Pole piece processing method

By heating the battery pole at a specific temperature, redistribute the binder and maintain the integrity of the active substances, the problem of low internal resistance and rate performance of the battery is solved, and the dynamic performance of the battery and the infiltration rate of the electrolyte are significantly improved. .

CN119069647AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310627314.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The fast charging performance of existing batteries is limited by high internal resistance and low rate performance. How to reduce internal resistance, improve rate performance, and improve the dynamic performance of secondary batteries has become the top priority.

Method used

By heating the electrode sheet, the temperature of the active layer is greater than or equal to the softening or melting temperature of the binder, and is less than the minimum temperature of the decomposition temperature, oxidation temperature and ignition temperature of the active substance, and redistribute the binder to form a uniform The capillary channel increases the infiltration rate of the electrolyte and keeps the crystal lattice of the active substance intact.

Benefits of technology

It reduces the internal resistance of the battery, improves the rate performance and dynamic performance of the battery, improves the adhesion and cohesion of the electrode sheet, improves the absorption rate of the electrolyte, and enhances the possibility of conductive paths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069647A_ABST
    Figure CN119069647A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary batteries, and particularly relates to a pole piece processing method. The pole piece comprises an active layer, the active layer comprises an active substance and a binder, and the treatment method comprises the following steps: heating the pole piece to raise the temperature of the active layer to a treatment temperature; the treatment temperature is higher than or equal to the softening temperature or the melting temperature of the binder, and the treatment temperature is lower than the lowest temperature of the decomposition temperature, the oxidation temperature and the ignition temperature of the active substance. The method can reduce the internal resistance of the battery, improve the rate capability of the battery and improve the dynamic performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery technology, and in particular relates to a method for processing a pole piece. Background Art

[0002] With the continuous deepening of secondary battery research and the continuous improvement of market demand, higher requirements are placed on the fast charging performance of batteries. Fast charging, that is, rapid charging, can generally make the battery reach or approach a fully charged state in a relatively short period of time. However, the current fast charging performance of batteries is often restricted by their poor dynamic performance such as high internal resistance and low rate. Therefore, how to reduce internal resistance, improve rate performance, and improve the dynamic performance of secondary batteries has become a top priority. Summary of the invention

[0003] In view of the above problems, the present application provides a method for processing a pole piece, which can reduce the internal resistance of the battery, enhance the battery rate performance, and improve the battery dynamics performance.

[0004] In the first aspect, the present application provides a method for processing an electrode, wherein the electrode comprises an active layer, wherein the active layer comprises an active substance and a binder, and the processing method comprises: heating the electrode to raise the temperature of the active layer to a processing temperature; the processing temperature is greater than or equal to the softening temperature or melting temperature of the binder, and the processing temperature is less than the lowest temperature among the decomposition temperature, oxidation temperature, and ignition temperature of the active substance.

[0005] In the electrode processing method of the embodiment of the present application, the electrode is heated to make the temperature of the active layer greater than or equal to the softening temperature or melting temperature of the binder, and the binder re-melts and penetrates into the active layer of the electrode, which plays a role in balancing the distribution of the binder in the upper and lower layers of the electrode, which helps to improve the electrode resistance of the electrode and enhance the dynamic performance; the balanced distribution of the binder in the electrode helps to improve the bonding force and cohesion of the electrode. Moreover, the high heat generated during heating can remove part of the binder on the surface of the electrode, and then form pores on the surface of the electrode; due to thermal expansion and contraction and the softening and fluidity of the binder, a small amount of pores are also regenerated inside the electrode after cooling. The generation of a small amount of pores constructs a capillary channel, which can increase the infiltration rate with the electrolyte, accelerate the transmission of lithium ions between the electrodes and the electrolyte, and can reduce the internal resistance of the battery, improve the battery rate performance, and improve the battery dynamic performance.

[0006] At the same time, the processing temperature is lower than the lowest temperature among the decomposition temperature, oxidation temperature and ignition temperature of the active material. Therefore, during the electrode processing, the etching or decomposition of the active material can be improved, which is beneficial for the active material in the electrode to maintain the integrity of the lattice, and thus is beneficial for maintaining the capacity of the electrode.

[0007] In some embodiments, the electrode sheet is a positive electrode sheet, and the processing temperature is less than or equal to the decomposition temperature of the binder.

[0008] According to the electron gain and loss of the active material in the electrode in the battery chemical reaction, the electrode can be divided into positive electrode and negative electrode, where the active material in the positive electrode loses electrons in the battery chemical reaction of charging, and the active material in the negative electrode gains electrons in the battery chemical reaction of charging. Due to the difference in active materials, the solubility of the active materials in the solvent is different in the positive electrode and the negative electrode, and the solubility of the binder in the solvent is different. Therefore, different types of solvents and binders are usually used in the production process of the active layer of the positive electrode and the negative electrode. Usually, oily solvents and oily binders are used in the production process of the active layer of the positive electrode, while aqueous solvents and aqueous binders are used for the negative electrode. The different volatilization rates of oily solvents and oily solvents make the migration of the binder different during the slurry drying process. Therefore, the distribution of the binder in the positive electrode is usually different from that of the negative electrode.

[0009] In practice, it is found that the binder in the positive electrode sheet floats less. Therefore, for the positive electrode sheet, the treatment temperature is greater than or equal to the softening temperature or melting temperature of the binder, and less than or equal to the decomposition temperature of the binder, so that the binder can be re-infiltrated into the sheet in a molten manner, and the binder does not decompose or only very little decomposes, so that the distribution of the binder between different layers of the sheet is balanced, which helps to improve the bonding and cohesion of the positive electrode sheet.

[0010] For the negative electrode sheet, the processing temperature is controlled to be greater than or equal to the softening temperature or melting temperature of the binder, and the processing temperature is less than the lowest temperature of the three temperatures of the decomposition temperature, oxidation temperature, and ignition temperature of the active material. Considering that the decomposition temperature of the binder is usually higher than the softening temperature or melting temperature of the binder, and lower than the decomposition temperature of the active material, therefore, for the negative electrode sheet, there may be a case where the processing temperature is greater than or equal to the decomposition temperature of the binder, or there may be a case where the processing temperature is less than the decomposition temperature of the binder. When the processing temperature of the negative electrode sheet is greater than or equal to the decomposition temperature of the binder, the excess binder on the surface can be removed, the bonding force can be balanced, and the negative electrode sheet is not easy to crack or powder during the cold pressing process. When the processing temperature of the negative electrode sheet is less than the decomposition temperature of the binder, the binder can be re-infiltrated into the sheet in a molten manner, and at the same time, the binder does not decompose or only a very small amount of the binder decomposes, so that the distribution of the adhesive between different layers of the sheet is balanced, which helps to improve the bonding force and cohesion of the positive electrode sheet.

[0011] In some embodiments, the processing temperature is 160-400° C.; in other embodiments, the processing temperature is 180-370° C. This temperature range is greater than or equal to the softening temperature or melting temperature of a common binder and less than the decomposition temperature of a common active substance. Therefore, for ease of operation, the processing temperature can be set within this temperature range.

[0012] In some embodiments, the pole piece is a positive pole piece, and the treatment temperature is 160-260°C, or 280-400°C. Depending on the type of binder used in the positive pole piece, a suitable treatment temperature can be used. For example, the melting temperature of polyvinylidene fluoride (PVDF), a common binder for positive pole pieces, is 166-170°C, and the thermal decomposition temperature is greater than 310°C, so a treatment temperature of 160-260°C can be used; polyimide (PI) softens at ≥300°C, and the thermal decomposition temperature is greater than 500°C, so a treatment temperature of 280-400°C can be used; according to different binders, a suitable treatment temperature is selected within this temperature range, so that the binder can be re-infiltrated into the pole piece in a molten manner, and at the same time, the binder does not decompose or only a very small amount of the binder decomposes, so that the distribution of the adhesive between different layers of the pole piece is balanced, which helps to improve the bonding and cohesion of the positive pole piece.

[0013] In some embodiments, the electrode is a negative electrode, and the treatment temperature is 180-350° C., optionally 200-350° C. This temperature is greater than or equal to the decomposition temperature of a common binder for negative electrode. For example, styrene-butadiene rubber (SBR), a common binder for negative electrode, will gradually decompose at a temperature above 220° C. At this treatment temperature, the excess binder on the surface can be removed, the bonding force can be balanced, and the problem of easy cracking and powdering of the negative electrode during the cold pressing process can be improved.

[0014] In some embodiments, the heating time is 0.02 to 0.3 seconds, and optionally 0.02 to 0.2 seconds. The treatment method in the embodiment of the present application has a high heating rate, which can quickly make the surface and internal temperature of the active layer reach the treatment temperature. The binder absorbs heat in a short time, which not only makes the binder more evenly distributed in the active layer, but also has a high treatment efficiency.

[0015] In some embodiments, the heating treatment method includes laser irradiation treatment. Laser irradiation treatment is to use a laser to generate a laser beam and use the laser beam for irradiation. The laser has the characteristics of excellent monochromaticity, extremely small divergence, and extremely high brightness, and can make the temperature of the active layer reach the required temperature in a very short time. Moreover, the pole piece processing method of the embodiment of the present application can quickly complete the processing of the pole piece at one time by using a laser on one side or both sides of the pole piece, and can be integrated on existing equipment without adding a lot of extra time and equipment. The original pole piece production capacity can be maintained at a low cost.

[0016] In some embodiments, the pole piece includes a first surface and a second surface arranged opposite to each other; the laser irradiation processing step includes: using a first laser beam to perform laser irradiation processing on the first surface, and using a second laser beam to perform laser irradiation processing on the second surface; there is a spacing between the first laser beam and the second laser beam in a direction parallel to the first surface and the second surface.

[0017] In the embodiment of the present application, there is a gap between the first laser beam and the second laser beam in the direction parallel to the first surface and the second surface, that is, the first laser beam and the second laser beam are staggered for irradiation on both sides of the pole piece, and the laser heads for generating laser beams are located on both sides of the pole piece but not directly facing each other. The two are separated by a certain distance in the plane direction of the pole piece, which is beneficial to control the temperature of the pole piece and improve the problem of overheating of the pole piece in a short period of time.

[0018] In some embodiments, in the laser irradiation treatment step, the maximum size of the laser spot falling on the surface of the pole piece is greater than or equal to the minimum size of the pole piece surface. In the embodiment of the present application, the maximum size of the laser spot is greater than or equal to the minimum size on the pole piece surface. Under this condition, the pole piece can be simultaneously and comprehensively irradiated in the direction of the minimum size on the pole piece surface in one laser irradiation treatment, so that the adhesive in this direction is melted almost at the same time, which helps to improve the uniformity of the adhesive after redistribution.

[0019] In some embodiments, the laser irradiation treatment step includes: moving the pole piece relative to the laser spot falling on the surface of the pole piece, and the speed of the moving treatment is 10 to 200 m / min, optionally 30 to 200 m / min. In the embodiment of the present application, the processing process of the pole piece can be in a dynamic state, the pole piece moves relative to the laser spot, and the laser briefly heats the pole piece, which can increase the temperature of the active layer in the pole piece, but the rising temperature will not be too high. In actual operation, the pole piece can be placed on the winding guide roller and the unwinding guide roller, and the winding guide roller is used to pull the pole piece to achieve the movement of the pole piece. The speed of the pole piece movement can be controlled by the operating speed of the winding guide roller. By controlling the movement of the pole piece, the laser irradiation treatment of the entire roll of pole piece can be completed in one winding and unwinding process, with a high processing speed, which helps to improve production capacity and is convenient and easy to process.

[0020] In some embodiments, the power of the laser irradiation treatment is 100-8000 W, optionally 1000-7000 W. The heating speed can be adjusted by changing the power. At high movement speeds, the laser power is increased accordingly to meet the rapid heating of the pole piece in a shorter dwell time.

[0021] In some embodiments, before the heating step, a step of drying the electrode piece is included.

[0022] In some embodiments, before the heating treatment step, a step of forming the pole piece is included. Optionally, the forming treatment includes one or both of cold pressing treatment and hot pressing treatment.

[0023] In some embodiments, before the heating step, a step of cutting the pole piece is included.

[0024] In the production process of the pole piece, the active material is generally mixed with a binder, a solvent and other necessary components to form a slurry. The slurry is coated on the current collector and dried to form a pole piece including a current collector and an active layer. After drying, the pole piece is usually subjected to a forming treatment such as cold pressing or hot pressing to increase the compaction density of the active layer and enhance the bonding force between the active layer and the current collector, and finally cut into a desired shape. The pole piece processing method of the embodiment of the present application is applicable to each process of pole piece production. This process can be performed after coating and drying, after forming, and after cutting. A wide range of materials can be processed and low requirements are placed on the pole piece. Moreover, after the pole piece is cut, the pole piece has residual stress and burrs are generated during cutting. After being treated by the method of the embodiment of the present application, the residual stress is released in advance to soften the burrs.

[0025] In a second aspect, the present application provides a pole piece, which is obtained by processing according to the above processing method.

[0026] The pole piece obtained by the above-mentioned treatment method has improved binder floating phenomenon, wherein the binder is redistributed and has good uniformity in the active layer, the bonding force and cohesion between the components in the active layer of the pole piece are improved, and the stress between the components is released; at the same time, the pole piece has a higher porosity, which helps to increase the absorption rate of the electrolyte; the possibility of electrons forming a conductive path increases, and the resistivity of the pole piece decreases, resulting in a decrease in internal resistance, which helps to improve the battery kinetic performance.

[0027] In a third aspect, the present application provides a battery, comprising the above-mentioned electrode.

[0028] The battery of the embodiment of the present application includes the above-mentioned pole piece, which can be a positive pole piece, a negative pole piece, or both a positive pole piece and a negative pole piece. Under the action of the treated pole piece, the battery has good battery dynamics performance, such as rate performance, low K value (voltage drop per unit time of the battery), low DC impedance and other advantages.

[0029] In a fourth aspect, the present application provides an electrical device, wherein the electrical device comprises the above-mentioned battery.

[0030] The battery disclosed in the embodiments of the present application can be used in electrical devices that use the battery as a power source, or various energy storage systems that use the battery as an energy storage element. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 SEM images of the positive electrode sheet provided in Example 1 of the present application before (a) and after (b) laser treatment;

[0033] Figure 2 SEM images of the negative electrode sheet provided in Example 1 of the present application before (a) and after (b) laser treatment;

[0034] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application;

[0035] Figure 4 A schematic diagram of a battery pack according to an embodiment of the present application;

[0036] Figure 5 for Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown;

[0037] Figure 6 A schematic diagram of a battery according to an embodiment of the present application;

[0038] Figure 7 for Figure 6 An exploded view of a battery according to an embodiment of the present application is shown;

[0039] Figure 8 A schematic diagram of an electrical device using a battery as a power source according to an embodiment of the present application.

[0040] Description of reference numerals:

[0041] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0042] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0044] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0045] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0046] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0047] In the description of the embodiments of the present application, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple, respectively.

[0048] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0049] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0050] With the continuous deepening of lithium-ion battery research and the continuous improvement of market demand, higher requirements are placed on the fast charging (fast charging) performance of batteries. The fast charging performance of batteries is closely related to their internal resistance, rate performance, and dynamic performance. Therefore, how to reduce internal resistance, improve rate performance, and improve dynamic performance has become a top priority.

[0051] In order to improve the performance of the above aspects, improvements can be made from the active materials, conductive agents, binders, electrolytes, and separators in the battery pole pieces. For example, the related art sequentially performs microwave heating and radiation irradiation on the lithium-ion battery pole pieces. However, in this method, the high-energy particles of the radiation can cause lattice distortion and rearrangement of some active materials with poor structural stability, thereby affecting the capacity, such as lithium nickel cobalt manganese oxide; the residual free radicals caused by cross-linking have the possibility of degrading the capacity of the pole piece. For example, the related art uses a micro-gravure to coat an aqueous solution of CMC (sodium carboxymethyl cellulose) or an NMP (N-methylpyrrolidone) solution of PVDF (polyvinylidene fluoride) on the positive or negative electrode sheet that has been rolled, and then rolls it again after drying. During the gravure coating, a slight rebound expansion will occur, causing the material particles in the pole piece to slightly "rotate", thereby achieving the effect of relieving the internal stress of the entire pole piece, which is more conducive to lithium ion embedding and improving dynamic performance. However, this method may have the problem of thickness rebound in the long term, affecting the stability of the electrode; and because the surface of the electrode is coated with a layer of adhesive, the surface resistance is too high, which increases the resistance of the electrode and makes the DC internal resistance of the lithium-ion battery using this electrode higher. Since it needs to be dried twice, the production cycle becomes longer.

[0052] In addition, there are related technologies that use carbon coating structures in active materials, add high specific surface area conductive agents such as carbon nanotubes, graphene, etc. to the conductive agent, introduce conductive binders into the binder, introduce primers on the current collector, etc. These methods are all based on the raw materials of the pole piece, and there are still the following problems: during the preparation of the slurry, the rapid evaporation of the solvent causes the binder to easily migrate to the surface, causing the binder to float, thereby deteriorating the surface dynamics and affecting the wettability of the pole piece. At present, double-layer coating can be used to compensate for this problem, but this method requires the preparation of two slurries at the same time, which consumes more equipment. Therefore, how to quickly and effectively improve the floating of the binder in the pole piece and improve the dynamic performance of the battery at the same time has become a technical breakthrough.

[0053] To this end, by heating the surface of the electrode and controlling the heating temperature so that the temperature is greater than or equal to the softening temperature or melting temperature of the adhesive, the adhesive is removed or re-infiltrated into the electrode by ablation or melting, thereby balancing the distribution of adhesive in the upper and lower layers of the electrode, helping to improve the diaphragm resistance of the electrode and enhance the dynamic performance; the balanced distribution of the adhesive in the electrode helps to improve the bonding strength and cohesion of the electrode.

[0054] The high heat generated during heating can remove part of the binder on the surface of the pole piece, and then form pores on the surface of the pole piece; due to thermal expansion and contraction, as well as the softening and fluidity of the binder, a small amount of pores are also regenerated inside the pole piece after cooling. The generation of a small amount of pores constructs capillary channels, which can increase the infiltration rate with the electrolyte, accelerate the transmission of lithium ions between the electrodes and the electrolyte, and improve the battery dynamics performance.

[0055] Under the action of high temperature, the burrs on the electrode caused by cutting can be shrunk and softened, making them less sharp and reducing the risk of piercing the isolation membrane, thereby improving the battery K value (voltage drop per unit time) and self-discharge rate.

[0056] At the same time, the temperature is controlled to be lower than the lowest temperature among the decomposition temperature, oxidation temperature and ignition temperature of the active material, so that the active material in the electrode can maintain the integrity of the lattice, which is beneficial to maintaining the capacity of the electrode.

[0057] In this way, by performing a specific heating treatment on the electrode, the dried electrode can be "reactivated" and the binder can be evenly distributed, which can release the stress between the components in the electrode, help increase the porosity of the electrode, and improve the absorption rate of the electrolyte; the possibility of electrons forming a conductive path is increased, which is beneficial to reduce the resistivity of the electrode, reduce the internal resistance of the battery, and help improve the battery dynamic performance.

[0058] The present application is further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application.

[0059] An embodiment of the present application provides a method for processing an electrode, which includes an active layer, and the active layer includes an active substance and a binder. The processing method of the embodiment of the present application includes: heating the electrode to raise the temperature of the active layer to a processing temperature; the processing temperature is greater than or equal to the softening temperature or melting temperature of the binder, and the processing temperature is less than the lowest temperature among the decomposition temperature, oxidation temperature, and ignition temperature of the active substance.

[0060] In the embodiments of the present application, the active material on the pole piece is the medium for electron transfer during the battery chemical reaction. The active material usually forms an active layer with an adhesive and other materials, and is arranged on at least one side of the current collector of the pole piece. The binder is a polymer compound used to bind the various components in the active layer (such as active materials and other substances) and the current collector to each other. It mainly plays the role of bonding and maintaining the firmness of the active material in the active layer, enhancing the contact between the active layer and the current collector, and enhancing the contact between the various substances in the active layer. The binder is mixed with the active material, solvent and other necessary components to form a slurry. After the solvent evaporates, the slurry is dried to form an active layer. During the drying process, the evaporation of the solvent makes it easy for the binder to migrate to the surface of the active layer, causing the binder to float, thereby deteriorating the surface dynamics, affecting the wettability of the pole piece, and ultimately affecting the electrochemical performance of the pole piece.

[0061] Heating the active layer to the processing temperature means that at least the surface temperature of the active layer is heated to the processing temperature. The surface of the active layer refers to the outermost layer of the active layer in contact with the outside world. Usually, the pole piece includes a current collector and an active layer arranged on at least one side of the current collector, so the surface of the active layer is usually also the surface of the pole piece. Generally, the area within 40% of the thickness of the pole piece along the thickness direction of the pole piece and from the outside to the inside can be regarded as the surface of the pole piece. The active layer is usually thin, and during the heating process, the temperature of the surface of the active layer is usually close to or the same as the temperature inside the active layer, and the temperature difference is small. At this time, the temperature inside the active layer can also reach the processing temperature.

[0062] The softening temperature is the temperature at which the three-dimensional long-range ordered state of the macromolecular chain structure of a non-crystalline polymer changes to a disordered viscous flow state. The melting temperature is the temperature at which the three-dimensional long-range ordered state of the macromolecular chain structure of a crystalline polymer changes to a disordered viscous flow state, also known as the melting point, which is the lower limit of the molding processing temperature of crystalline polymers. Generally speaking, the melting temperature range is relatively narrow, while the softening temperature range is relatively wide.

[0063] For polymer materials, the decomposition temperature refers to the temperature at which the molecular chains of polymers in a viscous flow state will degrade more rapidly or even significantly degrade when the temperature rises further; for inorganic materials, the decomposition temperature refers to the temperature at which the molecular structure of inorganic materials is destroyed or the lattice is distorted, although no combustion reaction occurs. The oxidation temperature is the minimum temperature required for a substance to undergo an oxidation reaction. The ignition temperature, also known as the ignition temperature, is the minimum temperature at which a substance burns.

[0064] In the electrode processing method of the embodiment of the present application, the electrode is heated so that the temperature of the active layer is greater than or equal to the softening temperature or melting temperature of the binder, and the binder re-melts and penetrates into the active layer of the electrode, which plays a role in balancing the distribution of the binder in the upper and lower layers of the electrode, which helps to improve the electrode resistance of the electrode and enhance the dynamic performance; the balanced distribution of the binder in the electrode helps to improve the bonding force and cohesion of the electrode. Moreover, the high heat generated during heating can remove part of the binder on the surface of the electrode, and then form pores on the surface of the electrode; due to thermal expansion and contraction and the softening and fluidity of the binder, a small amount of pores are also regenerated inside the electrode after cooling. The generation of a small amount of pores constructs a capillary channel, which can increase the infiltration rate with the electrolyte, accelerate the transmission of lithium ions between the electrodes and the electrolyte, and improve the battery dynamic performance.

[0065] At the same time, the processing temperature is lower than the lowest temperature among the decomposition temperature, oxidation temperature and ignition temperature of the active material. Therefore, during the electrode processing, the etching or decomposition of the active material can be improved, which is beneficial for the active material in the electrode to maintain the integrity of the lattice, and thus is beneficial for maintaining the capacity of the electrode.

[0066] In some embodiments, the electrode piece is a positive electrode piece, and the processing temperature is less than or equal to the decomposition temperature of the binder.

[0067] According to the electron gain and loss of the active material in the electrode in the battery chemical reaction, the electrode can be divided into positive electrode and negative electrode, where the active material in the positive electrode loses electrons in the battery chemical reaction of charging, and the active material in the negative electrode gains electrons in the battery chemical reaction of charging. Due to the difference in active materials, the solubility of the active materials in the solvent is different in the positive electrode and the negative electrode, and the solubility of the binder in the solvent is different. Therefore, different types of solvents and binders are usually used in the production process of the active layer of the positive electrode and the negative electrode. Usually, oily solvents and oily binders are used in the production process of the active layer of the positive electrode, while aqueous solvents and aqueous binders are used for the negative electrode. The different volatilization rates of oily solvents and oily solvents make the migration of the binder different during the slurry drying process. Therefore, the distribution of the binder in the positive electrode is usually different from that of the negative electrode.

[0068] In practice, it is found that the binder in the positive electrode sheet floats less. Therefore, for the positive electrode sheet, the treatment temperature is greater than or equal to the softening temperature or melting temperature of the binder, and less than or equal to the decomposition temperature of the binder, so that the binder can be re-infiltrated into the sheet in a molten manner, and the binder does not decompose or only very little decomposes, so that the distribution of the binder between different layers of the sheet is balanced, which helps to improve the bonding and cohesion of the positive electrode sheet.

[0069] For the negative electrode sheet, the processing temperature is controlled to be greater than or equal to the softening temperature or melting temperature of the binder, and the processing temperature is less than the lowest temperature of the three temperatures of the decomposition temperature, oxidation temperature, and ignition temperature of the active material. Considering that the decomposition temperature of the binder is usually higher than the softening temperature or melting temperature of the binder, and lower than the decomposition temperature of the active material, therefore, for the negative electrode sheet, there may be a case where the processing temperature is greater than or equal to the decomposition temperature of the binder, or there may be a case where the processing temperature is less than the decomposition temperature of the binder. When the processing temperature of the negative electrode sheet is greater than or equal to the decomposition temperature of the binder, the excess binder on the surface can be removed, the bonding force can be balanced, and the negative electrode sheet is not easy to crack or powder during the cold pressing process. When the processing temperature of the negative electrode sheet is less than the decomposition temperature of the binder, the binder can be re-infiltrated into the sheet in a molten manner, and at the same time, the binder does not decompose or only a very small amount of the binder decomposes, so that the distribution of the adhesive between different layers of the sheet is balanced, which helps to improve the bonding force and cohesion of the positive electrode sheet.

[0070] In some embodiments, the treatment temperature is 160 to 400°C; in other embodiments, the treatment temperature is 180 to 370°C. For example, the treatment temperature includes but is not limited to any one of 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 370°C, 380°C, and 400°C, or a range between any two of them. The treatment temperature can be measured by an infrared thermometer or other temperature tester. The treatment temperature can be measured by an infrared thermometer or other temperature tester. This temperature interval is greater than or equal to the softening temperature or melting temperature of a common binder, and is less than the decomposition temperature of a common active substance. Therefore, for ease of operation, the treatment temperature can be set in this temperature interval.

[0071] In some embodiments, the electrode is a positive electrode, and the processing temperature is 160-260°C, including but not limited to any point value of 160°C, 180°C, 200°C, 220°C, 240°C, 260°C or any range value between two thereof; in other embodiments, the electrode is a positive electrode, and the processing temperature is 280-400°C, including but not limited to any point value of 280°C, 300°C, 320°C, 340°C, 360°C, 370°C, 380°C, 400°C or any range value between two thereof. Depending on the type of binder used in the positive electrode, a suitable processing temperature can be used. For example, the melting temperature of polyvinylidene fluoride (PVDF), a commonly used binder for positive electrode sheets, is 166-170°C, and its thermal decomposition temperature is greater than 310°C, so a treatment temperature of 160-260°C can be used; polyimide (PI) will soften at ≥300°C, and its thermal decomposition temperature is greater than 500°C, so a treatment temperature of 280-400°C can be used; selecting a suitable treatment temperature within this temperature range according to different binders can allow the binder to re-infiltrate into the sheet in a molten form, while at the same time, the binder does not decompose or only very little decomposes, so that the distribution of the adhesive between different layers of the sheet is balanced, which helps to improve the bonding strength and cohesion of the positive electrode sheet.

[0072] In some embodiments, the electrode is a negative electrode, and the processing temperature is 180-350°C, optionally 200-350°C, including but not limited to any one of 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 350°C or any range between two thereof. The temperature is greater than or equal to the decomposition temperature of the common binder for the negative electrode. For example, styrene-butadiene rubber (SBR), a common binder for the negative electrode, will gradually decompose at a temperature above 220°C. At this processing temperature, the excess binder on the surface can be removed, the bonding force can be balanced, and the problem of easy cracking and powdering of the negative electrode during the cold pressing process can be improved.

[0073] In some embodiments, the heating time is 0.02 to 0.3 s, optionally 0.02 to 0.2 s, including but not limited to any one of 0.02 s, 0.04 s, 0.06 s, 0.08 s, 0.1 s, 0.12 s, 0.14 s, 0.16 s, 0.18 s, 0.2 s, 0.22 s, 0.24 s, 0.26 s, 0.28 s, and 0.3 s, or a range between any two of them.

[0074] In the embodiment of the present application, the heating time refers to the time for the surface of the active layer to be heated to the processing temperature. The shorter the heating time, the faster the heating speed. The heating time can be recorded by a temperature sensor. The processing method in the embodiment of the present application has a high heating rate, which can quickly make the surface and internal temperatures of the active layer reach the processing temperature. The binder absorbs heat in a short time, which can not only make the binder more evenly distributed in the active layer, but also has a high processing efficiency.

[0075] In some embodiments, the thickness of the active layer is 50 to 300 μm before the heat treatment; in other embodiments, the thickness of the active layer is 50 to 200 μm before the heat treatment. For example, the thickness of the pole piece may include but is not limited to any point value of 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm or any range value between two of them. Generally, the thickness of the pole piece can be measured by a micrometer, a laser thickness gauge, a thickness scanning thickness gauge, etc.

[0076] Due to the influence of heat conduction and diffusion, the method of the embodiment of the present application can process various single-sided or double-sided pole pieces with an actual coating thickness of 50 to 300 μm. At the appropriate thickness, the surface and interior of the active layer can reach the required processing temperature under rapid heating, reducing the temperature difference between the surface and interior of the active layer. When the surface and interior of the active layer have similar or the same processing temperatures, the melting and flow of the binder are more uniform, thereby improving the uniformity of the distribution of the binder in the pole piece. The method of the embodiment of the present application can process a wide range of materials and has low requirements for pole pieces.

[0077] Moreover, in terms of thickness, the electrode sheet processing method of the embodiment of the present application has little effect on the thickness of the electrode sheet due to the small number of newly generated pores. That is, after the processing, the thickness of the electrode sheet changes little.

[0078] In some embodiments, before the heat treatment, the surface density of the active layer is 0.05 to 0.6 mg / mm 2 For example, the surface density of the active layer may include but is not limited to 0.05 mg / mm 2 , 0.1mg / mm 2 , 0.15mg / mm 2 , 0.2mg / mm 2 , 0.25mg / mm 2 , 0.3mg / mm 2 , 0.35mg / mm 2 , 0.4mg / mm 2 、0.45mg / mm 2 , 0.5mg / mm 2 , 0.55mg / mm2 , 0.6mg / mm 2 Any point value in or any range between two values. Surface density refers to the mass of the sheet coating per unit surface area, which can be obtained by testing with an X / β-ray surface density meter. Due to the influence of heat conduction and diffusion, the method of the embodiment of the present application can handle the actual coating thickness with a surface density of 0.05 to 0.6 mg / mm 2 At a suitable surface density, the binder in the active layer can be effectively heated, ablated or melted into the electrode. At the same time, the surface density mainly affects the internal resistance and capacity of the electrode. Generally, within a certain range, the internal resistance of the electrode decreases with the increase of the surface density. Increasing the surface density of the electrode helps to reduce the internal resistance of the electrode, thereby improving the capacity of the electrode. The active layer of the embodiment of the present application has a suitable surface density, and the electrode has low internal resistance and high capacity.

[0079] In some embodiments, the electrode is a positive electrode, and before the heating treatment, the surface density of the active layer is 0.08 to 0.6 mg / mm 2 , optionally 0.1 to 0.5 mg / mm 2 For example, the surface density of the active layer may include but is not limited to 0.08 mg / mm 2 , 0.1mg / mm 2 , 0.15mg / mm 2 , 0.2mg / mm 2 , 0.25mg / mm 2 , 0.3mg / mm 2 , 0.35mg / mm 2 , 0.4mg / mm 2 、0.45mg / mm 2 , 0.5mg / mm 2 , 0.55mg / mm 2 , 0.6mg / mm 2 Any point value in or any range between two values.

[0080] In some embodiments, the electrode is a negative electrode, and before the heating treatment, the surface density of the active layer is 0.05 to 0.3 mg / mm 2 , optionally 0.05 to 0.2 mg / mm 2 For example, the surface density of the active layer may include but is not limited to 0.05 mg / mm 2 , 0.1mg / mm 2 , 0.15mg / mm 2 , 0.2mg / mm 2 , 0.25mg / mm 2 , 0.3mg / mm 2Any point value in or any range between two values.

[0081] Generally, the active materials of the positive and negative electrodes have different densities, and many positive electrode active materials have higher density than negative electrode active materials; and the positive and negative electrodes usually have different gram capacities. Under the same surface density, the capacity of the negative electrode is larger than that of the positive electrode. In order to make the positive and negative electrode capacities roughly the same, the surface density of the negative electrode is usually set to be slightly smaller than the surface density of the positive electrode.

[0082] In some embodiments, the heating treatment method includes laser irradiation treatment. Laser irradiation treatment is to use a laser to generate a laser beam and use the laser beam for irradiation. The laser has the characteristics of excellent monochromaticity, extremely small divergence, and extremely high brightness, and can make the temperature of the active layer reach the required temperature in a very short time. Moreover, the pole piece processing method of the embodiment of the present application can quickly complete the processing of the pole piece at one time by using a laser on one side or both sides of the pole piece, and can be integrated on existing equipment without adding a lot of extra time and equipment. The original pole piece production capacity can be maintained at a low cost.

[0083] In some embodiments, the pole piece includes a first surface and a second surface arranged opposite to each other; the laser irradiation treatment step includes: using a first laser beam to perform laser irradiation treatment on the first surface, and using a second laser beam to perform laser irradiation treatment on the second surface; there is a spacing between the first laser beam and the second laser beam in a direction parallel to the first surface and the second surface.

[0084] In the embodiment of the present application, there is a gap between the first laser beam and the second laser beam in the direction parallel to the first surface and the second surface, that is, the first laser beam and the second laser beam are staggered for irradiation on both sides of the pole piece, and the laser heads for generating laser beams are located on both sides of the pole piece but not directly facing each other. The two are separated by a certain distance in the plane direction of the pole piece, which is beneficial to control the temperature of the pole piece and improve the problem of overheating of the pole piece in a short period of time.

[0085] In some embodiments, in the laser irradiation treatment step, the maximum size of the laser spot falling on the surface of the pole piece is greater than or equal to the minimum size on the surface of the pole piece. The laser spot is the area (usually circular or rectangular) formed at the focal point after the laser beam is focused, and the laser power density is most concentrated at the laser spot. The maximum size of the laser spot is also usually called the laser spot width, which is usually the diameter (circular) or diagonal size (rectangular) of the area. The maximum size of the laser spot can usually be set directly in the laser generator. The minimum size on the surface of the pole piece refers to the shortest distance of the pole piece on the surface. The pole piece is usually rectangular, and the minimum size on the surface of the pole piece refers to the width of the pole piece, which is also usually called the membrane area width. In the embodiment of the present application, the maximum size of the laser spot is greater than or equal to the minimum size on the surface of the pole piece. Under this condition, the pole piece can be simultaneously and comprehensively irradiated in the direction of the minimum size on the surface of the pole piece in one laser irradiation treatment, so that the adhesive in this direction is melted almost at the same time, which helps to improve the uniformity of the adhesive after it is fully distributed. For example, the maximum size of the laser spot falling on the surface of the pole piece can be adjusted to 50-220 mm, including but not limited to any point value of 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 120 mm, 140 mm, 160 mm, 180 mm, 200 mm, 220 mm or any range value between two of them. This size can meet the processing requirements of most pole pieces.

[0086] In some embodiments, in the laser irradiation treatment step, the distance between the laser used to generate the laser beam and the surface of the pole piece is 10 to 50 cm, including but not limited to any point value of 10 cm, 15 cm, 20 cm, 25 cm, 30 cm, 35 cm, 40 cm, 45 cm, 50 cm or any range value between two of them. The appropriate distance can effectively utilize laser irradiation to heat up the pole piece, and is also conducive to controlling the temperature of the pole piece, improving the problem of pole piece overheating and the need to use higher power and longer laser irradiation, which increases costs.

[0087] In some embodiments, the laser irradiation treatment step includes: moving the pole piece relative to the laser spot falling on the pole piece surface, and the moving speed is 10 to 200 m / min; in some embodiments, the moving speed is 30 to 200 m / min. For example, the speed of the moving process includes but is not limited to any point value among 10m / min, 15m / min, 20m / min, 25m / min, 30m / min, 35m / min, 40m / min, 45m / min, 50m / min, 55m / min, 60m / min, 65m / min, 70m / min, 75m / min, 80m / min, 85m / min, 90m / min, 95m / min, 100m / min, 110m / min, 120m / min, 130m / min, 140m / min, 150m / min, 160m / min, 170m / min, 180m / min, 190m / min, and 200m / min, or a range value between any two of them. In the embodiment of the present application, the processing process of the pole piece can be in a dynamic state, the pole piece moves relative to the laser spot, and the laser briefly heats the pole piece, which can increase the temperature of the active layer in the pole piece, but the rising temperature will not be too high. In actual operation, the pole piece can be placed on the winding guide roller and the unwinding guide roller, and the winding guide roller is used to pull the pole piece to achieve movement of the pole piece. The speed of movement of the pole piece can be controlled by the operating speed of the winding guide roller. By controlling the movement of the pole piece, the laser irradiation treatment of the entire roll of pole piece can be completed in one winding and unwinding process, with a high processing speed, which helps to improve production capacity and is convenient and easy to process. During the movement process, the time that the pole piece passes through the laser light source is usually less than 0.2s, which is enough to redistribute the adhesive in the active layer, while reducing heat accumulation and unnecessary side reactions.

[0088] In some embodiments, the power of the laser irradiation treatment is 100-8000W, optionally 1000-7000W, and optionally 2000-6500W. For example, the power of the laser irradiation treatment includes but is not limited to any point value of 100W, 500W, 1000W, 1500W, 2000W, 2500W, 3000W, 3500W, 4000W, 4500W, 5000W, 5500W, 6000W, 6500W, 7000W, 7500W, 8000W or any range value between two of them. The heating speed can be adjusted by changing the power. At high movement speed, the laser power increases accordingly to meet the rapid heating of the pole piece in a shorter residence time.

[0089] In some embodiments, the laser irradiation treatment includes one or both of pulsed laser irradiation treatment and continuous laser irradiation treatment. Pulsed laser refers to a light pulse emitted by a laser using a pulsed working mode, and there is a certain interval between two adjacent light pulses. Continuous laser is a continuous and uninterrupted laser emitted by a continuous laser. Whether the pole piece is subjected to pulsed laser irradiation or continuous laser irradiation, the active layer can reach the required processing temperature in a short time.

[0090] In some embodiments, the binder includes one or more of an oil-soluble binder, a water-soluble binder, and an emulsion-type binder.

[0091] In some embodiments, the oil-soluble binder includes one or more of polyvinylidene fluoride, polyimide, polytetrafluoroethylene, polybutyl acrylate, and polyacrylonitrile.

[0092] In some embodiments, the water-soluble binder includes one or more of carboxymethyl cellulose, carboxymethyl cellulose salt, polyacrylic acid, polyacrylic acid salt, polyvinyl alcohol, sodium alginate, and cyclodextrin.

[0093] In some embodiments, the emulsion binder includes one or more of styrene-butadiene rubber, vinyl acetate resin, acrylic resin, and chlorinated rubber.

[0094] According to the different types of active materials in the pole piece, different binders can be selected, and the appropriate processing temperature can be determined according to the softening temperature or melting temperature, or decomposition temperature of the binder. For example, in the case where the pole piece is a positive pole piece, polyvinylidene fluoride can usually be selected as a binder, and its processing temperature can be set to 160-260°C, more specifically, it can be set to 180-250°C, including but not limited to any point value of 160°C, 180°C, 200°C, 220°C, 240°C, 250°C, 260°C or any range value between the two; polyimide is selected as a binder, and its processing temperature can be set to 280-400°C, more specifically, it can be set to 300-380°C, including but not limited to any point value of 280°C, 300°C, 320°C, 340°C, 360°C, 370°C, 380°C, 400°C or any range value between the two. For another example, in the case where the electrode is a negative electrode, styrene-butadiene rubber can usually be selected as a binder, and the processing temperature can be set to 180-350°C, more specifically 200-350°C, such as 200-300°C, including but not limited to any one of 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 350°C or a range between any two of them.

[0095] In some embodiments, the mass content of the binder in the active layer includes but is not limited to 0.5% to 10%, such as 1% to 5%, for example, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, any one of the points or any range values ​​between two of them, and can also be set to other contents as needed.

[0096] In some embodiments, the electrode is a positive electrode, and the active material includes one or more of metal inorganic active materials and organic active materials.

[0097] In some embodiments, the metal inorganic active material includes one or more of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0098] In some embodiments, the organic active material includes one or more of quinone compounds, carboxylate compounds, anhydride compounds, and amide compounds.

[0099] In some embodiments, the electrode is a negative electrode, and the active material includes one or more of a carbon-based active material, a titanium-based active material, a silicon-based active material, a nitride, and metallic lithium.

[0100] In some embodiments, the carbon-based material includes one or more of graphite, hard carbon, soft carbon, mesocarbon microbeads, and graphene.

[0101] In some embodiments, the titanium-based active material includes one or more of lithium titanate and titanium dioxide.

[0102] In some embodiments, the silicon-based active material includes one or more of silicon, silicon dioxide.

[0103] In some embodiments, the nitride includes lithium nitride.

[0104] In some embodiments, the mass content of the active substance in the active layer includes but is not limited to 90% to 98%, such as 95% to 98%, for example, any point value of 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or a range value between any two of them, and can also be set to other contents as needed.

[0105] In some embodiments, before the heating step, a step of drying the electrode sheet is included.

[0106] In some embodiments, before the heating step, a step of forming the pole piece is included. In some embodiments, the forming process includes one or both of cold pressing and hot pressing.

[0107] In some embodiments, before the heating step, a step of cutting the pole piece is included.

[0108] In the production process of the pole piece, the active material is generally mixed with a binder, a solvent and other necessary components to form a slurry. The slurry is coated on the current collector and dried to form a pole piece including a current collector and an active layer. After drying, the pole piece is usually subjected to a forming treatment such as cold pressing or hot pressing to increase the compaction density of the active layer and enhance the bonding force between the active layer and the current collector, and finally cut into a desired shape. The pole piece processing method of the embodiment of the present application is applicable to each process of pole piece production. This process can be performed after coating and drying, after forming, and after cutting. A wide range of materials can be processed and low requirements are placed on the pole piece. Moreover, after the pole piece is cut, the pole piece has residual stress and burrs are generated during cutting. After being treated by the method of the embodiment of the present application, the residual stress is released in advance to soften the burrs.

[0109] In some embodiments, the pole piece further includes a current collector, and the active layer is disposed on at least one side of the current collector. The current collector on the pole piece is used as a substrate for the active layer to attach and to transmit electrons in the battery chemical reaction. The current collector includes but is not limited to a metal current collector, a carbon current collector, a conductive resin current collector, a composite current collector of metal and resin, and more specifically, copper, nickel, titanium, iron and their respective alloys, stainless steel, carbon fiber, carbon nanotube (CNT), graphite, and the like.

[0110] In some embodiments, the active layer also includes a conductive agent. The conductive agent collects microcurrents between the active materials and between the active materials and the current collector to improve the electronic conductivity. At the same time, the conductive agent can also promote the infiltration of the electrolyte into the positive electrode. The conductive agent includes but is not limited to acetylene black (SP), carbon nanotubes, conductive carbon black (super-P), Ketjen black, carbon fiber, graphene, etc. Due to the softening flow of the binder, the conductive agent will also move during the electrode processing. The conductive agent has good affinity with the conductive agent and a large specific surface area. It is easier to form a conductive path at the moment of movement, which can significantly improve the conductivity of the electrode and improve the battery DCR (direct current resistance).

[0111] In some embodiments, the mass content of the conductive agent in the active layer includes but is not limited to 0.5% to 10%, such as 1% to 5%, for example, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, any one of the point values ​​or the range value between any two of them, and can also be set to other contents as needed.

[0112] In some embodiments, the active layer may further include a thickener, such as carboxymethyl cellulose (CMC). The mass content of the thickener in the active layer includes, but is not limited to, 0.5% to 5%, such as 1% to 5%, including but not limited to any one of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%, or any range between two of them, and may also be set to other contents as needed.

[0113] The embodiment of the present application also provides a pole piece, which is obtained by processing according to the above processing method.

[0114] The electrode obtained by the above-mentioned treatment method has a redistributed binder and has good uniformity in the active layer. The bonding force and cohesion between the components in the active layer of the electrode are improved, and the stress between the components is released; at the same time, the electrode has a higher porosity, which helps to increase the absorption rate of the electrolyte; the possibility of electrons forming a conductive path increases, and the resistivity of the electrode decreases, resulting in a decrease in internal resistance, which helps to improve the battery kinetic performance.

[0115] The embodiment of the present application also provides a battery. The battery includes the above-mentioned pole piece.

[0116] The battery of the embodiment of the present application includes the above-mentioned pole piece, which can be a positive pole piece, a negative pole piece, or both a positive pole piece and a negative pole piece. Under the action of the treated pole piece, the battery has good battery dynamics performance, such as high rate performance, low K value (voltage drop per unit time of the battery), low DC impedance, etc.

[0117] In some embodiments, the battery of the embodiment of the present application includes one or more of a primary battery and a secondary battery. Batteries can be divided into primary batteries and secondary batteries according to whether the battery can be recharged and reused. A primary battery cannot be recharged to restore it after discharge, and a secondary battery can continue to be used by activating the active material by charging after the battery is discharged. The pole piece of the embodiment of the present application can be applied to both primary batteries and secondary batteries, and has a wide range of uses.

[0118] In some embodiments, the battery of the embodiments of the present application includes one or more of a battery cell, a battery module, and a battery pack. In the case where the battery is a secondary battery, the secondary battery is divided into a battery cell, a battery module, and a battery pack according to different packaging forms. Among them, the battery cell is the most basic unit of a secondary battery, including an electrode assembly and an electrolyte. The electrode assembly is usually composed of a positive electrode sheet, a negative electrode sheet, and a separator. The battery cell mainly relies on the movement of metal ions in the electrolyte between the positive electrode sheet and the negative electrode sheet to work. In some battery packaging technologies, one or more battery cells can be integrated into a battery module first, and then one or more battery modules can be assembled into a battery pack. In other battery packaging technologies, one or more battery cells can also be directly installed in a box to form a battery pack, eliminating the intermediate state of the battery module, thereby reducing the mass of the battery pack and increasing the energy density of the battery.

[0119] In some embodiments, the battery further includes an electrolyte. The electrolyte can serve as a carrier for ion transport in the battery.

[0120] In some embodiments, the electrolyte may be a solid electrolyte, such as a polymer electrolyte, an inorganic solid electrolyte, etc., but is not limited thereto. The electrolyte may also be an electrolyte solution. The electrolyte solution includes a solvent and a lithium salt dissolved in the solvent.

[0121] Among them, the solvent can be a non-aqueous organic solvent, such as ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB) and ethyl butyrate (EB) One or more, preferably two or more.

[0122] The lithium salt can be one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalatoborate), LiBOB (lithium bis(oxalatoborate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorooxalatophosphate) and LiTFOP (lithium tetrafluorooxalatophosphate), for example, one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiBOB (lithium bis(oxalatoborate), LiDFOB (lithium difluorooxalatoborate), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) and LiFSI (lithium bis(fluorosulfonyl)imide).

[0123] The electrolyte may also contain other additives, such as vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), succinonitrile (SN), adiponitrile (ADN), glutaronitrile (GLN), hexanetrinitrile (HTN), 1,3-propane sultone (1,3-PS), vinyl sulfate (DTD), methylene disulfonate (MMDS), 1-propylene-1,3-sultone (PST), 4-methylethylene sulfate (PCS), 4-ethylethylene sulfate (PES), 4-propylethylene sulfate (PEGLST), propylene sulfate (TS), 1,4-butane sultone (1,4-BS), ethylene sulfite (DTO), dimethyl sulfite (DMS), diethyl sulfite (DES), sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl) phosphate (TMSP) and tris(trimethylsilyl) borate (TMSB), but are not limited thereto.

[0124] In some embodiments, the battery further includes a separator stacked between the positive electrode sheet and the negative electrode sheet. In some batteries, a separator is required to separate the positive electrode sheet from the negative electrode sheet so that electrons in the battery cannot pass freely, preventing the two electrodes from contacting and short-circuiting, while allowing ions in the electrolyte to pass freely between the positive and negative electrodes.

[0125] The isolation membrane can be any known porous structure isolation membrane with electrochemical stability and mechanical stability, such as a single-layer or multi-layer film of one or more of glass fiber, non-woven fabric, polyethylene (PE), polypropylene (PP) and polyvinylidene fluoride (PVDF).

[0126] The positive electrode sheets and the negative electrode sheets are alternately stacked, and a separation film is set between the positive electrode sheets and the negative electrode sheets to play an isolating role, so as to obtain a battery cell, or the battery cell can be obtained after winding. The battery cell is placed in a casing, an electrolyte is injected, and it is sealed to obtain a battery cell. Multiple battery cells are first integrated to form a battery module, which can provide higher voltage and capacity, and has a specific functional output; then the battery module is installed in the battery box, and a battery management system is usually added to form a battery pack, which is usually a product provided to users. Alternatively, multiple battery cells can be directly installed in the box to form a battery pack.

[0127] refer to Figure 3 , which is an example of a battery module 4. In the battery module 4, a plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.

[0128] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.

[0129] refer to Figure 4 and Figure 5 , which is taken as an example of a battery pack 1. The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3, and the upper box body 2 can be covered on the lower box body 3 to form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0130] In some embodiments, the battery may include an outer packaging, which may be used to encapsulate the electrode assembly consisting of the positive electrode sheet, the negative electrode sheet, the separator, and the electrolyte.

[0131] The outer packaging of the battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0132] The shape of the battery can be cylindrical, square or any other shape. For example, Figure 6 A square-structured battery is used as an example.

[0133] In some embodiments, reference Figure 7The outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can form an electrode assembly 52 through a winding process or a lamination process. One or more electrode assemblies 52 are encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52.

[0134] The embodiment of the present application also provides an electrical device, which includes the above-mentioned battery. The battery disclosed in the embodiment of the present application can be used in an electrical device using a battery as a power source, or in various energy storage systems using a battery as an energy storage element. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, for example, game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like. As the electrical device, the battery cell, battery module, or battery pack in the battery can be selected according to its use requirements.

[0135] Figure 8 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the battery, a battery pack or a battery module can be used.

[0136] The following describes the invention in conjunction with specific embodiments.

[0137] Example 1

[0138] 1) Preparation of positive electrode

[0139] Lithium iron phosphate was selected as the positive electrode active material, and was dispersed in NMP (N-methylpyrrolidone) with conductive carbon black and PI (polyimide) at a mass ratio of 97wt%, 1wt%, and 2wt%, and then coated on both sides of aluminum foil and dried, and then cold pressed to obtain CW (surface density) = 360mg / 1540.25mm 2 , the total thickness of the positive electrode sheet is 97μm and the membrane area width is 100mm.

[0140] 2) Laser treatment of the positive electrode surface

[0141] The positive electrode plate is uniformly passed between the upper and lower lasers at a moving speed of 180m / min for laser irradiation heating. The distance between the laser and the electrode plate is 10cm, and the two lasers are misaligned on both sides of the positive electrode plate; the laser spot width is 200mm, the laser continuous heating power is 6500W, and the heating time is 0.067s. The final temperature (i.e., the treatment temperature) of the surface of the positive electrode plate after laser irradiation heating is 340℃.

[0142] SEM images of the positive electrode before and after laser treatment Figure 1 As shown in the figure, it can be seen that after laser treatment, the positive electrode plate has not been etched.

[0143] 3) Preparation of negative electrode sheet

[0144] 95wt% of the negative electrode active material artificial graphite, 1.0wt% of the conductive carbon black, 2.0wt% of the binder styrene butadiene rubber (SBR) and 2.0wt% of the thickener sodium carboxymethyl cellulose (CMC) were mixed, added with deionized water, stirred, and dispersed to form the negative electrode slurry. Then the negative electrode slurry was coated on the Cu foil, and after both sides were completed, it was dried and cold pressed to obtain a total CW = 160mg / 1540.25mm 2 , the negative electrode plate has a thickness of 67μm and a membrane area width of 105mm.

[0145] 4) Laser treatment of the negative electrode surface

[0146] The negative electrode plate is uniformly passed between the upper and lower lasers at a moving speed of 120m / min for laser irradiation heating. The distance between the laser and the negative electrode plate is 20cm, and the two lasers are misaligned on both sides of the negative electrode plate; the laser spot width is 105mm, the laser continuous heating power is 6000W, and the heating time is 0.053s. The final temperature of the surface of the negative electrode plate after laser irradiation heating is 300℃.

[0147] SEM images of the negative electrode before and after laser treatment Figure 2 As shown in the figure, it can be seen that after laser treatment, the negative electrode plate is not etched.

[0148] Example 2

[0149] 1) Preparation of positive electrode

[0150] Lithium nickel cobalt manganese oxide with a nickel-cobalt-manganese molar ratio of 8:1:1 was selected as the positive electrode active material, and was dispersed in NMP (N-methylpyrrolidone) with conductive carbon black and PVDF at a mass ratio of 96wt%, 2wt%, and 2wt% and coated on both sides of aluminum foil in sequence and dried to obtain CW=660mg / 1540.25mm 2The positive electrode sheet is then cold pressed to obtain a positive electrode sheet with a total electrode layer thickness of 130μm and a membrane area width of 200mm.

[0151] 2) Laser treatment of the positive electrode surface

[0152] The positive electrode plate is uniformly passed between the upper and lower lasers at a moving speed of 80m / min for laser irradiation heating. The continuous laser heating power is 3000W, and the heating time (heating time) is 0.075s. The distance between each laser and the positive electrode plate is 15cm, and the two lasers are misaligned on both sides of the positive electrode plate; the laser spot width is 100mm. The final temperature of the surface of the positive electrode plate after laser irradiation heating is 250℃.

[0153] 3) Preparation of negative electrode sheet

[0154] 95wt% of the negative electrode active material artificial graphite, 1wt% of silicon, 0.5wt% of conductive carbon black, 2.0wt% of the binder styrene butadiene rubber (SBR) and 1.5wt% of the thickener sodium carboxymethyl cellulose (CMC) were mixed, added with deionized water, stirred, and dispersed to form a negative electrode slurry. Then the negative electrode slurry was coated on the Cu foil, and after both sides were completed, it was dried and cold pressed to obtain CW = 420mg / 1540.25mm 2 , the negative electrode plate has a thickness of 190μm and a membrane area width of 210mm.

[0155] 4) Laser treatment of the negative electrode surface

[0156] The negative electrode plate was uniformly passed between the upper and lower lasers at a moving speed of 200m / min for laser irradiation heating. The distance between the laser and the electrode plate was 35cm, and the two lasers were misaligned on both sides of the positive electrode plate; the laser spot width was 210mm, the laser continuous heating power was 2000W, and the heating time was 0.063s. The final temperature of the surface of the negative electrode plate after laser irradiation heating was 275℃.

[0157] Example 3

[0158] The rest is the same as Example 1, except that the final heating temperatures of the positive and negative electrode sheets are 370°C and 260°C respectively, the corresponding laser continuous heating powers are 4500W and 4000W respectively, the movement speed of the positive electrode sheet is 60m / min, the movement speed of the negative electrode sheet is 80m / min, and the heating times of the positive electrode sheet and the negative electrode sheet are 0.2s and 0.079s respectively.

[0159] Example 4

[0160] The rest is the same as Example 2, the only difference is that the final heating temperatures of the positive and negative electrode sheets are 180° C. and 200° C. respectively, and the corresponding laser continuous heating powers are 1800W and 1300W respectively.

[0161] Comparative Example 1

[0162] The difference from Example 1 is that the positive and negative electrode plates are not laser processed, that is, steps 2) and 4) of Example 1 are not performed.

[0163] Comparative Example 2

[0164] The difference from Example 2 is that the positive and negative electrode plates are not laser processed, that is, steps 2) and 4) of Example 2 are not performed.

[0165] Comparative Example 3

[0166] The difference from Example 1 is that the heating temperature of the positive electrode plate is greater than the decomposition temperature of the active material therein, and the surface laser treatment of the negative electrode plate is not performed. Specifically, step 2) in Example 1 is replaced by the following steps:

[0167] The laser was adjusted to 10 side-by-side rectangular spots acting perpendicularly on the surface of the positive electrode plate. The width of these 10 side-by-side rectangular spots was 10 mm perpendicular to the direction of movement of the positive electrode plate, and the length was 15 mm parallel to the direction of movement of the positive electrode plate. The laser was 5 cm away from the plate, the laser instantaneous pulse power was 8000 W, the laser pulse time was 0.005 s, the pulse time interval was 0.008 s, the movement speed of the positive electrode plate was 35 m / min, the heating time was 0.025 s, and the instantaneous temperature of the surface of the positive electrode plate after laser irradiation and heating was 600 ° C, resulting in etching and forming holes on the surface of the positive electrode plate.

[0168] Other implementation conditions and methods are consistent with those in Example 1.

[0169] Comparative Example 4

[0170] The difference from Example 2 is that the heating temperature of the negative electrode plate is greater than the decomposition temperature of the active material therein, and the surface laser treatment of the positive electrode plate is not performed. Specifically, step 4) in Example 2 is replaced by the following steps:

[0171] The laser was adjusted to 8 parallel rectangular spots acting perpendicularly on the surface of the negative electrode. The width of the 8 parallel rectangular spots was 25 mm perpendicular to the direction of movement of the negative electrode, and the length was 30 mm parallel to the direction of movement of the negative electrode. The laser was 6 cm away from the electrode, the movement speed of the negative electrode was 30 m / min, the instantaneous pulse power of the laser was 7500 W, the laser pulse time was 0.005 s, the pulse time interval was 0.005 s, the total heating time was 0.030 s, and the instantaneous temperature of the surface of the negative electrode after laser irradiation and heating was 550 ° C, resulting in etching and forming holes on the surface of the negative electrode.

[0172] Other implementation conditions and methods are consistent with those of Example 2.

[0173] The surface treatment conditions of the pole pieces of each embodiment and comparative example are shown in Tables 1 and 2 below.

[0174] Table 1. Surface treatment conditions of the electrode in Example 1, Example 3, Comparative Example 1 and Comparative Example 3

[0175]

[0176]

[0177] Table 2. Surface treatment conditions of the electrode in Example 2, Example 4, Comparative Example 2 and Comparative Example 4

[0178]

[0179]

[0180] The performance tests were performed on the positive electrode sheets and negative electrode sheets after treatment in the embodiments and comparative examples, and the results are shown in Tables 3 and 4 below.

[0181] Table 3. Test results of electrode performance in Example 1, Example 3, Comparative Example 1, and Comparative Example 3

[0182]

[0183]

[0184] Table 4. Test results of electrode performance in Example 2, Example 4, Comparative Example 2, and Comparative Example 4

[0185]

[0186]

[0187] The data in Tables 3 and 4 are processed to obtain the electrode performance change rates of Example 1, Example 3, and Comparative Example 3 compared with Comparative Example 1, as well as the electrode performance change rates of Example 2, Example 4, and Comparative Example 4 compared with Comparative Example 2. The results are shown in Tables 5 and 6 below.

[0188] Table 5. Change rate of pole piece performance of Example 1, Example 3, and Comparative Example 3 compared with Comparative Example 1

[0189]

[0190]

[0191] Table 6. Change rate of pole piece performance of Example 2, Example 4, and Comparative Example 4 compared with Comparative Example 2

[0192]

[0193] From the test results of Examples 1 to 4 and Comparative Examples 1 to 2 in Tables 3 to 6 above, it can be seen that after the heat treatment, the resistance of the electrode sheet decreases significantly, among which the decrease of the negative electrode sheet is higher than that of the positive electrode sheet; the adhesion and cohesion of the electrode sheet are slightly improved; the absorption rate of the electrode sheet to the electrolyte is greatly improved, and the porosity of the electrode sheet is slightly improved; and after the heat treatment, the gram capacity of the electrode sheet does not decrease. In addition, after the heat treatment, no significant change in the thickness of the electrode sheets of Examples 1 to 4 was found. The results show that appropriate heating treatment of the electrode sheet can effectively improve the performance of the electrode sheet, with little side effects, and will not cause significant capacity loss and potential risk of lithium dendrites.

[0194] At the same time, it can be seen from the test results of Comparative Examples 3 to 4 that after the heating treatment, if the temperature of the electrode is too high and etching occurs, not only will the adhesion and cohesion of the electrode fail to be effectively improved, but the gram capacity of the electrode will also drop significantly, indicating that the heating temperature has a great influence on the electrochemical properties of the electrode, and inappropriate heating temperature will bring side effects to the electrode.

[0195] The positive and negative electrode sheets of the above embodiments and comparative examples were cut into pieces, and the electrode sheets were combined with a polyethylene / polypropylene / polyethylene three-layer separator and 1 mol·L containing vinylene carbonate (VC), tris(trimethylsilyl) phosphate (TMSP), ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). -1 Lithium hexafluorophosphate (LiPF6) electrolyte solution is assembled into a lithium-ion battery with a positive and negative electrode pair, and the corresponding performance is shown in the table below.

[0196] Table 7. Lithium-ion battery performance test results

[0197]

[0198] The data in Table 7 were processed to obtain the performance change rates of the lithium ion batteries of Example 1, Example 3, and Comparative Example 3 compared with Comparative Example 1, and the performance change rates of the lithium ion batteries of Example 2, Example 4, and Comparative Example 4 compared with Comparative Example 2. The results are shown in the following table.

[0199] Table 8. Lithium-ion battery performance change rate

[0200]

[0201]

[0202] In Table 7, “4C discharge rate retention rate” indicates the retention rate of the discharge capacity of the lithium-ion battery at 4C rate compared to the discharge capacity at 1C rate;

[0203] "SOC" is the state of charge, which is used to reflect the remaining capacity of the battery. Its numerical value is defined as the ratio of the remaining capacity to the battery capacity;

[0204] The "K value" represents the voltage drop of the battery per unit time.

[0205] It can be seen from the above table that the lithium-ion positive and negative electrode plates treated by the methods of Examples 1 to 4, after being assembled into lithium-ion batteries, are compared with the untreated group (Comparative Examples 1 to 2), and compared with Comparative Examples 3 to 4 in which the electrode plates are etched due to excessively high electrode plate temperatures after heating treatment. Under the same system, their rate performance, K value, and DC impedance are all improved, indicating that the electrode plate treatment methods of Examples 1 to 4 reduce the electrode plate resistance and improve the infiltration rate of the electrolyte, thereby significantly improving the kinetic performance of the lithium-ion battery while ensuring good bonding strength. At the same time, the treatment method is simple, less time-consuming and energy-consuming, and can be used in large-scale production.

[0206] Appendix: The relevant performance test methods in Table 3 and Table 4 above are as follows:

[0207] (1) Electrode resistance

[0208] Use Yuanneng Technology's diaphragm resistor to test the diaphragm resistance. Cut small discs with a diameter of 10 mm on the left, middle, and right of the electrode. Turn on the indicator light of the Yuanneng Technology electrode resistor, place the small disc in the appropriate position of the "probe" of the electrode resistor, click the "Start" button, and wait for the reading to stabilize before reading. Each small disc tests two positions, and finally calculates the average value of the six measurements, which is the electrode resistance of the electrode.

[0209] (2) Adhesion test

[0210] Cut the pole piece into 20*100mm 2The test specimens of different sizes are kept for later use; the double-sided tape is used to adhere the side of the specimen to be tested, and it is compacted with a roller to make the double-sided tape fit the specimen completely; the other side of the double-sided tape of the specimen is adhered to the stainless steel surface, and one end of the specimen is bent in the opposite direction with a bending angle of 180°; the high-speed rail tensile testing machine is used for testing, one end of the stainless steel is fixed to the clamp below the tensile testing machine, the bent end of the specimen is fixed to the clamp above, the angle of the specimen is adjusted to ensure that the upper and lower ends are in a vertical position, and then the specimen is stretched at a speed of 50 mm / min until the specimen is completely peeled off from the substrate, and the displacement and force in the process are recorded. It is generally believed that the force when the force is balanced is the bonding force of the electrode.

[0211] (3) Electrode electrolyte absorption rate

[0212] Fix the electrode on a clean glass plate, use a capillary with an inner diameter of 0.3mm to absorb the electrolyte at a height of 3mm, and then make vertical contact with the electrode to allow the electrode to absorb the electrolyte. Measure the time it takes to absorb the electrolyte and obtain the electrolyte absorption rate by conversion.

[0213] (4) Pole cohesion test

[0214] Cut the pole piece into 20*100mm 2 The test specimens of different sizes are kept aside for later use; the specimens are attached to the surface of stainless steel with double-sided tape, and the single-sided tape is attached to the surface of the specimen, with the excess part being bent at an angle of 180°; the high-speed rail tensile testing machine is used for testing, one end of the stainless steel is fixed to the lower fixture of the tensile testing machine, the bent end of the specimen is fixed to the upper fixture, the angle of the specimen is adjusted to ensure that the upper and lower ends are in a vertical position, and then the specimen is stretched at a speed of 50 mm / min until the tape is completely peeled off from the specimen, and the displacement and force in the process are recorded. It is generally believed that the force when the force is balanced is the cohesive force of the electrode.

[0215] (5) Pole piece porosity test

[0216] Cut the pole piece into 20 pieces of 14mm diameter circular double-sided pole pieces, record the pole piece weight and thickness, and calculate the volume density. Put the circular double-sided pole piece into the sample cup of the true density porosity tester, use helium replacement, and combine Archimedes' law and Bohr's law to obtain the true volume of the pole piece, and then calculate the true density. Porosity is equal to (1-volume density / true density)*100%.

[0217] (6) Electrode gram capacity test

[0218] Wash one side of the positive or negative electrode with N-methylpyrrolidone or deionized water, punch it into a single-sided circular electrode with a diameter of 14 mm and weigh it; at the same time, weigh the weight of the corresponding current collector substrate under the 14 mm diameter circular sheet (circular current collector). The active layer loading is obtained based on the weight of the circular electrode and the corresponding circular current collector. The mass of the active material is calculated according to the formula. The 2032 button battery is equipped with a negative electrode shell, nickel foam, a 16 mm diameter lithium sheet, an 18 mm diameter Celgard2325 isolation membrane, and 0.1 g 1 mol·L -1 LiPF6 EC:DMC:EMC (mass ratio 1:1:1) electrolyte, 14mm diameter single-sided circular pole piece (active material side facing the separator), 2032 button cell matching positive electrode shell assembled into 2032 button cell. The assembled button cell was tested after standing for 12 hours. For button cells with negative pole pieces, the battery was discharged at a current of 0.05C to the lower limit of the material voltage, and then charged at a current of 0.1C to the upper limit of the material voltage, and the charging capacity was recorded; the charging capacity was divided by the mass of the active material to obtain the gram capacity of the negative pole piece; for button cells with positive pole pieces, the battery was charged at a current of 0.1C to the upper limit of the material voltage, and then discharged at a current of 0.1C to the upper limit of the material voltage, and the discharge capacity was recorded; the discharge capacity was divided by the mass of the active material to obtain the gram capacity of the positive pole piece.

[0219] (7) Determination of K value

[0220] The cell was charged to 20% capacity, and then the cell voltage OCV1 was recorded. Then, the cell was placed at 25°C for 48 hours, and the cell voltage OCV2 was measured again. The K value is (OCV1-OCV2) / 48, and the unit is mV / h.

[0221] (8) Discharge rate test

[0222] Proceed as follows:

[0223] After the battery cell has been stationary for 30 minutes at 25°C, it is discharged at a constant current of 0.33C to 2.5V (Example 2, Example 4 and Comparative Example 2 are discharged at a constant current to 2.8V); after standing at 25°C for 1 hour, it is charged at a constant current of 0.33C to 3.65V (Example 2, Example 4 and Comparative Example 2 are charged at a constant current to 4.25V); and constant voltage charging is performed at 3.65V (or 4.25V) until the cut-off current is 0.05C.

[0224] Repeat the above steps once, let it stand for 30 minutes at 25°C, and then discharge it at 1C to 2.5V (Example 2, Example 4 and Comparative Example 2 discharge to 2.8V). After standing at 25°C for 1 hour, charge it at 0.33C constant current to 3.65V (Example 2, Example 4 and Comparative Example 2 charge it at 4.25V); charge it at 3.65V (or 4.25V) constant voltage to a cutoff current of 0.05C. After standing at 25°C for 30 minutes, discharge it at 4C to 2.5V (Example 2, Example 4 and Comparative Example 2 discharge it to 2.8V). Finally, let it stand for 30 minutes at 25°C.

[0225] The discharge capacity during the test was recorded, and the 4C discharge rate retention rate was calculated based on the discharge capacity at 4C and 1C.

[0226] (9) DC impedance test

[0227] Proceed as follows:

[0228] After the battery cell was left standing at 25°C for 30 minutes, it was charged to 3.65V at 0.33C constant current (4.25V in Example 2, Example 4 and Comparative Example 2); then it was charged to a cut-off current of 0.05C at a constant voltage, at which time the battery's state of charge (SOC) was 100%. After standing at 25°C for 5 minutes, it was discharged at 0.33C constant current, with a cut-off current of 0.5C, and the SOC was adjusted to 50%. After standing at 25°C for 1 hour, the voltage V1 was recorded. After discharging at 5C constant current for 30 seconds, the voltage V2 and the current I of the 5C constant current discharge were recorded.

[0229] Let stand for 40 seconds at 25°C, and charge at a constant current of 3.75C for 30 seconds. After standing for 1 hour at 25°C, charge at a constant current of 0.33C to 3.65V (Example 2, Example 4 and Comparative Example 2 are charged to 4.25V at a constant current); charge at a constant voltage of 3.65V (or 4.25V), with a cut-off current of 0.05C. Let stand for 5 minutes at 25°C, and record the voltage V1'. Then discharge at 0.33C, with a cut-off current of 0.9C, and adjust the SOC to 50%. After standing for 1 hour at 25°C, discharge at 5C for 30 seconds, and record the voltage V2' and the current I' of the 5C constant current discharge.

[0230] Let stand for 40 seconds at 25℃, and charge at 3.75C constant current for 30 seconds. After standing for 5 minutes at 25℃, the above steps can be repeated multiple times.

[0231] The DC impedance of the battery cell at 25°C, 50% SOC, and 5C constant current discharge for 30s = (V2-V1) / I = (V2'-V1') / I'.

[0232] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A method for processing a pole piece, wherein the pole piece comprises an active layer, wherein the active layer comprises an active material and a binder, wherein: The treatment method includes: heating the pole piece to raise the temperature of the active layer to a treatment temperature; the treatment temperature is greater than or equal to the softening temperature or melting temperature of the binder, and the treatment temperature is less than the lowest temperature among the decomposition temperature, oxidation temperature, and ignition temperature of the active material.

2. The method for processing a pole piece according to claim 1, characterized in that: The electrode sheet is a positive electrode sheet, and the processing temperature is less than or equal to the decomposition temperature of the binder.

3. The method for processing a pole piece according to claim 1 or 2, characterized in that: The treatment temperature is 160-400°C, optionally 180-370°C.

4. The method for processing a pole piece according to any one of claims 1 to 3, characterized in that: The pole piece is a positive pole piece, and the processing temperature is 160-260°C or 280-400°C.

5. The method for processing a pole piece according to claim 1 or 3, characterized in that: The pole piece is a negative pole piece, and the processing temperature is 180-350°C, and optionally 200-350°C.

6. The method for processing a pole piece according to any one of claims 1 to 5, characterized in that: The heating time is 0.02 to 0.3 s, and optionally 0.02 to 0.2 s.

7. The method for processing a pole piece according to any one of claims 1 to 6, characterized in that: The heating treatment includes laser irradiation treatment.

8. The method for processing a pole piece according to claim 7, characterized in that: The surface of the pole piece includes a first surface and a second surface arranged opposite to each other; the laser irradiation treatment step includes: using a first laser beam to perform laser irradiation treatment on the first surface, and using a second laser beam to perform laser irradiation treatment on the second surface; there is a spacing between the first laser beam and the second laser beam in a direction parallel to the first surface and the second surface.

9. The method for processing a pole piece according to claim 7 or 8, characterized in that: In the laser irradiation processing step, the maximum size of the laser spot falling on the surface of the pole piece is greater than or equal to the minimum size of the surface of the pole piece.

10. The method for processing a pole piece according to any one of claims 7 to 9, characterized in that: The laser irradiation treatment step includes: moving the pole piece relative to the laser spot falling on the surface of the pole piece, and the speed of the moving treatment is 10 to 200 m / min, and optionally 30 to 200 m / min.

11. The method for processing a pole piece according to any one of claims 7 to 10, characterized in that: The power of the laser irradiation treatment is 100-8000W, and optionally 1000-7000W.

12. The method for processing a pole piece according to any one of claims 1 to 11, characterized in that: Before the heating step, a step of drying the electrode sheet is included.

13. The method for processing a pole piece according to any one of claims 1 to 12, characterized in that: Before the heating treatment step, a step of forming the pole piece is included. Optionally, the forming treatment includes one or both of cold pressing treatment and hot pressing treatment.

14. The method for processing a pole piece according to any one of claims 1 to 13, characterized in that: Before the heating step, a step of cutting the pole piece is included.

15. A pole piece, characterized in that: The pole piece is obtained by processing according to any one of claims 1 to 14.

16. A battery, characterized in that: The battery comprises the electrode piece as claimed in claim 15.

17. An electrical device, characterized in that: The electrical device comprises the battery as claimed in claim 16.

Citation Information

Patent Citations

  • Electrode and preparation method thereof, electrochemical device and electronic device

    CN115398667A

  • Negative pole piece, preparation method thereof and battery

    CN116130602A

  • Electrode plate for nonaqueous electrolytic solution secondary battery, and its manufacturing method as well as nonaqueous electrolytic solution secondary battery

    JP2007265889A