into a sheet, the sheet sample is subjected to XRD testing. It should be noted that the small amount of conductive agent that may be contained in the test sample does not affect the comparison of the OI values ​​of the negative electrode active materials in the first and second negative electrode active layers.

[0605] 3. The powder compaction density of the negative electrode material in each negative electrode active layer.

[0606] Negative electrode material: disassemble the battery, extract the powder of the first negative electrode active layer (referred to as the first negative electrode material) and the powder of the second negative electrode active layer (referred to as the second negative electrode material), dry them, and obtain the powder samples to be tested.

[0607] Method: According to the standard GB / T24533-2009, the pressure is measured by the electronic pressure tester UTM7305. Weigh the negative electrode material with a mass of M and add a bottom area of ​​A1 (A1 = 1.327 cm 2 ) in a mold, pressurize to pressure P (P=3T), maintain pressure for 30s, then release pressure, maintain for 10s, then record the thickness D, and calculate the powder compaction density of the negative electrode material under pressure P, powder compaction density = M / (A1×D).

[0608] (2) Negative electrode sheet and its preparation process test

[0609] 1. Powder resistivity and conductivity of different negative electrode active layers.

[0610] Powder resistivity of the second negative electrode active layer (lower layer) and the first negative electrode active layer (upper layer).

[0611] Method: Use a powder resistance tester. Disassemble the battery cell and remove the negative electrode. Scrape 20g of powder from the upper and lower layers of the negative electrode respectively. Use a powder resistance tester to test the powder resistivity under 3T pressure.

[0612] If the powder resistivity of the upper layer powder (first negative electrode active layer) is lower than the powder resistivity of the lower layer powder (second negative electrode active layer), it can also be considered that the conductivity of the first negative electrode active layer is higher than the conductivity of the second negative electrode active layer.

[0613] 2. The thickness of the lithium replenishment layer on one side (the thickness of the lithium replenishment layer on one side of the negative electrode current collector in the lithium replenishment negative electrode sheet after roller pressing).

[0614] Method: Obtain the single-side thickness data of the lithium replenishment layer based on the cross-sectional SEM image of the lithium replenishment negative electrode sheet (see the method for obtaining the cross-sectional SEM image of the negative electrode sheet) or a laser thickness gauge.

[0615] 3. Compacted density of lithium-supplemented negative electrode sheets and surface density based on the total amount on both sides

[0616] (1) Punch the lithium-supplemented negative electrode sheet into a piece with an area of ​​A (1540.25mm 2 ) and measure the weight m and thickness L of the small disc;

[0617] (2) Take another lithium-supplemented negative electrode sheet, wipe off the surface membrane layer and remove the remaining empty current collector foil, and also punch it into an area of ​​1540.25mm 2 The mass of the empty foil is M0 and the thickness is L0;

[0618] (3) The sum of the double-sided density of the lithium-replenishing layer on the first negative electrode active layer in the lithium-replenishing negative electrode sheet of the tested embodiment is recorded as ρ A The total thickness of the lithium supplement layer on both sides is recorded as d D ;

[0619] (4) Calculation:

[0620] Compaction density PD of lithium-supplemented negative electrode sheet A =(M-M0-ρ A ×d D ) / [A×(L-L0-d D )].

[0621] Surface density of lithium-supplemented negative electrode sheet (based on the total amount on both sides) = (M-M0-ρ A ×d D ) / A.

[0622] 4. After lithium replenishment, the thickness of the lithium replenishment residual layer formed by the residue and the coverage percentage of the lithium replenishment residual layer relative to the first negative electrode active layer.

[0623] (1) The thickness of the lithium supplement residual layer on one side of the negative electrode current collector.

[0624] Samples: The battery cells were disassembled, and the negative electrode sheets were removed. A plasma quenching method was used to obtain a cross-section perpendicular to the thickness of the negative electrode sheet. This cross-section corresponds to the cross-section of the negative electrode sheet. Method: A scanning electron microscope (SEM, Sigma 300, ZEISS, Germany) combined with an energy dispersive spectrometer (EDS) was used to observe the cross-sectional morphology of the negative electrode sheet and to measure and analyze the thickness of the lithium-supplemented residual layer on one side.

[0625] (2) The percentage of the coverage area of ​​the lithium supplement residual layer relative to the first negative electrode active layer (measured on a single side of the negative electrode current collector).

[0626] For the negative electrode sheets in lithium-ion secondary batteries, the battery cells are disassembled and the negative electrode sheets are removed. The surface of the negative electrode sheets is observed using a scanning electron microscope (SEM) combined with an energy dispersive spectrometer (EDS). The coverage area of ​​the lithium-replenishing residual layer can be identified. The area of ​​the lithium-replenishing residual layer is divided by the area of ​​the first negative electrode active layer to calculate the percentage of coverage of the lithium-replenishing residual layer relative to the first negative electrode active layer (measured on a single side of the negative electrode current collector). When the lithium-replenishing layer is provided on both sides of the negative electrode current collector, the "percentage of the coverage area of ​​the lithium-replenishing residual layer on both sides relative to the first negative electrode active layer" is the average of the coverage percentages on both sides.

[0627] 5. Compaction density and surface density of negative electrode sheets in lithium-ion secondary batteries

[0628] For the negative electrode sheets in lithium-ion secondary batteries, the batteries are fully discharged, the cells are disassembled, the negative electrode sheets are taken out, and then punched into small discs to test the compaction density and surface density.

[0629] (1) Compaction density of negative electrode sheet:

[0630] Compaction density test analysis: The negative electrode sheet is punched into an area of ​​A (1540.25mm 2 ) small disc, measure the weight m and thickness L of the small disc, take another negative electrode sheet, wipe off the surface membrane layer and the remaining empty collector foil, and also punch out the area of ​​1540.25mm 2 The mass of the empty foil is M0, and the thickness is L0, then the compaction density PD=(M-M0) / [A×(L-L0).

[0631] (2) Surface density of negative electrode:

[0632] Measured by the total area density on both sides, the area density of the negative electrode sheet = PD×(L-L0).

[0633] 6. Thermal analysis

[0634] The battery cell was disassembled and the electrode was taken out. 10 mg of powder on the upper layer and 10 mg of powder on the lower layer of the electrode were scraped off respectively. The test was performed using a thermogravimetric analyzer in a nitrogen atmosphere at a temperature range of 25°C to 600°C at a heating rate of 5°C / min, and the weight loss data at different temperature stages were recorded.

[0635] The "350°C to 450°C mass loss" corresponds to the temperature range in which SBR loses weight. SBR floats during the electrode drying process, and controlling the amount of floating material can optimize dynamics.

[0636] (III) Negative electrode lithium replenishment amount and lithium replenishment efficiency

[0637] The following test analysis involves the electrolyte, unless otherwise specified: the electrolyte composition in Example 1.

[0638] 1. Confirmation of the NP ratio of lithium-ion secondary batteries and whether lithium replenishment is successful.

[0639] Negative electrode capacity: Fully charge the battery, disassemble the cell, take the negative electrode, and punch it into small discs with a diameter of 14 mm (corresponding to area A N ), separate the small disc and the lithium sheet with an isolation film, add electrolyte and package it into 4 button half-cells; use a 0.1C rate to charge and discharge within the voltage range of 0.005V~2V for 1 cycle, and take the average of the discharge capacity of the 4 batteries to get the negative electrode capacity C N , negative electrode surface capacity = negative electrode capacity ÷ area A N .

[0640] Positive electrode capacity: disassemble the battery cell, take the positive electrode and punch it into small discs with a diameter of 14mm (corresponding to area A P ), separate the small disc and the lithium sheet with an isolation film, add electrolyte and package it into 4 button half-cells; use a 0.1C rate to charge and discharge for 1 cycle in the voltage range of 2.5V~3.65V, and take the average of the discharge capacity of the 4 batteries to get the positive electrode capacity C P , positive electrode surface capacity = positive electrode capacity ÷ area A P .

[0641] NP ratio of lithium-ion secondary battery = negative electrode surface capacity / positive electrode surface capacity; N Equal to A P In the case of , the following formula can also be used: NP ratio = C N / C P .

[0642] By comparing the NP ratio (NP1) of the lithium-ion secondary battery prepared in the embodiment with the NP ratio (NP2) of the corresponding lithium-ion secondary battery prepared by omitting the lithium replenishment step, if NP1>NP2, it can be considered that the negative electrode plate has achieved successful lithium replenishment.

[0643] 2. C N_A / (C Li / g ×ρ A +C P_A ) test analysis

[0644] Among them, C N_A is the preset surface capacity of the negative electrode, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

[0645] Among them, the negative electrode preset surface capacity C N_A = Theoretical gram capacity of negative electrode active material × surface density of negative electrode active material in negative electrode sheet,

[0646] Positive electrode preset surface capacity C P_A = Theoretical gram capacity of positive electrode active material × surface density of positive electrode active material in positive electrode sheet,

[0647] ρ A It can be calculated based on the ratio between the mass of both sides of the lithium supplement layer (i.e., the mass of the lithium foil on both sides) and the average spreading area of ​​the lithium supplement layer on the surface on which it is located (on the first negative electrode active layer), and the spreading area includes the covered area and the uncovered area;

[0648] Theoretical gram capacity of lithium C Li / g Calculated at 3860mAh / g.

[0649] The preset range of each embodiment is: 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3.

[0650] (IV) Battery performance test

[0651] 1. Battery internal resistance

[0652] At 25°C, a lithium-ion secondary battery is charged at a constant current of 1 / 3C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After 5 minutes of rest, the battery is discharged at a constant current of 1 / 3C for 90 minutes. After 120 minutes of rest, the voltage V1 is recorded. The battery is then discharged at 4C for 30 seconds, and the voltage V2 is recorded. The internal resistance DCR of the battery is calculated as (V2-V1) / 4C.

[0653] 2. Cycle life test: At 25 °C, charge the lithium-ion secondary battery to be tested at a constant current of 1 / 3C until 3.65V, then charge it at a constant voltage of 3.65V until the current reaches 0.05C, leave it standing for 5 minutes, and then discharge it at 1 / 3C until 2.5V. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery, and simultaneously record the discharge capacity Cn of the battery after the nth cycle. Then, the battery capacity retention rate Pn = Cn / C0 × 100%, and the battery capacity retention rate is obtained.

[0654] In this test process, the first cycle corresponds to n = 1, the second cycle corresponds to n = 2,... the 1000th cycle corresponds to n = 1000.

[0655] Refer to the "Capacity Retention Rate after 1000 Cycles" in the corresponding table below.

[0656] Table 1.

[0657]

[0658] In Table 1, for each embodiment, the powder resistivity of the first negative electrode material (upper layer) is lower than that of the second negative electrode material (lower layer), R1 < R2, and the conductivity of the first negative electrode active layer is higher than that of the second negative electrode active layer.

[0659] Table 2.

[0660]

[0661] Table 3.

[0662]

[0663] In Table 3, OI1 is the OI value of the raw material of the first negative electrode active material, OI2 is the OI value of the raw material of the second negative electrode active material; R1 is the powder resistivity of the first negative electrode material, and R2 is the powder resistivity of the second negative electrode material.

[0664] Table 4.

[0665]

[0666] In Table 4, "First negative electrode active layer (upper layer) D v 501" corresponds to the D v 50 test result of the raw material of the first negative electrode active material, and "Second negative electrode active layer (lower layer) D v 502" corresponds to the Dv50 test result of the raw material of the second negative electrode active material; disassemble the battery cell, take the negative electrode sheet, and separately extract the D v 50 test results of the first negative electrode active material and the second negative electrode active material are close to those in Table 4.

[0667] (V) Test analysis results

[0668] The negative electrode active layers of the negative electrode sheets of Examples 1-13 all adopt a double-layer design, wherein the upper layer corresponds to the first negative electrode active layer and the lower layer corresponds to the second negative electrode active layer. Examples 1-13 all perform negative electrode lithium replenishment treatment on the first negative electrode active layer.

[0669] The NP ratios of the lithium-ion secondary batteries of Examples 1-13 were all higher than those of lithium-ion secondary batteries that had not been treated with lithium replenishment, indicating that lithium replenishment was successfully achieved in all of Examples 1-13. The NP ratios of the lithium-ion secondary batteries of Examples 1-13 were all within the range of 1.05 to 1.3, and further within the range of 1.1 to 1.3. Taking Example 1-4 as an example, the NP ratio of the lithium-ion secondary battery (approximately 1.28) was higher than the NP ratio of the lithium-ion secondary battery in Comparative Example 5 (1.12).

[0670] After lithium replenishment treatment, the negative electrode sheets of each example were disassembled and tested. A residual layer of inactive lithium, including lithium oxides, was detected on the negative electrode surface. However, disassembly of the battery for the unreplenished negative electrode sheet of Comparative Example 5 (see Comparative Example 5) revealed no similar lithium replenishment residue.

[0671] Examples 1-13 all satisfy the requirement that the powder resistivity R1 of the upper negative electrode material is lower than the powder resistivity R2 of the lower negative electrode material, and that the upper layer has a higher conductivity than the lower layer. Both R1 and R2 are within the range of 1 mΩ·cm to 20 mΩ·cm.

[0672] Compared with the corresponding control examples without lithium supplementation treatment, the lithium ion secondary batteries prepared in Examples 1-13 have a higher capacity retention rate after 1000 cycles and have a significantly extended cycle life.

[0673] In addition, the lithium-ion secondary batteries prepared in Examples 1-13 have low internal resistance, high capacity retention after 1000 cycles, and both long cycle life and excellent battery kinetics.

[0674] The thickness of the lithium-supplemented residual layer in each embodiment is less than 0.1 μm, and further less than 0.08 μm.

[0675] In both Examples 1 and 3-4, the binder content in the upper layer is lower than that in the lower layer. When both the upper and lower layers contain SBR, the mass loss of the first negative electrode active layer at 350°C to 450°C is lower than that of the second negative electrode active layer. Compared to Comparative Examples 1-4, the powder resistivity of the upper negative electrode material in Examples 1 and 3-4 is significantly reduced, significantly improving battery kinetics. See Table 1-2 for details.

[0676] In both Examples 1-2 and 4, the upper layer conductive agent content was higher than the lower layer conductive agent content. Compared to Comparative Examples 1-4, the upper layer negative electrode material powder resistivity in Examples 1-2 and 4 was significantly reduced, significantly optimizing battery kinetics. See Table 1-2 for details.

[0677] In Example 4, both the first and second negative electrode active layers are also provided with a lithium-containing binder, CMC-Li. This lithium-containing binder improves conductivity, low powder resistivity, and a very low internal resistance of the battery, while also maintaining a high cycle capacity retention rate. The introduction of a lithium-containing binder improves the lithium ion conductivity of the first negative electrode active layer and enhances lithium replenishment efficiency. Furthermore, the lithium provided by the lithium-containing binder can occupy some active sites, helping to reduce lithium consumption during film formation.

[0678] Examples 5-8 and Comparative Examples 5-7 adjust the OI value of the negative electrode active material of the upper and / or lower layers. When the first negative electrode active material of the upper layer has a lower OI value, the lithium ion diffusion kinetics is better, which can improve the lithium replenishment efficiency. Example 1 also has a significantly reduced battery internal resistance relative to Comparative Examples 3, 6, and 7, and the battery kinetics is significantly improved. Please refer to Table 3. Comparative Example 7 adjusts the OI value, resulting in the upper layer powder resistivity R1 being higher than the lower layer powder resistivity R2, resulting in a decrease in lithium replenishment efficiency, an increase in battery internal resistance, and a decrease in battery cycle life.

[0679] Examples 9-13 and Comparative Example 8 adjust the D of the negative electrode active materials in the upper and lower layers. v 50 value. When the upper first negative electrode active material has a lower Dv50, solid-phase diffusion paths are reduced, improving battery kinetics. The lithium-ion secondary batteries prepared in Examples 9-13 all exhibit high cycle capacity retention, long cycle life, and low internal resistance. See Table 4 for details.

[0680] The compaction density of the lithium-supplemented negative electrode sheets of Examples 1-13 all met the requirements of 1.3 g / cm 3 ~1.8g / cm 3 , partially meet 1.4g / cm 3 ~1.6 g / cm 3 , the surface density (on both sides) meets 10mg / cm 2 ~26mg / cm 2 , partially meet 15mg / cm 2 ~20mg / cm 2 , which can improve the energy density of lithium-ion secondary batteries, so that the battery has both high energy density and high lithium replenishment efficiency. Taking Examples 9-13 as an example, the compaction density of the lithium replenishment negative electrode sheets all meets 1.3g / cm 3 ~1.8 g / cm 3 , the surface density (on both sides) meets 10 mg / cm2 ~26mg / cm 2 Taking Example 1 as an example, the compaction density of the lithium-supplemented negative electrode sheet is 1.45 g / cm 3 , the surface density (double side) is 17.4 mg / cm 2 .

[0681] In each of Examples 1-13, the negative electrode sheets were disassembled from the fully discharged batteries, and the measured compaction density was 1.08 g / cm 3 ~1.71 g / cm 3 Within the range, some meet 1.17g / cm 3 ~1.52 g / cm 3 , the surface density is 10 mg / cm 2 ~26mg / cm 2 Within the range, some meet 15 mg / cm 2 ~20mg / cm 2 .

[0682] Based on Example 1, the D values ​​of the first negative electrode active material and the second negative electrode active material were adjusted. v 50 combination (in the second negative electrode active layer located in the lower layer, the second negative electrode active material is controlled to use a combination of large particle materials and small particle materials, and only a single type of small particle material is used in the upper layer), so that the powder compaction density of the second negative electrode material is higher than the powder compaction density of the first negative electrode material, and the second negative electrode active layer is given a higher compaction density during the cold pressing process of the electrode piece, and the overall compaction density remains basically unchanged. The resulting lithium ion secondary battery has a long cycle life and a high energy density.

[0683] In addition, by using a separator with a ceramic coating, taking a ceramic coating with a thickness of 1 μm formed on both sides of the separator as an example, the other parameters are consistent with those of Examples 1-4, and lithium-ion secondary batteries with long cycle life can be obtained. In addition, the battery kinetic performance is good.

[0684] Based on Examples 1-8, the type of positive electrode active material is adjusted, and the ternary positive electrode material NCM811 is replaced as an example. The other parameters are consistent with Examples 1-8, and lithium-ion secondary batteries with long cycle life can be obtained. In addition, the battery kinetic performance is good.

[0685] The above description of the various embodiments and examples tends to emphasize the differences between the various embodiments and examples. The similarities or similarities between them can be referenced and will not be repeated here for the sake of brevity. The various technical features of the above-described embodiments and examples can be combined in any way. To keep the description concise, not all possible combinations of the various technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0686] It should be noted that the present application is not limited to the above-mentioned embodiments and examples. The above-mentioned embodiments and examples are only examples, and the embodiments and examples that have the same structure as the technical idea and play the same role and effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. The above-described embodiments and examples only express several embodiments and examples of the present application, and their descriptions are relatively detailed, but they cannot be understood as limiting the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art are applied to the embodiments or examples, and other methods of constructing by combining some of the constituent elements in the embodiments or examples are also included in the scope of the present application.

Claims

1. A lithium ion secondary battery, characterized in that: It comprises a negative electrode plate; the negative electrode plate comprises a negative electrode current collector and a second negative electrode active layer and a first negative electrode active layer sequentially arranged on at least one side of the negative electrode current collector; The negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer; The negative electrode plate is treated with negative electrode lithium supplementation.

2. The lithium ion secondary battery according to claim 1, characterized in that: The negative electrode plate meets one or more of the following characteristics: The powder resistivity of the first negative electrode active layer is 1 mΩ·cm to 100 mΩ·cm; The powder resistivity of the second negative electrode active layer is 1 mΩ·cm to 100 mΩ·cm.

3. The lithium ion secondary battery according to claim 2, characterized in that: The negative electrode plate meets one or more of the following characteristics: The powder resistivity of the first negative electrode active layer is 1 mΩ·cm to 20 mΩ·cm; The powder resistivity of the second negative electrode active layer is 1 mΩ·cm to 20 mΩ·cm.

4. The lithium ion secondary battery according to claim 1, characterized in that: In the negative electrode sheet, a lithium supplement residual layer exists on a surface of the first negative electrode active layer away from the second negative electrode active layer, and the lithium supplement residual layer contains inactive lithium; The negative electrode plate meets one or more of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.1 μm on a single side of the negative electrode current collector; Based on a single side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer is less than or equal to 98%.

5. The lithium ion secondary battery according to claim 4, characterized in that: The negative electrode plate meets one or more of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.08 μm on a single side of the negative electrode current collector; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer is 30% to 70%.

6. The lithium ion secondary battery according to claim 4, characterized in that: The negative electrode plate meets one or more of the following characteristics: The thickness of the lithium supplement residual layer is less than 0.05 μm on a single side of the negative electrode current collector; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement residual layer relative to the first negative electrode active layer is 50% to 70%.

7. The lithium ion secondary battery according to claim 1, characterized in that: The negative electrode plate meets one or more of the following characteristics: The first negative electrode active layer includes a first binder, the second negative electrode active layer includes a second binder, and the mass fraction of the first binder in the first negative electrode active layer is lower than the mass fraction of the second binder in the second negative electrode active layer; The first negative electrode active layer includes a first conductive agent, and the second negative electrode active layer includes a second conductive agent. The mass fraction of the first conductive agent in the first negative electrode active layer is higher than the mass fraction of the second conductive agent in the second negative electrode active layer.

8. The lithium ion secondary battery according to claim 7, characterized in that: The negative electrode plate meets one or more of the following characteristics: The mass fraction of the first binder in the first negative electrode active layer is 1% to 15%; The mass fraction of the second binder in the second negative electrode active layer is 1% to 15%; The mass fraction of the first conductive agent in the first negative electrode active layer is 0.1% to 10%; The mass fraction of the second conductive agent in the second negative electrode active layer is 0.1% to 10%.

9. The lithium ion secondary battery according to claim 7, characterized in that: In a thermogravimetric test conducted in a nitrogen atmosphere, the mass loss of the first negative electrode active layer at 350° C. to 450° C. is lower than that of the second negative electrode active layer.

10. The lithium ion secondary battery according to claim 9, characterized in that: The negative electrode plate meets one or more of the following characteristics: The mass fraction of styrene-butadiene rubber in the first negative electrode active layer is lower than the mass fraction of styrene-butadiene rubber in the second negative electrode active layer; The mass fraction of styrene-butadiene rubber in the first negative electrode active layer is 0.1% to 10%; The mass fraction of styrene-butadiene rubber in the second negative electrode active layer is 0.1% to 10%.

11. The lithium ion secondary battery according to claim 7, characterized in that: The first binder includes a lithium-containing binder.

12. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The first negative electrode active layer comprises a first graphite material, and the second negative electrode active layer comprises a second graphite material; The OI value of the first graphite material is lower than the OI value of the second graphite material; wherein the OI value refers to the intensity ratio of the (004) crystal plane to the (110) crystal plane in the powder X-ray diffraction spectrum.

13. The lithium ion secondary battery according to claim 12, characterized in that: The negative electrode plate meets one or more of the following characteristics: The OI value of the first graphite material is 3-7; The OI value of the second graphite material is 3-7.

14. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The first negative electrode active layer comprises a first negative electrode active material, and the second negative electrode active layer comprises a second negative electrode active material; The D of the first negative electrode active material v 50 lower than the D of the second negative electrode active material v 50; among them, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the multi-particle mixture reaches 50%.

15. The lithium ion secondary battery according to claim 14, characterized in that: The negative electrode plate meets one or more of the following characteristics: The D of the first negative electrode active material v 50Satisfies 5μm≤D v 50≤15μm; The D of the second negative electrode active material v 50Satisfy 10μm≤D v 50≤18μm.

16. The lithium ion secondary battery according to claim 15, characterized in that: The D of the first negative electrode active material v 50Satisfies 7μm≤D v 50≤13μm.

17. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The ratio of the thickness of the first negative electrode active layer to the sum of the thickness of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f H , satisfying 20%≤f H ≤70%.

18. The lithium ion secondary battery according to claim 17, characterized in that: 30%≤f H ≤50%。 19. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The constituent material of the first negative electrode active layer is recorded as the first negative electrode material, and the constituent material of the second negative electrode active layer is recorded as the second negative electrode material; The negative electrode plate meets one or two of the following characteristics: The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer; The powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

20. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The negative electrode plate meets one or two of the following characteristics: When the battery is fully discharged, the compaction density of the negative electrode sheet is 1.08 g / cm 3 ~ 1.71 g / cm 3 ; When the battery is fully discharged, the surface density of the negative electrode is 10 mg / cm 2 ~ 26 mg / cm 2 .

21. The lithium ion secondary battery according to claim 20, characterized in that: The negative electrode plate meets one or two of the following characteristics: When the battery is fully discharged, the compaction density of the negative electrode sheet is 1.17 g / cm 3 ~ 1.52 g / cm 3 ; When the battery is fully discharged, the surface density of the negative electrode is 15 mg / cm 2 ~ 20 mg / cm 2 .

22. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The lithium-ion secondary battery also includes a positive electrode plate. The NP ratio of the lithium-ion secondary battery is 1.05-1.3, and the NP ratio of the lithium-ion secondary battery is equal to the ratio of the negative electrode surface capacity to the positive electrode surface capacity.

23. The lithium ion secondary battery according to claim 22, characterized in that: The NP ratio of the lithium ion secondary battery is 1.1-1.

3.

24. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The lithium-ion secondary battery also includes an electrolyte; The electrolyte includes additives, and the additives include one or more of vinylene carbonate and sulfur-containing additives; the sulfur-containing additives include one or more of vinyl sulfate, vinyl sulfite, and propylene sulfite.

25. The lithium ion secondary battery according to any one of claims 1 to 11, characterized in that: The lithium-ion secondary battery also includes a positive electrode plate, which includes a positive electrode active material, and the positive electrode active material includes one or more of a ternary positive electrode material, a modified form of a ternary positive electrode material, lithium iron phosphate, a modified form of lithium iron phosphate, lithium iron manganese phosphate, and a modified form of lithium iron manganese phosphate; the modified form includes one or more of a doping modification and a coating modification.

26. The lithium ion secondary battery according to claim 25, characterized in that: The positive electrode active material includes carbon-coated lithium iron phosphate, which includes a lithium iron phosphate body and a carbon coating layer located on at least a portion of the surface of the lithium iron phosphate body, and the carbon coating layer includes one or more of soft carbon, hard carbon and amorphous carbon.

27. A lithium-supplemented negative electrode sheet, characterized in that: It includes a negative electrode current collector and a second negative electrode active layer, a first negative electrode active layer and a lithium supplement layer sequentially arranged on at least one side of the negative electrode current collector; The lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer.

28. The lithium supplemented negative electrode sheet according to claim 27, characterized in that: The lithium supplement layer includes single substance lithium.

29. The lithium-supplemented negative electrode sheet according to claim 28, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: Measured on one side of the negative electrode current collector, the thickness of the lithium supplement layer is less than the sum of the thicknesses of the first negative electrode active layer and the second negative electrode active layer; Calculated on a single side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active layer is less than or equal to 98%.

30. The lithium-supplemented negative electrode sheet according to claim 28, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The thickness of the lithium supplement layer is less than 8.5 μm on a single side of the negative electrode current collector; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active layer is 30% to 70%.

31. The lithium-supplemented negative electrode sheet according to claim 28, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The thickness of the lithium supplement layer is 1 μm to 4.8 μm on a single side of the negative electrode current collector; Based on one side of the negative electrode current collector, the coverage area percentage of the lithium supplement layer relative to the first negative electrode active layer is 50% to 70%.

32. The lithium supplemented negative electrode sheet according to any one of claims 27 to 31, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The first negative electrode active layer and the second negative electrode active layer in the lithium supplemented negative electrode sheet meet the characteristics described in the lithium ion secondary battery according to any one of claims 2 to 3 and 7 to 11; The compaction density of the lithium supplemented negative electrode sheet is 1.3 g / cm 3 ~1.8g / cm 3 ; The surface density of the lithium supplemented negative electrode sheet is 10 mg / cm 2 ~26mg / cm 2 .

33. The lithium supplemented negative electrode sheet according to claim 32, characterized in that: The lithium-supplemented negative electrode sheet meets one or more of the following characteristics: The compaction density of the lithium supplemented negative electrode sheet is 1.4 g / cm 3 ~1.6g / cm 3 ; The surface density of the lithium supplemented negative electrode sheet is 15 mg / cm 2 ~20mg / cm 2 .

34. The lithium supplemented negative electrode sheet according to any one of claims 27 to 31, characterized in that: The first negative electrode active layer comprises a first graphite material, and the second negative electrode active layer comprises a second graphite material; The OI value of the first graphite material is lower than the OI value of the second graphite material; wherein the OI value refers to the intensity ratio of the (004) crystal plane to the (110) crystal plane in the powder X-ray diffraction spectrum.

35. The lithium-supplemented negative electrode sheet according to claim 34, characterized in that: Meet one or more of the following characteristics: The OI value of the first graphite material is 3-7; The OI value of the second graphite material is 3-7.

36. The lithium supplemented negative electrode sheet according to any one of claims 27 to 31, characterized in that: The first negative electrode active layer comprises a first negative electrode active material, and the second negative electrode active layer comprises a second negative electrode active material; The D of the first negative electrode active material v 50 lower than the D of the second negative electrode active material v 50; among them, D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the multi-particle mixture reaches 50%.

37. The lithium-supplemented negative electrode sheet according to claim 36, characterized in that: Meet one or more of the following characteristics: The D of the first negative electrode active material v 50Satisfies 5μm≤D v 50≤15μm; The D of the second negative electrode active material v 50Satisfy 10μm≤D v 50≤18μm.

38. The lithium supplemented negative electrode sheet according to claim 37, characterized in that: The D of the first negative electrode active material v 50Satisfies 7μm≤D v 50≤13μm.

39. The lithium supplemented negative electrode sheet according to any one of claims 27 to 31, characterized in that: The ratio of the thickness of the first negative electrode active layer to the sum of the thickness of the first negative electrode active layer and the second negative electrode active layer on one side of the negative electrode current collector is denoted as f H , satisfying 20%≤f H ≤70%.

40. The lithium-supplemented negative electrode sheet according to claim 39, characterized in that: 30%≤f H ≤50%。 41. The lithium supplemented negative electrode sheet according to any one of claims 27 to 31, characterized in that: The constituent material of the first negative electrode active layer is recorded as the first negative electrode material, and the constituent material of the second negative electrode active layer is recorded as the second negative electrode material; The lithium-supplemented negative electrode sheet meets one or two of the following characteristics: The compaction density of the second negative electrode active layer is higher than the compaction density of the first negative electrode active layer; The powder compaction density of the second negative electrode material in the second negative electrode active layer is higher than the powder compaction density of the first negative electrode material in the first negative electrode active layer.

42. A component for preparing a lithium ion secondary battery, characterized in that: It comprises an electrode assembly and an electrolyte, wherein the electrode assembly comprises a positive electrode sheet, a lithium-supplemented negative electrode sheet and a separator, and the separator is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; The lithium-supplemented negative electrode sheet is the lithium-supplemented negative electrode sheet described in any one of claims 27 to 41.

43. A method for preparing a lithium ion secondary battery, characterized in that: The steps include: The positive electrode sheet, the separator and the lithium-supplemented negative electrode sheet are assembled into an electrode assembly, so that the separator is arranged between the positive electrode sheet and the lithium-supplemented negative electrode sheet; wherein the lithium-supplemented negative electrode sheet comprises a negative electrode current collector and a second negative electrode active layer, a first negative electrode active layer and a lithium-supplemented layer arranged in sequence on at least one side of the negative electrode current collector; the lithium-supplemented negative electrode sheet satisfies one or both of the following characteristics (i) and (ii): (i) the electrical conductivity of the first negative electrode active layer is higher than the electrical conductivity of the second negative electrode active layer; (ii) the powder resistivity of the first negative electrode active layer is lower than the powder resistivity of the second negative electrode active layer; The electrode assembly is placed in the housing cavity of the shell, and an electrolyte is injected to allow the electrolyte to soak the positive electrode sheet and the lithium-supplemented negative electrode sheet, and then the lithium-ion secondary battery is obtained.

44. The method for preparing a lithium ion secondary battery according to claim 43, characterized in that: The lithium replenishment layer in the lithium replenishment negative electrode sheet satisfies the following formula: 1.05≤C N_A / (C Li / g ×ρ A +C P_A )≤1.3; Among them, C N_A is the preset surface capacity of the negative electrode, C P_A is the preset surface capacity of the positive electrode, ρ A is the surface density of the lithium supplement layer on the first negative electrode active layer based on the total amount on both sides, C Li / g is the theoretical gram capacity of lithium.

45. The method for preparing a lithium ion secondary battery according to claim 43, characterized in that: The lithium-supplemented negative electrode sheet is prepared by a method comprising the following steps: The second negative electrode active layer is formed on at least one side surface of the negative electrode substrate, the first negative electrode active layer is formed on the surface of the second negative electrode active layer away from the negative electrode substrate, and the lithium supplement layer is added on the surface of the first negative electrode active layer away from the second negative electrode active layer.

46. ​​The method for preparing a lithium ion secondary battery according to any one of claims 43 to 45, characterized in that: The prepared lithium ion secondary battery is the lithium ion secondary battery described in any one of claims 1 to 11.

47. An electrical device, characterized in that: The invention comprises at least one of the lithium ion secondary battery described in any one of claims 1 to 26 and the lithium ion secondary battery prepared by the method for preparing a lithium ion secondary battery described in any one of claims 43 to 45.

Citation Information

Patent Citations

  • Silicon-based negative electrode plate, fabrication method thereof and lithium ion battery

    CN109888266A

  • Negative lithium supplementing pole piece and lithium ion battery

    CN112331928A

  • Negative plate and lithium ion battery

    CN112635712A

  • Negative electrode, and preparation method and application thereof

    CN113224263A

  • Lithium supplement negative plate and lithium ion battery

    CN114068867A

Cited By

  • New energy cell pole piece core characteristic identification method based on coating technology and application

    CN121299036A